Light conversion material and preparation method thereof
By preparing light conversion materials combined with Y2O3:Eu3+, BaMgAl10O17:Eu2+ and CaSrAl2SiO7:Eu3+, etc., the light conversion efficiency, stability and compatibility problems in the prior art are solved, and efficient light conversion and long-term stability are achieved. Improve the application effect in agriculture and photovoltaic fields.
Patent Information
- Application Number
- CN202410995786.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure CN119081695A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of materials, and in particular to a light conversion material and a preparation method thereof. Background Art
[0002] In the existing technology, light conversion materials have shown broad application prospects in many fields, such as agriculture, photovoltaics, etc. However, there are still some defects in the current light conversion materials, which are mainly reflected in the following aspects:
[0003] Photoconversion efficiency: The photoconversion efficiency of some light-conversion materials is not high enough to fully convert light of a specific wavelength into light required by plants or efficiently used by photovoltaic cells. This limits the application effect of light-conversion materials in improving photosynthesis efficiency or photovoltaic cell performance.
[0004] Stability issues: When many light-conversion materials are used for a long time or exposed to certain environmental conditions (such as high temperature, high humidity, ultraviolet radiation, etc.), their light conversion performance will gradually decline or even fail. This stability issue seriously affects the long-term application effect of light-conversion materials.
[0005] Poor dispersion: When some light-converting materials are added to substrates such as resin, they tend to be unevenly dispersed. This not only affects the performance of the light-converting materials, but may also have an adverse effect on other properties of the substrate.
[0006] Poor compatibility: Some light-converting materials have poor compatibility with substrates such as resins, which leads to agglomeration and stratification during the preparation process. This not only increases the difficulty and cost of preparation, but may also affect the performance and quality of the final product.
[0007] In order to solve the above problems, the applicant proposes a light conversion material and a preparation method thereof. Summary of the invention
[0008] The object of the present invention is to provide a light conversion material and a preparation method thereof to solve the problems in the prior art.
[0009] To achieve the above object, the present invention provides the following technical solution: a method for preparing a light conversion material, the specific steps are as follows:
[0010] S1. Preparation of Y2O3:Eu 3+ ;
[0011] S2. Preparation of BaMgAl 10 O 17 :Eu 2+
[0012] S3, mixing aluminum oxide and silicon dioxide in a molar ratio of 2:1 and calcining to obtain aluminosilicate;
[0013] S4, putting the aluminosilicate, strontium carbonate, calcium carbonate, barium oxide and europium oxide prepared in step S3 into a mortar and grinding them thoroughly for 1 hour;
[0014] S5. Add boric acid to the obtained powder, mix it, and calcine it in a tube furnace for 3 hours. Then cool it naturally to room temperature to obtain the light conversion material CaSrAl2SiO7:Eu 3+ ;
[0015] S6, use a high-speed mixer to mix Y2O3:Eu 3+ 、CaSrAl2SiO7:Eu 3+ 、BaMgAl 10 O 17 :Eu 2+ XT-SZ light conversion material is made by mixing in different proportions.
[0016] Optionally, the step S1 includes preparing Y2O3:Eu 3+ The steps are as follows:
[0017] S1-1, dissolving Eu2O3 and Y2O3 in concentrated nitric acid in a molar ratio of 9:1;
[0018] S1-2, adding oxalic acid with a concentration of 1.49 mol / L as a precipitant to obtain a rare earth oxalic acid precursor;
[0019] S1-3, calcining the rare earth oxalate precursor at 1300℃ in a tube furnace for 3h, and cooling it naturally to room temperature to obtain Y2O3:Eu 3+ Solid powder.
[0020] Optionally, the step S2 includes preparing BaMgAl 10 O 17 :Eu 2+ The steps are as follows: S2-1, put europium oxide, barium oxide, magnesium oxide and aluminum oxide in a certain proportion in a mortar and grind them thoroughly for 1 hour;
[0021] S2-2, the obtained powder was placed in a tube furnace and calcined at 1300℃ for 3h to obtain BaMgAl 10 O 17 :Eu 2+ Precursor raw materials;
[0022] S2-3, BaMgAl 10 O 17 :Eu 2+ 2% NH4Cl flux was added to the precursor raw material, and secondary sintering was performed in CS2 reducing gas atmosphere at 1250℃-1450℃ for 2h, and then naturally cooled to room temperature to obtain BaMgAl 10 O17 :Eu 2+ powder.
