Prepreg sheet suitable for high-frequency circuit, core board of prepreg sheet, laminated circuit board, preparation method and preparation device
By staggering the inorganic microsphere adjustment layer on the glass fiber cloth of the high-frequency circuit board and using ultrasonic induced distribution, the signal transmission instability caused by the glass fiber effect is solved, and Dk uniformity and high-frequency circuit board are achieved The accuracy of signal transmission simplifies the preparation process.
Patent Information
- Application Number
- CN202410623931.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing high-frequency circuit boards have different dielectric constants due to the periodic pattern of the fiberglass cloth, which triggers the glass fiber effect, resulting in unstable signal transmission and reduced accuracy. The existing improvement methods such as increasing fiber density or circuit design occupying space, exist. Through hole difficulty and signal delay issues.
Using an interlaced glass fiber cloth, and covering the inorganic microsphere adjustment layer on the Z-side, ultrasonic wave induced the distribution of inorganic microspheres to form a gradient density, reduce the periodic changes of the Dk of the glass fiber cloth, improve the glass fiber effect, and improve the accuracy of signal transmission. sex.
The uniformity of glass fiber cloth Dk is achieved, phase deviation is avoided, signal transmission accuracy of high-frequency circuit boards is improved, and the preparation process is simplified and yield is improved.
Smart Images

Figure CN119081320A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of circuit boards, and in particular relates to a prepreg sheet suitable for high-frequency circuits and a preparation method, device and circuit board thereof. Background Art
[0002] In recent years, technologies such as 5G, AI, and self-driving cars have developed rapidly. Correspondingly, the performance requirements for high-frequency and high-speed circuit boards have become more stringent and urgent.
[0003] Most existing circuit boards include low-dielectric-constant, low-dielectric-loss organic materials such as polytetrafluoroethylene (PTFE) to ensure transmission performance. Circuit boards are usually also designed with glass fiber cloth to enhance the mechanical properties of the entire board. However, the periodic changes in the glass fiber weaving pattern will cause the glass fiber effect, that is, the difference in dielectric constant (Dk) in small areas of the entire circuit board material, leading to problems such as stepped impedance structure, differential-to-common-mode conversion, and waveform distortion at the receiving end, especially at high frequencies.
[0004] There are currently two main methods to reduce the glass fiber effect:
[0005] 1) The weaving method of the glass fiber cloth is improved, and a higher weaving density or wider fibers are used for dense arrangement. The fiber is opened or flattened. Although the Dk difference is eliminated, the amount of glass fiber used is increased, resulting in an increase in the overall Dk. At the same time, the design of high-density glass fiber leads to greater difficulty in through-hole preparation and higher through-hole roughness during subsequent through-hole preparation.
[0006] 2) Circuit design uses Zig-Zag routing, wider routing, angled routing and other methods to reduce the difference in signal transmission between lines. Although it can reduce or eliminate the glass fiber effect of differential lines, the field of circuit board technology tends to pursue high integration and miniaturization. This method of improving the glass fiber effect will occupy more circuit board volume, which is more wasteful of circuit board design space. At the same time, it may increase chamfers, thereby causing problems such as signal delays.
[0007] The patent document with application number 202010956221.1 discloses a PCB board with differential lines, a manufacturing method and an electronic device. The PCB board includes: a first transmission medium layer, including a glass fiber sheet woven into a grid and an adhesive material embedded in the grid, and a first transmission line is opened on the surface of the first transmission medium layer; a second transmission medium layer, a glass fiber sheet woven into a grid and an adhesive material embedded in the grid, the grid of the second transmission medium layer is parallel to and opposite to the grid of the first transmission medium layer, and the second transmission medium layer is opened on the surface close to the first transmission medium layer. The first transmission line and the second transmission line have the same width and constitute a differential pair; a prepreg, the prepreg is bonded to the relative surfaces of the first transmission medium layer and the second transmission medium layer.
[0008] Although the multi-layer transmission method of the above patented technology reduces the difference in signal transmission to a certain extent, the complex laminated structure is prone to defects such as delamination and air holes in actual production and manufacturing, thereby reducing the efficiency of use.
[0009] In summary, the present invention aims to develop a prepreg sheet suitable for high-frequency circuits that can improve the glass fiber effect, in order to solve the defects of the prior art. Summary of the invention
[0010] In view of the problems in the related art, the present invention proposes a prepreg sheet suitable for high-frequency circuits, which can improve the Dk periodic variation problem caused by the periodic pattern of glass fiber cloth, thereby ensuring the signal transmission accuracy of high-frequency circuit boards. The present invention also discloses a core board and a laminated circuit board including the prepreg sheet, and the present invention also discloses a preparation method and a preparation device of the prepreg sheet.
