Silicone rubber material and preparation method thereof

The silicone rubber material with aerogel and reinforcing fillers addresses noise reduction and mechanical strength issues by converting sound energy into heat and reinforcing structural integrity.

CN119081414APending Publication Date: 2024-12-06GOERTEK INC
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411215055.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Current silicone rubber materials suffer from poor noise reduction effects due to reduced mechanical properties and filler compatibility issues, such as increased density, hardness, and microsphere breakage, leading to inadequate sound insulation and damping performance.

Method used

A silicone rubber material comprising 100-200 parts of methyl vinyl silicone rubber base, 2-20 parts of aerogel noise reduction filler, 2-40 parts of reinforcing filler, 3-5 parts of hydrogenated silicone oil, and 0.05-1 part of inhibitor, with aerogel fillers having a nanoporous structure to dissipate sound energy and reinforcing fillers enhancing mechanical strength.

Benefits of technology

The material achieves improved noise reduction and mechanical damping performance by incorporating aerogel fillers that convert sound energy into heat energy and reinforcing fillers that enhance structural integrity, addressing the noise reduction and mechanical damping performance issues, enhancing the noise reduction and mechanical damping performance issues, and improving the material's sound insulation and structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081414A_ABST
    Figure CN119081414A_ABST
Patent Text Reader

Abstract

The invention discloses a silicone rubber material and a preparation method thereof, and belongs to the technical field of organic polymer materials, and the silicone rubber material comprises the following components in parts by mass: 100-200 parts of methyl vinyl silicone rubber-based rubber, 2-20 parts of an aerogel noise reduction filler, 2-40 parts of a reinforcing filler, 3-5 parts of hydrogen-containing silicone oil, 0.05-5 parts of a catalyst, and 0.05-1 part of an inhibitor. The noise reduction effect of the silicone rubber material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic polymer materials, and in particular to a silicone rubber material and a preparation method thereof. Background Art

[0002] The rapid development of science and technology has brought about rapid changes in people's lives, but it has also brought about factors that harm the social environment and human health, such as noise, water and air pollution. In particular, noise pollution not only causes serious damage to human hearing system, sleep, communication, physiology and psychology, work and life, but also has a significant impact on the aging speed, service life and accuracy of mechanical structures, buildings, instruments and meters.

[0003] As a viscoelastic polymer damping material, silicone rubber has the characteristics of viscous liquid dissipating energy under certain motion conditions and elastic solid storing energy. It has high damping and certain noise reduction effects. However, at present, foamed silicone usually forms a porous structure by physical foaming, chemical foaming, and hollow microsphere filling. Among them, the physical foaming and chemical foaming methods, the mechanical properties of the foamed silicone will be significantly reduced compared with the vulcanized silicone rubber in the unfoamed state due to the existence of internal pores, especially the tensile strength and tear strength. The hollow microsphere filling method mainly includes inorganic microspheres and organic polymer microspheres. The inorganic microspheres are mainly hollow glass microspheres, which have certain noise reduction and sound insulation effects, but will increase the density and hardness of the silicone, reduce the elongation at break, and have a certain microsphere breakage rate after silicone injection molding, resulting in a significant reduction in the noise reduction effect. The main disadvantage of organic polymer microsphere filling is that the microspheres have low strength and are deformed or damaged by heat, resulting in the noise reduction effect of the silicone after molding not reaching the theoretical value. Filled foamed silicone is affected by the dispersibility and compatibility of the filler. Stratification, sedimentation or agglomeration may occur in the silicone, which will also affect the noise reduction effect of the silicone after molding. The noise reduction effect of the current silicone rubber material still needs to be improved. Summary of the invention

[0004] The main purpose of the present invention is to provide a silicone rubber material and a preparation method thereof, aiming to solve the technical problem that the current silicone rubber material has a poor noise reduction effect.

[0005] To achieve the above-mentioned purpose, the present invention provides a silicone rubber material, which comprises, by weight, 100-200 parts of methyl vinyl silicone rubber base, 2-20 parts of aerogel noise reduction filler, 2-40 parts of reinforcing filler, 3-5 parts of hydrogenated silicone oil, 0.05-5 parts of catalyst, and 0.05-1 part of inhibitor.