[0023] Optionally, the ratio of the components in step S2-1 is 12-14 parts of europium oxide, 18-20 parts of barium oxide, 50-55 parts of magnesium oxide, and 13-15 parts of aluminum oxide.
[0024] Optionally, the S6 step includes Y2O3:Eu 3+ 1-6 parts, CaSrAl2SiO7:Eu 3+ 1-4 parts, BaMgAl 10 O 17 :Eu 2+ For 1 portion.
[0025] A light conversion material is prepared by the method for preparing a light conversion material according to any one of claims 1 to 4.
[0026] Beneficial effect: The main emission peaks of the XT-SZ light-conversion material prepared by the patented method are mainly located at about 450nm (blue light region) and 620nm (red light region). 3+ As the ratio increases, the relative intensity ratio of red and blue light of the main emission peak of XT-SZ shows a positive correlation. 3+ 、CaSrAl2SiO7:Eu 3+ 、BaMgAl 10 O 17 :Eu 2+ When the ratio is 2:2:1 and 6:4:1, the relative intensity ratio of red and blue light increases significantly. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Example (a) Y2O3:Eu 3+ XRD pattern of (b) Y2O3:Eu 3+ The full spectrum of XPS;
[0028] Figure 2 Example (a) Y2O3:Eu 3+ Excitation spectrum of (b) Y2O3:Eu 3+ Emission spectrum (c) Fluorescence image under UV light (d) Y2O3:Eu 3+ CIE diagram of
[0029] Figure 3 It is the embodiment of the present invention Y2O3:Eu 3+ Thermogravimetric analysis curve of
[0030] Figure 4 Example (a) BaMgAl10 O 17 :Eu 2+ XRD pattern of (b)BaMgAl 10 O 17 :Eu 2+ The full spectrum of XPS;
[0031] Figure 5 Example (a) BaMgAl 10 O 17 :Eu 2+ Excitation spectrum of (b) BaMgAl 10 O 17 :Eu 2+ Emission spectrum (c) Fluorescence image under UV light (d) BaMgAl 10 O 17 :Eu 2+ CIE diagram of
[0032] Figure 6 The present invention embodiment BaMgAl 10 O 17 :Eu 2+ Thermogravimetric analysis curve of
[0033] Figure 7 Example (a) of the present invention CaSrAl2SiO7:Eu 3+ XRD spectrum (b) CaSrAl2SiO7:Eu 3+ XPS full spectrum;
[0034] Figure 8 Example (a) of the present invention CaSrAl2SiO7:Eu 3+ Excitation spectrum (b) CaSrAl2SiO7:Eu 3+ Emission spectrum (c) Fluorescence image under UV light (d) CaSrAl2SiO7:Eu 3+ CIE diagram of
[0035] Fig. 9 The embodiment of the present invention is CaSrAl2SiO7:Eu 3+ Thermogravimetric analysis curve;
[0036] Fig.10 is the particle size distribution diagram of XT-SZ treated with 5 kinds of embodiments of the present invention;
[0037] Fig.11 It is the XRD result diagram of the sample of the embodiment of the present invention;
[0038] Fig.12 These are SEM images of XT-SZ light conversion materials processed in Example 5 of the present invention. DETAILED DESCRIPTION
[0039] The following describes the preferred embodiments of the present invention with reference to the drawings in the specification, so that the technical content is clearer and easier to understand. The present invention can be embodied in many different forms of embodiments, and the protection scope of the present invention is not limited to the embodiments mentioned in the text.
[0040] Example 1
[0041] Preparation of Y2O3:Eu 3+
[0042] 31.67g Eu2O3 and 2.26g Y2O3 were dissolved in 55.6g concentrated nitric acid at a molar ratio of 9:1, and 67mL 1.49mol / L oxalic acid was added as a precipitant to obtain a rare earth oxalic acid precursor. The precursor was calcined at 1300℃ for 3h in a tube furnace and cooled naturally to room temperature to obtain Y2O3:Eu 3+ Solid powder.
[0043] Preparation of BaMgAl 10 O 17 :Eu 2+
[0044] 21.12g europium oxide, 13.34g barium oxide, 9.65g magnesium oxide and 6.76g aluminum oxide were ground in a mortar for 1 hour and calcined in a tube furnace at 1300℃ for 3 hours to prepare BaMgAl 10 O 17 :Eu 2+ The precursor raw material is added with 2% NH4Cl flux, and then sintered for 2 hours at 1250-1450℃ in CS2 reducing gas atmosphere, and then cooled naturally to room temperature to obtain BaMgAl 10 O 17 :Eu 2+ powder.
