Method and device for efficiently recovering indium from indium-rich slag
Through the combination of carbon thermal reduction and vacuum distillation, the problems of complex processes and high cost in the prior art are solved, and efficient separation and recovery of high-purity indium are achieved, which simplifies the process and reduces energy consumption.
Patent Information
- Application Number
- CN202411199486.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-29
AI Technical Summary
In the prior art, the process of recovering indium from indium-rich slag is complex and costly, and the solution processing volume is large, making it difficult to efficiently separate indium from other impurity metals.
Carbon-thermal reduction combined with vacuum distillation, through alkaline leaching, carbonaceous reduction and vacuum distillation steps, carbonaceous reduction and sodium acetate promote the generation of carbonaceous compounds, enhance the reduction capacity, and distillation in multi-layer disc cylinder Zinc, lead and indium are separated in the furnace.
The process flow is simplified, the separation efficiency between indium and impurity metal is improved, high-purity indium products are obtained, energy consumption and raw material use are reduced, and the recycling capacity of valuable metals is improved.
Smart Images

Figure CN119082470A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of valuable metal recovery, and in particular to a method for efficiently recovering indium from indium-rich slag. Background Art
[0002] Indium has become one of the most important metal materials in the modern electronics industry due to its excellent physical and chemical properties. Indium does not have independent deposits and is often associated with minerals such as zinc and lead ores. It can only be recovered as a by-product from the smelting process, and a relatively complex smelting process is required to separate indium from it. A large amount of indium-containing raw materials are produced every year in the lead-zinc smelting system. The zinc oxide produced by the lead system undergoes three-stage countercurrent leaching of neutral leaching-low acid leaching-high acid leaching. The indium in the raw material is mainly enriched in the weak acid leaching supernatant, and further neutralized and precipitated to obtain indium-rich slag, which is rich in indium and other scattered metals and has a high recovery value. The currently commonly used indium extraction process is indium-rich slag leaching-extraction-strip extraction-replacement-casting, which has the disadvantages of long process and high cost.
[0003] The Chinese patent application publication number CN104451205A discloses a method for recovering metallic indium from indium-containing materials, which includes leaching with sulfuric acid - removing impurities from the solution - reducing trivalent iron with oxalic acid - extracting - stripping - replacing - casting to obtain an indium ingot with an indium content of more than 99%. Although this method can obtain indium ingot products with a relatively high purity, the process flow is complicated and the solution processing volume is large. Summary of the invention
[0004] The present invention combines the wet process and the pyrometallurgical process, and adopts the method of carbon thermal reduction combined with vacuum distillation to recover the valuable metal indium in the indium-rich slag, which effectively solves the problems of complex process flow and large solution treatment volume in the prior art, and efficiently separates indium from other impurity metals in the indium-rich slag to obtain a high-purity indium product.
[0005] The technical scheme adopted by the present invention is: a method for efficiently recovering indium from indium-rich slag, comprising the following steps: S1, alkaline leaching: crushing the indium-rich slag into powder and then performing alkaline leaching to dissolve the arsenic therein in the alkali; adding a sodium hydroxide solution with a concentration of 80 to 120 g / L to the indium-rich slag at a liquid-solid ratio of (3 to 5): 1, heating and stirring at 50 to 80°C for 2 to 3 hours, filtering to obtain arsenic-free leaching slag, at which the arsenic leaching rate is greater than 98%; S2, carbon thermal reduction: treating S1 The arsenic removal leaching residue obtained in the above step is crushed and ground into a powder with a particle size of less than 200 meshes, and mixed with a carbonaceous reducing agent and sodium acetate in a certain proportion to obtain a mixed powder, and reduced in an atmosphere furnace at 1200-1350°C for 2-5 hours to obtain a reduction product; S3, vacuum distillation: the reduction product obtained in S2 is vacuum distilled at 1050-1150°C, with a vacuum degree of <10Pa, for 2-6 hours, so that zinc, lead, and indium are volatilized to obtain crude zinc, crude lead, and crude indium. Due to the inclusion of lead sulfate, the arsenic removal leaching residue will release high-energy active sulfur oxides in the heated material, and then continue to combine with the carbonaceous reducing agent at high temperature to generate a strongly reducing carbonyl sulfide compound, which can enhance the reducing ability of carbon; at the same time, the addition of sodium acetate further promotes the formation of carbonyl sulfide compounds, so that the direct recovery rates of zinc, lead, and indium are all greater than 98%.