[0006] In one embodiment, the aerogel noise reduction filler includes at least one of silica aerogel powder, alumina aerogel powder, graphene aerogel powder, and all-carbon aerogel powder.

[0007] In one embodiment, the particle size of the aerogel noise reduction filler is 10-100 μm.

[0008] In one embodiment, the viscosity of the methyl vinyl silicone rubber base is 10-10000 mPa·s.

[0009] In one embodiment, the reinforcing filler includes fumed silica and / or precipitated silica;

[0010] and / or, the catalyst comprises a platinum catalyst;

[0011] And / or, the inhibitor comprises an acetylenic alcohol inhibitor.

[0012] In addition, to achieve the above object, the present invention also provides a method for preparing a silicone rubber material, which is used to prepare the silicone rubber material as described above, and the method for preparing the silicone rubber material comprises:

[0013] Preparation of aerogel noise reduction filler;

[0014] Take appropriate amounts of methyl vinyl silicone rubber base, aerogel noise reduction filler, reinforcing filler and catalyst and mix them evenly to prepare component A;

[0015] Take appropriate amounts of methyl vinyl silicone rubber base, aerogel noise reduction filler, reinforcing filler, hydrogen-containing silicone oil and inhibitor and mix them evenly to prepare component B;

[0016] The component A and the component B are mixed and molded to obtain a silicone rubber material.

[0017] In one embodiment, the step of preparing the aerogel noise reduction filler comprises:

[0018] crushing the aerogel raw material into particles to obtain aerogel particles;

[0019] The aerogel particles are treated with a silane coupling agent, dried, crushed, and sieved to obtain noise reduction filler powder;

[0020] The noise reduction filler powder is added into cyclosiloxane and stirred to obtain an aerogel noise reduction filler.

[0021] In one embodiment, the cyclosiloxane includes at least one of hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, and dodecamethylcyclohexasiloxane.

[0022] In one embodiment, the silane coupling agent includes a vinyl group, an epoxy group or a methacryloxy group.

[0023] In one embodiment, the molding comprises thermoforming or injection molding.

[0024] The silicone rubber material provided by the present invention includes, by mass, 100-200 parts of methyl vinyl silicone rubber base, 2-20 parts of aerogel noise reduction filler, 2-40 parts of reinforcing filler, 3-5 parts of hydrogen-containing silicone oil, 0.05-5 parts of catalyst, and 0.05-1 part of inhibitor. The aerogel noise reduction filler contains aerogel, and the aerogel has a nanoporous network structure formed by many pores inside, and a nano-skeleton composed of nano-scale colloidal particles aggregated together. The pores of the aerogel are filled with gaseous dispersion medium. When sound waves propagate to the interface of the aerogel noise reduction filler, the gas molecules in the pores vibrate and dissipate part of the energy of the sound waves. The gas molecules close to the pore wall are not easy to move due to friction and viscosity, so that part of the sound energy is converted into heat energy, and heat exchange is carried out with other components through the nano-skeleton to consume sound energy, thereby improving the noise reduction effect. The silicone rubber material also includes reinforcing fillers, which can make up for the decrease in tear strength caused by the formation of pores in the silicone rubber by the aerogel noise reduction filler, and meet the use requirements of the silicone rubber material in different environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present drawings or related technologies, the drawings required for use in the embodiments or related technical descriptions will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present drawings. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.

[0026] Figure 1 Schematic diagram of the process of preparing the silicone rubber material according to an embodiment of the present invention;

[0027] Figure 2 A schematic diagram of a brief process for preparing an aerogel noise reduction filler according to an embodiment of the present invention;

[0028] Figure 3 The attenuation test results of Examples 1-3 of the present invention and the comparative example are shown in FIG.

[0029] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0030] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0031] Hereinafter, the silicone rubber material and the method for preparing the same of the present invention are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the accompanying drawings and the following description are provided for those skilled in the art to fully understand the present invention and are not intended to limit the subject matter described in the claims.

