Polyolefin composition with high rigidity and high toughness and low cost
Through the combination of polypropylene impact copolymer, polyolefin elastomer and filler, the bending modulus and impact strength of polyolefin materials are improved, and the compromise problem between toughness and rigidity of existing polypropylene materials is solved, achieving high Low cost effect.
Patent Information
- Application Number
- CN202411341279.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-12-06
AI Technical Summary
Existing polypropylene materials have limitations in improving toughness and rigidity, and are costly, making it difficult to meet the needs of high physical properties and low cost materials.
Compositions using 50-90% polypropylene impact copolymer, 5-25% polyolefin elastomer and 5-30% filler, specifically including 60-80% homopolypolypropylene and 20-40% Ethylene-α-olefin copolymers, as well as 85-95% homopolymer polypropylene and 5-15% ethylene-α-olefin copolymers, improve the formulation and process to improve the flexural modulus and impact strength of the material.
The high rigidity and high toughness of the polyolefin composition and products are achieved, while the amount of elastomer used is reduced, the production cost is reduced, and the requirements of high physical properties and low cost are met.
Smart Images

Figure BDA0005059764120000141
Abstract
Description
Technical Field
[0001] The present invention relates to a polyolefin composition and an article made from the polyolefin composition. Background Art
[0002] Due to the trade-off between toughness and stiffness, the use of pure polyolefin materials in engineering applications is relatively limited. For example, in common industrial applications, polyethylene materials have higher toughness and lower stiffness, so they are mostly used to produce consumables such as packaging bottles, bucket toys, etc. with lower physical property requirements. Polypropylene has higher stiffness than polyethylene, but lower toughness than polyethylene, so it is mostly used in white appliance housings. For automotive component materials with higher requirements, existing industrial solutions are mostly based on modified materials with engineering plastics or polyolefins as the base material.
[0003] The industry has developed several solutions to improve the overall physical properties of polypropylene materials. The most widely used solution is to improve the overall physical properties of polypropylene materials by adding fillers and elastomers at the same time. Fillers are responsible for improving the rigidity of polypropylene materials, and elastomers are responsible for improving the toughness of polypropylene materials. However, the modification technology is also subject to the influence of polypropylene substrates and blending technology, as well as the formulation ratio. Its ability to improve physical properties has its limitations, and the price of rubber elastomers is relatively high compared to polypropylene materials, which is not conducive to reducing production costs. Therefore, materials with high physical properties and low costs are still the focus of the industry to be broken through.
[0004] Therefore, there is still a need to find a polyolefin composition that has both high rigidity and high toughness and low cost. Summary of the invention
[0005] To this end, the present invention provides a polyolefin composition comprising, based on the weight of the polyolefin composition:
[0006] A) 50 to 90 wt.% of a polypropylene impact copolymer, the polypropylene impact copolymer comprising a first polypropylene impact copolymer and a second polypropylene impact copolymer,
[0007] B) 5 to 25% by weight of a polyolefin elastomer, and
[0008] C) 5-30% by weight of fillers,
[0009] wherein the first polypropylene impact copolymer comprises 60-80 wt% homopolypropylene and 20-40 wt% ethylene-α-olefin copolymer, based on the weight of the first polypropylene impact copolymer, and
[0010] The second polypropylene impact copolymer comprises 85-95 wt % of homopolypropylene and 5-15 wt % of ethylene-α-olefin copolymer, based on the weight of the second polypropylene impact copolymer.
[0011] The present invention also relates to an article made from the polyolefin composition.
[0012] The polyolefin composition and its products of the present invention have the following beneficial effects: (1) the polyolefin composition and its products have excellent rigidity and toughness; (2) the polyolefin composition and its products use a low amount of elastomer toughening agent, thereby reducing production costs. DETAILED DESCRIPTION
[0013] Polyolefin composition
[0014] According to the present invention, the polyolefin composition comprises, based on the weight of the polyolefin composition:
[0015] A) 50 to 90 wt.% of a polypropylene impact copolymer, the polypropylene impact copolymer comprising a first polypropylene impact copolymer and a second polypropylene impact copolymer,
[0016] B) 5 to 25% by weight of a polyolefin elastomer, and
[0017] C) 5-30% by weight of fillers,
[0018] wherein the first polypropylene impact copolymer comprises 60-80 wt% homopolypropylene and 20-40 wt% ethylene-α-olefin copolymer, based on the weight of the first polypropylene impact copolymer, and
[0019] The second polypropylene impact copolymer comprises 85-95 wt % of homopolypropylene and 5-15 wt % of ethylene-α-olefin copolymer, based on the weight of the second polypropylene impact copolymer.
