Metal component with large-thickness and high-density hardened layer on surface and preparation method of metal component
By using the secondary laser remelting method during the laser remelting process, the spot and heat input are regulated, and the problems of solidification and cracks of the melt pool are solved, and a surface hardening layer with high hardness and high density is obtained, which improves efficiency and Reduces energy consumption.
Patent Information
- Application Number
- CN202411195275.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
During laser remelting, in order to obtain a dense hardened layer with high thickness and high hardness, the prior art requires higher heat input, but this can easily lead to loosening and microcracks when the molten pool solidifies, reducing hardness and wear-resistant properties. In addition, increasing the spot overlap rate will reduce efficiency and increase energy consumption.
The secondary laser remelting method is used to regulate the spot of the secondary laser remelting completely overlap with the primary laser remelting, and reduce the heat input of the secondary laser remelting to ensure that the spot completely covers the spot of the primary laser remelting to eliminate the center. Solidification loose zones and cracks.
A surface hardened layer with high thickness, high hardness and denseness is realized, which improves hardness and wear resistance and corrosion resistance, reduces energy consumption and improves efficiency.
Smart Images

Figure CN119082644A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface engineering, and in particular to a metal component with a thick and high-density hardened layer on the surface and a preparation method thereof. Background Art
[0002] Laser remelting can obtain a surface layer with ultra-fine structure, the same composition as the matrix, and complete metallurgical bonding on the surface of the steel matrix through the mechanism of rapid melting, which can significantly improve the surface hardness and wear and corrosion resistance of steel components. It is considered to be a very promising surface strengthening method.
[0003] However, when a thicker hardened layer is required, a higher heat input is required. At this time, when the molten pool solidifies, it is easy to form looseness and microcracks in the center. The higher the heat input, the larger the solidification loose zone, and the more serious the solidification cracks, which will significantly reduce the hardness and wear and corrosion resistance of the remelted layer.
[0004] In order to eliminate solidification defects, it is necessary to increase the overlap rate between the light spots so that the next light spot can eliminate the defects at the solidification center of the previous molten pool. However, increasing the spot overlap rate will reduce efficiency and increase energy consumption. At the same time, the next light spot will have a serious thermal impact on the previously formed solidified structure, reducing the hardness of the remelted layer. The greater the heat input during remelting, the higher the overlap rate required, and the more serious the thermal impact, which greatly reduces the hardness of the remelted layer. This problem affects the application scope of laser remelting strengthening.
[0005] Therefore, in order to expand the application scope of laser remelting, an efficient laser strengthening method is needed to obtain a thick, high-hardness and dense hardened layer. Summary of the invention
[0006] In view of the deficiencies in the prior art, an object of the present invention is to provide a metal component having a thick and dense hardened layer and a preparation method thereof.
[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0008] In a first aspect, the present invention provides a method for preparing a thick and dense hardened layer on the surface of a metal component, comprising:
[0009] Performing a laser remelting on the surface of the metal component to form a remelting layer;
[0010] A secondary laser remelting is continued on the surface of the remelting layer to form the hardened layer, the heat input of the secondary laser remelting is lower than that of the primary laser remelting, and all the light spots of the secondary laser remelting are concentric with the primary laser remelting, and the light spots of the secondary laser remelting completely cover the light spots of the primary laser remelting.
[0011] In a second aspect, the present invention also provides a metal component having a thick and high-density hardened layer obtained by the above-mentioned preparation method.
[0012] Based on the above technical solution, compared with the prior art, the beneficial effects of the present invention include:
[0013] The preparation method provided by the present invention utilizes a secondary laser remelting method. By adjusting the light spot of the secondary laser remelting to completely overlap with the primary laser remelting and adjusting the heat input of the secondary laser remelting to be lower, the remelting layer formed by the primary laser remelting is further strengthened and adjusted, and the problems of a large area of solidified loose area and serious solidification cracks in the center of the remelting area are solved, which significantly reduces the hardness and wear and corrosion resistance of the remelting layer. A surface hardened layer with large thickness, high hardness and good density can be obtained, and at the same time, the efficiency is high, the surface is smooth, and the energy consumption is reduced.
