Adhesive composition and preparation method thereof, pressure-sensitive adhesive and protective film
By using unsaturated bond-containing acrylate copolymers and radiation crosslinking initiators in the adhesive, combining antistatic agents and silicone compounds to form chemical bonds and conductive layers, the high-speed peeling force and pollution problems are solved, and low peeling is achieved Force and residual adhesive compositions are suitable for optical devices under high temperature and humidity conditions.
Patent Information
- Application Number
- CN202411211097.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to maintain low peeling force and no residual glue under high-speed peeling conditions, and common solutions are prone to contamination of the surface of the adhesive under high temperature and humidity conditions.
Using an acrylic ester copolymer containing unsaturated bonds as the main resin, combining radiation crosslinking initiator, antistatic agent and organic silicon compound containing carbon-carbon double bonds, to form chemical bonds through radiation crosslinking to fix diluents and silicone compounds. Reduce the peeling force and high-speed peeling force, and form a conductive layer to resist static electricity.
An adhesive composition with low peeling force and no residual glue under high-speed peeling conditions is realized, avoiding contamination and residual glue on the surface of the adhered, and is suitable for applications under high temperature and humidity conditions.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of optical protective films, and in particular, relates to an adhesive composition and a preparation method thereof, a pressure-sensitive adhesive and a protective film. Background Art
[0002] Many display and electronic devices need to be attached with surface protection films, which can prevent the surface of these components from being damaged during processing, assembly, inspection, and transportation. The protective film is often used as an intermediate transition protection and then peeled off from the surface of the adherend. The peeling force of the protective film is closely related to the peeling speed. The faster the peeling speed, the greater the peeling force. A relatively large peeling force will have an adverse effect on the appearance of the adherend, such as causing deformation of the adherend surface or degradation caused by uneven microscopic force.
[0003] Therefore, the relatively small variation range of the peeling force of the protective film on the adherend has an important impact on the appearance and usability of the adherend, that is, the protective film needs to have a relatively low peeling force under high-speed peeling conditions. The above performance requires that the protective film adhesive layer has relatively large flexibility, and the change of the adhesive layer stress can keep up with the rapid change of strain. However, greater flexibility often leads to lower cohesion, which will cause precipitation under high temperature, humidity or long-term use, thereby causing surface contamination of the adherend.
[0004] A common solution is to add polyether-modified silicone compounds to the adhesive layer to reduce the surface energy of the adhesive layer and the interaction between the adhesive layer and the surface of the adherend. This approach often results in too low peeling force or warping, which weakens the protective effect of the protective film. On the other hand, polyether-modified silicone is a polymer, which is easy to precipitate onto the surface of the adherend under high temperature, humidity or long-term use, causing pollution.
[0005] Chinese patent CN201410367592.0 discloses an adhesive sheet and an optical component. The adhesive resin composition provided by the patent contains a (meth) acrylic polymer, and the (meth) acrylic polymer is composed of at least a (meth) acrylic monomer having an alkyl group with 1 to 14 carbon atoms and a (meth) acrylic monomer having a hydroxyl group as raw monomers. The adhesive composition contains an ionic compound and an organopolysiloxane with an oxyalkylene chain. In order to achieve light peeling and low pollution, the patent adds an iron-based catalyst to accelerate the crosslinking reaction and prevent the precipitation of organopolysiloxane with an oxyalkylene chain and other small molecules or oligomers. However, the crosslinking method of the invention is heating crosslinking. High-efficiency catalysts can accelerate the crosslinking reaction. However, due to the processing time limit, the crosslinking speed is slower than radiation crosslinking, and it takes a certain amount of time for the crosslinking to be complete. A heating and aging process is often required to ensure that the crosslinking is complete. In this process, oligomers and small molecules diffuse and precipitate, especially organic silicon compounds have low surface energy and are easy to diffuse to the surface of the material, which may contaminate the adherend.
[0006] Chinese patent CN200980125812.6 discloses an acrylic composition for optical elements, a protective film for optical elements, a polarizer and a liquid crystal display. The composition provided by the invention contains a compound with a photopolymerizable group, an antistatic agent and a photoinitiator in the chain. By adding an appropriate amount of an antistatic agent and a predetermined proportion of a polymerization initiator to a composition containing a photopolymerizable acrylic polymer (which is cross-linked by irradiation with radiation such as ultraviolet rays (UVs)), the aging process can be skipped during the cross-linking process, thereby simplifying the preparation method. The acrylate pressure-sensitive adhesive provided by the invention contains an acrylic polymer with a photopolymerizable group, an antistatic agent and a photoinitiator. Because the acrylic polymer contains a photopolymerizable group, the cross-linking density can be fully increased, small molecules and oligomers can be prevented from precipitating, and contamination of the adherend can be avoided. However, the components provided by the patent cannot effectively reduce the high-speed peeling force, and cannot solve the problem of high high-speed peeling force of the pressure-sensitive adhesive layer.
[0007] Therefore, it is very necessary to develop an adhesive composition with no residual glue, low peeling force and low high-speed peeling force. Summary of the invention
[0008] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to provide an adhesive composition and a preparation method thereof, a pressure-sensitive adhesive and a protective film, wherein the adhesive composition provided by the present invention has low peeling force and low high-speed peeling force, and has no residual adhesive.
[0009] In the first aspect of the present invention, the present invention provides an adhesive composition, which, according to an embodiment of the present invention, comprises the following components in parts by weight: (A) 100 to 150 parts of an acrylate copolymer, (B) 5 to 30 parts of a diluent, (C) 0.2 to 2 parts of a radiation crosslinking initiator, (D) 0.02 to 1 part of an antistatic agent, and (E) 0.1 to 4 parts of an organosilicon compound containing a carbon-carbon double bond; wherein the (A) acrylate copolymer contains an unsaturated bond, and the (A) acrylate copolymer has an average functionality of 3 to 50.
[0010] According to the adhesive composition of the above embodiment of the present invention, an acrylate copolymer containing unsaturated bonds (such as carbon-carbon double bonds) is used as the main resin. The acrylate copolymer provided by the present invention has a lower glass transition temperature and a certain polarity, and can generate electrostatic attraction between the surface of the adherend, thereby improving the pressure-sensitive properties of the adhesive composition. Under the action of the radiation cross-linking initiator, the unsaturated bonds (such as carbon-carbon double bonds) in the acrylate copolymer can react with the diluent to form new chemical bonds, and the cross-linking effect is good, and the precipitation of low molecular weight polymers can be avoided, and residual glue can be reduced and pollution can be avoided. The amount of diluent used can also be reduced to prevent the poor appearance caused by the aggregation of diluents. The antistatic agent has good electrical conductivity, can form a conductive layer on the surface of the adherend, can be connected to the current in the environment, and the accumulated charge is released, thereby achieving the purpose of antistatic. The organosilicon compound has a lower surface tension, can reduce the surface energy of the adhesive composition, weaken the interaction with the adherend surface, and then can reduce the peeling force and high-speed peeling force of the adhesive composition. Moreover, the organosilicon compound containing unsaturated bonds (such as carbon-carbon double bonds) can also form chemical bonds with the diluent and acrylate copolymer, fixing the organosilicon compound in the network structure of the polymer without precipitation, thereby preventing the adhesive composition from contaminating the adherend.