[0020] The sum of the percentages of the various components in the polyolefin composition is 100% by weight.
[0021] According to the present invention, the polyolefin composition has a flexural modulus measured according to ISO 178 of from 1600 MPa to 2200 MPa.
[0022] According to the present invention, the polyolefin composition has a thermal conductivity of 30-40 kJ / m 2 Izod notched impact strength.
[0023] According to the present invention, the polyolefin composition has a thermal conductivity of 30-40 kJ / m2 The simply supported beam notched impact strength.
[0024] The polyolefin composition of the present invention can be formulated in any mixer commonly used in the art, for example in a twin-screw extruder (such as a Leistriz twin-screw extruder with a screw diameter of 40 mm).
[0025] Polypropylene impact copolymer
[0026] According to the present invention, the polyolefin composition comprises 50-90 wt% of a polypropylene impact copolymer, such as 65-85 wt% of a polypropylene impact copolymer, based on the weight of the polyolefin composition. The polypropylene impact copolymer comprises a first polypropylene impact copolymer and a second polypropylene impact copolymer.
[0027] In one embodiment, the polypropylene impact copolymer comprises 60 to 95 weight percent of a first polypropylene impact copolymer and 5 to 40 weight percent of a second polypropylene impact copolymer, based on the total weight of the polypropylene impact copolymer.
[0028] In a preferred embodiment, the polypropylene impact copolymer comprises 70-90 wt% of a first polypropylene impact copolymer and 10-30 wt% of a second polypropylene impact copolymer, based on the total weight of the polypropylene impact copolymer.
[0029] According to the present invention, the first polypropylene impact copolymer has a melt flow rate of 15 to 45 g / 10 min, for example, 20 to 40 g / 10 min, measured according to ASTM D12382 at 30°C / 2.16 kg.
[0030] According to the present invention, the second polypropylene impact copolymer has a melt flow rate of 50 to 80 g / 10 min, such as 55 to 70 g / 10 min, measured according to ASTM D12382 at 30°C / 2.16 kg.
[0031] According to the present invention, the first polypropylene impact copolymer and the second polypropylene impact copolymer each independently have a strength of 0.85-0.95 g / cm 3 density.
[0032] According to the present invention, the first polypropylene impact copolymer has a flexural modulus measured according to ISO 178 of 800 MPa to 1200 MPa.
[0033] According to the present invention, the second polypropylene impact copolymer has a flexural modulus measured according to ISO 178 of 1400 to 2000 MPa.
[0034] In one embodiment, in the first polypropylene impact copolymer and the second polypropylene impact copolymer, the homopolypropylene each independently has a tacticity index of 80% or more, or a tacticity index of 85% or more, or a tacticity index of 90% or more, or a tacticity index of 95% or more.
[0035] In one embodiment, in the first polypropylene impact copolymer and the second polypropylene impact copolymer, the α-olefin in the ethylene-α-olefin copolymer independently has 2 to 8 carbon atoms. Preferably, the α-olefin is selected from propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene or 1-octene. In a preferred embodiment, the α-olefin is propylene.
[0036] In one embodiment, in the first and second polypropylene impact copolymers, the ethylene-α-olefin copolymers each independently comprise 10-75 wt% ethylene derived monomer units, such as 20-40 wt% or 30-50 wt% ethylene derived monomer units.
[0037] In one embodiment, in the first polypropylene impact copolymer and the second polypropylene impact copolymer, the ethylene-α-olefin copolymer each independently has an intrinsic viscosity of 1.5 to 8.5 dl / g, such as 2.0 to 4.0 dl / g.
[0038] Herein, intrinsic viscosity is measured using a Crystex instrument from Polymer Char according to the soluble fraction test method.
[0039] According to the present invention, the ethylene-α-olefin copolymer is present as a dispersed phase in the homopolypropylene continuous phase of the polypropylene impact copolymer.
[0040] Each polypropylene impact copolymer can be prepared according to conventional methods in the art. In the method for preparing the polypropylene impact copolymer, the polymerization temperature is preferably 200° C. or lower, more preferably 100° C. or lower. In the method for preparing the polypropylene impact copolymer, the polymerization pressure is preferably 10 MPa or lower, more preferably 5 MPa or lower.