[0014] The above description is only an overview of the technical solution of the present invention. In order to enable those skilled in the art to more clearly understand the technical means of the present application and implement them according to the contents of the specification, the following is a description of the preferred embodiments of the present invention in conjunction with detailed drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a test diagram of the average hardness from the surface to the inside of the molten pool center of the hardened layer provided by a typical implementation case of the present invention and a typical comparison case;
[0016] Figure 2 is a test diagram of the average hardness from the surface to the inside of the molten pool center of the hardened layer provided by another typical embodiment of the present invention and another typical comparison case;
[0017] Figure 3 It is a test diagram of the average hardness from the surface to the inside of the molten pool center of the hardened layer provided by another typical implementation case of the present invention and another typical comparison case;
[0018] Figure 4 is a test diagram of the average hardness from the surface to the inside of the molten pool center of the hardened layer provided by another typical implementation case of the present invention and another typical comparison case;
[0019] Figure 5 is a comparison chart of the surface average hardness test of the hardened layer provided by multiple typical implementation cases of the present invention and multiple typical control cases;
[0020] Figure 6 It is a surface morphology photograph of a spot area of a laser remelting at a low heat input level provided by a typical implementation case of the present invention;
[0021] Figure 7This is a surface morphology photograph of a spot area of a laser remelting at a high heat input level provided in a typical implementation case of the present invention. DETAILED DESCRIPTION
[0022] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution, its implementation process and principle will be further explained as follows.
[0023] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0024] Moreover, relational terms such as “first” and “second” are merely used to distinguish one component or method step from another with the same name, but do not necessarily require or imply any such actual relationship or order between these components or method steps.
[0025] The embodiment of the present invention provides a method for preparing a thick and dense hardened layer on the surface of a metal component, more specifically, a surface strengthening method for eliminating a central solidification loose zone, avoiding the generation of serious solidification cracks, and significantly improving the hardness and wear and corrosion resistance of the remelted layer, which comprises the following steps:
[0026] Performing a laser remelting on the surface of the metal component to form a remelting layer;
[0027] A secondary laser remelting is continued on the surface of the remelting layer to form the hardened layer, the heat input of the secondary laser remelting is lower than that of the primary laser remelting, and all the light spots of the secondary laser remelting are concentric with the primary laser remelting, and the light spots of the secondary laser remelting completely cover the light spots of the primary laser remelting.
[0028] The above technical solution includes two situations. One is that the position and diameter of the spot of the secondary laser remelting are exactly the same as those of the primary laser remelting, that is, the two completely overlap and only differ in heat input; the other situation is that the spot of the secondary laser remelting is concentric with that of the primary laser remelting, but the diameter can be slightly larger than that of the primary laser remelting.
[0029] In the present invention, the key technical means lies in the relationship between the size of the heat input and the position relationship of the light spots of the two laser remeltings. The light spot of the second laser remelting needs to be concentric and completely cover the light spot of the first laser remelting. If the heat input of the two is equal, the loose solidification in the central area cannot be eliminated. Even if the heat input of the second laser remelting is larger, the loose solidification will be more serious. The second remelting light spot needs to be concentric with the first laser remelting to eliminate the solidification transport in the central area. The size of the second light spot can be slightly larger or equal to the first one, but not smaller, otherwise the hardness of the position not illuminated twice will be low; if there is a center offset, the same result may occur.
[0030] For example, in some embodiments, the first laser remelting and the second laser remelting are both performed in a combination of multiple passes, and the path of the first laser remelting is completely consistent with the path of the second laser remelting, and in any pass, the spot size and the spot center position of the first laser remelting are completely consistent with those of the second laser remelting.
[0031] In the above technical scheme, the key to achieving surface hardening processing with large thickness and excellent hardness lies in that the light spot during the second remelting is completely overlapped with that during the first remelting (both the light spot size and the light spot position overlap) or has a larger diameter, and concentrically covers the light spot during the first remelting, so as to avoid the softening zone that is not remelted for the second time but annealed during the second remelting; and the heat input of the second remelting is smaller than that of the first remelting. When a larger heat input is used for the first remelting, there is no need to use the method of increasing the overlap rate in the prior art (generally the overlap rate can be controlled at about 40%) to eliminate the defects at the center of the solidification of the previous molten pool, but the secondary remelting method is used to eliminate the central defects, thereby reducing energy consumption and improving the surface hardness of the remelted layer.