[0045] Preparation of CaSrAl2SiO7:Eu 3+
[0046] 20.2g of aluminum oxide and 6g of silicon dioxide were mixed and calcined in a molar ratio of 2:1 to obtain aluminosilicate. 25g of aluminosilicate, 8.2g of strontium carbonate, 6.7g of calcium carbonate, 8.9g of barium oxide, and 10.55g of europium oxide were put into a mortar and ground for 1h. 5g of boric acid was added and mixed. The mixture was calcined at 1300°C for 3h in a tubular furnace and naturally cooled to room temperature to obtain a light conversion material.
[0047] Preparation of XT-SZ
[0048] Use high speed mixer to mix Y2O3:Eu 3+ 、CaSrAl2SiO7:Eu 3+、BaMgAl 10 O 17 :Eu 2+ The XT-SZ light conversion materials were prepared by mixing in ratios of 1:1:1, 2:1:1, 2:2:1, 4:2:1, and 6:4:1 (respectively represented by XT-SZ1, XT-SZ2, XT-SZ3, XT-SZ4, and XT-SZ5).
[0049] XRD test on the sample: lay the sample flat on the quartz tank, press the sample, use Cu-Kα ray (wavelength 0.15416nm), voltage 40kV, current 40mA, scanning speed 0.02° / min, test range 5-90°. XPS test: press the sample into small pieces, put the table into the sample delivery room to evacuate, set WaitObject to 20s, turn on the X-ray gun, narrow spectrum passenergy is 30eV (step length 0.1eV), full spectrum passenergy 150eV (step length 1.0eV). Fluorescence spectrum test: use xenon lamp as excitation light source, configure R928 photomultiplier tube, excitation and emission light slit width 5nm, dissolve the light conversion material in the cuvette, set the excitation wavelength, start wavelength and end wavelength, and measure the corresponding fluorescence spectrum. TG test: The sample is evenly distributed on the sample plate, and the test is carried out in a nitrogen flow, with a flow rate of 10mL / min for nitrogen replacement, and the temperature is increased from 25℃ to 800℃ at a rate of 10℃ / min, and the relationship between the sample mass and temperature is recorded. SEM test: A small piece of double-sided tape is fixed on an aluminum short rod, and the sample powder is sprinkled on the surface of the short rod and dispersed, and the particle shape and surface characteristics of the sample are measured, and the SEM is used to take pictures, and the voltage is 20kV.
[0050] Y2O3:Eu 3+ Performance
[0051] The fluorescent host is Y2O3:Eu 3+ , which is a cubic crystal structure, and its luminescence mainly comes from its internal structure, Eu 3+ ion as the central ion and Y2O3 crystal as the main body. XRD was used to further analyze the Y2O3:Eu 3+ The crystal structure, such as Figure 1 (a), the spectrum clearly shows strong diffraction peaks at 20.48°, 29.11°, 33.81°, 48.56° and 57.61°. These typical characteristic peaks correspond to the (211), (222), (400), (440) and (622) crystal planes of THT, respectively. The crystal structure of the phosphor is quite uniform, indicating that Y2O3:Eu 3+ Solids were formed with no side products or residual products.
[0052] Y2O3:Eu was tested by XPS 3+ The chemical valence and composition of the surface, such as Figure 2 As shown in (b), it can be seen from the full XPS spectrum that the peaks of binding energy at 156.4 eV, 284.8 eV, 527.88 eV, and 1133.59 eV correspond to Y3d, C1s, O1s, and Eu3d, respectively.
[0053] Y2O3:Eu 3+ Optical properties
[0054] like Figure 2 As shown in (a), the optimal excitation spectrum of the red light conversion material Ex = 365nm is first determined by backscanning the excitation wavelength, and the emission spectrum of the light conversion material is tested with the excitation wavelength Ex = 365nm as the benchmark. Figure 2 (b) It can be seen that the light conversion material can emit red light at 618nm. The fluorescence data show that with the addition of the light conversion material, the light conversion material can convert the ultraviolet light from the sun into the red light required for plant growth. Figure 2 As shown in (c) and 2(d), the light-converting material can be observed to exhibit visible red fluorescence under UV light, and the CIE chromaticity coordinates are calculated based on the emission spectrum data, which are located in the red region.