[0041] According to the present invention, the method for preparing the polypropylene impact copolymer can be a continuous polymerization method or a batch polymerization method. In addition, the polymerization reaction is carried out in two stages, or in three or more stages.
[0042] When preparing a polypropylene impact copolymer, it can be prepared by two or more stage polymerization, and the copolymer can generally be obtained by preparing homopolypropylene using a Ziegler-Natta catalyst in the first stage and copolymerizing ethylene and α-olefin in the second stage.
[0043] In one embodiment, polymerization is performed in the first stage of preparing the first polypropylene impact copolymer by adjusting the polymerization temperature and the residence time so that the proportion of the homopolypropylene continuous phase is in the range of 60-80 wt %, and then ethylene and α-olefin are introduced and polymerized in the second stage so that the proportion of the dispersed phase is in the range of 20-40 wt %.
[0044] In one embodiment, polymerization is performed in the first stage of preparing the second polypropylene impact copolymer by adjusting the polymerization temperature and the residence time so that the proportion of the homopolypropylene continuous phase is in the range of 85-95 wt %, and then ethylene and α-olefin are introduced and polymerized in the second stage so that the proportion of the dispersed phase is in the range of 5-15 wt %.
[0045] The stage of preparing polypropylene can be carried out in two or more series reactors, each reactor is operated under the same conditions (such as hydrogen level, comonomer, temperature, type or percentage of external electron donor, etc.) to prepare the same type of polypropylene, or is operated under different conditions to prepare polypropylene such as bimodal molecular weight distribution. Similarly, there can be two or more reactors in series for the second stage, and these reactors can be operated under the same conditions to prepare the same type of ethylene-alpha-olefin copolymers, or are operated under different conditions to prepare ethylene-alpha-olefin copolymers with differences in some features such as molecular weight or comonomer content. Most preferably, the first stage of preparing the continuous phase of polypropylene is carried out in a bulk polymerization process, and the preparation of the ethylene-alpha-olefin copolymer finely dispersed in the continuous phase range is carried out in one or more gas phase reactors in the second stage.
[0046] The polymerization temperature in both the first stage and the second stage is preferably 200° C. or less, more preferably 100° C. or less. The polymerization pressure is preferably 10 MPa or less, more preferably 5 MPa or less. In addition, the polymerization time per polymerization stage or the residence time in the case of continuous polymerization is usually 0.25 to 5 hours.
[0047] Examples of the polymerization method include a solution polymerization method in which an inert hydrocarbon compound such as cyclohexane and heptane is used as a solvent, a bulk polymerization method in which liquefied propylene is used, and a gas phase polymerization method in which no liquid alkane is involved. Examples of preferred polymerization methods include both bulk polymerization methods and gas phase polymerization methods. The polymerization methods are known to those skilled in the art.
[0048] In a preferred embodiment, the first polypropylene impact copolymer is, for example, Advanced Achieved TM PP 8285E1.
[0049] In a preferred embodiment, the second polypropylene impact copolymer is, for example, ExxonMobil TM PP7935E1.
[0050] Polyolefin elastomer
[0051] According to the present invention, the polyolefin composition comprises 5-25 wt% of polyolefin elastomer, such as 5-15 wt% of polyolefin elastomer, based on the weight of the polyolefin composition.
[0052] In one embodiment, the polyolefin elastomer has a melt flow rate of 1 to 15 g / 10 min, measured according to ASTM D1238 190° C. / 2.16 kg.
[0053] In one embodiment, the polyolefin elastomer has a glass transition temperature of -55°C to -50°C and a melting point of 40°C to 90°C.
[0054] The polyolefin elastomer comprises one or more ethylene-based elastomers. The polyolefin elastomer comprises monomer units derived from ethylene and monomer units derived from a group consisting of C3-C 12 Monomer units of one or more comonomers of an α-olefin. The α-olefin comonomer may be selected from propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene or 1-decene. In a preferred embodiment, the α-olefin is 1-octene.