[0032] "Scope" disclosed in the present invention is defined in the form of lower limit and upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a particular range. The scope defined in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a particular parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3,4 and 5 are listed, the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present invention, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0033] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the technical solutions of the present invention are further described below in conjunction with the accompanying drawings and embodiments. However, the present invention is not limited to the embodiments listed, and should also include any other known changes within the scope of the rights claimed by the present invention.

[0034] Liquid silicone rubber (LSR) has excellent electrical insulation properties and aging resistance, high mechanical strength, high temperature resistance, skin-friendliness, and softness, so it has been widely used. Compared with plastic materials, silicone rubber, as a viscoelastic polymer damping material, has the characteristics of viscous liquid dissipating energy under a certain state of motion and elastic solid storing energy. It has higher damping and a certain noise reduction effect.

[0035] By foaming silicone rubber to form a porous structure, silicone rubber can have good heat insulation, sound insulation and high impact resistance. When sound waves reach the interface of porous sound-absorbing materials, the air molecules in the pores of the material vibrate and dissipate energy. In addition, the air close to the pore wall is not easy to move due to friction and viscosity, so part of the sound energy is converted into heat energy and heat exchange with the material, thereby consuming the sound energy.

[0036] At present, foamed silica gel is usually formed into a porous structure by physical foaming, chemical foaming, and hollow microsphere filling. Among them, the physical foaming and chemical foaming methods, the mechanical properties of the foamed silica gel will be significantly reduced compared with the vulcanized silicone rubber in the unfoamed state due to the existence of internal pores, especially the tensile strength and tear strength will be significantly reduced. The hollow microsphere filling method mainly includes inorganic microspheres and organic polymer microspheres. The inorganic microspheres are mainly hollow glass microspheres, which have a certain noise reduction and sound insulation effect, but will increase the density and hardness of the silica gel, reduce the elongation at break, and have a certain microsphere breakage rate after silica gel injection molding, resulting in a significant reduction in the noise reduction effect. The main disadvantage of organic polymer microsphere filling is that the microspheres have low strength and are deformed or damaged by heat, resulting in the noise reduction effect of the silica gel after molding not reaching the theoretical value. The filled foamed silica gel is affected by the dispersibility and compatibility of the filler, and stratification, sedimentation or agglomeration may occur in the silica gel, which will also affect the noise reduction effect of the silica gel after molding.

[0037] Based on this, an embodiment of the present invention provides a silicone rubber material, which includes, by mass, 100-200 parts of methyl vinyl silicone rubber base, 2-20 parts of aerogel noise reduction filler, 2-40 parts of reinforcing filler, 3-5 parts of catalyst, 3-5 parts of hydrogenated silicone oil, and 0.05-1 part of inhibitor.

[0038] Methyl vinyl silicone rubber base is a substance formed by copolymerization of dimethyl siloxane and a small amount of vinyl siloxane. The introduction of a small amount of vinyl can improve the heat aging resistance and high temperature compression deformation resistance of silicone rubber materials. In this embodiment, the mass fraction of methyl vinyl silicone rubber base is 100-200 parts, for example, 100 parts, 110 parts, 120 parts, 130 parts, 140 parts, 150 parts, 160 parts, 170 parts, 180 parts, 190 parts, 200 parts, etc. Methyl vinyl silicone rubber base is the basic substance for forming silicone rubber materials and affects the basic properties of silicone rubber materials.

[0039] Optionally, the viscosity of the methyl vinyl silicone rubber base is 10-10000mPa·s, for example, 10mPa·s, 100mPa·s, 500mPa·s, 1000mPa·s, 5000mPa·s, 8000mPa·s, 10000mPa·s, etc. The viscosity of the methyl vinyl silicone rubber base is low, the resistance that needs to be overcome during processing is small, the processing difficulty is small, the strength and hardness are low, but the texture is soft. The viscosity of the methyl vinyl silicone rubber base is high, the resistance that needs to be overcome during processing is large, the processing difficulty is large, the hardness is high, but the mechanical strength is high. According to the different application scenarios of the silicone rubber material, a methyl vinyl silicone rubber base with an appropriate viscosity can be selected to prepare different silicone rubber products.