[0011] Furthermore, by limiting the mass fraction of (A) acrylate copolymer to between 100 and 150 parts, sufficient pressure-sensitive effect can be provided. If the amount of acrylate copolymer is too little, the pressure sensitivity of the adhesive layer is insufficient; if it is too much, the crosslinking is insufficient and there is a risk of residual glue. By limiting the mass fraction of (B) diluent to between 5 and 30 parts, the diluent and the unsaturated bonds in the acrylate copolymer are effectively crosslinked under the action of the radiation crosslinking initiator, which can reduce the generation of residual glue and improve the pressure-sensitive properties of the adhesive composition. By limiting the mass fraction of the radiation crosslinking initiator to between 0.2 and 2 parts, it can ensure that an appropriate amount of free radicals are generated under radiation conditions, thereby initiating an effective crosslinking reaction between the unsaturated bonds in the acrylate copolymer and the diluent, reducing unreacted polymer segments, and thus reducing the risk of residual glue. By limiting the mass fraction of the antistatic agent to between 0.02 and 1 parts, the uniform distribution of the antistatic agent in the adhesive composition can be ensured to form an effective conductive path, thereby significantly improving the antistatic performance of the adhesive composition, and avoiding the residue of the antistatic agent on the surface of the adherend, thereby reducing the contamination of the adherend. By limiting the mass fraction of the organosilicon compound containing carbon-carbon double bonds to between 0.1 and 4 parts, it can be ensured that the adhesive forms a uniform and smooth coating on the surface of the adherend, thereby improving the apparent quality of the product; it can also avoid excessive organosilicon compounds, maintain the pressure sensitivity of the adhesive composition, and ensure that it can adhere quickly and firmly when it contacts the adherend.
[0012] Furthermore, by limiting the average functionality of the (A) acrylate copolymer to between 3 and 50, the number of epoxy groups can be effectively controlled, thereby controlling the peeling force of the adhesive composition within an appropriate range. This can ensure the bonding force between the adhesive composition and the adherend, and make the adhesive composition easy to peel, thus meeting the actual application requirements.
[0013] Therefore, the adhesive composition provided by the present invention has low peeling force, low high-speed peeling force, and no residual adhesive.
[0014] In addition, the adhesive composition according to the above embodiment of the present invention may also have the following additional technical features:
[0015] In some embodiments of the present invention, the number average molecular weight of the (A) acrylic ester copolymer is 40,000 to 400,000. This can avoid the occurrence of adhesive residue and improve construction efficiency.
[0016] In some embodiments of the present invention, the raw material components of the (A) acrylic acid ester copolymer include (F) acrylic acid ester polymer and (G) monomer containing carboxyl group and carbon-carbon double bond. Thus, it is beneficial to obtain an adhesive composition with low peel force, low high-speed peel force and no residual adhesive.
[0017] In some embodiments of the present invention, based on the total mass of the (A) acrylic ester copolymer, the mass proportion of the (G) monomer containing a carboxyl group and a carbon-carbon double bond is 0.5% to 5%. Thus, an appropriate amount of carboxyl groups can be introduced to adjust the polarity of the acrylic ester copolymer, which helps to enhance the interaction between the adhesive composition and the adherend, thereby improving the wettability of the adhesive, and further reducing the peeling force of the adhesive composition.
[0018] In some embodiments of the present invention, the monomer containing (G) a carboxyl group and a carbon-carbon double bond includes at least one of acrylic acid, methacrylic acid, carboxyethyl acrylate, mono-2-(methacryloyloxy)ethyl phthalate, and mono-[2-[(2-methyl-acryloyl)oxy]ethyl] succinate. Thus, an appropriate amount of carboxyl groups can be introduced, the polarity of the acrylate copolymer can be adjusted, and the interaction between the adhesive composition and the adherend can be enhanced, thereby improving the wettability of the adhesive, and further reducing the peeling force of the adhesive composition.
[0019] In some embodiments of the present invention, the raw material components of the (F) acrylic acid ester polymer include a first methacrylate monomer, a second methacrylate monomer and (H) a monomer containing an epoxy group and a carbon-carbon double bond, wherein the first methacrylate monomer has a structural formula of CH 2 =C(CH 3 )COOR 1 , R 1 is an alkyl group having 4 to 22 carbon atoms, and the structural formula of the second methacrylate monomer is CH 2 =C(CH 3 )COOR 2 , R 2 The alkyl group has a carbon number of 1 to 3. Thus, the adhesion strength and durability of the adhesive can be significantly improved, and the peeling force can be effectively reduced.
[0020] In some embodiments of the present invention, the first methacrylate monomer includes at least one of butyl acrylate, butyl methacrylate, hexyl acrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, n-octyl acrylate, isooctyl acrylate, isononyl acrylate, decyl acrylate, isodecyl acrylate, dodecyl acrylate, dodecyl methacrylate, tridecyl acrylate, tridecyl methacrylate, tetradecyl acrylate, heptadecanyl acrylate, octadecyl acrylate, and behenyl acrylate. Thus, while ensuring that the adhesive composition has significant pressure sensitivity, the peeling force of the adhesive composition can also be reduced.
[0021] In some embodiments of the present invention, the second methacrylate monomer includes at least one of methyl methacrylate, ethyl methacrylate and propyl methacrylate, thereby significantly improving the adhesion strength and durability of the adhesive and effectively reducing the peeling force.
[0022] In some embodiments of the present invention, the (H) monomer containing an epoxy group and a carbon-carbon double bond includes at least one of glycidyl acrylate, glycidyl methacrylate and allyl glycidyl ether. Thus, the adhesion strength and durability of the adhesive can be significantly improved, and the peeling force can be effectively reduced.
[0023] In some embodiments of the present invention, the (C) radiation crosslinking initiator includes at least one of α-hydroxyketone compounds and benzyl ketal compounds. Thus, the unsaturated bonds (such as C=C double bonds) in the acrylate copolymer can be induced to undergo a crosslinking reaction with the diluent to form new chemical bonds, and the diluent can be fixed in the acrylate copolymer network to prevent its precipitation, thereby reducing the residual adhesive in the adhesive composition.