[0055] Y2O3:Eu 3+ Thermal stability
[0056] When light-converting materials are incorporated into agricultural films to prepare light-converting agricultural films, a processing temperature of 200°C is required. Therefore, the thermal stability of light-converting materials is also an important factor in determining whether they can be used in light-converting agricultural films. Figure 3 As shown, the red light conversion material maintains good thermal stability in the range of 0-800°C and can exist stably when preparing light conversion agricultural film.
[0057] BaMgAl 10 O 17 :Eu 2+ Performance
[0058] BaMgAl 10 O 17 :Eu 2+ It is a hexagonal close-packed crystal, Eu 2+ ion is the central ion, replacing the Ba in the mirror layer 2+ The samples prepared by high temperature solid phase method were further analyzed by XRD. 10 O 17 :Eu 2+ The crystal structure of the powder. Figure 4(a), the spectrum clearly shows strong diffraction peaks at 18.80°, 20.13°, 31.94°, 33.54°, 35.76°, 42.06°, 44.28° and 66.48°. These typical characteristic peaks correspond to the (101), (102), (110), (107), (114), (205), (208) and (220) crystal planes, respectively. 10 O 17 :Eu 2+ It is the main phase, but there are a small amount of Al2O3 and BaAl2O4 impurity peaks, which may be caused by the synthesis temperature not being high enough. The effect is not significant. The peak intensity is very strong, indicating that the crystallization performance is improving. The body color of the sample is white, belonging to the hexagonal crystal system, and its unit cell parameters are: a = 0.5612 (6) nm, c = 2.2782 (9) nm, V = 0.6205 (2) nm 3 .
[0059] The surface element distribution of the blue light-converting material was tested by XPS, such as Figure 4 As shown in (b), it can be seen from the full XPS spectrum that the peaks of binding energy at 73.73 eV, 101.53 eV, 284.45 eV, 530.65 eV, 780.19 eV, 1135.27 eV, and 1303.47 eV correspond to Al2p, Si2p, C1s, O1s, Ba3d, Eu3d, and Mg1s, respectively.
[0060] BaMgAl 10 O 17 :Eu 2+ Optical properties
[0061] like Figure 5 As shown in (a) and (b), the optimal excitation spectrum of the blue light conversion material Ex = 340nm is first determined by backscanning the excitation wavelength. The emission spectrum of the blue light conversion material is tested with the excitation wavelength Ex = 340nm as the benchmark. It can be seen that the fluorescence intensity of the emission spectrum reaches the maximum at 456nm. The light conversion material can convert the ultraviolet light irradiated by the sun into the blue light required for plant growth. Figure 5 As shown in (c) and (d), the solid powder can be observed to exhibit visual blue fluorescence under UV light, and the CIE chromaticity coordinates are calculated based on the emission spectrum data, which are located in the blue area.
[0062] BaMgAl 10 O 17 :Eu 2+ Thermal stability
[0063] Thermogravimetric analysis curve Figure 6It can be seen that the light conversion material remains intact at 800°C without any mass loss and has good thermal stability. Therefore, the inorganic blue light conversion material can meet the temperature requirements for preparing agricultural film.
[0064] CaSrAl2SiO7:Eu 3+ Characterization
[0065] like Figure 7 (a) CaSrAl2SiO7:Eu was further analyzed by XRD. 3+ The crystal structure of the solid powder tested the diffraction peaks at 10-80°. There are strong diffraction peaks at 2θ=18°, 25°, 31°, 34°, and 35°. It can be seen that CaSrAl2SiO7:Eu 3 + The solid powder was successfully prepared. The chemical valence and composition of its surface were tested by XPS. Figure 7 As shown in (b), it can be seen from the full XPS spectrum that the peaks of binding energy at 73.94 eV, 101.89 eV, 133.39 eV, 284.52 eV, 347.23 eV, 531.28 eV, 780.5 eV, and 1124.74 eV correspond to Al2p, Si2p, Sr3d, C1s, Ca2p, O1s, Ba3d, and Eu3d, respectively.
[0066] CaSrAl2SiO7:Eu 3+ Optical properties
[0067] CaSrAl2SiO7:Eu was analyzed 3+ The fluorescent property of solid powder is that its own chromophore group absorbs green light, thereby inducing the energy level transition of the π electrons in the molecule to emit fluorescence. Figure 8 As shown in (a) and (b), the optimal excitation spectrum Ex = 550nm of the green-to-red light-converting material was first determined by backscanning the excitation wavelength, and CaSrAl2SiO7:Eu was tested with the excitation wavelength Ex = 550nm as the benchmark. 3+ The emission spectrum of the fluorescence reaches its maximum at 620nm, emitting red fluorescence. Figure 8 As shown in (c) and (d), CaSrAl2SiO7:Eu is irradiated by UV light. 3+ Powder, no fluorescence was observed, and the CIE chromaticity coordinates were calculated using the emission spectrum data, which were located in the red region.