[0055] The polyolefin elastomer may include at least 70 weight percent, at least 75 weight percent, at least 80 weight percent, at least 81 weight percent, at least 82 weight percent, or at least 83 weight percent ethylene-derived monomer units, wherein the weight percent is based on the total weight of the ethylene-derived monomer units and the alpha-olefin-derived monomer units. The polyolefin elastomer may include up to 95 weight percent, up to 94 weight percent, up to 93 weight percent, up to 92 weight percent, up to 90 weight percent, or up to 88 weight percent ethylene-derived monomer units, wherein the weight percent is based on the total weight of the ethylene-derived monomer units and the alpha-olefin-derived monomer units.
[0056] The polyolefin elastomer may include at least 5 wt%, at least 6 wt%, at least 7 wt%, at least 8 wt%, at least 9 wt%, at least 10 wt%, or at least 12 wt% α-olefin derived monomer units, wherein the weight percentage is based on the total weight of ethylene derived monomer units and α-olefin derived monomer units. The polyolefin elastomer may include up to 30 wt%, up to 25 wt%, up to 22 wt%, up to 20 wt%, up to 19 wt%, up to 18 wt%, or up to 17 wt% α-olefin derived monomer units, wherein the weight percentage is based on the total weight of ethylene derived monomer units and α-olefin derived monomer units. In some embodiments, the polyolefin elastomer may include 5-25 wt% α-olefin derived monomer units, or 9-18 wt% α-olefin derived monomer units, wherein the weight percentage is based on the total weight of ethylene derived monomer units and α-olefin derived monomer units.
[0057] In a preferred embodiment, the polyolefin elastomer is an ethylene-octene copolymer, such as Engage 8200 from Dow.
[0058] In a preferred embodiment, the polyolefin elastomer may have a weight average molecular weight (Mw) of 50,000 to 5,000,000 g / mol, 75,000 to 1,000,000 g / mol, 100,000 to 500,000 g / mol, or 125000 to 300000 g / mol. The molecular weight distribution (MWD, equal to Mw / Mn) of the polyolefin elastomer may be 1 to 40, 1 to 15, 1.8 to 5, or 1.8 to 3.
[0059] The polyolefin elastomer can be prepared according to conventional methods in the art. For example, the polyolefin elastomer can be prepared by reacting the monomers at a temperature of 0° C. to 200° C. for a period of 1 minute to 10 hours in the presence of a catalyst system. Preferably, uniform conditions are used, such as a continuous solution process or a bulk polymerization process using excess monomer as a diluent. The catalyst system used to prepare the polyolefin elastomer can be a metallocene-based compound.
[0060] filler
[0061] According to the present invention, the polyolefin composition comprises 5-30 wt% filler, such as 10-20 wt% filler, based on the weight of the polyolefin composition.
[0062] In one embodiment, the filler includes talc, calcium carbonate, calcium hydroxide, barium sulfate, mica, calcium silicate, clay, kaolin, silica, alumina, wollastonite, magnesium carbonate, magnesium hydroxide, titanium oxide, zinc oxide, zinc sulfate, or a combination thereof.
[0063] In a preferred embodiment, the filler is talc, which may have a size of about 1 μm to about 100 μm. The talc is, for example, HTP Ultra 5L from Imifabi.
[0064] According to the present invention, the polyolefin composition may further comprise additives generally known in the art, such as dispersants, lubricants, flame retardants, antioxidants, antistatic agents, light stabilizers, ultraviolet light absorbers, carbon black, nucleating agents, plasticizers and coloring agents such as dyes or pigments. The additive may be present in the polyolefin composition in an amount of 0.1-5% by weight, based on the weight of the polyolefin composition.
[0065] In a preferred embodiment, the polyolefin composition comprises, based on the weight of the polyolefin composition:
[0066] A) 50 to 90 wt.% of a polypropylene impact copolymer, the polypropylene impact copolymer comprising a first polypropylene impact copolymer and a second polypropylene impact copolymer,
[0067] B) 5 to 25% by weight of a polyolefin elastomer, and
[0068] C) 5-30% by weight of fillers,
[0069] wherein the first polypropylene impact copolymer comprises 60-80 wt % of homopolypropylene and 20-40 wt % of ethylene-α-olefin copolymer, based on the weight of the first polypropylene impact copolymer,
[0070] wherein the second polypropylene impact copolymer comprises 85-95 wt % homopolypropylene and 5-15 wt % ethylene-α-olefin copolymer, based on the weight of the second polypropylene impact copolymer, and
[0071] The polypropylene impact copolymer comprises 60-95 wt % of a first polypropylene impact copolymer and 5-40 wt % of a second polypropylene impact copolymer, based on the total weight of the polypropylene impact copolymer.
