Low-VOC (volatile organic compound) fragrant long glass fiber reinforced polypropylene material and preparation method thereof

By adding low VOC polypropylene resin, compatibilizer, glass fiber and fragrance-type silicone masterbatch to long glass fiber reinforced polypropylene materials, combined with the twin screw extrusion mechanism, the odor control of long glass fiber reinforced polypropylene materials is solved. The problem has achieved the combination of low VOC and fragrance, improving the comfort and market application prospects of the car interior.

CN119081282APending Publication Date: 2024-12-06QINGDAO GON TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411200746.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Long glass fiber reinforced polypropylene material produces irritating odors in a high-temperature and closed environment of automobiles, affecting health, and the existing technology is difficult to effectively control odors, especially when adding fragrance agents to the production process, small odor molecules will be extracted, the effect is Not good.

Method used

Using low-VOC fragrance long glass fiber reinforced polypropylene material, including low-VOC polypropylene resin, low-VOC compatibility agent, low-VOC glass fiber and fragrance silicone masterbatch, it is prepared through the twin-screw extrusion mechanism to control odor output The ratio of added fragrance masterbatches to meet the needs of low odor and good comfort.

Benefits of technology

Effectively reduce the VOC content of the material, and continuously release the fragrance by adding fragrance-type silicone masterbatches, improve the comfort of the car interior, and have the characteristics of simplicity and efficiency. It can flexibly adjust the fragrance intensity according to customer needs, and has a good market Application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a low-VOC (volatile organic compound) fragrant long glass fiber reinforced polypropylene material and a preparation method thereof. The material comprises the following components in parts by weight: 50-80 parts of low-VOC polypropylene resin; 5-10 parts by weight of a low VOC compatilizer; 10-40 parts by weight of a low VOC glass fiber; 0.5 to 1.5 parts by weight of an auxiliary agent; and 0-10 parts by weight of fragrant silicone master batch. According to the preparation method of the material, the VOC content of the material can be effectively reduced, meanwhile, by adding a proper amount of fragrant silicone master batch, the material can continuously release fragrance in the using process, and the comfort level of automotive trim is improved. In addition, the method also has the advantages of simplicity, convenience and high efficiency, can flexibly adjust the fragrance intensity according to customer requirements, and has a good market application prospect. The low-VOC fragrance type long glass fiber reinforced polypropylene composite material is high in performance, can provide different fragrances according to requirements of customers, has a certain price advantage, and is beneficial to production management and cost control of the customers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer material modification, and specifically relates to a low-VOC fragrant long glass fiber reinforced polypropylene material and a preparation method thereof. Background Art

[0002] Long glass fiber reinforced polypropylene (LGFPP) is a composite material formed by adding glass fibers with a length of 10 to 25 mm to polypropylene. Due to its three-dimensional spatial cross-distribution of long glass fibers, long glass fiber reinforced polypropylene has significantly higher tensile strength, impact strength and hardness than ordinary polypropylene. It has excellent dimensional stability and creep resistance. It also has good fatigue resistance and weather resistance, and can maintain stable mechanical properties at extreme temperatures. Compared with metal materials, long glass fiber reinforced polypropylene has higher specific strength and specific stiffness, which makes it an ideal choice for replacing metals, especially in the field of automotive manufacturing.

[0003] However, due to the strong odor of the raw materials themselves and the strong shearing effect of the screw during the modification process, the modified glass fiber reinforced polypropylene material produced will produce a strong irritating odor in the high temperature and closed environment of the car, affecting people's health. Therefore, low-odor or fragrant long glass fiber reinforced polypropylene reinforced materials came into being. For example, application number / patent number: CN2020103842011, a low-odor and low-VOC long glass fiber reinforced polypropylene composite material and its preparation method are proposed; application number / patent number: CN2018116284641, a low-VOC long-lasting fragrant glass fiber reinforced polypropylene material and its preparation method are proposed.

[0004] In addition to PP and additives, the source of odor in ordinary glass fiber reinforced polypropylene materials is mainly glass fiber. The small odor molecules produced by screw shearing will be partially removed by vacuum, thereby reducing the VOC content. However, due to its special production process (LFT) and appearance, the glass fiber is directly pulled out from the die head without passing through the screw, and its odor control is much more difficult than that of ordinary glass fiber reinforced polypropylene materials. At present, there are few patents in the field of scented LGFPP, and most of them are to prepare low-VOC LGFPP by controlling odor output or adding fragrances during the production process. The latter method will not only remove the small odor molecules during the vacuum process, but also remove the small fragrance molecules released during the screw shearing process, resulting in poor results. Summary of the invention

[0005] The purpose of the present invention is to provide a low-VOC fragrance-type long glass fiber reinforced polypropylene material and a preparation method thereof, to control the output of odor and the addition ratio of fragrance masterbatch, so as to meet the demand for low odor and good comfort of automotive interior materials, and to solve the problems raised in the above-mentioned background technology.

