Solvent-free rapid tackifying polyacrylate / polyurethane system adhesive and preparation method thereof
Patent Information
- Application Number
- CN202411239815.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-06
AI Technical Summary
The existing organic solvent-based acrylate adhesives pollute the environment, waste energy, and have poor safety. The water-based acrylate adhesive has a low curing rate and a low solids content.
Develop a solvent-free rapid adhesion-enhancing polyacrylate/polyurethane system adhesive, which consists of liquid polyether polyols, acrylate monomers, thermal initiators, isocyanate ethyl acrylate, polyurethane synthesis catalyst, photoinitiators and polyisocyanates, through Preparation of specific mixing and photocuring steps.
The pollution and safety problems of organic solvent-based adhesives are solved, the curing film formation rate and solid content of water-based adhesives are improved, and the preparation of low-energy and high-efficiency adhesives are achieved.
Smart Images

Figure CN119081594A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, and in particular to a solvent-free rapid tackifying polyacrylate / polyurethane system adhesive and a preparation method thereof. Background Art
[0002] In recent years, organic solvent-based acrylic adhesives have occupied most of the market in the entire adhesive field. However, with the continuous development of the economy, the defects of organic solvent-based adhesives such as environmental pollution, energy waste, and poor safety have gradually been exposed; although water-based acrylic adhesives do not contain organic solvents, are harmless to the human body, and do not pollute the environment, their curing film-forming rate is low, and their solid content is low, and their transportation costs are high; while solvent-free acrylic adhesives have a solid content of 100%, almost zero VOC emissions, and contain extremely low levels of flammable, toxic and harmful substances. They are also environmentally friendly adhesives with fast viscosity increase rate and low energy consumption. Therefore, the research on solvent-free acrylic adhesives has extremely high practical value.
[0003] Therefore, it is urgent to propose a solvent-free rapid tackifying polyacrylate / polyurethane system adhesive and a preparation method to solve the above technical problems. Summary of the invention
[0004] The purpose of the present invention is to solve the problems of environmental pollution, energy waste, poor safety, etc. formed by conventional technologies. A brief summary of the present invention is given below to provide a basic understanding of certain aspects of the present invention. It should be understood that this summary is not an exhaustive summary of the present invention. It is not intended to determine the key or important parts of the present invention, nor is it intended to limit the scope of the present invention.
[0005] The technical solution of the present invention:
[0006] A solvent-free fast-tackifying polyacrylate / polyurethane system adhesive, which is composed of liquid polyether polyol, acrylate monomer, thermal initiator, isocyanate ethyl acrylate, polyurethane synthesis catalyst, photoinitiator and polyisocyanate;
[0007] The mass fraction of liquid polyether polyol is 40-60 parts, the mass fraction of acrylate monomer is 30-60 parts, the mass fraction of thermal initiator is 0.1-0.4 parts, the mass fraction of isocyanate ethyl acrylate is 3-10 parts, the mass fraction of polyurethane synthesis catalyst is 0.02-0.06 parts, the mass fraction of photoinitiator is 0.1-0.3 parts, and the mass fraction of polyisocyanate is 3.5-14 parts.
[0008] Preferably, the liquid polyether polyol is composed of one or more of polyethylene glycol, polypropylene glycol and polybutylene glycol.
[0009] Preferably, the acrylate monomer is composed of one or more of butyl methacrylate, methyl methacrylate, methacrylic acid, hydroxyethyl methacrylate, butyl acrylate, isooctyl acrylate, acrylic acid, and hydroxyethyl acrylate.
[0010] Preferably, the thermal initiator is one or more of benzoyl peroxide, dodecyl peroxide, tert-butyl peroxide-2-ethylhexanoate, and azobisisobutyronitrile.
[0011] Preferably, the polyurethane synthesis catalyst is composed of one or more of dibutyltin dilaurate, didodecylsulfide dibutyltin, and octyltin maleate.