[0072] In yet another preferred embodiment, the polyolefin composition comprises, based on the weight of the polyolefin composition:
[0073] A) 65 to 85 weight percent of a polypropylene impact copolymer, the polypropylene impact copolymer comprising a first polypropylene impact copolymer and a second polypropylene impact copolymer,
[0074] B) 5-15% by weight of a polyolefin elastomer, and
[0075] C) 10-20% by weight of fillers,
[0076] wherein the first polypropylene impact copolymer comprises 60-80 wt % of homopolypropylene and 20-40 wt % of ethylene-α-olefin copolymer, based on the weight of the first polypropylene impact copolymer,
[0077] wherein the second polypropylene impact copolymer comprises 85-95 wt % homopolypropylene and 5-15 wt % ethylene-α-olefin copolymer, based on the weight of the second polypropylene impact copolymer, and
[0078] The polypropylene impact copolymer comprises 60-95 wt % of a first polypropylene impact copolymer and 5-40 wt % of a second polypropylene impact copolymer, based on the total weight of the polypropylene impact copolymer.
[0079] In yet another preferred embodiment, the polyolefin composition comprises, based on the weight of the polyolefin composition:
[0080] A) 65 to 85 weight percent of a polypropylene impact copolymer, the polypropylene impact copolymer comprising a first polypropylene impact copolymer and a second polypropylene impact copolymer,
[0081] B) 5-15% by weight of a polyolefin elastomer, and
[0082] C) 10-20% by weight of fillers,
[0083] wherein the first polypropylene impact copolymer comprises 60-80 wt % of homopolypropylene and 20-40 wt % of ethylene-α-olefin copolymer, based on the weight of the first polypropylene impact copolymer,
[0084] wherein the second polypropylene impact copolymer comprises 85-95 wt % homopolypropylene and 5-15 wt % ethylene-α-olefin copolymer, based on the weight of the second polypropylene impact copolymer, and
[0085] The polypropylene impact copolymer comprises 70-90 wt % of a first polypropylene impact copolymer and 10-30 wt % of a second polypropylene impact copolymer, based on the total weight of the polypropylene impact copolymer.
[0086] Products
[0087] The present invention relates to an article made of the polyolefin composition. The polyolefin composition disclosed herein can be used to prepare any article, such as instrument components and automotive components. Such components can be made by common plastic preparation processes, such as thermoforming, blow molding or injection molding. Preferably, the polyolefin composition of the present invention can be used for (injection) molding automotive components, i.e. automotive interior or exterior components. The term "automotive component" used in the present invention means that it is a molded three-dimensional article for automotive interior or exterior. Typical automotive components are bumpers, body panels, rocker panels, side trims, pillars, pedal assists, spoilers, fenders, instrument panels, etc. The term "exterior" means that the article is not part of the automotive interior, but part of the automotive exterior. Therefore, preferred automotive exterior components are selected from bumpers, pedal assists, body panels, fenders and spoilers. In contrast, the term "interior" means that the article is part of the automotive interior, not part of the automotive exterior. Therefore, preferred automotive interior components are selected from instrument panels, pillars and glove boxes.
[0088] In order to mix the individual components of the polyolefin composition, conventional processing blending equipment can be used, for example internal mixer, two-roll rubber mill, co-kneader or twin screw extruder. The polymeric material coming out of the extruder is generally in the form of pellets. Preferably these pellets are further processed then, for example by injection molding to produce goods, for example automotive interior or exterior components (such as automobile bumpers).
[0089] According to the present invention, the article made from the polyolefin composition has a flexural modulus measured according to ISO 178 of 1600 to 2200 MPa.
[0090] According to the present invention, the article made of the polyolefin composition has a thermal conductivity of 30-40 kJ / m 2 Izod notched impact strength.
[0091] According to the present invention, the article made of the polyolefin composition has a thermal conductivity of 30-40 kJ / m 2 The simply supported beam notched impact strength.
[0092] The various descriptive elements and numerical ranges describing the polyolefin compositions may be combined with other descriptive elements and numerical ranges to describe the invention; furthermore, for a given element, any upper numerical limit may be combined with any lower numerical limit described herein.