[0006] To achieve the above objectives, the present invention provides a low-VOC scented long glass fiber reinforced polypropylene material on one hand, which comprises: 50-80 parts by weight of low-VOC polypropylene resin; 5-10 parts by weight of low-VOC compatibilizer; 10-40 parts by weight of low-VOC glass fiber; 0.5-1.5 parts by weight of additive; and 0-10 parts by weight of scented silicone masterbatch.

[0007] Preferably, the scented silicone masterbatch comprises: 30-60 parts by weight of low VOC polypropylene resin; 30-60 parts by weight of silicone; and 0.1-10 parts by weight of scented liquid.

[0008] Preferably, the material comprises: 65 parts by weight of low-VOC polypropylene resin; 5 parts by weight of low-VOC compatibilizer; 30 parts by weight of low-VOC glass fiber; 1 part by weight of auxiliary agent; and 0 parts by weight of scented silicone masterbatch.

[0009] Preferably, the material comprises: 65 parts by weight of low-VOC polypropylene resin; 5 parts by weight of low-VOC compatibilizer; 30 parts by weight of low-VOC glass fiber; 1 part by weight of auxiliary agent; and 1 part by weight of scented silicone masterbatch.

[0010] Preferably, the material comprises: 65 parts by weight of low-VOC polypropylene resin; 5 parts by weight of low-VOC compatibilizer; 30 parts by weight of low-VOC glass fiber; 1 part by weight of auxiliary agent; and 2 parts by weight of scented silicone masterbatch.

[0011] Preferably, the material comprises: 65 parts by weight of low-VOC polypropylene resin; 5 parts by weight of low-VOC compatibilizer; 30 parts by weight of low-VOC glass fiber; 1 part by weight of auxiliary agent; and 5 parts by weight of scented silicone masterbatch.

[0012] Preferably, the material comprises: 65 parts by weight of low-VOC polypropylene resin; 5 parts by weight of low-VOC compatibilizer; 30 parts by weight of low-VOC glass fiber; 1 part by weight of auxiliary agent; and 10 parts by weight of scented silicone masterbatch.

[0013] Another aspect of the present invention provides a method for preparing a low-VOC fragrant long glass fiber reinforced polypropylene material, comprising the following steps:

[0014] Prepare masterbatch A by mixing low VOC polypropylene resin, low VOC compatibilizer and additives;

[0015] The mixed materials are added into a twin-screw extruder for melt extrusion to form a low-VOC long glass fiber reinforced polypropylene material;

[0016] Prepare B masterbatch by mixing low VOC polypropylene resin, silicone and fragrance liquid;

[0017] The mixed materials are added into a twin-screw extruder for melt extrusion to form a scented silicone masterbatch;

[0018] During the injection molding process, different proportions of scented silicone masterbatch are added to the low VOC long glass fiber reinforced polypropylene material according to the required fragrance level.

[0019] Preferably, during the preparation of the masterbatch A, the temperatures of the zones of the twin-screw extruder are 180-220°C for the first stage, 220-250°C for the second stage, 230-250°C for the third stage, and 220-250°C for the die head.

[0020] Preferably, during the preparation of the B masterbatch, the temperatures of the zones of the twin-screw extruder are 180-210°C in the first zone, 210-230°C in the second zone, 210-220°C in the third zone, and 210-230°C in the die head.

[0021] Technical effects and advantages of the present invention: The low-VOC fragrance-type long glass fiber reinforced polypropylene material and the preparation method thereof proposed by the present invention have the following advantages compared with the prior art:

[0022] The material of the present invention comprises the following components: 50-80 parts by weight of low-VOC polypropylene resin; 5-10 parts by weight of low-VOC compatibilizer; 10-40 parts by weight of low-VOC glass fiber; 0.5-1.5 parts by weight of auxiliary agent; 0-10 parts by weight of scented silicone masterbatch. The preparation method of this material can effectively reduce the VOC content of the material, and by adding an appropriate amount of scented silicone masterbatch, the material can continuously release fragrance during use, thereby improving the comfort of the car interior. In addition, this method also has the advantages of being simple and efficient, and can flexibly adjust the intensity of the fragrance according to customer needs, and has good market application prospects. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0024] The invention provides a low-VOC fragrant long glass fiber reinforced polypropylene material. The material comprises: 50-80 parts by weight of low-VOC polypropylene resin (PP); 5-10 parts by weight of low-VOC compatibilizer (PP-g); 10-40 parts by weight of low-VOC glass fiber; 0.5-1.5 parts by weight of auxiliary agent; and 0-10 parts by weight of fragrant silicone masterbatch.