[0012] Preferably, the photoinitiator is one or more of hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methylphenyl acetone, diphenyl (2.4.6-triformyl) phosphine oxide, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl) butanone.
[0013] Preferably, the polyisocyanate is composed of one or more of toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate), 4,4-diisocyanate dicyclohexylmethane, and HDI trimer.
[0014] Preferably: a method for preparing a solvent-free rapid tackifying polyacrylate / polyurethane system adhesive comprises the following steps:
[0015] Step 1, weighing acrylate monomer and part of thermal initiator, mixing them evenly to form a mixed solution for standby use;
[0016] Step 2: Put the liquid polyether polyol into a reaction vessel and apply nitrogen protection to the reaction system, stir and heat at the same time, add 10-20% of the mixed solution into the reaction vessel after stirring and heating, and start to drop the remaining mixed solution after 15-30 minutes, and the dropping time is 2-3 hours;
[0017] Step 3: After the mixed solution is completely added, keep warm and react for 0.5-1h;
[0018] Step 4: After the heat preservation is completed, the remaining thermal initiator is added, and the temperature is raised after the heat preservation for 2-3 hours, and the temperature is kept for 1-2 hours after the temperature is raised to obtain a solution;
[0019] Step 5, cooling the solution, adding a polyurethane synthesis catalyst to the reaction system after cooling, and then dripping ethyl isocyanate acrylate for 0.5-1h;
[0020] Step 6: After all the isocyanate ethyl acrylate is added, heat-retaining reaction is performed for 2-4 hours. After the heat-retaining reaction is completed, stirring and cooling are performed;
[0021] Step 7: After cooling, add photoinitiator and polyisocyanate, stir again, stir evenly, and then perform photocuring at 330-395nm ultraviolet wavelength for 30-90s;
[0022] Step 8: After light curing, the cured product is aged for 6-12 hours. After complete ripening, a polyacrylate / polyurethane system adhesive is obtained.
[0023] Preferably: the stirring rate is 100-200r / min, the heating temperature in step 2 is 65-80°C, the heating temperature in step 4 is 90-100°C, the cooling temperature in step 5 is 70-80°C, and the aging temperature in step 8 is 70-80°C.
[0024] The present invention has the following beneficial effects:
[0025] The invention solves the problems of organic solvent-based acrylic adhesives polluting the environment, wasting energy and having poor safety.
[0026] The present invention solves the problem that the water-based acrylic adhesive has a low curing film-forming rate and a low solid content. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Schematic diagram of the preparation of the solvent-free rapid tackifying polyacrylate / polyurethane system adhesive in Example 1. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is described below by the specific embodiments shown in the accompanying drawings. However, it should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0029] Specific implementation method 1: Combination Figure 1 The present embodiment is described as follows: a solvent-free rapid tackifying polyacrylate / polyurethane system adhesive of the present embodiment, wherein the solvent-free rapid tackifying polyacrylate / polyurethane system adhesive is composed of liquid polyether polyol, acrylate monomer, thermal initiator, isocyanate ethyl acrylate, polyurethane synthesis catalyst, photoinitiator and polyisocyanate;
[0030] The mass fraction of liquid polyether polyol is 40-60 parts, the mass fraction of acrylate monomer is 30-60 parts, the mass fraction of thermal initiator is 0.1-0.4 parts, the mass fraction of isocyanate ethyl acrylate is 3-10 parts, the mass fraction of polyurethane synthesis catalyst is 0.02-0.06 parts, the mass fraction of photoinitiator is 0.1-0.3 parts, and the mass fraction of polyisocyanate is 3.5-14 parts.
[0031] Specific implementation method 2: Combination Figure 1 The present embodiment is described as a solvent-free fast-tackifying polyacrylate / polyurethane system adhesive, wherein the liquid polyether polyol type is composed of one or more of polyethylene glycol, polypropylene glycol, and polybutylene glycol.