[0024] In some embodiments of the present invention, the (B) diluent includes at least one of a polyalkylene glycol containing at least one acrylate functional group and a polyalkylene glycol containing at least one allyl functional group. As a result, the polyalkylene glycol has low structural polarity, strong molecular mobility, and high flexibility, and can reduce the peel force of the adhesive composition, and reduce the high-speed peel force of the adhesive composition to a certain extent.
[0025] In some embodiments of the present invention, the (D) antistatic agent includes at least one of pyridinium antistatic agents, imidazolium antistatic agents, phosphonium antistatic agents, sulfonium antistatic agents, pyrrolidinium antistatic agents, guanidinium antistatic agents, ammonium antistatic agents, isourea antistatic agents, thiourea antistatic agents, piperidinium antistatic agents, pyrazolium antistatic agents, methyl carbonium antistatic agents, lithium ion antistatic agents, morpholinium antistatic agents, sorbitol antistatic agents, polyoxyethylene alkyl ether antistatic agents, and fatty acid polyol ester antistatic agents. Thus, the resistivity of the surface of the adhesive composition can be effectively reduced, the accumulation and generation of static electricity can be reduced, and the antistatic performance of the adhesive composition can be improved.
[0026] In some embodiments of the present invention, at least one of amide monomers, nitrogen-containing heterocyclic vinyl monomers, cyano-containing monomers, vinyl-containing monomers, aromatic vinyl-containing monomers, imide-containing monomers, and amino-containing monomers is further included. This is conducive to obtaining an adhesive composition with low peeling force and high-speed peeling force and no residual adhesive.
[0027] In some embodiments of the present invention, the amide monomer includes at least one of acrylamide, methacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, diacetone acrylamide, N-hydroxyethyl acrylamide, N-(isobutyloxy)methacrylamide, N-vinylformamide and N-vinylacetamide. This is conducive to obtaining an adhesive composition with low peel force and high-speed peel force and no residual adhesive.
[0028] In some embodiments of the present invention, the nitrogen-containing heterocyclic vinyl monomer includes at least one of N-vinyl pyrrolidone, vinyl pyridine, N-vinyl piperidone, vinyl piperazine, 2-vinyl pyrazine, N-vinyl imidazole, N-vinyl oxazolidinone, N-ethyl morpholine and N-vinyl caprolactam. This is conducive to obtaining an adhesive composition with low peel force and high-speed peel force and no residual adhesive.
[0029] In some embodiments of the present invention, the cyano group-containing monomer includes at least one of acrylonitrile and methacrylonitrile. This is conducive to obtaining an adhesive composition with low peel force and high-speed peel force and no residual adhesive.
[0030] In some embodiments of the present invention, the vinyl-containing monomer includes at least one of vinyl acetate, vinyl propionate and vinyl laurate. This is conducive to obtaining an adhesive composition with low peel force and high-speed peel force and no residual adhesive.
[0031] In some embodiments of the present invention, the aromatic vinyl-containing monomer includes at least one of styrene, chlorostyrene, chloromethylstyrene and α-methylstyrene. Thus, the cohesion and adhesion of the adhesive composition can be enhanced.
[0032] In some embodiments of the present invention, the imide group-containing monomer includes N-cyclohexylmaleimide, N-isopropylmaleimide and N-cyclohexylmaleimide. This is conducive to obtaining an adhesive composition with low peel force and high-speed peel force and no residual adhesive.
[0033] In some embodiments of the present invention, the amino-containing monomer includes at least one of dimethylaminoethyl acrylate, diethylaminoethyl methacrylate, dimethylaminoethyl acrylate and dimethylaminoethyl methacrylate. This is conducive to obtaining an adhesive composition with low peel force and high-speed peel force and no residual adhesive.
[0034] In the second aspect of the present invention, the present invention provides a method for preparing an adhesive composition, comprising: mixing (A) an acrylate copolymer, (B) a diluent, (C) a radiation crosslinking initiator, (D) an antistatic agent and an organosilicon compound to obtain an adhesive composition, wherein the (A) acrylate copolymer contains an unsaturated bond and the average functionality of the (A) acrylate copolymer is 3 to 50. Thus, an adhesive composition with low peel force, low high-speed peel force and no residual adhesive can be obtained.
[0035] In the third aspect of the present invention, the present invention provides a pressure-sensitive adhesive. According to an embodiment of the present invention, the pressure-sensitive adhesive is prepared using the adhesive composition described above. Therefore, when the pressure-sensitive adhesive is applied to a protective film, the peeling force is low, and under high-speed peeling conditions, the peeling force is also low, and the pressure-sensitive adhesive is easy to peel and there is no residual adhesive on the device surface after peeling, and is suitable for use on various optical devices and devices with high surface requirements.
[0036] In the fourth aspect of the present invention, the present invention proposes a protective film. According to an embodiment of the present invention, the protective film includes: a base film; a pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer is formed on at least one surface of the base film, wherein the pressure-sensitive adhesive layer includes the pressure-sensitive adhesive described above. As a result, the protective film is anti-static, has low peeling force, does not pollute the adherend, has low high-speed peeling force, protects the adherend surface during the peeling process or processing of the protective film, makes it have a good appearance, is flat and does not deform, and is suitable for use on various optical devices and devices with high surface requirements.
[0037] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. DETAILED DESCRIPTION
[0038] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below are exemplary and are intended to be used to explain the present invention, and cannot be understood as limiting the present invention.
[0039] In the first aspect of the present invention, the present invention provides an adhesive composition, which, according to an embodiment of the present invention, comprises the following components in parts by weight: (A) 100 to 150 parts of an acrylate copolymer, (B) 5 to 30 parts of a diluent, (C) 0.2 to 2 parts of a radiation crosslinking initiator, (D) 0.02 to 1 part of an antistatic agent, and (E) 0.1 to 4 parts of an organosilicon compound containing a carbon-carbon double bond; wherein the (A) acrylate copolymer contains an unsaturated bond, and the (A) acrylate copolymer has an average functionality of 3 to 50.
[0040] As an example, the mass fraction of the (A) acrylic ester copolymer can be 100 parts, 110 parts, 120 parts, 130 parts, 140 parts, 150 parts, etc.; the mass fraction of the (B) diluent can be 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, etc.; the mass fraction of the (C) radiation cross-linking initiator can be 0.2 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, etc.; the mass fraction of the (D) antistatic agent can be 0.02 parts, 0.05 parts, 0.1 parts, 0.5 parts, 1 parts, etc.; the mass fraction of the (E) organosilicon compound containing carbon-carbon double bonds can be 0.1 parts, 0.5 parts, 1 parts, 2 parts, 4 parts, etc.
