Method for gradually separating valuable metal antimony and bismuth from alkaline high-arsenic liquid

By step-by-step treatment in alkaline high arsenic liquid, including heating, filtration and deep alkalization, the separation and purification of antimony and bismuth were successfully achieved, solving the problem of difficult separation in the alkaline system and increasing the value The purity and safety of metals.

CN119082497APending Publication Date: 2024-12-06ZIJIN COPPER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411192998.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In alkaline systems, the separation of antimony, bismuth and arsenic is difficult, and the target metal and the non-target metal are prone to precipitate at the same time, resulting in low purity and content of the valuable metals, the existing technology process is complex and there are many control parameters.

Method used

The process is carried out step by step in alkaline high arsenic solution, including heating, addition of H2O2, filtration, deep alkalization, addition of sodium sulfide and sodium hydroxide, followed by heating and stirring to achieve the separation and purification of antimony and bismuth, and finally hydroxide oxidation Calcium precipitates arsenic to reduce impurities.

Benefits of technology

Deep separation and enrichment under alkaline conditions are achieved, and high-purity sodium antimonate is generated, which improves the purity and safety of the valuable metals and reduces the impact of water treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082497A_ABST
    Figure CN119082497A_ABST
Patent Text Reader

Abstract

The invention discloses a method for gradually separating valuable metal antimony and bismuth from alkaline high-arsenic liquid, which comprises the following steps: oxidizing the alkaline high-arsenic liquid by using H2O2 to precipitate antimony, then adding sodium sulfide to precipitate bismuth, and finally adding calcium hydroxide to causticize and precipitate arsenic. The deep separation of As, Sb and Bi under the alkaline condition is realized by utilizing the method disclosed by the invention; according to the method, enrichment and purification of Sb and Bi can be achieved under the alkaline condition, and the purity of valuable metal is increased; according to the method disclosed by the invention, the non-valent metal arsenic is fixed in a causticization manner, so that the safety of the arsenic is greatly improved. According to the method disclosed by the invention, S in the added sodium sulfide is fixed by adding calcium hydroxide, so that S in water is reduced, and the influence on subsequent water treatment is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resource recycling, and in particular to a method for separating valuable metals antimony and bismuth step by step from an alkaline high-arsenic solution. Background Art

[0002] At present, the separation methods of As, Sb and Bi in solution are mainly divided into separation in acidic liquid and separation in alkaline liquid. The separation of antimony, bismuth and arsenic in alkaline system mainly utilizes the difference in solubility of antimony, bismuth and arsenic compounds in solution, and separates them by adding different compounds to react and make arsenic, antimony and bismuth form precipitation. However, due to the similar properties of arsenic, antimony and bismuth, when adding compound precipitation, the target metal and non-target metal are easy to precipitate at the same time, which makes separation difficult. The resulting precipitate has too many metal impurities, which seriously affects the valuation coefficient and use conditions of the target metal precipitation. In order to increase the content and purity of valuable metals, chlorination leaching is often used to further remove impurities from valuable metals. This method is complicated and has many control parameters. Summary of the invention

[0003] In view of the deficiencies of the prior art, the present invention aims to provide a method for stepwise separation of valuable metals antimony and bismuth in an alkaline high-arsenic solution.

[0004] In order to achieve the above object, the present invention adopts the following technical solution:

[0005] A method for separating valuable metals antimony and bismuth step by step from an alkaline high-arsenic solution comprises the following steps:

[0006] S1, heating the alkaline high arsenic solution to 40-60°C, slowly adding H2O2 to the alkaline high arsenic solution several times according to the molar ratio of antimony: H2O2=1:2-4, and obtaining an oxidized solution after the reaction is completed;

[0007] S2, the oxidized liquid obtained in step S1 is allowed to stand and cool, and then filtered to obtain oxidation slag and oxidation liquid;

[0008] S3, add sodium hydroxide solution to the oxidizing solution for deep alkalization, the end point of adding alkali is pH = 12-13, and then according to the molar ratio of As:S 2- =2:5-10 add sodium sulfide;

[0009] S4, heating the mixed solution of the oxidation solution, sodium hydroxide and sodium sulfide obtained in step S3 to 60-70° C. for reaction, filtering after the reaction is completed, the filter residue is the bismuth precipitation residue, and the filtrate is the bismuth precipitation liquid;

[0010] S5, heating the bismuth precipitation solution obtained in step S4 to above 70°C and adding calcium hydroxide, the molar ratio (As+S 2- ):Ca(OH)2=1-1.5:1, stir the reaction to precipitate arsenic, filter and remove the residue, the filtrate is the arsenic precipitation liquid, and the filter residue is calcium arsenic residue.