[0032] Specific implementation method three: Combination Figure 1 To illustrate this embodiment, a solvent-free fast-tackifying polyacrylate / polyurethane system adhesive according to this embodiment also includes that the acrylate monomer is composed of one or more of butyl methacrylate, methyl methacrylate, methacrylic acid, hydroxyethyl methacrylate, butyl acrylate, isooctyl acrylate, acrylic acid, and hydroxyethyl acrylate.
[0033] Specific implementation method four: Combination Figure 1 The present embodiment is described as a solvent-free rapid tackifying polyacrylate / polyurethane system adhesive, wherein the thermal initiator is composed of one or more of benzoyl peroxide, dodecyl peroxide, tert-butyl peroxy-2-ethylhexanoate, and azobisisobutyronitrile.
[0034] Specific implementation method five: Combination Figure 1 The present embodiment is described as a solvent-free rapid tackifying polyacrylate / polyurethane system adhesive, wherein the polyurethane synthesis catalyst is composed of one or more of dibutyltin dilaurate, di(dodecylsulfide) dibutyltin, and octyltin maleate.
[0035] Specific implementation method six: Combination Figure 1 The present embodiment is described as a solvent-free fast-thickening polyacrylate / polyurethane system adhesive, wherein the photoinitiator is composed of one or more of hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methylphenyl acetone, diphenyl (2.4.6-triformyl) phosphine oxide, and 2-benzyl-2-dimethylamino-1-(4-morpholinephenyl) butanone.
[0036] Specific implementation method seven: Combination Figure 1The present embodiment is described as a solvent-free fast-tackifying polyacrylate / polyurethane system adhesive, wherein the polyisocyanate is composed of one or more of toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate), 4,4-diisocyanate dicyclohexylmethane, and HDI trimer.
[0037] Specific implementation method eight: Combination Figure 1 This embodiment is described. A method for preparing a solvent-free rapid tackifying polyacrylate / polyurethane system adhesive in this embodiment comprises the following steps:
[0038] Step 1, weighing acrylate monomer and part of thermal initiator, mixing them evenly to form a mixed solution for standby use;
[0039] Step 2: Put the liquid polyether polyol into a reaction vessel and apply nitrogen protection to the reaction system, stir and heat at the same time, add 10-20% of the mixed solution into the reaction vessel after stirring and heating, and start to drop the remaining mixed solution after 15-30 minutes, and the dropping time is 2-3 hours;
[0040] Step 3: After the mixed solution is completely added, keep warm and react for 0.5-1h;
[0041] Step 4: After the heat preservation is completed, the remaining thermal initiator is added, and the temperature is raised after the heat preservation for 2-3 hours, and the temperature is kept for 1-2 hours after the temperature is raised to obtain a solution;
[0042] Step 5, cooling the solution, adding a polyurethane synthesis catalyst to the reaction system after cooling, and then dripping ethyl isocyanate acrylate for 0.5-1h;
[0043] Step 6: After all the isocyanate ethyl acrylate is added, heat-retaining reaction is performed for 2-4 hours. After the heat-retaining reaction is completed, stirring and cooling are performed;
[0044] Step 7: After cooling, add photoinitiator and polyisocyanate, stir again, stir evenly, and then perform photocuring at 330-395nm ultraviolet wavelength for 30-90s;
[0045] Step 8: After light curing, the cured product is matured for 6-12 hours. After the matured product is fully matured, a polyacrylate / polyurethane system adhesive is obtained.
[0046] Specific implementation method nine: Combination Figure 1The present embodiment describes a method for preparing a solvent-free rapid tackifying polyacrylate / polyurethane system adhesive, wherein the stirring rate is 100-200 r / min, the heating temperature in step 2 is 65-80°C, the heating temperature in step 4 is 90-100°C, the cooling temperature in step 5 is 70-80°C, and the aging temperature in step 8 is 70-80°C.
[0047] The present invention is described in detail below in conjunction with various embodiments, but it should be noted that these embodiments are not limitations of the present invention, and any equivalent transformations or substitutions in functions, methods, or structures made by ordinary technicians in the field based on these embodiments are all within the scope of protection of the present invention.