[0040] Aerogel noise reduction material refers to an aerogel material used to enhance the noise reduction effect of silicone rubber. Aerogels are usually prepared by the sol-gel method, and a certain drying method is used to replace the liquid phase in the gel with gas to form a nanoporous structure. It can be understood that according to the noise reduction mechanism of different types of materials, noise reduction materials can be divided into damping materials, sound absorbing materials, and sound insulation materials. The principle of noise reduction of the silicone rubber material in this embodiment can be attributed to the sound absorption mechanism. When sound waves enter the porous structure of the aerogel, reflection and scattering will occur between the pores, and losses will occur and be converted into heat energy. The propagation of sound waves drives the gas molecules in the pores to rub against the pore walls, and the energy of the sound waves is lost, resulting in a sound absorption effect. The pores of aerogel are filled with gaseous dispersion medium. This special structure makes aerogel have extremely high porosity, extremely low density, extremely high specific surface area, ultra-high pore volume rate, high temperature resistance, high elasticity, strong adsorption, catalysis and other characteristics. Its nano-scale porous structure can have excellent sound absorption effect. The aerogel powder treated with silane coupling agent can form a chemical bond with silicone rubber and has good dispersibility.

[0041] In this embodiment, the mass fraction of aerogel noise reduction filler is 2-20 parts, for example, 2 parts, 5 parts, 8 parts, 10 parts, 13 parts, 15 parts, 18 parts, 20 parts, etc. The amount of aerogel noise reduction filler added will affect the noise reduction performance of the silicone rubber material. If the amount added is too little, it cannot play a sufficient noise reduction role. If the amount added is too much, it is easy to cause the filler particles to agglomerate, affecting the mechanical properties of the silicone rubber material. Controlling the mass fraction of aerogel noise reduction filler within the above range can not only improve the noise reduction effect of the silicone rubber material, but also will not affect the performance of the silicone rubber due to the decrease in the mechanical properties of the silicone rubber.

[0042] Optionally, the aerogel noise reduction filler includes at least one of silica aerogel powder, alumina aerogel powder, graphene aerogel powder, and all-carbon aerogel powder. The above-mentioned aerogel noise reduction fillers all have a nanoporous structure, which can play a role in improving the noise reduction effect. The above-mentioned aerogel powder is subjected to a certain treatment to obtain an aerogel noise reduction filler, which can form a chemical bond between the aerogel powder and the silicone rubber, thereby improving the dispersion effect of the aerogel powder.

[0043] Optionally, the particle size of the aerogel noise reduction filler is 10-100 μm, for example, 10 μm, 30 μm, 50 μm, 70 μm, 90 μm, 100 μm, etc. It is understandable that the particle size of the aerogel noise reduction filler will affect the strength and other mechanical properties of the silicone rubber material. The larger the particle size of the aerogel noise reduction filler, the worse the continuity of the composition of the silicone rubber material, resulting in a decrease in the strength of the silicone rubber material. A particle size that is too small is difficult to achieve during the preparation process, that is, the preparation is difficult. Aerogel noise reduction fillers of different particle sizes can be obtained by screening through sieves of different mesh sizes.

[0044] Reinforcing filler is a filler used to improve the strength performance of silicone rubber materials. In this embodiment, the mass fraction of reinforcing filler is 2-40 parts, for example, 2 parts, 5 parts, 10 parts, 20 parts, 30 parts, 35 parts, 40 parts, etc. It can be understood that the reinforcing filler can fill the gaps in the silicone rubber matrix, increase the density of silicone rubber, improve the hardness and tensile strength of silicone rubber, and the reinforcing filler and the silicone rubber matrix can also form an interface interaction to improve the mechanical strength of the silicon phase. If the amount of reinforcing filler added is too little, it will not play a role in improving the strength performance. If the amount added is too much, the dispersion of the reinforcing filler is difficult, and agglomeration may occur, affecting the noise reduction effect of silicone rubber.