[0041] According to the adhesive composition of the above embodiment of the present invention, the acrylate copolymer has a strong polarity and can generate electrostatic attraction with the surface of the adherend, thereby improving the pressure-sensitive properties of the adhesive composition. Under the action of the radiation cross-linking initiator, the unsaturated bonds (such as carbon-carbon double bonds) in the acrylate copolymer can undergo a cross-linking reaction with the diluent to form a new chemical bond, which can fix the diluent in the acrylate copolymer network to prevent its precipitation, reduce residual glue and avoid pollution. It can also reduce the amount of diluent used to prevent poor appearance caused by diluent aggregation.
[0042] Antistatic agents have good electrical conductivity and can form a conductive layer on the surface of the adherend, which can be connected to the current in the environment and release the accumulated charge, thereby achieving the purpose of antistatic. Organic silicon compounds containing carbon-carbon double bonds have low surface tension, which can reduce the surface energy of the adhesive composition and weaken the interaction with the adherend surface, thereby reducing the peeling force and high-speed peeling force of the adhesive composition. In addition, the unsaturated bonds (such as carbon-carbon double bonds) in organic silicon compounds can also form chemical bonds with diluents and acrylate copolymers, fixing the organic silicon compounds in the network structure of the polymer without precipitation, so that the adhesive composition does not contaminate the adherend.
[0043] Furthermore, by limiting the mass fraction of (A) acrylate copolymer to between 100 and 150 parts, sufficient pressure-sensitive effect can be provided to prevent viscosity reduction or residual glue; by limiting the mass fraction of (B) diluent to between 5 and 30 parts, the diluent and the unsaturated bonds in the acrylate copolymer are effectively cross-linked under the action of the radiation cross-linking initiator, which can reduce the generation of residual glue and improve the pressure-sensitive properties of the adhesive composition. By limiting the mass fraction of the radiation cross-linking initiator to between 0.2 and 2 parts, it can be ensured that an appropriate amount of free radicals are generated under radiation conditions, thereby initiating an effective cross-linking reaction between the unsaturated bonds in the acrylate copolymer and the diluent, reducing unreacted polymer segments, and thus reducing the risk of residual glue. By limiting the mass fraction of the antistatic agent to between 0.02 and 1 part, it can be ensured that the antistatic agent is evenly distributed in the adhesive composition to form an effective conductive path, thereby significantly improving the antistatic properties of the adhesive composition, and can also avoid the residue of the antistatic agent on the surface of the adherend, reducing the contamination of the adherend. By limiting the mass fraction of the organic silicon compound containing carbon-carbon double bonds to between 0.1 and 4 parts, it is possible to ensure that the adhesive forms a uniform and smooth coating on the surface of the adherend, thereby improving the apparent quality of the product; it is also possible to avoid excessive organic silicon compounds containing carbon-carbon double bonds, maintain the pressure sensitivity of the adhesive composition, and ensure that it can quickly bond when it contacts the adherend.
[0044] Furthermore, by limiting the average functionality of the (A) acrylic ester copolymer to between 3 and 50, for example, 3, 5, 10, 20, 40, 50, etc., the number of epoxy groups can be effectively controlled, thereby controlling the peeling force of the adhesive composition within a suitable range. In this way, the bonding force between the adhesive composition and the adherend can be ensured, and the adhesive composition can be easily peeled off, meeting the actual application requirements.
[0045] Therefore, the adhesive composition provided by the present invention has low peeling force and low high-speed peeling force, and has no residual adhesive.
[0046] According to some specific embodiments of the present invention, the number average molecular weight of the (A) acrylate copolymer is 40,000 to 400,000. For example, it can be 40,000, 100,000, 200,000, 400,000, etc. If the molecular weight of the acrylate copolymer is too low, the content of the oligomer in the adhesive composition will increase, and it will easily precipitate during processing and use, resulting in residual glue. If the molecular weight of the acrylate copolymer is too high, the viscosity of the acrylate copolymer will increase, causing inconvenience in construction, resulting in low construction efficiency, and even affecting the final performance of the product. Therefore, by limiting the molecular weight of the acrylate copolymer to the above range, the occurrence of residual glue can be avoided and the construction efficiency can be improved.
[0047] According to some specific embodiments of the present invention, the raw material components of the (A) acrylate copolymer include the raw material components of the acrylate copolymer containing epoxy groups include (F) acrylate polymer and (G) monomers containing carboxyl groups and carbon-carbon double bonds. In the adhesive composition, by introducing a monomer containing a carboxyl group to carry out a copolymerization reaction, specifically, the epoxy group in the acrylate copolymer can undergo an esterification reaction with the carboxyl group in the monomer containing a carboxyl group and a carbon-carbon double bond, and the carbon-carbon double bond in the monomer containing a carboxyl group and a carbon-carbon double bond is grafted into the acrylate copolymer, so that an acrylate copolymer containing unsaturated carbon-carbon double bonds can be obtained, which is conducive to obtaining an adhesive composition with lower peeling force and no residual adhesive.
[0048] According to some specific embodiments of the present invention, based on the total mass of the (A) acrylate copolymer, the mass proportion of the (G) monomer containing carboxyl and carbon-carbon double bonds is 0.5% to 5%. For example, it can be 0.5%, 1%, 5%, etc. If the amount of the monomer containing carboxyl and carbon-carbon double bonds is too low, the number of carboxyl groups will be less than the epoxy groups on the acrylate polymer, resulting in residual epoxy groups, which will increase the peeling force of the adhesive composition and even improve the high-speed peeling force of the adhesive composition; if the amount of the monomer containing carboxyl and carbon-carbon double bonds is too high, the number of carboxyl groups is more than the epoxy groups on the acrylate polymer, and the carboxyl group is a group with high polarity, which will also cause the peeling force to increase. Therefore, by limiting the mass proportion of the monomer containing carboxyl and carbon-carbon double bonds to the above range, an appropriate amount of carboxyl groups can be introduced, which can adjust the polarity of the acrylate copolymer, help enhance the interaction between the adhesive composition and the adherend, thereby improving the wettability of the adhesive, and then can reduce the peeling force and high-speed peeling force of the adhesive composition.
[0049] As an example, the (G) monomer containing a carboxyl group and a carbon-carbon double bond includes at least one of acrylic acid, methacrylic acid, carboxyethyl acrylate, mono-2-(methacryloyloxy)ethyl phthalate, and mono-[2-[(2-methyl-acryloyl)oxy]ethyl] succinate.