[0025] The scented silicone masterbatch comprises: 30-60 parts by weight of low VOC polypropylene resin; 30-60 parts by weight of silicone; and 0.1-10 parts by weight of scented liquid.

[0026] The material proposed by the present invention can effectively reduce the VOC content of the material. At the same time, by adding an appropriate amount of scented silicone masterbatch, the material can continuously release fragrance during use, thereby improving the comfort of the car interior. In addition, this method also has the advantages of being simple and efficient, and the intensity of the fragrance can be flexibly adjusted according to customer needs, and has good market application prospects.

[0027] Example 1

[0028] In this embodiment, a low-VOC scented long glass fiber reinforced polypropylene material is provided, which comprises: 65 parts by weight of low-VOC polypropylene resin; 5 parts by weight of low-VOC compatibilizer; 30 parts by weight of low-VOC glass fiber; 1 part by weight of auxiliary agent; and 0 parts by weight of scented silicone masterbatch.

[0029] Another aspect of the present invention provides a method for preparing a low-VOC fragrant long glass fiber reinforced polypropylene material, comprising the following steps:

[0030] Prepare masterbatch A by mixing low VOC polypropylene resin, low VOC compatibilizer and additives;

[0031] The mixed materials are added into a twin-screw extruder for melt extrusion to form a low-VOC long glass fiber reinforced polypropylene material;

[0032] Prepare B masterbatch by mixing low VOC polypropylene resin, silicone and fragrance liquid;

[0033] The mixed materials are added into a twin-screw extruder for melt extrusion to form a scented silicone masterbatch;

[0034] During the injection molding process, different proportions of scented silicone masterbatch are added to the low VOC long glass fiber reinforced polypropylene material according to the required fragrance level.

[0035] Preferably, during the preparation of the masterbatch A, the temperatures of the zones of the twin-screw extruder are 180°C for the first stage, 220°C for the second stage, 230°C for the third stage, and 220°C for the die head.

[0036] Preferably, during the preparation of the B masterbatch, the temperatures of the zones of the twin-screw extruder are 180° C. in the first zone, 210° C. in the second zone, 210° C. in the third zone, and 210° C. in the die head.

[0037] Example 2

[0038] In this embodiment, a low-VOC scented long glass fiber reinforced polypropylene material is provided, which comprises: 65 parts by weight of low-VOC polypropylene resin; 5 parts by weight of low-VOC compatibilizer; 30 parts by weight of low-VOC glass fiber; 1 part by weight of auxiliary agent; and 1 part by weight of scented silicone masterbatch.

[0039] Another aspect of the present invention provides a method for preparing a low-VOC fragrant long glass fiber reinforced polypropylene material, comprising the following steps:

[0040] Prepare masterbatch A by mixing low VOC polypropylene resin, low VOC compatibilizer and additives;

[0041] The mixed materials are added into a twin-screw extruder for melt extrusion to form a low-VOC long glass fiber reinforced polypropylene material;

[0042] Prepare B masterbatch by mixing low VOC polypropylene resin, silicone and fragrance liquid;

[0043] The mixed materials are added into a twin-screw extruder for melt extrusion to form a scented silicone masterbatch;

[0044] During the injection molding process, different proportions of scented silicone masterbatch are added to the low VOC long glass fiber reinforced polypropylene material according to the required fragrance level.

[0045] Preferably, during the preparation of the masterbatch A, the temperatures of the zones of the twin-screw extruder are 200°C for the first stage, 240°C for the second stage, 240°C for the third stage, and 240°C for the die head.

[0046] Preferably, during the preparation of the B masterbatch, the temperatures of the zones of the twin-screw extruder are 200° C. in the first zone, 220° C. in the second zone, 215° C. in the third zone, and 220° C. in the die head.

[0047] Example 3

[0048] In this embodiment, a low-VOC scented long glass fiber reinforced polypropylene material is provided, which comprises: 65 parts by weight of low-VOC polypropylene resin; 5 parts by weight of low-VOC compatibilizer; 30 parts by weight of low-VOC glass fiber; 1 part by weight of auxiliary agent; and 2 parts by weight of scented silicone masterbatch.