[0045] Optionally, the reinforcing filler includes fumed silica and / or precipitated silica. The average particle size of fumed silica is small, the average diameter of primary particles is 7-40nm, the specific surface area is large, and its internal structure is almost a completely tightly arranged three-dimensional structure, so it has low hygroscopicity, strong adsorption of particle surface, and strong reinforcing effect. Silicone rubber products added with fumed silica have good transparency, good mechanical properties, electrical properties, and heat resistance. Due to the influence of the molecular structure of the raw material sodium silicate, precipitated silica has more two-dimensional structures, its structure is loose, the molecular density is low, and there are many capillary structures in the aggregated state, which is easy to absorb moisture, affecting the reinforcement effect, but its resilience, compression set and processing performance are good. Different reinforcing fillers can be selected according to the different use requirements of silicone rubber materials.

[0046] The Si-H bonds in the hydrogen-containing silicone oil can undergo cross-linking reactions with other functional groups in silicone rubber, thereby forming a cross-linked structure between the silicone rubber molecular chains. This cross-linked structure can not only enhance the mechanical properties of silicone rubber, but also improve its heat resistance and weather resistance. In this embodiment, the mass fraction of the hydrogen-containing silicone oil is 3-5 parts, for example, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, etc. If the amount of hydrogen-containing silicone oil added is too little, it may cause incomplete cross-linking of the silicone rubber. If the amount of hydrogen-containing silicone oil added is too much, excessive cross-linking may occur. Optionally, the hydrogen content of the hydrogen-containing silicone oil is 0.5-1.5wt%.

[0047] The catalyst is used to promote the cross-linking of silicone rubber. The mass fraction of the catalyst in this embodiment is 0.05-5 parts, for example, 0.05 parts, 0.1 parts, 1 parts, 2 parts, 3 parts, 4 parts, 4.5 parts, 5 parts, etc. It is understandable that too little catalyst may lead to incomplete cross-linking, and too much catalyst may cause too fast reaction, which is difficult to control, or produce oversulfurization, resulting in a decrease in the performance of silicone rubber. Optionally, the catalyst of this embodiment includes a platinum catalyst. The platinum catalyst contains a platinum complex, such as a platinum-vinylsiloxane complex, which has good compatibility in silicone rubber and good storage stability.

[0048] The inhibitor is used to improve the stability of silicone rubber in a high temperature environment and to prevent the silicone rubber base from curing too quickly. The mass fraction of the inhibitor in this embodiment is 0.05-1 part, for example, 0.05 part, 0.1 part, 0.3 part, 0.5 part, 0.8 part, 1 part, etc. It is understandable that in the process of preparing the silicone rubber material, the inhibitor and the catalyst are added separately to prevent the silicone rubber base from directly curing. If the amount of the inhibitor added is too little, the inhibitory effect is not obvious, and if the amount added is too much, the mechanical properties and heat resistance of the silicone rubber will be reduced. Optionally, the inhibitor includes an acetylene alcohol inhibitor. The inhibitory effect of the acetylene alcohol inhibitor is strong. The acetylene alcohol inhibitors that can be used in this embodiment include ethynyl cyclopentanol, methyl butynol, methyl pentynol, etc.

[0049] The aerogel noise reduction filler of the present embodiment includes aerogel, and the interior of the aerogel has a nanoporous network structure formed by many pores, and a nano-skeleton composed of nano-scale colloidal particles aggregated together. The pores of the aerogel are filled with a gaseous dispersion medium. When sound waves propagate to the interface of the aerogel noise reduction filler, the gas molecules in the pores vibrate and dissipate part of the energy of the sound waves. The gas molecules close to the pore walls are not easy to move due to friction and viscosity, so that part of the sound energy is converted into heat energy, and heat exchange is carried out with other components through the nano-skeleton to consume sound energy, thereby improving the noise reduction effect. The silicone rubber material also includes a reinforcing filler, which can make up for the decrease in tear strength caused by the formation of pores in the silicone rubber by the aerogel noise reduction filler, and adapt to the use requirements of the silicone rubber material in different environments.

[0050] The present invention also provides a method for preparing a silicone rubber material. Figure 1 , Figure 1 The figure is a schematic flow chart of a method for preparing a silicone rubber material according to the present embodiment.