[0011] The technical solution of the present invention is as follows:
[0012] A prepreg sheet suitable for high-frequency circuits, comprising glass fiber cloth, the glass fiber cloth comprising staggered X-direction wire bundles and Y-direction wire bundles, the gaps between the wire bundles forming windows, the glass fiber cloth covering and adhering an adjustment layer on at least one side in the Z direction, the adjustment layer being filled with inorganic microspheres;
[0013] The inorganic microspheres of the adjustment layer are distributed in a density that gradually decreases toward the empty window along the Z direction, and the inorganic microspheres of the adjustment layer are distributed in a density that gradually increases toward the wire bundle along the Z direction.
[0014] The present invention improves the design of the structure of the prepreg sheet, designs high-density inorganic microspheres in the Z direction of the wire harness to reduce the high Dk effect of the X-direction wire harness and the Y-direction wire harness, designs low-density inorganic microspheres in the Z direction of the empty window to improve its low Dk effect, reduces the peak and valley values of the periodic change of the Dk value of the glass fiber cloth due to the arrangement of the wire harness and the gap, improves the glass fiber effect of the glass fiber cloth, and makes the prepreg sheet prepared by the present invention have overall Dk uniformity, avoids phase deviation caused by the periodic Dk change of the glass fiber cloth in the same circuit of the circuit board, improves the accuracy of signal transmission, and is particularly suitable for application in high-frequency and high-speed circuits; at the same time, the prepreg sheet of the present invention has a simple structure and a high preparation yield.
[0015] Preferably, the inorganic microspheres of the adjustment layer are distributed in a density gradually decreasing along the Z direction toward the empty window until a microsphere blank area is formed above the empty window;
[0016] The inorganic microspheres of the adjustment layer are distributed in a density that gradually increases toward the wire bundle along the Z direction until a microsphere-dense area is formed above the wire bundle;
[0017] The distribution of the inorganic microspheres in the area outside the microsphere blank area and the microsphere dense area tends to be uniform.
[0018] The inorganic microspheres of the prepreg sheet are further arranged with a density design, and the density arrangement of the inorganic microspheres can further reduce the Dk variation difference and further improve the accuracy of signal transmission.
[0019] Preferably, the adjustment layer comprises a low-polarity organic material and inorganic microspheres filled in the low-polarity organic material; the weight ratio of the low-polarity organic material to the inorganic microspheres is 10:1-3.
[0020] Preferably, the inorganic microspheres are hollow silica microspheres or hollow glass microspheres (HGM).
[0021] Preferably, the particle size of the hollow silica microspheres or hollow glass microspheres is 5 to 20 microns, and the sphere wall thickness of the hollow silica microspheres or hollow glass microspheres is ≥ 1 / 5 of the sphere radius.
[0022] Specifically, the purity of the hollow glass microspheres (HGM) is ≥99.9%.
[0023] Preferably, the inorganic microspheres are surface-modified with a silane coupling agent, specifically comprising the following steps:
[0024] A) preparing an ethanol solution of a silane coupling agent (such as KH550, etc.), wherein the mass concentration of the silane coupling agent is 0.1-0.3%, to obtain a modified solution;
[0025] B) the inorganic microspheres and the modified solution are mixed in a weight ratio of 25 to 35:100 and mixed at a speed of 1500 to 1700 r / min for 2 to 4 minutes;
[0026] C) After being evenly dispersed, the modified particles are immersed at a constant temperature of 35 to 45° C. for 40 to 50 minutes, washed, and dried to obtain inorganic microspheres modified with a silane coupling agent.
[0027] Surface silanization modification of inorganic microspheres can effectively prevent their agglomeration, which is beneficial to inducing their mobile distribution during the preparation process, thereby realizing the ideal density distribution design of inorganic microspheres in the present invention.
[0028] Preferably, the dielectric constant of the low-polarity organic material is ≤3, such as polyphenylene ether, polytetrafluoroethylene (PTFE), etc.
[0029] Preferably, the glass fiber cloth covers and adheres the adjustment layer on the upper side in the Z direction, the thickness of the adjustment layer is 2 to 4 mils, and covers and adheres the matrix layer on the lower side, the thickness of the matrix layer is 1 to 2 mils;
[0030] The matrix layer is filled with the same inorganic microspheres as the adjustment layer.
[0031] Preferably, the weaving specification of the glass fiber cloth adopts a weaving specification of glass fiber cloth with a warp and weft gap ≥ 1080.
[0032] Exemplary parameters are shown in the table below.
[0033]
[0034] The glass fiber cloth is more preferably of 106 weave specification, with larger gaps between wire bundles and less increase in overall Dk.
[0035] The glass fiber cloth is one of NE-glass fiber cloth, E-glass fiber cloth and flat E-glass fiber cloth, preferably NE-glass fiber cloth.
[0036] Preferably, the bundle is composed of round fibers, and a circular interface is more suitable for the induction of activation energy.