[0049] Another aspect of the present invention provides a method for preparing a low-VOC fragrant long glass fiber reinforced polypropylene material, comprising the following steps:

[0050] Prepare masterbatch A by mixing low VOC polypropylene resin, low VOC compatibilizer and additives;

[0051] The mixed materials are added into a twin-screw extruder for melt extrusion to form a low-VOC long glass fiber reinforced polypropylene material;

[0052] Prepare B masterbatch by mixing low VOC polypropylene resin, silicone and fragrance liquid;

[0053] The mixed materials are added into a twin-screw extruder for melt extrusion to form a scented silicone masterbatch;

[0054] During the injection molding process, different proportions of scented silicone masterbatch are added to the low VOC long glass fiber reinforced polypropylene material according to the required fragrance level.

[0055] Preferably, during the preparation of the masterbatch A, the temperatures of the zones of the twin-screw extruder are 220°C for the first stage, 250°C for the second stage, 250°C for the third stage, and 250°C for the die head.

[0056] Preferably, during the preparation of the B masterbatch, the temperatures of the zones of the twin-screw extruder are 210° C. in the first zone, 230° C. in the second zone, 220° C. in the third zone, and 230° C. in the die head.

[0057] Example 4

[0058] In this embodiment, a low-VOC scented long glass fiber reinforced polypropylene material is provided, which comprises: 65 parts by weight of low-VOC polypropylene resin; 5 parts by weight of low-VOC compatibilizer; 30 parts by weight of low-VOC glass fiber; 1 part by weight of auxiliary agent; and 5 parts by weight of scented silicone masterbatch.

[0059] Another aspect of the present invention provides a method for preparing a low-VOC fragrant long glass fiber reinforced polypropylene material, comprising the following steps:

[0060] Prepare masterbatch A by mixing low VOC polypropylene resin, low VOC compatibilizer and additives;

[0061] The mixed materials are added into a twin-screw extruder for melt extrusion to form a low-VOC long glass fiber reinforced polypropylene material;

[0062] Prepare B masterbatch by mixing low VOC polypropylene resin, silicone and fragrance liquid;

[0063] The mixed materials are added into a twin-screw extruder for melt extrusion to form a scented silicone masterbatch;

[0064] During the injection molding process, different proportions of scented silicone masterbatch are added to the low VOC long glass fiber reinforced polypropylene material according to the required fragrance level.

[0065] Preferably, during the preparation of the masterbatch A, the temperatures of the zones of the twin-screw extruder are 180°C for the first stage, 250°C for the second stage, 230°C for the third stage, and 250°C for the die head.

[0066] Preferably, during the preparation of the B masterbatch, the temperatures of the zones of the twin-screw extruder are 210° C. for the first zone, 210° C. for the second zone, 210° C. for the third zone, and 210° C. for the die head.

[0067] Example 5

[0068] In this embodiment, a low-VOC scented long glass fiber reinforced polypropylene material is provided, which comprises: 65 parts by weight of low-VOC polypropylene resin; 5 parts by weight of low-VOC compatibilizer; 30 parts by weight of low-VOC glass fiber; 1 part by weight of auxiliary agent; and 10 parts by weight of scented silicone masterbatch.

[0069] Another aspect of the present invention provides a method for preparing a low-VOC fragrant long glass fiber reinforced polypropylene material, comprising the following steps:

[0070] Prepare masterbatch A by mixing low VOC polypropylene resin, low VOC compatibilizer and additives;

[0071] The mixed materials are added into a twin-screw extruder for melt extrusion to form a low-VOC long glass fiber reinforced polypropylene material;

[0072] Prepare B masterbatch by mixing low VOC polypropylene resin, silicone and fragrance liquid;

[0073] The mixed materials are added into a twin-screw extruder for melt extrusion to form a scented silicone masterbatch;

[0074] During the injection molding process, different proportions of scented silicone masterbatch are added to the low VOC long glass fiber reinforced polypropylene material according to the required fragrance level.

[0075] Preferably, during the preparation of the masterbatch A, the temperatures of the zones of the twin-screw extruder are 220°C for the first zone, 240°C for the second zone, 240°C for the third zone, and 240°C for the die.

[0076] Preferably, during the preparation of the B masterbatch, the temperatures of the zones of the twin-screw extruder are 210° C. in the first zone, 220° C. in the second zone, 220° C. in the third zone, and 210° C. in the die head.