[0006] As a further improvement of the present invention, in S2, the mass ratio of the carbonaceous reducing agent: sodium acetate: dearsenicizing leaching residue is 20-25:1-3:100.
[0007] As a further improvement of the present invention, the carbonaceous reducing agent is coke powder or graphite powder.
[0008] As a further improvement of the present invention, in S3, the vacuum distillation adopts a multi-layer drum distillation furnace.
[0009] As a further improvement of the present invention, the bottom of the multi-layer drum type distillation furnace is a heating zone, and the middle and upper parts are condensation zones; the temperature of the bottom heating zone is 1010-1100°C, the temperature of the middle condensation zone is 650-750°C, the temperature of the upper condensation zone is 250-390°C, and the vacuum degree is <10Pa. Under this vacuum degree, the boiling and evaporation temperature of indium is 1000°C, the boiling and evaporation temperature of lead is 760°C, and the boiling and evaporation temperature of zinc is 400°C, so the temperature of the bottom heating zone is 1010-1100°C, and the middle temperature zone is set at 650-750°C, then indium is easily converted from gas to liquid and enriched on the bottom high-purity graphite sleeve, lead is easily converted from gas to liquid and enriched on the middle high-purity quartz sleeve, and the upper temperature zone is set at 250-350°C, then zinc is easily converted from gas to liquid and enriched on the upper high-purity quartz sleeve. The vacuum distillation process is carried out in a multi-layer disc-type distillation furnace. The materials are placed in a high-purity graphite crucible. As the temperature inside the distillation furnace rises, the low-boiling-point metals gradually evaporate to the condensation zone. Since the boiling points of zinc, lead and indium gradually increase, the upper tray in the condensation zone of the furnace is zinc, the middle tray in the condensation zone is lead, and the lower tray in the condensation zone is indium, while high-melting-point metals such as copper remain in the crucible.
[0010] As a further improvement of the present invention, the indium-rich slag is indium-rich waste slag remaining in the wet process, and the indium content in the indium-rich slag is 1.3-3.4%, the zinc content is 26.1-34.6%, the lead content is 9.3-11.8%, the iron content is 8.6-9.8%, the arsenic content is 2.0-2.7%, and the copper content is 0.4-0.6%.
[0011] As a further improvement of the present invention, a recovery device for efficiently recovering indium from indium-rich slag includes a distillation furnace, a vacuum tube is provided at the top of the distillation furnace, the distillation furnace includes a heating zone at the bottom, a condensation zone in the middle and a condensation zone at the top, a high-temperature resistance wire is provided in the distillation furnace, and the high-temperature resistance wire is respectively located in the heating zone and the condensation zone; a crucible is provided at the bottom of the distillation furnace, a sleeve and a tower plate stacked layer by layer are provided on the top of the crucible, and a top cover is provided on the topmost tower plate; the through holes of adjacent sleeves and tower plates are arranged in a staggered manner. The distillation container used is high-purity graphite and high-purity quartz, the tower plate and sleeve are located on the top of the crucible and stacked layer by layer, the sleeve is used for metal condensation, and the tower plate is used for metal separation.
[0012] As a further improvement of the present invention, the temperature of the bottom heating zone is 1010-1100°C, the temperature of the middle condensation zone is 650-750°C, and the temperature of the upper condensation zone is 250-390°C.