[0037] The present invention also discloses a method for preparing the above-mentioned prepreg sheet suitable for high-frequency circuits, comprising the following steps:
[0038] 1) low polarity organic material and inorganic microspheres are mixed in a weight ratio of 10:1-3, stirred evenly, and a slurry is prepared for standby use;
[0039] 2) Preheating the glass fiber cloth, then evenly spreading the slurry on the surface of the glass fiber cloth, and at the same time, arranging an ultrasonic wave emitting upward in the Z direction under the glass fiber cloth to treat it, and finally semi-curing it to obtain a prepreg sheet suitable for high-frequency circuits.
[0040] The present invention utilizes the reflection and diffraction behavior of ultrasonic waves on the glass fiber cloth and its gaps to achieve the adjustment of Dk. Specifically, since the X- and Y-direction bundles of the glass fiber cloth strongly reflect ultrasonic waves, the empty windows of the glass fiber cloth can pass ultrasonic waves. The ultrasonic waves that penetrate the empty windows form a pressure difference with the surroundings, thereby driving the inorganic microspheres to gather above the warp and weft lines of the glass fiber cloth along the Z direction. The ultrasonic wave energy gradually weakens as it moves away from the glass fiber cloth, thereby forming a gradient difference, resulting in a high density of inorganic microspheres near the X- and Y-direction bundles, a low density of inorganic microspheres near the empty windows, and a uniform distribution of inorganic microspheres away from the entire glass fiber cloth. Ultrasonic waves are utilized to achieve the induction and directional distribution and agglomeration of inorganic microspheres, so that the inorganic microspheres are periodically assembled according to the warp and weft lines of the glass fiber cloth, thereby adjusting and improving the glass fiber effect, so that the prepreg sheet prepared by the present invention has good Dk uniformity, so as to improve the accuracy of circuit signal transmission; at the same time, the preparation process steps of the present invention are simplified, the yield rate is high, and it is easy to scale up the technology to form stable industrial production.
[0041] Preferably, in step 1), the viscosity of the low-polarity organic material is controlled to be 10-100 mPa.s, which is beneficial to the subsequent induction of the movement of the inorganic microspheres.
[0042] Preferably, in step 2), the frequency of the ultrasonic wave is 40-60 kHz, and the radiating ultrasonic wave is continuously generated toward the adjusting layer slurry.
[0043] Preferably, in step 2), the surface of the glass fiber cloth is preheated to 50-60° C. before the slurry is applied, so that the surface of the glass fiber cloth has activation energy, which is beneficial for subsequent combination with the adjustment layer slurry and induces agglomeration of inorganic microspheres.
[0044] Preferably, the glass fiber cloth is firstly subjected to plasma cleaning before step 2), and the process parameters of the plasma cleaning are: nitrogen atmosphere, power 150-250W, and treatment time 3-10min.
[0045] Preferably, the specific operation of semi-curing is: using a standard medium-wave infrared heater with a power of 2000-2500W and irradiating with infrared rays with a radiation wavelength of 2-3 μm for 8-12 seconds, the slurry is in a semi-cured state.
[0046] Since there are a large number of open gaps (i.e., the windows) in the glass fiber cloth, the slurry will flow along the gaps to the bottom of the glass fiber cloth during the discharge process, and the matrix layer will be formed after semi-solidification. The glass fiber cloth can also be tensioned and controlled by the following traction mechanism so that the bottom of the glass fiber cloth does not contact the work surface, which is conducive to the flow and spreading of the slurry. A separate spreading process can also be set up.
[0047] The present invention also discloses a preparation device for producing the above-mentioned prepreg sheet suitable for high-frequency circuits, comprising a work surface, a feeding mechanism for quantitatively feeding the adjustment layer slurry to the glass fiber cloth, a coating scraper, an infrared heating mechanism, an infrared curing mechanism and a plurality of ultrasonic transducers;
[0048] A traction mechanism for pulling the glass fiber cloth forward in a certain direction is provided on the outer side of the work surface;
[0049] The infrared heating mechanism, the nozzle of the material discharging mechanism, the coating scraper, a plurality of ultrasonic transducers and the infrared curing mechanism are arranged in sequence along the advancing direction of the glass fiber cloth;
[0050] The nozzle of the material discharging mechanism, the coating scraper infrared heating mechanism and the infrared curing mechanism are arranged above the working table and operate in the direction of the working table;
[0051] The plurality of ultrasonic transducers are arranged below the working table, and the emission directions of the ultrasonic transducers are facing toward the working table.
[0052] Preferably, a pressure plate is provided between the coating scraper and the infrared curing mechanism, and the pressure plate is installed and fixed close to the coating scraper. The plurality of ultrasonic transducers located below the work surface are installed and arranged corresponding to the bottom of the pressure plate. The design of the pressure plate has a pressing and shaping effect on the top surface of the adjustment layer, which is beneficial for the adjustment layer to form a flat top surface.
[0053] Preferably, the pulling speed of the traction mechanism is 1-3 mm / s, the heating width of the infrared heating mechanism is 1-5 cm, and the width of the pressing plate is 5-10 cm.