[0051] In this embodiment, the preparation method of the silicone rubber material includes:

[0052] Step S10, preparing aerogel noise reduction filler;

[0053] It is understandable that the main component of the aerogel noise reduction filler is aerogel powder. After the aerogel raw material is processed into aerogel powder, surface treatment is performed so that the aerogel powder can be chemically combined with the silicone rubber.

[0054] Figure 2 A brief flow chart of the preparation of aerogel noise reduction filler in this embodiment is shown in FIG. Figure 2 As shown, in the process of preparing aerogel noise reduction filler, the aerogel raw material is first crushed into particles to obtain aerogel particles; the aerogel particles are treated with a silane coupling agent, dried, crushed, and sieved to obtain noise reduction filler powder; the noise reduction filler powder is added to cyclosiloxane and stirred to obtain aerogel noise reduction filler.

[0055] It is understandable that the aerogel raw material can be commercially available block or sheet aerogel, and the commercially available sheet or block aerogel is crushed into particles by physical grinding to obtain aerogel particles. The crushed aerogel particles are treated with a silane coupling agent, dried, and physically crushed into finer particles by ball milling. Different mesh sieves are used to sieve to obtain noise reduction filler powders of different particle sizes, and the powders are added to cyclosiloxane, mechanically stirred to a paste, and aerogel noise reduction filler is obtained. The mesh size of the sieve can include 40 mesh, 200 mesh, 300 mesh, 500 mesh, and 1000 mesh. After sieving, noise reduction filler powder with a particle size of 10-100 μm can be obtained.

[0056] Optionally, the silane coupling agent includes a vinyl group, an epoxy group or a methacryloxy group. The silane coupling agent can be represented by the general formula Y(CH2): n SiX3 represents that the Y end is a vinyl, epoxy, or methacryloxy structure. The vinyl, epoxy, or methacryloxy groups in the silane coupling agent can react with the functional groups in the silicone rubber base to produce chemical bonding.

[0057] Optionally, the cyclosiloxane includes at least one of hexamethylcyclotrisiloxane (D3), octamethylcyclotetrasiloxane (D4), and dodecamethylcyclohexasiloxane (D6). It is understood that the cyclosiloxane can be used as an intermediate for preparing silicone rubber, and further prepare silicone rubber materials with good noise reduction effect.

[0058] Step S20, taking appropriate amounts of methyl vinyl silicone rubber base, aerogel noise reduction filler, reinforcing filler, and catalyst and mixing them evenly to prepare component A;

[0059] It is understandable that using the inhibitor and the catalyst as different components can ensure the storage stability of the two components and prevent the silicone rubber base and other substances from reacting too quickly. According to the composition of the above silicone rubber material, the methyl vinyl silicone rubber base, aerogel noise reduction filler, and reinforcing filler in the total content can be distributed according to a certain proportion, and the catalyst can be added, mixed evenly, and vacuum degassed to obtain component A.

[0060] Step S30, taking appropriate amounts of methyl vinyl silicone rubber base, aerogel noise reduction filler, reinforcing filler, hydrogen-containing silicone oil, and inhibitor and mixing them evenly to prepare component B;

[0061] According to the composition of the silicone rubber material, the methyl vinyl silicone rubber base, aerogel noise reduction filler and reinforcing filler in the total content except component A can be distributed into component B, and hydrogen-containing silicone oil and inhibitor are added and mixed to obtain component B.

[0062] Step S40, mixing the component A and the component B, and molding them to obtain a silicone rubber material.

[0063] It is understandable that the ratio between component A and component B can be 1:1, and the mixed raw materials are prepared by hot pressing or injection molding to obtain the final silicone rubber material.