[0013] As a further improvement of the present invention, the crucible is a high-purity graphite crucible, and the sleeve at the bottom is made of high-purity graphite; the tray and sleeve at the middle and upper parts are made of high-purity quartz. The crucible and the bottom sleeve are made of high-purity graphite, which increases the hardness of the distillation container and extends its service life. At the same time, indium does not stick to graphite, which is convenient for collection. The middle and upper trays and sleeves are made of high-purity quartz, which is convenient for observing material distribution, and lead and zinc do not stick to quartz, which is convenient for the collection of lead and zinc.
[0014] The invention has the beneficial effects as follows: the process flow of the invention is short, and the efficient purification and recovery of zinc, lead and indium are realized through reduction and vacuum distillation; the invention has strong adaptability to materials and can process various types of indium-rich slag. Since the wet process retains lead sulfate, it can release high-energy active sulfur oxides in the high-temperature reduction process at the rear end, and then continue to combine with the carbonaceous reducing agent at high temperature to generate a strong reducing carbonyl sulfide compound, which can enhance the reducing ability of carbon; at the same time, the addition of sodium acetate promotes the release of high-energy active sulfur oxides, greatly improves the direct metal recovery rate, and effectively enhances the recovery capacity of valuable metals; in the vacuum distillation process, multi-layer disc distillation is adopted, and the evaporated metal will be repeatedly distilled and condensed in the tower plate and sleeve, thereby realizing the separation of substances and improving the separation efficiency of metals; at the same time, in the distillation process, based on the boiling point and volatility of different metals such as lead, zinc, and indium, highly pure products will be gradually separated, and the main grade of the obtained metal will be higher. In addition, multi-layer disc distillation can use less raw materials and energy consumption in the same time to obtain a larger yield of pure separations, which can greatly reduce the reaction temperature and reduce energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a schematic diagram of the present invention.
[0016] Figure 2 It is a schematic diagram of an embodiment of the recovery device disclosed in the present invention.
[0017] As shown in the figure: 1 vacuum cover, 2 top cover, 3 sleeve, 4 tower plate, 5 high temperature resistance wire, 7 crucible. DETAILED DESCRIPTION
[0018] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0019] As shown in the figure, a method for efficiently recovering indium from indium-rich slag comprises the following steps:
[0020] S1, alkaline leaching: crush the indium-rich slag into powder and then perform alkaline leaching to dissolve the arsenic in the alkali; add a sodium hydroxide solution with a concentration of 80-120 g / L to the indium-rich slag at a liquid-solid ratio of (3-5):1, heat and stir at 50-80°C for 2-3 hours, and filter to obtain arsenic-free leaching slag, at which the arsenic leaching rate is greater than 98%;
[0021] S2, carbon thermal reduction: crush and grind the dearsenicized leaching residue obtained in S1 into a powder with a particle size of less than 200 mesh, mix it evenly with a carbonaceous reducing agent and sodium acetate in a certain proportion to obtain a mixed powder, and reduce it in an atmosphere furnace at 1200-1350° C. for 2-5 hours to obtain a reduced product;
[0022] S3, vacuum distillation: the reduction product obtained in S2 is subjected to vacuum distillation at 1050-1150°C with a vacuum degree of <10Pa for 2-6h to volatilize zinc, lead and indium to obtain crude zinc, lead and indium.
[0023] Since the wet process retains lead sulfate, it can release high-energy active sulfur oxides during the high-temperature reduction process at the back end, and then continue to combine with carbonaceous reducing agents at high temperatures to generate highly reducing carbonyl sulfide compounds, which can enhance the reducing ability of carbon. At the same time, the addition of sodium acetate promotes the release of high-energy active sulfur oxides, greatly improves the direct metal recovery rate, and effectively enhances the recovery capacity of valuable metals; in the vacuum distillation process, multi-layer disc distillation is used, and the evaporated metal will be repeatedly distilled and condensed in the tower plate and sleeve, thereby realizing the separation of substances and improving the separation efficiency of metals; at the same time, based on the boiling points and volatility of different metals such as lead, zinc, and indium, the distillation process will gradually separate highly pure products, and the main metal grade obtained will be higher.