[0050] According to some specific embodiments of the present invention, the raw material components of the epoxy-containing acrylic polymer include a first methacrylate monomer, a second methacrylate monomer, and (H) a monomer containing an epoxy group and a carbon-carbon double bond, wherein the first methacrylate monomer has a structural formula of CH 2 =C(CH 3 )COOR 1 , R 1 is an alkyl group having 4 to 22 carbon atoms, and the structural formula of the second methacrylate monomer is CH 2 =C(CH 3 )COOR 2 , R2 The first methacrylate monomer, the second methacrylate monomer and the monomer containing epoxy group and carbon-carbon double bond are copolymerized, and the carbon-carbon double bond in the first methacrylate monomer, the carbon-carbon double bond in the second methacrylate monomer and the carbon-carbon double bond in the monomer containing epoxy group and carbon-carbon double bond are broken and then polymerized with each other to obtain an acrylate polymer containing epoxy group.
[0051] Furthermore, the first methacrylate monomer, as the main component in the preparation process of the acrylate polymer, has moderate intermolecular force, is easy to form stable and uniform adhesion, and can improve the pressure sensitivity of the adhesive composition. Moreover, the homopolymer of the first methacrylate monomer has a low glass transition temperature and low molecular polarity, so that the adhesive composition is not easy to have a strong interaction with the surface of the adherend during peeling, thereby ensuring low peeling force. The second methacrylate monomer can adjust the molecular weight and fluidity of the polymer during the preparation process of the acrylate polymer, which helps the adhesive composition to better penetrate into the micropores and irregular structures on the surface of the adherend to form a uniform bond; the monomer containing epoxy groups and carbon-carbon double bonds can provide epoxy groups in the adhesive composition, which can react with carbon bodies containing carboxyl groups and carbon-carbon double bonds, so that the acrylate copolymer is connected to carbon-carbon double bonds, so that the acrylate copolymer forms a cross-linked network through the initiator, diluent and organic silicon containing carbon-carbon double bonds, thereby improving cohesion and preventing residual glue.
[0052] Therefore, using an epoxy-containing acrylate polymer obtained by polymerizing a methacrylate monomer containing an alkyl group having 4-22 carbon atoms, a methacrylate monomer containing an alkyl group having 1-3 carbon atoms, and a monomer containing an epoxy group and a carbon-carbon double bond as the main component of the adhesive composition can significantly improve the adhesion strength and durability of the adhesive and effectively reduce the peel force.
[0053] As an example, the first methacrylate monomer includes at least one of butyl acrylate, butyl methacrylate, hexyl acrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, n-octyl acrylate, isooctyl acrylate, isononyl acrylate, decyl acrylate, isodecyl acrylate, dodecyl acrylate, dodecyl methacrylate, tridecyl acrylate, tridecyl methacrylate, tetradecyl acrylate, heptadecanyl acrylate, octadecyl acrylate, and behenyl acrylate. The second methacrylate monomer includes at least one of methyl methacrylate, ethyl methacrylate, and propyl methacrylate. The (H) monomer containing an epoxy group and a carbon-carbon double bond includes at least one of glycidyl acrylate, glycidyl methacrylate, and allyl glycidyl ether.
[0054] According to some specific embodiments of the present invention, the (C) radiation crosslinking initiator includes at least one of an α-hydroxyketone type compound and a benzyl ketal type compound. By selecting the above-mentioned radiation crosslinking initiator, during the radiation crosslinking process, the above-mentioned radiation crosslinking initiator can absorb radiation energy (such as ultraviolet light, electron beam or gamma ray), and then generate free radicals or ions, which can trigger the carbon-carbon double bonds, diluents, and organic silicon compounds containing carbon-carbon double bonds in the acrylate copolymer to undergo crosslinking reactions to form new chemical bonds, and the diluents and organic silicon compounds can be fixed in the acrylate copolymer network to prevent their precipitation, thereby reducing the residual adhesive of the adhesive composition.
[0055] According to some specific embodiments of the present invention, the (B) diluent includes at least one of a polyalkylene glycol containing at least one acrylate functional group and a polyalkylene glycol containing at least one allyl functional group. By selecting the above diluent, under the action of the radiation cross-linking initiator, the diluent can undergo a cross-linking reaction with the unsaturated bonds (such as C=C double bonds) in the acrylate copolymer to form a new chemical bond, and the diluent can be fixed in the acrylate copolymer network to prevent it from precipitating, thereby reducing the residual adhesive of the adhesive composition. In addition, the structural polarity of the polyalkylene glycol is low, the molecular mobility is strong, and the flexibility is large, which can reduce the peeling force of the adhesive composition, and reduce the high-speed peeling force of the adhesive composition to a certain extent.
[0056] It should be noted that a polyalkylene glycol containing at least one acrylate functional group is a polymer whose main chain is composed of polyalkylene glycol, and at least one acrylate group is connected to the end or side chain of the main chain. For example, there may be 1 acrylate group, 2 acrylate groups, 3 acrylate groups, or even multiple acrylate groups. Specifically, polyalkylene glycol is usually prepared by polycondensation of alkylene glycol monomers such as ethylene glycol and propylene glycol, and its molecular chain contains multiple repeated alkylene glycol units (-ORO-, where R is an alkylene group). The acrylate functional group is obtained by connecting acrylate or methacrylate to the end or side chain of polyalkylene glycol through an esterification reaction. The acrylate functional group has a double bond (C=C) and an ester group (-COO-) that can give the polymer excellent reactivity and can form chemical bonds with other molecules or polymer chains through free radical polymerization, crosslinking and other reactions.
[0057] Similarly, a polyalkylene glycol containing at least one allyl functional group is also a polymer, wherein the main chain is composed of polyalkylene glycol, and at least one allyl functional group is connected to the end or side chain of the main chain. For example, there may be 1 allyl functional group, 2 allyl functional groups, 3 allyl functional groups, or even multiple allyl functional groups. The presence of the allyl group enables the polymer to be connected or modified with other molecules or polymer chains through various chemical reactions (such as addition reactions, free radical polymerization, etc.).
[0058] According to some specific embodiments of the present invention, the (D) antistatic agent includes at least one of pyridinium antistatic agents, imidazolium antistatic agents, phosphonium antistatic agents, sulfonium antistatic agents, pyrrolidinium antistatic agents, guanidinium antistatic agents, ammonium antistatic agents, isourea antistatic agents, thiourea antistatic agents, piperidinium antistatic agents, pyrazolium antistatic agents, methyl carbonium antistatic agents, lithium ion antistatic agents, morpholinium antistatic agents, sorbitol antistatic agents, polyoxyethylene alkyl ether antistatic agents, and fatty acid polyol ester antistatic agents. By selecting the above antistatic agents, the resistivity of the surface of the adhesive composition can be effectively reduced, the accumulation and generation of static electricity can be reduced, and the antistatic performance of the adhesive composition can be improved.