[0054] The distance between the coating scraper and the work surface is adjustable to control the thickness of the finished product. Specifically, the distance between the coating scraper and the work surface can be fixed to two commonly used specifications of 3.94 mil and 5.90 mil, with a tolerance of 10%.
[0055] Based on the specific preparation method of the present invention, a preparation device is developed and designed, and multiple mechanisms and components are arranged and installed so that the multiple mechanisms and components form efficient synergy and can perform continuous production. The preparation device of the present invention has a streamlined structure and is easy to scale up in technology to form an industrial assembly line for mass production.
[0056] A core board (Core) suitable for high-frequency circuits comprises the above-mentioned prepreg sheet (PP), wherein copper foil is pressed on the upper and lower sides of the prepreg sheet.
[0057] The present invention also discloses a method for preparing a core board (Core), wherein the copper foils are pressed onto the upper and lower sides of the prepreg sheet and then sintered at a constant temperature of 250-300° C. to be completely cured to prepare the Core.
[0058] The invention also discloses a laminated circuit board, comprising the core board suitable for high-frequency circuits.
[0059] Preferably, the laminated circuit board includes at least 14 layers of laminated structure, which are set as L1 to L14, L1 is a signal layer (sig), L2 is a ground layer (GND), L3 is a signal layer, L4 is a ground layer, L5 is a signal layer, L6 is a ground layer, L7 is a signal layer, L8 is a signal layer, L9 is a ground layer, L10 is a signal layer, L11 is a ground layer, L12 is a signal layer, L13 is a ground layer, and L14 is a signal layer;
[0060] An insulating medium layer is provided between the layers. The core board is provided with two pieces, namely a first core board and a second core board. The copper foils on the upper and lower sides of the first core board are respectively used as the signal layer of L3 and the ground layer of L2. The copper foils on the upper and lower sides of the second core board are respectively used as the signal layer of L5 and the ground layer of L4. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 It is a schematic diagram of the structure of the prepreg sheet of the present invention;
[0062] Figure 2 It is a schematic diagram of reflection and diffraction of the distribution of inorganic microspheres induced by ultrasound of the present invention;
[0063] Figure 3 It is a schematic diagram of the process of preparing the prepreg sheet and core board of the present invention;
[0064] Figure 4 is a structural diagram of the glass fiber cloth involved in Examples 1 to 5;
[0065] Figure 5 It is a structural schematic diagram of the preparation device of the present invention;
[0066] Figure 6 This is a schematic diagram of the structure of the laminated structure obtained in Example 5.
[0067] Reference numerals
[0068] 1. Adjustment layer; 101. Microsphere blank area; 102. Microsphere dense area;
[0069] 2. Fiberglass cloth; 201. Empty window;
[0070] 3. Matrix layer;
[0071] 4. Infrared heating mechanism;
[0072] 5. Nozzle;
[0073] 6. Coating scraper;
[0074] 7. Press plate;
[0075] 8. Infrared curing mechanism;
[0076] 9. Work surface;
[0077] 10. Ultrasonic transducer. DETAILED DESCRIPTION
[0078] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0079] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0080] Reference Figure 5 The prepreg sheets of the following embodiments and comparative examples are produced by the preparation device, which includes a work surface, a feeding mechanism for quantitatively delivering the slurry to the NE-glass fiber cloth, a coating scraper, an infrared heating mechanism, an infrared curing mechanism and multiple ultrasonic transducers.
[0081] The outer side of the work surface is provided with a Figure 5 Traction mechanism moving forward in the direction of the arrow.
[0082] The infrared heating mechanism, the nozzle of the material discharging mechanism, the coating scraper, a plurality of ultrasonic transducers and the infrared curing mechanism are arranged in sequence along the forward direction of the NE-glass fiber cloth.
[0083] The infrared heating mechanism, the nozzle of the material discharging mechanism, the coating scraper and the infrared curing mechanism are arranged above the working table. The heating width of the infrared heating mechanism is 3 mm.
[0084] A pressing plate is provided between the coating scraper and the infrared curing mechanism, the pressing plate is fixedly installed close to the coating scraper and the bottom end is flush with the coating scraper, and the width of the pressing plate is 8 mm.
[0085] The plurality of ultrasonic transducers are disposed below the working table, the emission directions of the ultrasonic transducers are directed toward the working table, and the ultrasonic transducers are installed and arranged directly below the pressing plate.
[0086] The distance between the coating scraper and the work surface can be adjusted to control the thickness of the finished product. Specifically, the distance between the coating scraper and the work surface is set to 3.94 mil.
[0087] Example 1
[0088] Reference Figure 2 and Figure 3 , a method for preparing a prepreg sheet suitable for high-frequency circuits comprises the following steps:
[0089] 1) Surface modification of inorganic microspheres with silane coupling agent
[0090] The inorganic microspheres used in this embodiment are hollow glass microspheres (HGM, purity ≥99.9%), 4#DM30K-HGM of Shenzhen Dongyou New Material Technology Co., Ltd., with Dk of 1.4, average particle size of 7.8 microns, and ball wall thickness ≥1 / 5 ball radius.