[0048] Example 1
[0049] Step 1: Weigh 10g of butyl acrylate, 40g of isooctyl acrylate, 5g of hydroxyethyl acrylate, 5g of acrylic acid, and 0.24g of azobisisobutyronitrile, mix well to form a mixed solution for standby use;
[0050] Step 2: Weigh 60g of PEG500 into a reaction vessel and apply nitrogen protection to the reaction system. Stir at a rate of 200r / min and heat to 65°C, then add 20% of the mixed solution into the reaction vessel, and start to drop the remaining mixed solution after 30min, and the dropping time is 3h;
[0051] Step 3: After the mixed solution is completely added, keep warm and react for 1 hour;
[0052] Step 4: Add the remaining 0.06 g of azobisisobutyronitrile, keep warm for 3 hours, then raise the temperature to 90°C and keep warm at 90°C for 1 hour;
[0053] Step 5: After the reaction system in step 4 is cooled to 70° C., 0.02 g of dibutyltin dilaurate is weighed and added to the reaction system, and then 7 g of ethyl isocyanate acrylate is weighed and added dropwise for 0.5 h;
[0054] Step 6: After all the ethyl isocyanate acrylate is added, heat and react for 4 hours, stir and cool to discharge;
[0055] Step 7: Weigh 0.3g TPO, 4g HDI, and 10g HDI trimer, stir evenly with the product in step 6 at a rate of 100r / min, and then perform photocuring at a UV wavelength of 395nm for 30s;
[0056] Step 8: The photocured product is placed at 70° C. for aging for 6 hours, and a polyacrylate / polyurethane system adhesive is obtained after complete aging.
[0057] Example 2
[0058] Step 1: Weigh 12g of butyl methacrylate, 15g of methyl methacrylate, 3g of hydroxyethyl methacrylate, and 0.16g of benzoyl peroxide, mix them evenly to form a mixed solution for standby use;
[0059] Step 2: Weigh 60g of PTMEG1000 into a reaction vessel and apply nitrogen protection to the reaction system. Stir at a rate of 200r / min and heat to 80°C, then add 10% of the mixed solution in step 1 into the reaction vessel, and start adding the remaining mixed solution dropwise after 15min, and the addition time is 2h;
[0060] Step 3: After the mixed solution is completely added, keep warm and react for 0.5h;
[0061] Step 4: Add the remaining 0.04 g of benzoyl peroxide, keep warm for 2 h, then raise the temperature to 100 °C and keep warm at 100 °C for 1 h;
[0062] Step 5: After the reaction system in step 4 is cooled to 80° C., 0.03 g of octyltin maleate is weighed and added to the reaction system, and then 6.5 g of ethyl isocyanate acrylate is weighed and added dropwise for 1 hour;
[0063] Step 6: After all the ethyl isocyanate acrylate is added, heat and react for 4 hours, stir and cool to discharge;
[0064] Step 7: Weigh 0.3g 1173, 1g TDI, and 2.5g HDI trimer, stir evenly with the product in step 6 at a rate of 100r / min, and then perform photocuring at a UV wavelength of 330nm for 90s;
[0065] Step 8: The photocured product is placed at 80° C. for aging for 12 hours, and a polyacrylate / polyurethane system adhesive is obtained after complete aging.