[0064] In this embodiment, aerogel raw materials are processed to prepare aerogel noise reduction filler, and a chemical bond is formed between aerogel powder and silicone rubber, which is helpful for the dispersion of aerogel powder and the improvement of the strength of silicone rubber material. The prepared silicone rubber material contains a nanoporous structure. When sound waves propagate to the interface of the aerogel noise reduction filler, the gas molecules in the pores vibrate and dissipate part of the energy of the sound waves, while the gas molecules close to the pore walls are not easy to move due to friction and viscosity, so that part of the sound energy is converted into heat energy, and heat exchange is carried out with other components through the nano-skeleton to consume sound energy, thereby improving the noise reduction effect. The silicone rubber material also includes reinforcing fillers, which can make up for the decrease in tear strength caused by the formation of pores in the silicone rubber by the aerogel noise reduction filler, and adapt to the use requirements of silicone rubber materials in different environments.

[0065] The present invention is described in detail below with reference to specific embodiments.

[0066] Example 1

[0067] The commercially available block silica aerogel is crushed into particles by physical grinding. The crushed silica aerogel particles are treated with KH560 silane coupling agent, dried, ball milled for 30 minutes, and sieved with a 300-mesh sieve to obtain silica aerogel powder. The silica aerogel powder is added to octamethylcyclotetrasiloxane (D4) and mechanically stirred for 10 minutes until it becomes a paste.

[0068] Component A includes the following raw materials, by mass: 100 parts of methyl vinyl silicone rubber base (viscosity 400 mPa·s), 4 parts of fumed silica, 5 parts of 300 mesh silica aerogel paste, and 0.1 parts of platinum catalyst;

[0069] Component B includes the following raw materials: 100 parts of methyl vinyl silicone rubber base (viscosity 400 mPa·s), 10 parts of fumed silica, 5 parts of 300 mesh silica aerogel paste, 3 parts of hydrogenated silicone oil, and 0.05 parts of inhibitor.

[0070] Example 2

[0071] The commercially available block silica aerogel was crushed into particles by physical grinding. The crushed silica aerogel particles were treated with KH560 silane coupling agent, dried, ball milled for 30 minutes, and sieved with a 500-mesh sieve to obtain silica aerogel powder. The silica aerogel powder was added to octamethylcyclotetrasiloxane (D4) and mechanically stirred for 10 minutes until it became a paste.

[0072] Component A includes the following raw materials, by mass: 100 parts of methyl vinyl silicone rubber base (viscosity 400 mPa·s), 4 parts of fumed silica, 5 parts of 500 mesh silica aerogel paste, and 0.1 parts of platinum catalyst;

[0073] Component B includes the following raw materials: 100 parts of methyl vinyl silicone rubber base (viscosity 400 mPa·s), 10 parts of fumed silica, 5 parts of 500 mesh silica aerogel paste, 3 parts of hydrogenated silicone oil, and 0.05 parts of inhibitor.

[0074] Example 3

[0075] The commercially available block alumina aerogel was crushed into particles by physical grinding. The crushed alumina aerogel particles were treated with KH560 silane coupling agent, dried, ball milled for 50 minutes, and sieved with a 500-mesh sieve to obtain alumina aerogel powder. The alumina aerogel powder was added to octamethylcyclotetrasiloxane (D4) and mechanically stirred for 20 minutes until it became a paste.

[0076] Component A includes the following raw materials, by mass: 100 parts of methyl vinyl silicone rubber base (viscosity 400 mPa·s), 2 parts of fumed silica, 5 parts of 500 mesh alumina aerogel paste, and 0.1 parts of platinum catalyst;

[0077] Component B includes the following raw materials: 100 parts of methyl vinyl silicone rubber base (viscosity 400 mPa·s), 8 parts of fumed silica, 5 parts of 500 mesh alumina aerogel paste, 3 parts of hydrogenated silicone oil, and 0.05 parts of inhibitor.

[0078] Comparative Example

[0079] Component A includes the following raw materials in parts by mass: 100 parts of methyl vinyl silicone rubber base (viscosity 400 mPa·s), 4 parts of fumed silica, and 0.1 parts of platinum catalyst;

[0080] Component B includes the following raw materials: 100 parts of methyl vinyl silicone rubber base (viscosity 400 mPa·s), 10 parts of fumed silica, 3 parts of hydrogenated silicone oil, and 0.05 parts of inhibitor.