[0091] 1-A) preparing an ethanol solution of a silane coupling agent KH550, wherein the mass concentration of the silane coupling agent is 0.13%, to obtain a modified solution;
[0092] 1-B) Inorganic microspheres and modified solution were mixed in a planetary mixer at a weight ratio of 30:100 at a rotation speed of 1600 r / min for 3 min;
[0093] 1-C) The uniformly dispersed material is placed in a constant temperature magnetic stirrer, immersed and modified at a constant temperature of 40° C. for 45 minutes, washed, and dried to obtain inorganic microspheres modified with a silane coupling agent.
[0094] 2) The viscosity of the low-polarity organic material PTFE (Dk is 2.1) is controlled to be 40 mPa.s, and the low-polarity organic material and the modified inorganic microspheres are mixed at a weight ratio of 10:1 and stirred evenly to obtain a slurry for standby use.
[0095] 3) NE-glass cloth plasma cleaning
[0096] Use NE-glass fiber cloth with a weaving specification of 1080 (such as Figure 4 As shown), Dk is 4.6, the wire harness of NE-glass fiber cloth is composed of round fibers, and the specific parameters are as follows:
[0097]
[0098] The process parameters of plasma cleaning are: nitrogen atmosphere, power 200W, and processing time 5min.
[0099] 4) The NE-glass fiber cloth is connected to the traction mechanism of the preparation device at a pulling speed of 1 mm / s. The surface of the NE-glass fiber cloth is preheated to 50° C. by the infrared heating mechanism.
[0100] 5) The preheated NE-glass fiber cloth passes through the nozzle of the discharge mechanism, and the nozzle conveys the slurry prepared in step 2) to the NE-glass fiber cloth. The slurry flows along the gap to the bottom of the NE-glass fiber cloth, and then passes through the coating scraper. The coating scraper is 3.94 mil away from the upper surface of the ultrasonic transducer. The coating scraper controls the slurry to be evenly spread on the surface of the NE-glass fiber cloth;
[0101] At the same time, an ultrasonic wave is provided below the NE-glass fiber cloth to be emitted upward in the Z direction to process the NE-glass fiber cloth, that is, the ultrasonic transducer generates radiating ultrasonic waves (such as Figure 2 The frequency is 40kHz.
[0102] 6) Curing
[0103] The NE-glass fiber cloth is pulled into the semi-curing station and is first irradiated with infrared light with a radiation wavelength of 2.5μm for 10s. The slurry is in a semi-cured state. The NE-glass fiber cloth forms an adjustment layer with a thickness of 2.5mil on the Z-upward side and a matrix layer with a thickness of 1.44mil on the lower side, thus obtaining a prepreg sheet with a thickness of 3.94mil suitable for high-frequency circuits.
[0104] The prepreg sheet prepared in this example is designated as "UT-1080PP".
[0105] Reference Figure 1 The prepreg sheet (UT-1080PP) suitable for high-frequency circuits prepared in this embodiment includes NE-glass fiber cloth, and the NE-glass fiber cloth includes staggered X-direction wire bundles and Y-direction wire bundles, and the gaps between the wire bundles form windows.
[0106] The NE-glass cloth covers and adheres the adjustment layer on the upper side in the Z direction, and the adjustment layer includes a low-polarity organic material (PTFE) and inorganic microspheres (HGM) filled in the low-polarity organic material; the NE-glass cloth covers and adheres the matrix layer on the lower side in the Z direction, and the matrix layer is filled with the same inorganic microspheres as the adjustment layer.
[0107] The inorganic microspheres of the adjustment layer are distributed in a density that gradually decreases along the Z direction toward the empty window until a microsphere blank area is formed above the empty window; the inorganic microspheres of the adjustment layer are distributed in a density that gradually increases along the Z direction toward the wire bundle until a microsphere dense area is formed above the wire bundle; the distribution of the inorganic microspheres in the area outside the microsphere blank area and the microsphere dense area tends to be uniform.
[0108] Example 2
[0109] A core board (Core) is prepared by laminating copper foil with a thickness of 0.69 mil on the upper and lower sides of the "UT-1080PP" prepared in Example 1, and sintering at a constant temperature of 280°C to completely solidify it, so as to obtain a core with a thickness of 5.90 mil.
[0110] The core board prepared in this embodiment is set as "UT-1080Core".
[0111] Comparative Example 1
[0112] Compared with Example 1, there is no ultrasonic treatment, and the other operations are the same. The obtained prepreg sheet is designated as "1080PP".
[0113] Comparative Example 2
[0114] Copper foil with a thickness of 0.69 mil was pressed onto the upper and lower sides of the "1080PP" prepared in Comparative Example 1, and sintered at a constant temperature of 280°C for complete curing, thereby obtaining a Core with a thickness of 5.90 mil, which was designated as "1080Core".