[0024] Example 1, a method for efficiently recovering indium from indium-rich slag, is carried out according to the following steps:
[0025] In this embodiment, the indium content in the indium-rich slag is 1.36%, the zinc content is 27.2%, the lead content is 9.3%, the iron content is 9.1%, the arsenic content is 2.2%, and the copper content is 0.4%.
[0026] (1) Alkaline leaching: The indium-rich slag is subjected to alkaline leaching. A sodium hydroxide solution with a concentration of 60 g / L is added to the indium-rich slag at a liquid-to-solid ratio of 4:1. After heating and stirring at 60°C for 3 h, leached slag is obtained, and the arsenic leaching rate is greater than 98.9%.
[0027] (2) Carbon thermal reduction: The dearsenicated leaching residue is crushed and ground into a powder with a particle size of less than 200 mesh, mixed with a carbonaceous reducing agent and sodium acetate in a certain proportion to obtain a mixed powder, and reduced in an atmosphere furnace at 1250°C for 4 hours to obtain a reduced product. Among them, the mass ratio of the carbonaceous reducing agent to the dearsenicated leaching residue is 22:100, and the mass ratio of sodium acetate to the dearsenicated leaching residue is 1:100. The atmosphere furnace needs to maintain a nitrogen atmosphere in the process of heating and heating to protect the reduced product and prevent oxidation.
[0028] (3) Vacuum distillation: The reduction product is subjected to vacuum distillation at 1060° C., a middle temperature of 690° C., an upper temperature of 350° C., a vacuum degree of 6.3 Pa, and a time of 5 hours to volatilize zinc, lead, and indium to obtain crude zinc, crude lead, and crude indium.
[0029] Example 2, a method for efficiently recovering indium from indium-rich slag, is carried out according to the following steps:
[0030] In this embodiment, the indium content in the indium-rich slag is 1.4%, the zinc content is 25.4%, the lead content is 10.1%, the iron content is 8.7%, the arsenic content is 2.3%, and the copper content is 0.5%.
[0031] (1) Alkaline leaching: The indium-rich slag is subjected to alkaline leaching. A sodium hydroxide solution with a concentration of 70 g / L is added to the indium-rich slag at a liquid-to-solid ratio of 5:1. After heating and stirring at 70°C for 2 h, leached slag is obtained, and the arsenic leaching rate is greater than 98.5%.
[0032] (2) Carbon thermal reduction: The dearsenicated leaching residue is crushed and ground into a powder with a particle size of less than 200 mesh, mixed with a carbonaceous reducing agent and sodium acetate in a certain proportion to obtain a mixed powder, and reduced in an atmosphere furnace at 1300°C for 3 hours to obtain a reduced product. Among them, the mass ratio of the carbonaceous reducing agent to the dearsenicated leaching residue is 25:100, and the mass ratio of sodium acetate to the dearsenicated leaching residue is 1.5:100. The atmosphere furnace needs to maintain a nitrogen atmosphere in the process of heating and heating to protect the reduced product and prevent oxidation.
[0033] (3) Vacuum distillation: Vacuum distillation: The reduction product is subjected to vacuum distillation at 1080°C, with a middle temperature of 700°C, an upper temperature of 380°C, a vacuum degree of 4.8 Pa, and a time of 6 hours to volatilize zinc, lead, and indium to obtain crude zinc, crude lead, and crude indium.
[0034] The following table is a component analysis table of each link of Example 1 and Example 2
[0035] Example Product Composition Analysis Table / %
[0036]
[0037]
[0038] From the analysis in the above table, it can be seen that in the treated indium-rich slag, the direct recovery rate of indium exceeds 95%, the direct recovery rate of lead exceeds 96%, and the direct recovery rate of zinc exceeds 95%, all of which have relatively high direct recovery rates.
[0039] Those skilled in the art should be aware that the protection scheme of the present invention is not limited to the above-mentioned embodiments, and various arrangements, combinations and transformations can be performed on the basis of the above-mentioned embodiments. Without violating the spirit of the present invention, various transformations of the present invention fall within the protection scope of the present invention.