[0059] According to some specific embodiments of the present invention, the (E) organosilicon compound containing carbon-carbon double bonds has a low surface tension, can reduce the surface energy of the adhesive composition, weaken the interaction with the surface of the adherend, and thus can reduce the peel force and high-speed peel force of the adhesive composition. The use of organosilicon compounds containing double bonds can also form chemical bonds with diluents and acrylate copolymers, fix the organosilicon compounds in the network structure of the polymer, and prevent precipitation, so that the adhesive composition does not contaminate the adherend.
[0060] According to some specific embodiments of the present invention, the adhesive composition further comprises at least one of an amide monomer, a nitrogen-containing heterocyclic vinyl monomer, a cyano-containing monomer, a vinyl-containing monomer, an aromatic vinyl-containing monomer, an imido-containing monomer, and an amino-containing monomer. The addition of an amide monomer can increase the flexibility and cohesion of the adhesive composition, thereby improving its adhesion performance. The addition of a nitrogen-containing heterocyclic vinyl monomer can enhance the interaction between the adhesive composition and the adherend and improve the adhesion strength. The addition of a cyano-containing monomer can reduce the viscosity of the adhesive composition and help improve its processing performance. The addition of a vinyl-containing monomer can adjust the molecular weight and molecular weight distribution of the adhesive composition. The addition of an aromatic vinyl-containing monomer can enhance the cohesion and adhesion of the adhesive composition. The addition of an imido-containing monomer can improve the adhesion and crosslinking of the adhesive composition. The addition of an amino-containing monomer can react with an acidic substance to form an ionic bond or a covalent bond, thereby enhancing the adhesion of the adhesive. This is conducive to obtaining an adhesive composition with low peel force, low high-speed peel force and no residual adhesive.
[0061] As an example, the amide monomer includes at least one of acrylamide, methacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, diacetone acrylamide, N-hydroxyethyl acrylamide, N-(isobutyloxy)methacrylamide, N-vinyl formamide and N-vinyl acetamide. The nitrogen-containing heterocyclic vinyl monomer includes at least one of N-vinyl pyrrolidone, vinyl pyridine, N-vinyl piperidone, vinyl piperazine, 2-vinyl pyrazine, N-vinyl imidazole, N-vinyl oxazolidinone, N-ethylmorpholine and N-vinyl caprolactam. The cyano-containing monomer includes at least one of acrylonitrile and methacrylonitrile, wherein the CAS number of methacrylonitrile is 126-98-7. The vinyl-containing monomer includes at least one of vinyl acetate, vinyl propionate and vinyl laurate. The aromatic vinyl-containing monomer includes at least one of styrene, chlorostyrene, chloromethylstyrene and α-methylstyrene. The monomer containing an imido group includes at least one of N-cyclohexylmaleimide, N-isopropylmaleimide and N-cyclohexylmaleimide. The monomer containing an amino group includes at least one of dimethylaminoethyl acrylate, diethylaminoethyl methacrylate, dimethylaminoethyl acrylate and dimethylaminoethyl methacrylate.
[0062] According to some specific embodiments of the present invention, the adhesive composition further includes at least one of a solvent and an auxiliary agent.
[0063] In some embodiments of the present invention, the solvent includes at least one of ethyl acetate, butyl acetate, butanone, acetone, N,N-dimethylformamide, dimethylacetamide, benzene and toluene, thereby helping the components in the adhesive composition to form a uniform system.
[0064] In some embodiments of the present invention, the auxiliary agent includes at least one of a catalyst promoter, a surfactant, a plasticizer, a filler, an antioxidant, an anti-aging agent and a processing aid.
[0065] In the second aspect of the present invention, a method for preparing an adhesive composition is provided, which comprises mixing (A) an acrylate copolymer, (B) a diluent, (C) a radiation crosslinking initiator, (D) an antistatic agent and (E) an organosilicon compound containing a carbon-carbon double bond to obtain an adhesive composition, wherein the (A) acrylate copolymer contains an unsaturated bond and the average functionality of the (A) acrylate copolymer is 3 to 50.
[0066] According to the preparation method of the embodiment of the present invention, by mixing (A) acrylate copolymer, (B) diluent, (C) radiation crosslinking initiator, (D) antistatic agent and (E) organosilicon compound containing carbon-carbon double bond, an adhesive composition can be obtained. In the adhesive composition, an acrylate copolymer containing unsaturated bonds (such as carbon-carbon double bonds) is used as the main resin, and the acrylate copolymer has a strong polarity, can generate electrostatic attraction between the surface of the adherend, and improves the pressure-sensitive properties of the adhesive composition. Under the action of the radiation crosslinking initiator, the unsaturated bonds (such as carbon-carbon double bonds) in the acrylate copolymer can react with the diluent to form new chemical bonds, and the crosslinking effect is good, and the precipitation of low molecular weight polymers can be avoided, and residual glue can be reduced and pollution can be avoided. The amount of diluent used can also be reduced to prevent the poor appearance caused by the aggregation of the diluent. The antistatic agent has good electrical conductivity, can form a conductive layer on the surface of the adherend, can be connected to the current in the environment, and the accumulated charge is released, thereby achieving the purpose of antistatic. Organic silicon compounds have low surface tension, which can reduce the surface energy of the adhesive composition, weaken the interaction with the surface of the adherend, and thus reduce the peeling force and high-speed peeling force of the adhesive composition. In addition, organic silicon compounds with carbon-carbon double bonds can also form chemical bonds with diluents and acrylate copolymers, fixing the organic silicon compounds in the network structure of the polymer without precipitation, so that the adhesive composition does not contaminate the adherend.
[0067] In the third aspect of the present invention, the present invention provides a pressure-sensitive adhesive. According to an embodiment of the present invention, the pressure-sensitive adhesive is prepared by using the pressure-sensitive adhesive composition described above. Therefore, when the pressure-sensitive adhesive is applied to a protective film, the peeling force is low, and under the condition of high-speed peeling, the peeling force is also low, and it is easy to peel and there is no residual adhesive on the surface of the device after peeling, and it is suitable for use on various optical devices and devices with high surface requirements. Moreover, the pressure-sensitive adhesive can be radiation cross-linked, which is energy-saving and environmentally friendly.
[0068] In the fourth aspect of the present invention, the present invention proposes a protective film. According to an embodiment of the present invention, the protective film includes: a base film; a pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer is formed on at least one surface of the base film, wherein the pressure-sensitive adhesive layer includes the pressure-sensitive adhesive described above. As a result, the protective film is anti-static, has low peeling force, does not pollute the adherend, has low high-speed peeling force, protects the adherend surface during the peeling process or processing of the protective film, makes it have a good appearance, is flat and does not deform, and is suitable for use on various optical devices and devices with high surface requirements.