[0115] Example 3
[0116] Reference Figure 2 and Figure 3 , a method for preparing a prepreg sheet suitable for high-frequency circuits comprises the following steps:
[0117] 1) Surface modification of inorganic microspheres with silane coupling agent
[0118] The inorganic microspheres used in this embodiment are hollow glass microspheres (HGM, purity ≥99.9%), 4#DM30K-HGM from Shenzhen Dongyou New Material Technology Co., Ltd., with a Dk of 1.4, an average particle size of 13.8 microns, and a ball wall thickness ≥1 / 5 of the ball radius.
[0119] 1-A) preparing an ethanol solution of a silane coupling agent KH550, wherein the mass concentration of the silane coupling agent is 0.25%, to obtain a modified solution;
[0120] 1-B) Inorganic microspheres and modified solution were mixed in a planetary mixer at a weight ratio of 30:100 at a rotation speed of 1600 r / min for 3 min;
[0121] 1-C) The uniformly dispersed material is placed in a constant temperature magnetic stirrer, immersed and modified at a constant temperature of 40° C. for 45 minutes, washed, and dried to obtain inorganic microspheres modified with a silane coupling agent.
[0122] 2) The viscosity of the low-polarity organic material PTFE (Dk is 2.1) is controlled to be 70 mPa.s, and the low-polarity organic material and the modified inorganic microspheres are mixed at a weight ratio of 10:2 and stirred evenly to obtain a slurry for standby use.
[0123] 3) NE-glass cloth plasma cleaning
[0124] Use NE-glass fiber cloth with a weaving specification of 106 (such as Figure 4 As shown), Dk is 4.6, the wire harness of NE-glass fiber cloth is composed of round fibers, and the specific parameters are as follows:
[0125]
[0126] The process parameters of plasma cleaning are: nitrogen atmosphere, power 200w, and processing time 5min.
[0127] 4) The NE-glass fiber cloth is connected to the traction mechanism of the preparation device at a pulling speed of 2 mm / s. The surface of the NE-glass fiber cloth is preheated to 55° C. by the infrared heating mechanism.
[0128] 5) The preheated NE-glass fiber cloth passes through the nozzle of the discharge mechanism, and the nozzle conveys the slurry prepared in step 2) to the NE-glass fiber cloth. The slurry flows along the gap to the bottom of the NE-glass fiber cloth, and then passes through the coating scraper. The coating scraper is 3.94 mil away from the upper surface of the ultrasonic transducer. The coating scraper controls the slurry to be evenly spread on the surface of the NE-glass fiber cloth;
[0129] At the same time, an ultrasonic wave is provided below the NE-glass fiber cloth to be emitted upward in the Z direction to process the NE-glass fiber cloth, that is, the ultrasonic transducer generates radiating ultrasonic waves (such as Figure 2 As shown), the frequency is 50kHz.
[0130] 6) Curing
[0131] The NE-glass fiber cloth is pulled into the semi-curing station and is first irradiated with infrared light with a radiation wavelength of 2.5μm for 10s. The slurry is in a semi-cured state. The NE-glass fiber cloth forms an adjustment layer with a thickness of 2.5mil on the Z-upward side and a matrix layer with a thickness of 1.44mil on the lower side, thus obtaining a prepreg sheet with a thickness of 3.94mil suitable for high-frequency circuits.
[0132] The prepreg sheet prepared in this example is designated as "UT-106PP".
[0133] Reference Figure 1 The prepreg sheet (UT-106PP) suitable for high-frequency circuits prepared in this embodiment includes NE-glass fiber cloth, and the NE-glass fiber cloth includes staggered X-direction wire bundles and Y-direction wire bundles, and the gaps between the wire bundles form windows.
[0134] The NE-glass cloth covers and adheres the adjustment layer on the upper side in the Z direction, and the adjustment layer includes a low-polarity organic material (PTFE) and inorganic microspheres (HGM) filled in the low-polarity organic material; the NE-glass cloth covers and adheres the matrix layer on the lower side in the Z direction, and the matrix layer is filled with the same inorganic microspheres as the adjustment layer.
[0135] The inorganic microspheres of the adjustment layer are distributed in a density that gradually decreases along the Z direction toward the empty window until a microsphere blank area is formed above the empty window; the inorganic microspheres of the adjustment layer are distributed in a density that gradually increases along the Z direction toward the wire bundle until a microsphere dense area is formed above the wire bundle; the distribution of the inorganic microspheres in the area outside the microsphere blank area and the microsphere dense area tends to be uniform.
[0136] Example 4
[0137] A core board (Core) is prepared by laminating copper foil with a thickness of 0.69 mil on the upper and lower sides of the "UT-106PP" prepared in Example 3, and sintering at a constant temperature of 280°C to completely solidify it, so as to obtain a core with a thickness of 5.90 mil.
[0138] The core board prepared in this embodiment is set as "UT-106Core".
[0139] Comparative Example 3
[0140] Compared with Example 3, there is no ultrasonic treatment, and the other operations are the same. The obtained prepreg sheet is designated as "106PP".