[0066] Example 3
[0067] Step 1: Weigh 22g of butyl acrylate, 4g of methacrylic acid, 4g of hydroxyethyl methacrylate, and 0.08g of dodecyl peroxide, mix them evenly to form a mixed solution for standby use;
[0068] Step 2: Weigh 40g of PPG1000 into a reaction vessel and apply nitrogen protection to the reaction system. Stir at a rate of 200r / min and heat to 70°C, then add 15% of the mixed solution in step 1 into the reaction vessel, and start adding the remaining mixed solution dropwise after 20min, and the dropping time is 2h;
[0069] Step 3: After the mixed solution is completely added, keep warm and react for 0.5h;
[0070] Step 4: Add the remaining 0.02 g of dodecyl peroxide, keep warm for 2 hours, then raise the temperature to 90°C and keep warm at 90°C for 2 hours;
[0071] Step 5: After the reaction system in step 4 is cooled to 80° C., 0.05 g of dibutyltin(dodecylsulfide) is weighed and added to the reaction system, and then 3 g of ethyl isocyanate acrylate is weighed and added dropwise for 0.5 h;
[0072] Step 6: After all the isocyanate ethyl acrylate is added, heat and react for 2 hours, stir and cool to discharge;
[0073] Step 7: Weigh 0.1g 369, 1.7g HMDI, and 2.5g HDI trimer, stir evenly with the product in step 6 at a rate of 100r / min, and then perform photocuring at a UV wavelength of 395nm for 60s;
[0074] Step 8: The photocured product is placed at 80° C. for aging for 12 hours, and a polyacrylate / polyurethane system adhesive is obtained after complete aging.
[0075] Example 4
[0076] Step 1: Weigh 15g of butyl acrylate, 20g of isooctyl acrylate, 5g of hydroxyethyl acrylate, and 0.12g of tert-butyl peroxy-2-ethylhexanoate, mix them evenly to form a mixed solution for standby use;
[0077] Step 2: Weigh 30g PEG500 and 20g PPG1000 into a reaction vessel and apply nitrogen protection to the reaction system. Stir at a rate of 200r / min and heat to 75°C, then add 20% of the mixed solution in step 1 into the reaction vessel, and start to dropwise add the remaining mixed solution after 20min, and the dropping time is 3h;
[0078] Step 3: After the mixed solution is completely added, keep warm and react for 0.5h;
[0079] Step 4: add the remaining 0.03 g of tert-butyl peroxy-2-ethylhexanoate, keep the temperature for 2 hours, then raise the temperature to 100°C and keep the temperature at 100°C for 1 hour;
[0080] Step 5: After the reaction system in step 4 is cooled to 80° C., 0.06 g of octyltin maleate is weighed and added to the reaction system, and then 10 g of ethyl isocyanate acrylate is weighed and added dropwise for 1 hour;
[0081] Step 6: After all the ethyl isocyanate acrylate is added, heat and react for 3 hours, stir and cool to discharge;
[0082] Step 7: Weigh 0.3 g 184, 3 g IPDI, and 3.3 g HDI trimer, stir evenly with the product in step 6 at a rate of 100 r / min, and then perform photocuring at a UV wavelength of 330 nm for 30 s;
[0083] Step 8: The photocured product is placed at 80° C. for aging for 12 hours, and a polyacrylate / polyurethane system adhesive is obtained after complete aging.
[0084] Example 5
[0085] Step 1: Weigh 12g of butyl methacrylate, 15g of isooctyl acrylate, 3g of hydroxyethyl methacrylate, and 0.08g of azobisisobutyronitrile, mix well to form a mixed solution for standby use;
[0086] Step 2: Weigh 20g PEG500 and 20g PTMEG1000 into a reaction vessel and apply nitrogen protection to the reaction system. Stir at a rate of 200r / min and heat to 65°C, then add 10% of the mixed solution in step 1 into the reaction vessel, and start adding the remaining mixed solution dropwise after 30min, and the addition time is 3h;
[0087] Step 3: After the mixed solution is completely added, keep warm and react for 1 hour;
[0088] Step 4: Add the remaining 0.02 g of azobisisobutyronitrile, keep warm for 3 hours, then raise the temperature to 90°C and keep warm at 90°C for 1 hour;
[0089] Step 5: After the reaction system in step 4 is cooled to 70° C., 0.02 g of dibutyltin dilaurate is weighed and added to the reaction system, and then 5 g of ethyl isocyanate acrylate is weighed and added dropwise for 0.5 h;
[0090] Step 6: After all the isocyanate ethyl acrylate is added, heat and react for 4 hours, stir and cool to discharge;
[0091] Step 7: Weigh 0.2g 369 and 6.7g HDI trimer, stir evenly with the product in step 6 at a rate of 100r / min, and then perform photocuring at a UV wavelength of 395nm for 60s;
[0092] Step 8: The photocured product is placed at 70° C. for aging for 9 hours, and a polyacrylate / polyurethane system adhesive is obtained after complete aging.