[0068] CaSrAl2SiO7:Eu 3+ Thermal stability
[0069] like Fig. 9As shown in the figure, with the increase of temperature, the mass loss of the light conversion material changes. At 800°C, the mass loss of the light conversion material is 8.16%. In the temperature range of 0-800°C, although the inorganic light conversion material collapses, the impact is not significant, and it can still exist stably when preparing light conversion agricultural film.
[0070] XT-SZ Performance
[0071] Particle size distribution
[0072] Fig.10 Figure ae shows the particle size distribution of XT-SZ light conversion materials after five treatments. Figure ae shows the particle size distribution of XT-SZ1 to XT-SZ5, with particle sizes ranging from 2-6.5um, 2-8um, 2-6um, 2-7um, and 1.5-6um, respectively. The average particle sizes are 395±96nm, 455±133nm, 407±95nm, 441±136nm, and 352±119nm, respectively. The five treatments have good dispersibility.
[0073] Phase analysis of XT-SZ
[0074] The XRD characteristics of the samples are as follows Fig.11 As shown in the figure, the samples prepared in different proportions are consistent with the characteristic peaks of BaMgAl10O17 (PDF#26-0163) and (Y0.95Eu0.05)2O3 (PDF#25-1011), and there are special diffraction peaks belonging to Ca3Al2Si3O12 and Sr0.8Ba0.2CO3, which proves the successful preparation of the mixed light conversion material. The characteristic peaks at 29.2°, 33.8°, 48.5°, and 57.6° correspond to the (222), (400), (440), and (622) crystal planes, respectively. It can be seen from the figure that the diffraction peaks are strong, sharp, and symmetrical, indicating that the crystallinity of (Y0.95Eu0.05)2O3 is good. Although the samples are mixed in different proportions, no new diffraction peaks appear, indicating that there is no obvious effect on the physical structure of the samples. It is just that after a certain content is increased, the angle of the diffraction peak appears slightly shifted.
[0075] Morphological analysis of XT-SZ
[0076] The morphology of the five treated XT-SZ light conversion materials was characterized by scanning electron microscopy. The main component of the red light conversion material is Y2O3:Eu 3+ , a rod-like structure, Fig.12 ae can be seen that with the Y2O3:Eu 3+ As the ratio increases, the number of rod-like structures gradually increases.
[0077] Excitation and emission spectroscopy
[0078] like Fig.12As shown in (a), the monitoring wavelength is 616nm. It can be seen that the excitation spectra of the prepared light conversion materials are all a relatively wide spectrum, ranging from 250-400nm, indicating that the excitation light between 250-400nm can excite this series of light conversion materials to emit light, and the maximum excitation peak position is at 325nm.
[0079] The emission spectra of five treated XT-SZ were tested with an excitation wavelength of Ex = 325 nm. Fig.12 (b) It can be seen that the positions and shapes of the emission spectra of the five treatments are basically the same, and can be divided into two parts: blue light of 400-500nm and red light of 580-660nm. 2+ 4f 6 The energy of the 5d state is higher than that of the 4f state. 7 The energy of the excited state is low, so most of the Eu 2+ In the activated materials, the forbidden ff transition is not observed, but the 4f-5d transition is observed. 7 -4f 6 The transition of 5d is a transition between configurations. In addition, the 5d energy level is easily affected by the surrounding ion coordination field and the matrix structure, so the 4f 7 -4f 6 The transition between 5d is stronger. Therefore, the emission spectrum is located at the emission peak around 450nm, which is caused by Eu 2+ The excited state electron 4f 6 5d transitions to the ground state 4f 7 Resulting in the emission of Eu 2+ The main emission peak of the blue fluorescence is located at about 450nm. The emission peak at 620nm is due to the energy from the excited state ( 5 d0) to the ground state ( 7 f2) transformation, the energy transfer can make Eu 3+ Sensitive, showing inherent Eu 3+The red fluorescence emission of XT-SZ1 is located at 450nm (blue light region), and the second strongest emission peak is located at 620nm (red light region). The relative intensity ratio of red and blue light is about 0.5. XT-SZ2 is located at 450nm (blue light region) and the second strongest emission peak is located at 620nm (red light region). The relative intensity ratio of red and blue light is about 0.7. XT-SZ3 is located at 620nm (red light region) and the second strongest emission peak is located at 450nm (blue light region). The relative intensity ratio of red and blue light is about 1.3. XT-SZ4 is located at 450nm (blue light region) and the second strongest emission peak is located at 620nm (red light region). The relative intensity ratio of red and blue light is about 0.9. XT-SZ5 exhibits the strongest emission peak at 620nm (red light region), and the second strongest emission peak at 450nm (blue light region). The relative intensity ratio of red and blue light is about 2.2.