[0077] As shown in Table 1:

[0078]

[0079] As shown in the table above, as the amount of scented masterbatch increases, the odor level gradually increases. The odor output and the addition ratio of scented masterbatch can be controlled during the production process, further promoting the development of lightweight technology, which provides more market opportunities for LGFPP, and its odor improvement problem is a top priority. This low-VOC scented long glass fiber reinforced polypropylene material composite material has high performance and low odor. It can provide different fragrances according to customer needs. It is simple and efficient, has certain price advantages, and is conducive to customer production management and cost control.

[0080] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A low VOC fragrance-type long glass fiber reinforced polypropylene material, characterized in that: The materials include: 50-80 parts by weight of low VOC polypropylene resin; 5-10 parts by weight of low VOC compatibilizer; 10-40 parts by weight of low VOC glass fiber; 0.5-1.5 parts by weight of auxiliary agent; Scented silicone masterbatch 0-10 parts by weight.

2. The low VOC fragrance-type long glass fiber reinforced polypropylene material according to claim 1, characterized in that: The scented silicone masterbatch comprises: 30-60 parts by weight of low VOC polypropylene resin; Silicone 30-60 parts by weight; Aroma liquid 0.1-10 parts by weight.

3. The low VOC fragrance-type long glass fiber reinforced polypropylene material according to claim 1, characterized in that: The materials include: 65 parts by weight of low VOC polypropylene resin; 5 parts by weight of low VOC compatibilizer; 30 parts by weight of low VOC glass fiber; 1 part by weight of auxiliary agent; Scented silicone masterbatch 0 parts by weight.

4. The low VOC fragrance-type long glass fiber reinforced polypropylene material according to claim 1, characterized in that: The materials include: 65 parts by weight of low VOC polypropylene resin; 5 parts by weight of low VOC compatibilizer; 30 parts by weight of low VOC glass fiber; 1 part by weight of auxiliary agent; 1 part by weight of scented silicone masterbatch.

5. The low VOC fragrance-type long glass fiber reinforced polypropylene material according to claim 1, characterized in that: The materials include: 65 parts by weight of low VOC polypropylene resin; 5 parts by weight of low VOC compatibilizer; 30 parts by weight of low VOC glass fiber; 1 part by weight of auxiliary agent; 2 parts by weight of scented silicone masterbatch.

6. The low VOC fragrance-type long glass fiber reinforced polypropylene material according to claim 1, characterized in that: The materials include: 65 parts by weight of low VOC polypropylene resin; 5 parts by weight of low VOC compatibilizer; 30 parts by weight of low VOC glass fiber; 1 part by weight of auxiliary agent; 5 parts by weight of scented silicone masterbatch 7. The low VOC fragrance-type long glass fiber reinforced polypropylene material according to claim 1, characterized in that: The materials include: 65 parts by weight of low VOC polypropylene resin; 5 parts by weight of low VOC compatibilizer; 30 parts by weight of low VOC glass fiber; 1 part by weight of auxiliary agent; 10 parts by weight of scented silicone masterbatch.

8. A method for preparing a low-VOC aroma-type long glass fiber reinforced polypropylene material according to any one of claims 1 to 7, characterized in that: The following steps are involved: Prepare masterbatch A by mixing low VOC polypropylene resin, low VOC compatibilizer and additives; The mixed materials are added into a twin-screw extruder for melt extrusion to form a low-VOC long glass fiber reinforced polypropylene material; Prepare B masterbatch by mixing low VOC polypropylene resin, silicone and fragrance liquid; The mixed materials are added into a twin-screw extruder for melt extrusion to form a scented silicone masterbatch; During the injection molding process, different proportions of scented silicone masterbatch are added to the low VOC long glass fiber reinforced polypropylene material according to the required fragrance level.

9. The preparation method according to claim 8, characterized in that: During the preparation of the A masterbatch, the temperatures of the various zones of the twin-screw extruder are 180-220°C in the first stage, 220-250°C in the second stage, 230-250°C in the third stage, and 220-250°C in the die head.

10. The preparation method according to claim 8, characterized in that: During the preparation of the B masterbatch, the temperatures of the various zones of the twin-screw extruder are 180-210° C. for the first stage, 210-230° C. for the second stage, 210-220° C. for the third stage, and 210-230° C. for the die head.

Citation Information

Patent Citations

  • Low VOC glass fiber enhanced polypropylene material with long lasting fragrance and preparation method thereof

    CN109851916A

  • Low-odor low-VOC long glass fiber reinforced polypropylene composite material and preparation method thereof

    CN111533993A

  • Low-odor long-glass-fiber reinforced micro-foamed polypropylene composite material and preparation method thereof

    CN111748149A