[0081] The above comparative examples and embodiments 1-3 are all mixed in a ratio of 1:1 between component A and component B, and are formed into in-ear earplugs by hot pressing. The earplugs after forming are tested by a special acoustic test device method (ATF) and with reference to the ETSI TS103 640 test mark. The attenuation test results are shown in Table 1 and Figure 3 . Figure 3 The horizontal axis is the frequency (in Hz), and the vertical axis is the attenuation (in dB). Figure 3 The curves in FIG. 1 show the attenuation variation trends of various embodiments or comparative examples at different frequencies.

[0082] Table 1

[0083] 2000Hz 3000Hz 3750Hz 4000Hz 8000Hz 20000Hz Comparative Example 23 32 32 29 24 35 Example 1 24 36 43 40 27 42 Example 2 25 36 41 38 28 40 Example 3 25 34 40 38 28 40

[0084] Combined with Table 1 and Figure 3 It can be seen that the earplugs molded in Examples 1-3 with added aerogel noise reduction fillers have a greater attenuation than the comparative example in the frequency range of 2000 Hz to 20000 Hz, that is, the noise reduction effect is significantly improved.

[0085] The serial numbers of the above embodiments of the present invention are for description only and do not represent the advantages or disadvantages of the embodiments.

[0086] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A silicone rubber material, characterized in that: Calculated by mass, the silicone rubber material includes 100-200 parts of methyl vinyl silicone rubber base, 2-20 parts of aerogel noise reduction filler, 2-40 parts of reinforcing filler, 3-5 parts of hydrogenated silicone oil, 0.05-5 parts of catalyst, and 0.05-1 part of inhibitor.

2. The silicone rubber material according to claim 1, characterized in that: The aerogel noise reduction filler includes at least one of silica aerogel powder, alumina aerogel powder, graphene aerogel powder and all-carbon aerogel powder.

3. The silicone rubber material according to claim 1, characterized in that: The particle size of the aerogel noise reduction filler is 10-100 μm.

4. The silicone rubber material according to claim 1, characterized in that: The viscosity of the methyl vinyl silicone rubber base is 10-10000 mPa·s.

5. The silicone rubber material according to claim 1, characterized in that: The reinforcing filler comprises fumed silica and / or precipitated silica; and / or, the catalyst comprises a platinum catalyst; And / or, the inhibitor comprises an acetylenic alcohol inhibitor.

6. A method for preparing a silicone rubber material, characterized in that: Used for preparing the silicone rubber material according to any one of claims 1 to 5, the preparation method of the silicone rubber material comprising: Preparation of aerogel noise reduction filler; Take appropriate amounts of methyl vinyl silicone rubber base, aerogel noise reduction filler, reinforcing filler and catalyst and mix them evenly to prepare component A; Take appropriate amounts of methyl vinyl silicone rubber base, aerogel noise reduction filler, reinforcing filler, hydrogen-containing silicone oil and inhibitor and mix them evenly to prepare component B; The component A and the component B are mixed and molded to obtain a silicone rubber material.

7. The method for preparing a silicone rubber material according to claim 6, characterized in that: The steps of preparing the aerogel noise reduction filler include: crushing the aerogel raw material into particles to obtain aerogel particles; The aerogel particles are treated with a silane coupling agent, dried, crushed, and sieved to obtain noise reduction filler powder; The noise reduction filler powder is added into cyclosiloxane and stirred to obtain an aerogel noise reduction filler.

8. The method for preparing a silicone rubber material according to claim 7, characterized in that: The cyclosiloxane includes at least one of hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane and dodecamethylcyclohexasiloxane.

9. The method for preparing a silicone rubber material according to claim 7, characterized in that: The silane coupling agent includes a vinyl group, an epoxy group or a methacryloxy group.

10. The method for preparing a silicone rubber material according to any one of claims 6 to 9, characterized in that: The molding includes hot pressing molding or injection molding.

Citation Information

Cited By

  • Medium-high frequency sound-absorbing noise-reducing light organic silicon coating and application thereof

    CN122037778A

  • A medium-high frequency sound-absorbing noise-reducing lightweight organic silicon coating and application thereof