[0011] Furthermore, in step S1, the reaction time is 1-2h.

[0012] Furthermore, in step S3, the mass concentration of the sodium hydroxide solution is 32%.

[0013] Furthermore, in step S4, the reaction time is 1-3 hours.

[0014] Further, in step S4, the reaction is stirred for 1-2 hours.

[0015] The beneficial effects of the present invention are:

[0016] (1) The method of the present invention is used to achieve deep separation of As, Sb and Bi under alkaline conditions;

[0017] (2) The method of the present invention can achieve the enrichment and purification of Sb and Bi under alkaline conditions, generate sodium antimonate with higher purity, and produce bismuth slag containing bismuth>15%, arsenic<1%, and antimony<0.1%, thereby increasing the purity of valuable metals;

[0018] (3) The method of the present invention fixes the priceless metal arsenic by causticization, which greatly improves its safety.

[0019] (4) The method of the present invention also fixes the S in the added sodium sulfide by adding calcium hydroxide, thereby reducing the S in the water and reducing the impact on subsequent water treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Flowchart of methods according to various embodiments of the present invention. DETAILED DESCRIPTION

[0021] The present invention will be further described below in conjunction with the accompanying drawings. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to this embodiment.

[0022] Example 1

[0023] This embodiment provides a method for separating valuable metals antimony and bismuth step by step from an alkaline high-arsenic solution. Figure 1 As shown, the specific process is:

[0024] Oxidation: Slowly add 5.5gH2O2 (the molar ratio of antimony to H2O2 is 1:4) to 1L of alkaline high-arsenic solution at a temperature of about 60°C, react for 1h, and the sodium antimonate content in the filtered residue is about 98%, of which the bismuth and arsenic contents are less than 0.1%, and the antimony content in the filtered oxidation solution is <0.1g / L.

[0025] Bismuth precipitation: add 32% sodium hydroxide solution to the oxidizing solution to deeply alkalize to pH = 12.5, then add 130g of Na2S (As: S 2- The molar ratio is 2:6), and the reaction is carried out at 60°C for 1 hour, and then filtered to obtain bismuth precipitate residue and bismuth precipitate liquid. The bismuth content in the bismuth precipitate residue is 17.5%, the As content is less than 1%, and the antimony content is less than 0.1%. The bismuth precipitate residue mainly contains bismuth sulfide and bismuth hydroxide.

[0026] Arsenic precipitation: Heat the bismuth precipitation solution to 70°C and add 68g Ca(OH)2 ((As+S 2- ):Ca(OH)2 in a molar ratio of 1:1), and after reacting for 1 hour, the arsenic precipitate residue and the arsenic precipitate liquid were obtained by filtration. The arsenic content in the arsenic precipitate residue was about 18%, the As content in the arsenic precipitate liquid was only 3.582g / L, the sulfide content was less than 1g / L, and the Ca content was less than 0.1g / L.

[0027] The composition changes of the alkaline high-arsenic solution in this embodiment are shown in Table 1.

[0028] Table 1

[0029]

[0030] Example 2

[0031] This embodiment provides a method for separating valuable metals antimony and bismuth step by step from an alkaline high-arsenic solution. Figure 1 As shown, the specific process is:

[0032] Oxidation: Slowly add 4.6gH2O2 (the molar ratio of antimony to H2O2 is 1:4) to 1L of alkaline high-arsenic solution at a temperature of about 60°C, react for 1h, and the sodium antimonate content in the filtered residue is about 98%, of which the bismuth and arsenic contents are less than 0.1%, and the antimony content in the filtered oxidation solution is <1g / L.

[0033] Bismuth precipitation: add 32% sodium hydroxide solution to the oxidizing solution to deeply alkalize to pH = 12.8, then add 143g of Na2S (As: S 2- The molar ratio is 2:6), and the reaction is carried out at 60°C for 1 hour, and then filtered to obtain bismuth precipitate residue and bismuth precipitate liquid. The bismuth content of the bismuth precipitate residue is 16.8%, the As content is 0.8%, and the antimony content is less than 0.1%.