Claims
1. A method for efficiently recovering indium from indium-rich slag, characterized in that The steps include: S1, alkaline leaching: crush the indium-rich slag into powder and then perform alkaline leaching to dissolve the arsenic in the alkali; add a sodium hydroxide solution with a concentration of 80-120 g / L to the indium-rich slag at a liquid-solid ratio of (3-5):1, heat and stir at 50-80°C for 2-3 hours, and filter to obtain arsenic-free leaching slag, at which the arsenic leaching rate is greater than 98%; S2, carbon thermal reduction: crush and grind the dearsenicized leaching residue obtained in S1 into a powder with a particle size of less than 200 mesh, mix it evenly with a carbonaceous reducing agent and sodium acetate in a certain proportion to obtain a mixed powder, and reduce it in an atmosphere furnace at 1200-1350° C. for 2-5 hours to obtain a reduced product; S3, vacuum distillation: the reduction product obtained in S2 is subjected to vacuum distillation at 1050-1150°C with a vacuum degree of <10Pa for 2-6h to volatilize zinc, lead and indium to obtain crude zinc, lead and indium.
2. A method for efficiently recovering indium from indium-rich slag according to claim 1, characterized in that In S2, the mass ratio of the carbonaceous reducing agent: sodium acetate: dearsenicized leaching residue is 20-25:1-3:
100.
3. A method for efficiently recovering indium from indium-rich slag according to claim 2, characterized in that The carbonaceous reducing agent is coke powder or graphite powder.
4. The method for efficiently recovering indium from indium-rich slag according to claim 1, characterized in that In S3, the vacuum distillation adopts a multi-layer drum distillation furnace.
5. A method for efficiently recovering indium from indium-rich slag according to claim 4, characterized in that The bottom of the multi-layer disc-type distillation furnace is a heating zone, and the middle and upper parts are condensation zones; the temperature of the bottom heating zone is 1010-1100°C, the temperature of the middle condensation zone is 650-750°C, the temperature of the upper condensation zone is 250-390°C, and the vacuum degree is <10Pa.
6. A method for efficiently recovering indium from indium-rich slag according to any one of claims 1 to 5, characterized in that The indium-rich slag is waste slag rich in indium remaining in a wet process, wherein the indium content in the indium-rich slag is 1.3-3.4%, the zinc content is 26.1-34.6%, the lead content is 9.3-11.8%, the iron content is 8.6-9.8%, the arsenic content is 2.0-2.7%, and the copper content is 0.4-0.6%.
7. A recovery device for efficiently recovering indium from indium-rich slag using the method described in any one of claims 1 to 6, comprising a distillation furnace, a vacuum tube (1) being provided at the top of the distillation furnace, characterized in that The distillation furnace comprises a heating zone at the bottom, a condensation zone in the middle and a condensation zone at the top. A high-temperature resistance wire (5) is arranged in the distillation furnace, and the high-temperature resistance wire is respectively located in the heating zone and the condensation zone; a crucible (7) is arranged at the bottom of the distillation furnace, and sleeves (3) and tower plates (4) stacked layer by layer are arranged on the top of the crucible, and a top cover (2) is arranged on the topmost tower plate; the through holes of adjacent sleeves and tower plates are arranged in a staggered manner.
8. The recovery device according to claim 7, characterized in that The temperature of the bottom heating zone is 1010-1100°C, the temperature of the middle condensation zone is 650-750°C, and the temperature of the upper condensation zone is 250-390°C.
9. The recovery device according to claim 7, characterized in that The crucible is a high-purity graphite crucible, the sleeve at the bottom is made of high-purity graphite; the tower plate and sleeve at the middle and upper parts are made of high-purity quartz.
Citation Information
Patent Citations
Method for preparing sponge indium with indium-rich slag produced in lead-zinc smelting process
CN102586608A
Method for recovering indium back-extraction liquid purification residue
CN102978410A
Method of recycling indium and germanium from germanium vacuum distillation residues
CN107746965A
Recovering method of indium in carbothermic reduction indium containing slags
CN110117724A
Method for recovering indium from indium-containing matter
JP1993311267A