[0080] From the above analysis, it can be seen that with the Y2O3:Eu 3+ As the ratio increases, the relative intensity ratio of red and blue light of the main emission peak of XT-SZ shows a positive correlation. 3+ 、CaSrAl2SiO7:Eu 3+ 、BaMgAl 10 O 17 :Eu 2+ When the ratio is 2:2:1 and 6:4:1, the relative intensity ratio of red and blue light increases significantly.
[0081] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any figure mark in the claims should not be regarded as limiting the claims involved.
[0082] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a light conversion material, characterized in that: The specific steps are as follows: S1. Preparation of Y2O3:Eu 3+ ; S2. Preparation of BaMgAl 10 O 17 :Eu 2+ S3, mixing aluminum oxide and silicon dioxide in a molar ratio of 2:1 and calcining to obtain aluminosilicate; S4, putting the aluminosilicate, strontium carbonate, calcium carbonate, barium oxide and europium oxide prepared in step S3 into a mortar and grinding them thoroughly for 1 hour; S5. Add boric acid to the obtained powder, mix it, and calcine it in a tube furnace for 3 hours. Then cool it naturally to room temperature to obtain the light conversion material CaSrAl2SiO7:Eu 3+ ; S6, use a high-speed mixer to mix Y2O3:Eu 3+ 、CaSrAl2SiO7:Eu 3+ 、BaMgAl 10 O 17 :Eu 2+ XT-SZ light conversion material is made by mixing in different proportions.
2. The method for preparing a light conversion material according to claim 1, characterized in that: Including the specific preparation of Y2O3:Eu in step S1 3+ The steps are as follows: S1-1, dissolving Eu2O3 and Y2O3 in concentrated nitric acid in a molar ratio of 9:1; S1-2, adding oxalic acid with a concentration of 1.49 mol / L as a precipitant to obtain a rare earth oxalic acid precursor; S1-3, calcining the rare earth oxalate precursor at 1300℃ in a tube furnace for 3h, and cooling it naturally to room temperature to obtain Y2O3:Eu 3+ Solid powder.
3. The method for preparing a light conversion material according to claim 1, characterized in that: Including the specific preparation of BaMgAl in the S2 step 10 O 17 :Eu 2+ The steps are as follows: S2-1, put europium oxide, barium oxide, magnesium oxide and aluminum oxide in a certain proportion in a mortar and grind them thoroughly for 1 hour; S2-2, the obtained powder was placed in a tube furnace and calcined at 1300°C for 3h to obtain BaMgAl 10 O 17 :Eu 2+ Precursor raw materials; S2-3, BaMgAl 10 O 17 :Eu 2+ 2% NH4Cl flux was added to the precursor raw material, and secondary sintering was performed in CS2 reducing gas atmosphere at 1250℃-1450℃ for 2h, and then naturally cooled to room temperature to obtain BaMgAl 10 O 17 :Eu 2+ powder.
4. The method for preparing a light conversion material according to claim 1, characterized in that: The proportions of the components in step S2-1 are 12-14 parts of europium oxide, 18-20 parts of barium oxide, 50-55 parts of magnesium oxide, and 13-15 parts of aluminum oxide.
5. The method for preparing a light conversion material according to claim 1, characterized in that: Including Y2O3:Eu in step S6 3+ 1-6 parts, CaSrAl2SiO7:Eu 3+ 1-4 parts, BaMgAl 10 O 17 :Eu 2+ For 1 portion.
6. A light conversion material, characterized in that: The light-converting material is prepared by the method for preparing the light-converting material according to any one of claims 1 to 4.
Citation Information
Patent Citations
Red light-blue light dual-emission composited optical transfer material, and preparation method and application of red light-blue light dual-emission composited optical transfer material
CN106566536A
Fluorescent lamp for general illumination