[0034] Arsenic precipitation: Heat the bismuth precipitation solution to 70°C and add 84g Ca(OH)2 ((As+S 2+ ):Ca(OH)2 molar ratio=1:1), after reacting for 1h, arsenic precipitate residue and arsenic precipitate liquid are obtained by filtration. The arsenic content in the arsenic precipitate residue is about 18%, the As content in the arsenic precipitate liquid is only 3.687g / L, the sulfide content is less than 1g / L, and the Ca content is less than 0.1g / L.

[0035] The composition changes of the alkaline high-arsenic solution in this embodiment are shown in Table 2.

[0036] Table 2

[0037]

[0038] Example 3

[0039] This embodiment provides a method for separating valuable metals antimony and bismuth step by step from an alkaline high-arsenic solution. Figure 1 As shown, the specific process is:

[0040] Oxidation: Slowly add 7.6g H2O2 (the molar ratio of antimony to H2O2 is 1:4) to 1L of alkaline high-arsenic solution at a temperature of about 60°C, react for 1h, and the sodium antimonate content in the filtered residue is about 98%, of which the bismuth and arsenic contents are less than 0.1%, and the antimony content in the filtered oxidation solution is <0.1g / L.

[0041] Bismuth precipitation: add 32% sodium hydroxide solution to the oxidizing solution to deeply alkalize to pH = 13, then add 155g of Na2S (As: S 2- The molar ratio is 2:8), and the reaction is carried out at 60°C for 1 hour, and then filtered to obtain bismuth precipitate residue and bismuth precipitate liquid. The bismuth content in the bismuth precipitate residue is 17.3%, the As content is less than 1%, and the antimony content is less than 0.1%. The bismuth precipitate residue mainly contains bismuth sulfide and bismuth hydroxide.

[0042] Arsenic precipitation: Heat the bismuth precipitation solution to 70°C and add 78g Ca(OH)2 ((As+S 2+ ):Ca(OH)2 molar ratio=1.5:1), after reacting for 1h, arsenic precipitate residue and arsenic precipitate liquid were obtained by filtration. The arsenic content in the arsenic precipitate residue was about 18%, the As content in the arsenic precipitate liquid was only 2.954g / L, the sulfide content was less than 1g / L, and the Ca content was less than 0.1g / L.

[0043] The composition changes of the alkaline high-arsenic solution in this embodiment are shown in Table 3.

[0044] Table 3

[0045]

[0046] For those skilled in the art, various corresponding changes and modifications can be made according to the above technical solutions and concepts, and all of these changes and modifications should be included in the protection scope of the claims of the present invention.

Claims

1. A method for separating valuable metals antimony and bismuth step by step from an alkaline high-arsenic solution, characterized in that: The steps include: S1, heating the alkaline high arsenic solution to 40-60°C, slowly adding H2O2 to the alkaline high arsenic solution several times according to the molar ratio of antimony: H2O2=1:2-4, and obtaining an oxidized solution after the reaction is completed; S2, the oxidized liquid obtained in step S1 is allowed to stand and cool, and then filtered to obtain oxidation slag and oxidation liquid; S3, add sodium hydroxide solution to the oxidizing solution for deep alkalization, the end point of adding alkali is pH = 12-13, and then according to the molar ratio of As:S 2- =2:5-10 add sodium sulfide; S4, heating the mixed solution of the oxidation solution, sodium hydroxide and sodium sulfide obtained in step S3 to 60-70° C. for reaction, filtering after the reaction is completed, the filter residue is the bismuth precipitation residue, and the filtrate is the bismuth precipitation liquid; S5, heating the bismuth precipitation solution obtained in step S4 to above 70°C and adding calcium hydroxide, the molar ratio (As+S 2- ):Ca(OH)2=1-1.5:1, stir the reaction to precipitate arsenic, filter and remove the residue, the filtrate is the arsenic precipitation liquid, and the filter residue is calcium arsenic residue.

2. The method according to claim 1, characterized in that In step S1, the reaction time is 1-2h.

3. The method according to claim 1, characterized in that In step S3, the mass concentration of the sodium hydroxide solution is 32%.

4. The method according to claim 1, characterized in that: In step S4, the reaction time is 1-3 hours.

5. The method according to claim 1, characterized in that In step S4, the reaction is stirred for 1-2 hours.