[0141] Comparative Example 4
[0142] Copper foil with a thickness of 0.69 mil was pressed onto the upper and lower sides of the "106PP" prepared in comparative example 3, and sintered at a constant temperature of 280°C for complete solidification, thereby obtaining a core with a thickness of 5.90 mil, which was designated as "106Core".
[0143] Example 5
[0144] The preparation process of this embodiment involves NE-glass fiber cloth of the following specifications:
[0145]
[0146] A. Referring to the preparation method of Example 1, the NE-glass fiber cloth of specification 1080 was replaced with the NE-glass fiber cloth of specification 2216, without ultrasonic treatment, and the remaining operations were the same as those of Example 1 to produce "2216PP".
[0147] B. Referring to the preparation method of Example 1, the NE-glass fiber cloth of 1080 specification was replaced with the NE-glass fiber cloth of 3313 specification, without ultrasonic treatment, and the other operations were the same as those of Example 1 to prepare "3313PP";
[0148] Copper foil with a thickness of 0.69 mil was pressed on the upper and lower sides of 3313PP respectively, and sintered at a constant temperature of 280°C to fully solidify, thus obtaining a core with a thickness of 5.90, which was designated as "3313Core".
[0149] C. Referring to the preparation method of Example 1, the NE-glass fiber cloth of 1080 specification was replaced with the NE-glass fiber cloth of 2216 specification, without ultrasonic treatment, and the other operations were the same as those of Example 1 to prepare "2216PP";
[0150] Copper foil with a thickness of 0.69 mil was pressed on the upper and lower sides of 2216PP respectively, and sintered at a constant temperature of 280°C to fully solidify, thereby obtaining a core with a thickness of 5.90, which was designated as "2216Core".
[0151] D. After the PP and Core of the above steps A to C are prepared, the finished products of Examples 1 to 4 and Comparative Examples 1 to 4 are combined, and the Figure 6 For stacking, the differential trace spacing is 4 mil and the line width is 6 mil.
[0152] The laminated circuit board includes a 14-layer laminated structure, which is set as L1 to L14 from bottom to top, L1 is a signal layer (L1sig), L2 is a ground layer (L2 GND), L3 is a signal layer (L3 sig), L4 is a ground layer (L4 GND), L5 is a signal layer (L5sig), L6 is a ground layer (L6 GND), L7 is a signal layer (L7 sig), L8 is a signal layer (L8 sig), L9 is a ground layer (L9GND), L10 is a signal layer (L10 sig), L11 is a ground layer (L11 GND), L12 is a signal layer (L12 sig), L13 is a ground layer (L13 GND), and L14 is a signal layer (L14 sig), and the layer structure is made of copper foil with a thickness of 0.69 mil;
[0153] The copper foils on the upper and lower sides of the UT-1080Core prepared in Example 2 are used as the signal layer of L3 and the ground layer of L2 respectively;
[0154] The copper foils on the upper and lower sides of the UT-106Core prepared in Example 4 are used as the signal layer of L5 and the ground layer of L4 respectively;
[0155] The copper foils on the upper and lower sides of the 3313Core prepared in step B are used as the signal layer of L7 and the ground layer of L6 respectively;
[0156] The copper foils on the upper and lower sides of the 2216Core prepared in step C are used as the ground layer of L9 and the signal layer of L8 respectively;
[0157] The copper foils on the upper and lower sides of the 106Core prepared in Comparative Example 4 are used as the ground layer of L11 and the signal layer of L10 respectively;
[0158] The copper foils on the upper and lower sides of the 1080Core prepared in Comparative Example 2 are used as the ground layer of L13 and the signal layer of L12 respectively;
[0159] 1080PP prepared in Comparative Example 1 is sandwiched between L1 and L2, between L3 and L4, between L5 and L6, between L9 and L10, between L11 and L12, and between L13 and L14;
[0160] The 2216PP prepared in step A, the 1080PP prepared in comparative example 1 and the 2216PP prepared in step A are stacked in sequence from bottom to top between L7 and L8.
[0161] Performance Testing
[0162] Using a network analyzer (VNA), the loss data of differential stripline and single-ended microstrip line are tested using the Delta L method. The impedance and insertion loss parameters of different cores are obtained by testing the impedance values of single-ended and differential traces on the trace layer as shown in the following table:
[0163]
[0164] It can be seen that the effective Dk of the UT-1080Core and UT-106Core loops is significantly reduced after ultrasonic treatment, which in turn reduces impedance and insertion loss, and has a significant effect on signal transmission of high-frequency and high-speed devices.