[0093] Those skilled in the art can more easily understand the present invention according to the following embodiments:
[0094] Embodiment 1. A polyolefin composition comprising, based on the weight of the polyolefin composition:
[0095] A) 50 to 90 wt.% of a polypropylene impact copolymer, the polypropylene impact copolymer comprising a first polypropylene impact copolymer and a second polypropylene impact copolymer,
[0096] B) 5 to 25% by weight of a polyolefin elastomer, and
[0097] C) 5-30% by weight of fillers,
[0098] wherein the first polypropylene impact copolymer comprises 60-80 wt% homopolypropylene and 20-40 wt% ethylene-α-olefin copolymer, based on the weight of the first polypropylene impact copolymer, and
[0099] The second polypropylene impact copolymer comprises 85-95 wt % of homopolypropylene and 5-15 wt % of ethylene-α-olefin copolymer, based on the weight of the second polypropylene impact copolymer.
[0100] Embodiment 2. The polyolefin composition of embodiment 1, wherein the first polypropylene impact copolymer has a melt flow rate of 15 to 45 g / 10 min as determined according to ASTM D1238 230°C / 2.16 kg, and wherein the second polypropylene impact copolymer has a melt flow rate of 50 to 80 g / 10 min as determined according to ASTM D1238 230°C / 2.16 kg.
[0101] Embodiment 3. The polyolefin composition of embodiment 1 or 2, wherein in the first polypropylene impact copolymer and the second polypropylene impact copolymer, the homopolypropylene each independently has a tacticity index of 80% or more.
[0102] Embodiment 4. The polyolefin composition according to any one of embodiments 1-3, wherein in the first polypropylene impact copolymer and the second polypropylene impact copolymer, the α-olefin in the ethylene-α-olefin copolymer each independently has 2 to 8 carbon atoms.
[0103] Embodiment 5. The polyolefin composition according to any one of embodiments 1 to 4, wherein in the first polypropylene impact copolymer and the second polypropylene impact copolymer, the ethylene-α-olefin copolymer each independently comprises 10-75 wt% of ethylene-derived monomer units.
[0104] Embodiment 6. The polyolefin composition according to any one of embodiments 1-5, wherein in the first polypropylene impact copolymer and the second polypropylene impact copolymer, the ethylene-α-olefin copolymer each independently has an intrinsic viscosity of 1.5-8.5 dl / g.
[0105] Embodiment 7. The polyolefin composition according to any one of embodiments 1-6, wherein the first polypropylene impact copolymer has a flexural modulus of 800 MPa to 1200 MPa, as determined according to ISO 178, and wherein the second polypropylene impact copolymer has a flexural modulus of 1400 MPa to 2000 MPa, as determined according to ISO 178.
[0106] Embodiment 8. The polyolefin composition according to any one of embodiments 1-7, wherein the polyolefin elastomer has a melt flow rate of 1 to 15 g / 10 min as determined according to ASTM D1238 190°C / 2.16 kg.
[0107] Embodiment 9. The polyolefin composition of any one of embodiments 1-8, wherein the polyolefin elastomer has a glass transition temperature of -55°C to -50°C and a melting point of 40°C to 90°C.
[0108] Embodiment 10. The polyolefin composition according to any one of embodiments 1 to 9, wherein the polyolefin elastomer is an ethylene-α-olefin copolymer, preferably an ethylene-octene copolymer.
[0109] Embodiment 11. A polyolefin composition according to any one of Embodiments 1-10, wherein the filler comprises talc, calcium carbonate, calcium hydroxide, barium sulfate, mica, calcium silicate, clay, kaolin, silica, alumina, wollastonite, magnesium carbonate, magnesium hydroxide, titanium oxide, zinc oxide, zinc sulfate, or a combination thereof, preferably talc.
[0110] Embodiment 12. The polyolefin composition according to any one of embodiments 1-11,
[0111] wherein the polyolefin composition has a flexural modulus of 1600 MPa to 2200 MPa, measured according to ISO 178; and / or
[0112] The polyolefin composition has a thermal conductivity of 30-40 kJ / m2 as measured at room temperature according to ISO 180 / 1eA. 2 Izod notched impact strength; and / or
[0113] The polyolefin composition has a thermal conductivity of 30-40 kJ / m2 as measured at room temperature according to ISO 179 / 1eA. 2 The simply supported beam notched impact strength.
[0114] Embodiment 13. The polyolefin composition of any one of Embodiments 1-12, wherein the polypropylene impact copolymer comprises 60-95 wt% of the first polypropylene impact copolymer and 5-40 wt% of the second polypropylene impact copolymer, based on the total weight of the polypropylene impact copolymer.