[0069] As an example, the base film includes at least one of polyester such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate, cellulose-based polymers such as diacetyl cellulose and triacetyl cellulose, and polycarbonate-based polymers.
[0070] The scheme of the present disclosure will be explained below in conjunction with the examples. Those skilled in the art will appreciate that the following examples are only used to illustrate the present disclosure and should not be considered to limit the scope of the present disclosure. Where specific techniques or conditions are not indicated in the examples, the techniques or conditions described in the literature in this area or the product instructions are used. Where the manufacturers of reagents or instruments are not indicated, they are all conventional products that can be obtained commercially.
[0071] Example 1
[0072] 1. (F) Preparation of raw material mixed solution of acrylate polymer:
[0073] 60 parts of butyl acrylate, 20 parts of isooctyl acrylate, 10 parts of methyl acrylate, 1 part of glycidyl methacrylate, 1 part of N-(isobutyloxy)methacrylamide and 0.6 parts of azobisisobutyronitrile were mixed evenly and fully dissolved to obtain a raw material mixed solution of acrylate polymer.
[0074] 2. (A) Preparation of acrylic acid ester copolymer:
[0075] (1) Nitrogen is introduced into a four-necked flask equipped with a stirrer, a reflux condenser, a thermometer, a constant pressure dropping funnel and a nitrogen inlet tube until the air in the system is replaced by nitrogen, 80 g of butyl acetate and 25 g of the mixed solution in step 1 are added, nitrogen is introduced to remove oxygen from the mixture, the temperature is raised to 70° C., the temperature is kept for 0.5 hour, the remaining mixed solution is slowly added dropwise, the temperature is dropped for 3 hours, the temperature is kept for 6 hours, the temperature is raised to 120° C., the temperature is kept for 2 hours, and the temperature is naturally cooled to obtain (F) acrylate polymer.
[0076] (2) The (A) acrylic acid ester copolymer obtained in step (1) was heated to 90° C., and 0.5 g of acrylic acid, 0.0505 g of triphenylphosphine, and 0.011 g of p-hydroxyanisole were slowly added dropwise for 1 h. The mixture was kept warm for 6 hours, cooled naturally, and 220 g of ethyl acetate was added to obtain the (A) acrylic acid ester copolymer having an average functionality of 12.6 and a molecular weight of 170,000.
[0077] 3. Preparation of adhesive composition:
[0078] Take 100 parts of (A) acrylate copolymer, add 30 parts of (B) diluent, 0.5 parts of (C) radiation cross-linking initiator, 0.02 parts of (D) antistatic agent, 0.02 parts of organosilicon compound and ethyl acetate, mix well and obtain an adhesive composition, wherein the (B) diluent is polyethylene glycol 600 dimethacrylate; the (C) radiation cross-linking initiator is 1-hydroxy-cyclohexyl-phenyl-ketone; the (D) antistatic agent is lithium bistrifluoromethanesulfonyl imide; and the (E) organosilicon compound containing carbon-carbon double bonds is BYK-SILCLEAN 3710, wherein the polyether-modified polydimethylsiloxane containing acrylate functional groups as a component of BYK-SILCLEAN 3710 is supplied by BYK Chemical.
[0079] 4. Preparation of protective film:
[0080] The adhesive composition in step 3 was coated on a polyethylene terephthalate (PET) base film to a wet thickness of 80 μm, dried at 60° C. for 5 min to remove the solvent, and then irradiated at a radiation source of 500 mJ / cm 2 The protective film was obtained by irradiating for 5s under the conditions of .
[0081] The components of the adhesive compositions of Examples 2-10 and Comparative Examples 1-3 are the same as those of Example 1 except that some components are different from those of Example 1.
[0082] Some components of the adhesive compositions of Examples 1-10 and Comparative Examples 1-3 are shown in Table 1.
[0083] Table 1
[0084]
[0085] Testing and analysis
[0086] Under the same conditions, the protective films obtained in the above Examples 1-10 and Comparative Examples 1-3 were subjected to adhesive residue test, antistatic test, peeling force test and high-speed peeling force test respectively. The specific test methods are as follows:
[0087] (1) Residual adhesive test: According to the sample preparation method of standard GB / T2792-2014, the protective film is pasted on the steel plate, and the sample is placed in a 180°C forced air oven for high temperature treatment for 0.5 hours, restored to room temperature, and allowed to stand for 2 hours. The protective film is peeled off at a speed of 100 mm / min, and the residual adhesive on the surface of the adherend is observed. Among them, "△" indicates that the steel plate has slight residual adhesive, "○" indicates that the steel plate has no residual adhesive, and "×" indicates that the steel plate has residual adhesive.
[0088] (2) Antistatic test: Use ZC36 resistance meter to test the surface resistance of the protective film.
[0089] (3) Peel force test: Tested in accordance with the national standard GB / T2790-1995. Specifically, the surface protection film was cut into a size of 25 mm in width and 200 mm in length. After peeling off the release film, it was pasted on the surface of a standard mirror steel plate (50 mm in width, 150 mm in length, and 2 mm in thickness) with a 2KG hand roller, rolled three times, and left to stand for 30 minutes as the evaluation sample. The peel force test speed was 300 mm / min. The instrument gave the result directly without the need for calculation.
[0090] (4) High-speed peeling force test: Tested according to FINAT standard,
[0091] Cut the surface protection film into a size of 25mm in width and 200mm in length. After peeling off the release film, stick it to the surface of a standard mirror steel plate (50mm in width, 150mm in length, and 2mm in thickness) with a 2KG hand roller. Roll it three times and let it stand for 30 minutes. Use it as an evaluation sample. The peel force test speed is 30m / min. The instrument gives the result directly without the need for calculation.
[0092] The test results are shown in Table 2.
[0093] Table 2
[0094] Residue Antistatic / Ω Peel force / (g / 25mm) High-speed peeling force / (g / 25mm) Example 1 ○ <![CDATA[10 11 ]]> 15 125 Example 2 ○ <![CDATA[10 10 ]]> 12 116 Example 3 ○ <![CDATA[10 9 ]]> 10 102 Example 4 ○ <![CDATA[10 9 ]]> 15 76 Example 5 ○ <![CDATA[10 9 ]]> 18 84 Example 6 ○ <![CDATA[10 9 ]]> 9 96 Example 7 ○ <![CDATA[10 9 ]]> 10 115 Example 8 ○ <![CDATA[10 9 ]]> 18 88 Example 9 ○ <![CDATA[10 9 ]]> 11 109 Example 10 ○ <![CDATA[10 9 ]]> 14 118 Comparative Example 1 × <![CDATA[10 10 ]]> 26 192 Comparative Example 2 △ <![CDATA[10 12 ]]> 53 220 Comparative Example 3 ○ <![CDATA[10 11 ]]> 36 201
[0095] Combined with Table 1, it can be seen that compared with Comparative Examples 1-3, the protective films obtained in Examples 1-10 have the properties of antistatic, no residual adhesive, low peeling force, and low high-speed peeling force, and the effect is ideal, and it is suitable for use on various devices with high surface requirements. The polymers in Comparative Examples 1-2 do not contain C=C and cannot form chemical bonds with diluents. Although the diluents can be cross-linked, they have low cohesive force and will form residual adhesive. The polar components such as AA and GMA used in Comparative Example 3 have high contents, resulting in relatively large peeling force.