[0093] Example 6
[0094] Step 1: Weigh 25g of isooctyl acrylate, 10g of acrylic acid, 5g of hydroxyethyl acrylate, and 0.3g of azobisisobutyronitrile, mix well to form a mixed solution for standby use;
[0095] Step 2: Weigh 20g PEG500, 20g PPG1000, and 10g PTMEG1000 into a reaction vessel and apply nitrogen protection to the reaction system. Stir at a rate of 200r / min and heat to 70°C, then add 15% of the mixed solution in step 1 into the reaction vessel, and start adding the remaining mixed solution dropwise after 20min, and the addition time is 2h;
[0096] Step 3: After the mixed solution is completely added, keep warm and react for 1 hour;
[0097] Step 4: Add the remaining 0.1 g of azobisisobutyronitrile, keep warm for 3 hours, then raise the temperature to 90°C and keep warm at 90°C for 2 hours;
[0098] Step 5: After the reaction system in step 4 is cooled to 70° C., 0.03 g of dibutyltin dilaurate is weighed and added to the reaction system, and then 6 g of ethyl isocyanate acrylate is weighed and added dropwise for 1 hour;
[0099] Step 6: After all the ethyl isocyanate acrylate is added, heat and react for 3 hours, stir and cool to discharge;
[0100] Step 7: Weigh 0.25g 184, 4.5g HDI, and 3g HDI trimer, stir evenly with the product in step 6 at a rate of 100r / min, and then perform photocuring at a UV wavelength of 330nm for 30s;
[0101] Step 8: The photocured product is placed at 70° C. for aging for 12 hours, and a polyacrylate / polyurethane system adhesive is obtained after complete aging.
[0102] The performance test of the polyacrylate / polyurethane system adhesive obtained in Examples 1 to 6 was carried out, and the results are shown in the following table:
[0103]
[0104] The test temperature was from room temperature to 200°C, and the heating rate was 5°C / min.
[0105] Tensile strength and elongation at break test: Based on GB / T1040-2006 as the test standard, the molded samples were cut into 1BA-type specimens. Each group of test specimens has 5 specimens, with a thickness of 2-3mm, a test gauge length of 25mm, a fixture spacing of 58mm, a displacement rate of 100mm / min, and a test temperature of 25°C.
[0106] Adhesion strength test: GB / T2790-1995 is used as the test standard. The bonded PET film is cut into 25mm wide strips. The unbonded end of the PET film is bent 180° and clamped on a fixed chuck. The other end of the bonded PET film is clamped on another chuck. Each group of test strips has 5 samples. The separation rate of the chuck is 100mm / min. The test temperature is 25℃.
[0107] It should be noted that in the above embodiments, as long as the technical solutions are not contradictory, they can be arranged and combined, and those skilled in the art can exhaust all possibilities based on the mathematical knowledge of arrangement and combination. Therefore, the present invention will no longer describe the technical solutions after arrangement and combination one by one, but it should be understood that the technical solutions after arrangement and combination have been disclosed by the present invention.
[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A solvent-free rapid tackifying polyacrylate / polyurethane system adhesive, characterized in that: The solvent-free rapid tackifying polyacrylate / polyurethane system adhesive is composed of liquid polyether polyol, acrylate monomer, thermal initiator, isocyanate ethyl acrylate, polyurethane synthesis catalyst, photoinitiator and polyisocyanate; The mass fraction of liquid polyether polyol is 40-60 parts, the mass fraction of acrylate monomer is 30-60 parts, the mass fraction of thermal initiator is 0.1-0.4 parts, the mass fraction of isocyanate ethyl acrylate is 3-10 parts, the mass fraction of polyurethane synthesis catalyst is 0.02-0.06 parts, the mass fraction of photoinitiator is 0.1-0.3 parts, and the mass fraction of polyisocyanate is 3.5-14 parts.