[0115] Embodiment 14. A polyolefin composition comprising, based on the weight of the polyolefin composition:
[0116] A) 65 to 85 weight percent of a polypropylene impact copolymer, the polypropylene impact copolymer comprising a first polypropylene impact copolymer and a second polypropylene impact copolymer,
[0117] B) 5-15% by weight of a polyolefin elastomer, and
[0118] C) 10-20% by weight of fillers,
[0119] wherein the first polypropylene impact copolymer comprises 60-80 wt % of homopolypropylene and 20-40 wt % of ethylene-α-olefin copolymer, based on the weight of the first polypropylene impact copolymer,
[0120] wherein the second polypropylene impact copolymer comprises 85-95 wt % homopolypropylene and 5-15 wt % ethylene-α-olefin copolymer, based on the weight of the second polypropylene impact copolymer, and
[0121] The polypropylene impact copolymer comprises 60-95 wt % of a first polypropylene impact copolymer and 5-40 wt % of a second polypropylene impact copolymer, based on the total weight of the polypropylene impact copolymer.
[0122] Embodiment 15. An article made from the polyolefin composition according to any one of embodiments 1-14.
[0123] Embodiment 16. The article of embodiment 15, wherein the article is an automotive part, preferably an automotive bumper.
[0124] Embodiment 17. A method of making the article of embodiment 15 or 16, comprising melt extruding and injection molding the polyolefin composition according to any one of embodiments 1-14.
[0125] Example
[0126] The nature and purpose of the present invention will be further understood through the following examples. It should be understood that these examples are only for illustrative purposes and are not intended to limit the scope of the present invention.
[0127] Test Method
[0128] Flexural modulus (MPa) was measured according to ISO 178 standard method.
[0129] Izod notched impact strength (kJ / m 2 ) is measured according to ISO 180 / 1eA standard method.
[0130] Simple supported beam notched impact strength (kJ / m 2 ) is measured according to ISO 179 / 1eA standard method.
[0131] The melt flow rate (MFR) is measured according to ASTM D1238, 230°C / 2.16kg or ASTM D1238, 190°C / 2.16kg standard method.
[0132] The coefficient of linear thermal expansion in the flow direction (CLTE) is measured according to the ASTM E831 standard method.
[0133] Material
[0134] Advanced Achieved TM PP8285E1 is a polypropylene impact copolymer available from ExxonMobil Chemical.
[0135] ExxonMobil TM PP7935E1 is a polypropylene impact copolymer available from ExxonMobil Chemical.
[0136] Engage 8200 is a polyolefin elastomer available from Dow.
[0137] HTP Ultra 5L is a talc powder purchased from Imifabi.
[0138] Table 1 Composition of the polyolefin composition in the embodiment of the present invention
[0139] Example 1 <![CDATA[Advanced Achieved TM PP8285E1]]> 58% by weight <![CDATA[ExxonMobil TM PP7935E1]]> 16 wt% Engage 8200 10% by weight HTP Ultra 5L 16 wt% total 100% by weight
[0140] Example 1
[0141] The polyolefin composition of Example 1 of the present invention was formulated in a Leistriz twin-screw extruder with a screw diameter of 40 mm. Compounding was accomplished in the twin-screw extruder using mixing screw elements, with an extrusion process temperature of 210° C. and a die temperature of 230° C. The compound discharged from the extruder was pelletized. Table 2 shows the properties of the samples prepared from the polyolefin composition of Example 1 of the present invention.
[0142] Table 2 Performance of samples
[0143]
[0144] The data in Table 2 show that the various properties of the samples of the present invention meet the Nissan AS1 physical property standard, and in particular, the flexural modulus and impact strength thereof are much higher than the Nissan AS1 physical property standard, indicating that the product of the present invention has high rigidity and high toughness. At the same time, the polyolefin composition of the present invention uses a relatively low content of a relatively expensive polyolefin elastomer, thereby reducing production costs.
[0145] Although specific embodiments of the present invention are shown and described, it should be understood that other improvements, substitutions and alternatives are known to those skilled in the art. Such improvements, substitutions and alternative embodiments may be made without departing from the spirit and scope of the present invention which should be determined by the appended claims. Each feature of the present invention is described in the appended claims.