[0096] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", "some implementation schemes" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0097] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. An adhesive composition, characterized in that: The composition includes the following components in parts by weight: (A) 100 to 150 parts of an acrylic acid ester copolymer, (B) 5 to 30 parts of a diluent, (C) 0.2 to 2 parts of a radiation crosslinking initiator, (D) 0.02 to 1 part of an antistatic agent, and (E) 0.1 to 4 parts of an organic silicon compound containing a carbon-carbon double bond; The (A) acrylic ester copolymer contains unsaturated bonds, and the (A) acrylic ester copolymer has an average functionality of 3 to 50.
2. The adhesive composition according to claim 1, characterized in that: The number average molecular weight of the (A) acrylic acid ester copolymer is 40,000 to 400,000.
3. The adhesive composition according to claim 1 or 2, characterized in that: The raw material components containing (A) acrylic acid ester copolymer include (F) acrylic acid ester polymer and (G) monomer containing carboxyl group and carbon-carbon double bond.
4. The adhesive composition according to claim 3, characterized in that: Based on the total mass of the (A) acrylic ester copolymer, the mass proportion of the (G) monomer containing a carboxyl group and a carbon-carbon double bond is 0.5% to 5%; Optionally, the monomer containing (G) a carboxyl group and a carbon-carbon double bond includes at least one of acrylic acid, methacrylic acid, carboxyethyl acrylate, mono-2-(methacryloyloxy)ethyl phthalate, and mono-[2-[(2-methyl-acryloyl)oxy]ethyl] succinate.
5. The adhesive composition according to claim 4, characterized in that: The raw material components of the (F) acrylic acid ester polymer include a first methacrylate monomer, a second methacrylate monomer and (H) a monomer containing an epoxy group and a carbon-carbon double bond, wherein the first methacrylate monomer has a structural formula of CH2=C(CH3)COOR1, R1 is an alkyl group with a carbon number of 4-22, and the second methacrylate monomer has a structural formula of CH2=C(CH3)COOR2, R2 is an alkyl group with a carbon number of 1-3; Optionally, the first methacrylate monomer includes at least one of butyl acrylate, butyl methacrylate, hexyl acrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, n-octyl acrylate, isooctyl acrylate, isononyl acrylate, decyl acrylate, isodecyl acrylate, dodecyl acrylate, dodecyl methacrylate, tridecyl acrylate, tridecyl methacrylate, tetradecyl acrylate, heptadecanyl acrylate, octadecyl acrylate, and behenyl acrylate; Optionally, the second methacrylate monomer includes at least one of methyl acrylate, methyl methacrylate, ethyl methacrylate and propyl methacrylate; Optionally, the (H) monomer containing an epoxy group and a carbon-carbon double bond includes at least one of glycidyl acrylate, glycidyl methacrylate and allyl glycidyl ether.
6. The adhesive composition according to claim 1 or 2, characterized in that: The (C) radiation cross-linking initiator comprises at least one of an α-hydroxy ketone compound and a benzyl ketal compound; Optionally, the (B) diluent comprises at least one of a polyalkylene glycol containing at least one acrylate functional group and a polyalkylene glycol containing at least one allyl functional group; Optionally, the (D) antistatic agent includes at least one of pyridinium antistatic agents, imidazolium antistatic agents, phosphonium antistatic agents, sulfonium antistatic agents, pyrrolidinium antistatic agents, guanidinium antistatic agents, ammonium antistatic agents, isourea antistatic agents, thiourea antistatic agents, piperidinium antistatic agents, pyrazolium antistatic agents, methyl carbonium cation antistatic agents, lithium ion antistatic agents, morpholinium antistatic agents, sorbitol antistatic agents, polyoxyethylene alkyl ether antistatic agents, and fatty acid polyol ester antistatic agents.
7. The adhesive composition according to claim 1 or 2, characterized in that: It also includes at least one of an amide monomer, a nitrogen-containing heterocyclic vinyl monomer, a cyano-containing monomer, a vinyl-containing monomer, an aromatic vinyl-containing monomer, an imide-containing monomer, and an amino-containing monomer; Optionally, the amide monomer includes at least one of acrylamide, methacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, diacetone acrylamide, N-hydroxyethyl acrylamide, N-(isobutoxy)methacrylamide, N-vinylformamide and N-vinylacetamide; Optionally, the nitrogen-containing heterocyclic vinyl monomer includes at least one of N-vinylpyrrolidone, vinylpyridine, N-vinylpiperidone, vinylpiperazine, 2-vinylpyrazine, N-vinylimidazole, N-vinyloxazolidinone, N-ethylmorpholine and N-vinylcaprolactam; Optionally, the cyano group-containing monomer comprises at least one of acrylonitrile and methacrylonitrile; Optionally, the vinyl-containing monomer includes at least one of vinyl acetate, vinyl propionate and vinyl laurate; Optionally, the aromatic vinyl-containing monomer includes at least one of styrene, chlorostyrene, chloromethylstyrene and α-methylstyrene; Optionally, the imide group-containing monomer includes at least one of N-cyclohexylmaleimide, N-isopropylmaleimide and N-cyclohexylmaleimide; Optionally, the amino group-containing monomer includes at least one of dimethylaminoethyl acrylate, diethylaminoethyl methacrylate, dimethylaminoethyl acrylate and dimethylaminoethyl methacrylate.
8. A method for preparing an adhesive composition, characterized in that: include: (A) an acrylate copolymer, (B) a diluent, (C) a radiation crosslinking initiator, (D) an antistatic agent and an organosilicon compound are mixed to obtain an adhesive composition, wherein the (A) acrylate copolymer contains an unsaturated bond and the average functionality of the (A) acrylate copolymer is 3 to 50.
9. A pressure-sensitive adhesive, characterized in that: The pressure-sensitive adhesive is prepared from the adhesive composition described in claims 1 to 7 or the adhesive composition prepared by the method described in claim 8.
10. A protective film, characterized in that: The protective film comprises the pressure-sensitive adhesive according to claim 9.