[0165] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs may also change and modify the above implementation modes. Therefore, the present invention is not limited to the specific implementation modes disclosed and described above, and some modifications and changes to the present invention should also fall within the protection scope of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A prepreg sheet suitable for high-frequency circuits, comprising glass fiber cloth, wherein the glass fiber cloth comprises staggered X-direction wire bundles and Y-direction wire bundles, the gaps between the wire bundles form windows, and the glass fiber cloth is covered and adhered with an adjustment layer on at least one side in the Z direction, wherein the adjustment layer is filled with inorganic microspheres; The inorganic microspheres of the adjustment layer are distributed in a density that gradually decreases toward the empty window along the Z direction, and the inorganic microspheres of the adjustment layer are distributed in a density that gradually increases toward the wire bundle along the Z direction.
2. The prepreg sheet according to claim 1, characterized in that The inorganic microspheres of the adjustment layer are distributed in a density gradually decreasing along the Z direction toward the empty window until a microsphere blank area is formed above the empty window; The inorganic microspheres of the adjustment layer are distributed in a density that gradually increases toward the wire bundle along the Z direction until a microsphere-dense area is formed above the wire bundle; The inorganic microspheres are distributed evenly in areas other than the microsphere blank area and the microsphere dense area.
3. The prepreg sheet according to claim 1 or 2, characterized in that: The adjustment layer includes a low-polarity organic material and inorganic microspheres filled in the low-polarity organic material; The weight ratio of the low-polarity organic material to the inorganic microspheres is 10:1-3; The inorganic microspheres are hollow silica microspheres or hollow glass microspheres, the particle size of the hollow silica microspheres or hollow glass microspheres is 3 to 20 microns, and the wall thickness of the hollow silica microspheres or hollow glass microspheres is ≥ 1 / 5 of the ball radius; The hollow silica microspheres or hollow glass microspheres are surface-modified by a silane coupling agent.
4. The prepreg sheet according to claim 1 or 2, characterized in that: The glass fiber cloth covers and adheres the adjustment layer on the upper side in the Z direction, the thickness of the adjustment layer is 2 to 4 mils, and covers and adheres the matrix layer on the lower side, the thickness of the matrix layer is 1 to 2 mils, and the matrix layer is filled with inorganic microspheres; The weaving specification of the glass fiber cloth adopts a weaving specification of glass fiber cloth with a warp and weft gap of ≥1080.
5. A method for preparing a prepreg sheet suitable for high-frequency circuits, characterized in that: The following steps are involved: 1) low polarity organic material and inorganic microspheres are mixed in a weight ratio of 10:1-3, stirred evenly, and a slurry is prepared for standby use; 2) Preheating the glass fiber cloth, then evenly spreading the slurry on the surface of the glass fiber cloth, and at the same time, arranging an ultrasonic wave emitting upward in the Z direction under the glass fiber cloth to treat it, and finally semi-curing it to obtain a prepreg sheet suitable for high-frequency circuits.
6. The preparation method according to claim 5, characterized in that: In step 1), the viscosity of the low-polarity organic material is controlled to be 10 to 100 mPa.s; The glass fiber cloth is firstly plasma cleaned before step 2), and the process parameters of the plasma cleaning are: nitrogen atmosphere, power 150-250w, and treatment time 3-10min.
7. The preparation method according to claim 5 or 6, characterized in that: In step 2), The surface of the glass fiber cloth is preheated to 50-60° C. before the slurry is applied; The frequency of the ultrasonic wave is 40 to 60 kHz, and the radiant ultrasonic wave is continuously generated to the adjusting layer slurry; The specific operation of semi-curing is: use a standard medium-wave infrared heater with a power of 2000-2500W and irradiate with infrared light of a radiation wavelength of 2-3μm for 8-12s.
8. A device for preparing a prepreg sheet suitable for high-frequency circuits, used for preparing the prepreg sheet suitable for high-frequency circuits according to any one of claims 1 to 4, characterized in that: It includes a working table, a feeding mechanism for quantitatively feeding the adjustment layer slurry to the glass fiber cloth, a coating scraper, an infrared heating mechanism, an infrared curing mechanism and a plurality of ultrasonic transducers; A traction mechanism for pulling the glass fiber cloth forward in a certain direction is provided on the outer side of the work surface; The infrared heating mechanism, the nozzle of the material discharging mechanism, the coating scraper, a plurality of ultrasonic transducers and the infrared curing mechanism are arranged in sequence along the advancing direction of the glass fiber cloth; The nozzle of the material discharging mechanism, the coating scraper infrared heating mechanism and the infrared curing mechanism are arranged above the working table and operate in the direction of the working table; The plurality of ultrasonic transducers are arranged below the working table, and the emission directions of the ultrasonic transducers are facing toward the working table.
9. A core board suitable for high-frequency circuits, characterized in that: A prepreg sheet suitable for high-frequency circuits according to any one of claims 1 to 4; The core board is made by pressing copper foils on the upper and lower sides of the prepreg sheet and then sintering at a constant temperature of 250-300° C. to fully solidify it.
10. A laminated circuit board, characterized in that: The core board suitable for high-frequency circuits comprises the core board as claimed in claim 9.
Citation Information
Patent Citations
PCB with differential lines, manufacturing method and electronic equipment
CN112040637A