Claims
1. A polyolefin composition comprising, based on the weight of the polyolefin composition: A) 50 to 90 wt.% of a polypropylene impact copolymer, the polypropylene impact copolymer comprising a first polypropylene impact copolymer and a second polypropylene impact copolymer, B) 5 to 25% by weight of a polyolefin elastomer, and C) 5-30% by weight of fillers, wherein the first polypropylene impact copolymer comprises 60-80 wt% homopolypropylene and 20-40 wt% ethylene-α-olefin copolymer, based on the weight of the first polypropylene impact copolymer, and The second polypropylene impact copolymer comprises 85-95 wt % of homopolypropylene and 5-15 wt % of ethylene-α-olefin copolymer, based on the weight of the second polypropylene impact copolymer.
2. The polyolefin composition of claim 1, wherein the first polypropylene impact copolymer has a melt flow rate of 15 to 45 g / 10 min, as determined according to ASTM D1238 230°C / 2.16 kg, and wherein the second polypropylene impact copolymer has a melt flow rate of 50 to 80 g / 10 min, as determined according to ASTM D1238 230°C / 2.16 kg.
3. The polyolefin composition according to claim 1 or 2, wherein in the first polypropylene impact copolymer and the second polypropylene impact copolymer, the homopolypropylene each independently has a tacticity index of 80% or more.
4. The polyolefin composition according to any one of claims 1 to 3, wherein in the first polypropylene impact copolymer and the second polypropylene impact copolymer, the α-olefin in the ethylene-α-olefin copolymer each independently has 2 to 8 carbon atoms.
5. The polyolefin composition according to any one of claims 1 to 4, wherein in the first polypropylene impact copolymer and the second polypropylene impact copolymer, the ethylene-α-olefin copolymer each independently comprises 10 to 75 wt% of ethylene derived monomer units.
6. The polyolefin composition according to any one of claims 1 to 5, wherein in the first polypropylene impact copolymer and the second polypropylene impact copolymer, the ethylene-α-olefin copolymer each independently has an intrinsic viscosity of 1.5 to 8.5 dl / g.
7. The polyolefin composition according to any one of claims 1 to 6, wherein the first polypropylene impact copolymer has a flexural modulus determined according to ISO 178 of 800 to 1200 MPa, and wherein the second polypropylene impact copolymer has a flexural modulus determined according to ISO 178 of 1400 to 2000 MPa.
8. The polyolefin composition according to any one of claims 1 to 7, wherein the polyolefin elastomer has a melt flow rate of 1 to 15 g / 10 min, measured according to ASTM D1238 190°C / 2.16 kg.
9. The polyolefin composition according to any one of claims 1 to 8, wherein the polyolefin elastomer is an ethylene-α-olefin copolymer, preferably an ethylene-octene copolymer.
10. The polyolefin composition of any one of claims 1 to 9, wherein the polypropylene impact copolymer comprises 60 to 95 wt% of a first polypropylene impact copolymer and 5 to 40 wt% of a second polypropylene impact copolymer, based on the total weight of the polypropylene impact copolymer.
11. A polyolefin composition comprising, based on the weight of the polyolefin composition: A) 65 to 85 weight percent of a polypropylene impact copolymer, the polypropylene impact copolymer comprising a first polypropylene impact copolymer and a second polypropylene impact copolymer, B) 5-15% by weight of a polyolefin elastomer, and C) 10-20% by weight of fillers, wherein the first polypropylene impact copolymer comprises 60-80 wt % of homopolypropylene and 20-40 wt % of ethylene-α-olefin copolymer, based on the weight of the first polypropylene impact copolymer, wherein the second polypropylene impact copolymer comprises 85-95 wt % homopolypropylene and 5-15 wt % ethylene-α-olefin copolymer, based on the weight of the second polypropylene impact copolymer, and The polypropylene impact copolymer comprises 60-95 wt % of a first polypropylene impact copolymer and 5-40 wt % of a second polypropylene impact copolymer, based on the total weight of the polypropylene impact copolymer.
12. An article made from the polyolefin composition according to any one of claims 1 to 11.
13. A method for manufacturing the article of claim 12, comprising melt extruding and injection molding the polyolefin composition according to any one of claims 1 to 11.
Citation Information
Patent Citations
Polyolefin composition
CN105849178A
Heterophasic propylene copolymer composition
CN114846075A
Cited By
Polyolefin composition and honeycomb panel made therefrom
CN121249044A