2. The solvent-free rapid tackifying polyacrylate / polyurethane system adhesive according to claim 1, characterized in that: The liquid polyether polyol is composed of one or more of polyethylene glycol, polypropylene glycol and polybutylene glycol.
3. The solvent-free rapid tackifying polyacrylate / polyurethane system adhesive according to claim 1, characterized in that: The acrylic acid ester monomer is composed of one or more of butyl methacrylate, methyl methacrylate, methacrylic acid, hydroxyethyl methacrylate, butyl acrylate, isooctyl acrylate, acrylic acid, and hydroxyethyl acrylate.
4. The solvent-free rapid tackifying polyacrylate / polyurethane system adhesive according to claim 1, characterized in that: The thermal initiator is composed of one or more of benzoyl peroxide, dodecyl peroxide, tert-butyl peroxide-2-ethylhexanoate and azobisisobutyronitrile.
5. The solvent-free rapid tackifying polyacrylate / polyurethane system adhesive according to claim 1, characterized in that: The polyurethane synthesis catalyst is composed of one or more of dibutyltin dilaurate, didodecylsulfide dibutyltin, and octyltin maleate.
6. The solvent-free rapid tackifying polyacrylate / polyurethane system adhesive according to claim 1, characterized in that: The photoinitiator is composed of one or more of hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methylphenyl acetone, diphenyl (2.4.6-triformyl) phosphine oxide, and 2-benzyl-2-dimethylamino-1-(4-morpholinephenyl) butanone.
7. The solvent-free rapid tackifying polyacrylate / polyurethane system adhesive according to claim 1, characterized in that: The polyisocyanate is composed of one or more of toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, 4,4-diisocyanate dicyclohexylmethane and HDI trimer.
8. A method for preparing a solvent-free rapid tackifying polyacrylate / polyurethane system adhesive, characterized in that: The steps include: Step 1, weighing acrylate monomer and part of thermal initiator, mixing them evenly to form a mixed solution for standby use; Step 2: Put the liquid polyether polyol into a reaction vessel and apply nitrogen protection to the reaction system, stir and heat at the same time, add 10-20% of the mixed solution into the reaction vessel after stirring and heating, and start to drop the remaining mixed solution after 15-30 minutes, and the dropping time is 2-3 hours; Step 3: After the mixed solution is completely added, keep warm and react for 0.5-1h; Step 4: After the heat preservation is completed, the remaining thermal initiator is added, and the temperature is raised after the heat preservation for 2-3 hours, and the temperature is kept for 1-2 hours after the temperature is raised to obtain a solution; Step 5, cooling the solution, adding a polyurethane synthesis catalyst to the reaction system after cooling, and then dripping ethyl isocyanate acrylate for 0.5-1h; Step 6: After all the isocyanate ethyl acrylate is added, heat-retaining reaction is performed for 2-4 hours. After the heat-retaining reaction is completed, stirring and cooling are performed; Step 7: After cooling, add photoinitiator and polyisocyanate, stir again, stir evenly, and then perform photocuring at 330-395nm ultraviolet wavelength for 30-90s; Step 8: After light curing, the cured product is matured for 6-12 hours. After the matured product is fully matured, a polyacrylate / polyurethane system adhesive is obtained.
9. The method for preparing a solvent-free rapid tackifying polyacrylate / polyurethane system adhesive according to claim 8, characterized in that: The stirring rate is 100-200 r / min, the heating temperature in step 2 is 65-80°C, the heating temperature in step 4 is 90-100°C, the cooling temperature in step 5 is 70-80°C, and the aging temperature in step 8 is 70-80°C.
Citation Information
Cited By
Dynamic balance UV adhesive as well as preparation method and application thereof
CN120310441A