[0032] Specifically, since a thicker surface hardened layer is desired, the heat input during a remelting operation needs to be controlled to be larger to achieve a certain thickness. However, this will inevitably cause defects in the central solidification center. For details, see Figure 6 and Figure 7 As shown, when the heat input level is small, Figure 6 The solidification in the center of the spot irradiation area is loose and light, with no obvious cracking. In order to achieve a thicker hardened layer, a larger heat input is used. Figure 7As shown, the solidification looseness in the central area is serious, and the cracking phenomenon is obvious; during the second remelting, a lower heat input is used to supplement the central defects and eliminate the central solidification defects. And the spot diameter during the second remelting is equal to or slightly larger than that during the first remelting (for example, the second diameter is 100%-120% of the first diameter), avoiding the problem of low local hardness caused by incomplete coverage of the second remelting; and the heat input size of the second remelting is also relatively critical. If the same or higher heat input level is used, new central defects will continue to be generated, and the purpose of eliminating the central defects cannot be achieved; the heat input of the second remelting is controlled within a certain range to avoid serious solidification looseness and even cracking in the center of the molten pool; based on the above principle, the present invention can obtain a hardened layer with few defects, high hardness, smooth surface and uniformity.
[0033] The principle is that the greater the heat input, the larger and deeper the molten pool, the more severe the solidification porosity and cracking in the center of the molten pool, the larger the range, and the lower the hardness; however, if a large thickness is to be obtained, high heat input is required; therefore, a secondary remelting is performed to reduce the heat input of a single spot to a certain level so that solidification porosity or cracking does not occur in the center.
[0034] In some embodiments, in any pass of the laser remelting, the spot overlap rate is 30-50%, and the overlap rate between passes is 30-50%.
[0035] In some embodiments, the heat input of the secondary laser remelting is 40-70% of the heat input of the primary laser remelting.
[0036] In some embodiments, the average heat input per unit area of the laser remelting spot is 70-200 J / mm 2 The specific amount of heat input energy is generally related to the spot size, and considering that the energy density at the center and edge of the spot is very different, the average heat input per unit area is generally calculated based on the spot area.
[0037] In some embodiments, the pulse width of the laser remelting is 5 to 30 ms.
[0038] The average heat input per unit area of the secondary laser remelting spot is 10-40 J / mm 2 .
[0039] Pulse width is the duration of a pulse. The heat input of a single spot is proportional to the pulse width, but pulse width is not the only indicator that determines heat input. Usually, the product of current and pulse width determines heat input. The simplest way to control the heat input of a single spot is to control the pulse width. The heat input required for secondary remelting is small, so the pulse width is smaller. The general pulse width control range is shown above, but it is not limited to this range. Those skilled in the art can match the appropriate pulse width parameters based on actual conditions and different materials.
[0040] In some embodiments, the last spot irradiation of the first laser remelting and the second laser remelting are both outside the preset strengthening area of the metal component.
[0041] As some typical examples of the above technical solutions, the embodiments of the present invention can provide a technology for preparing a thick, high-hardness, dense laser-hardened layer, which can replace the traditional laser cladding or remelting technology and is used for surface strengthening of steel wear-resistant and corrosion-resistant components.
[0042] To achieve the above objectives, the following technical solutions can be adopted:
[0043] First, the surface of the steel component is cleaned to remove surface stains and oxide layer, and a thick remelting layer is prepared on its surface under the conditions of large spot and high heat input. The laser equipment, current, scanning speed, pulse frequency, pulse width, spot size, etc. can be flexibly selected, with a spot overlap rate of 30-50% and a pass overlap rate of 30-50%. Then, along exactly the same path, using the same spot and lower heat input, a second round of remelting treatment is carried out, with a heat input of 40-70% of the first remelting, to eliminate solidification looseness and microcracks. The last spot ends outside the workpiece to avoid residual complete molten pool and obtain a thick, highly dense surface hardened layer.
[0044] The second aspect of the embodiment of the present invention further provides a metal component having a thick and high-density hardened layer produced by the above-mentioned production method.
[0045] If you want to achieve a hardened layer with a large thickness (usually 0.5mm and above is considered to be a large thickness), a large spot heat input is usually required, but this will cause loose solidification in the center of the remelted layer, and the hardness and corrosion resistance will decrease. This is the basic technical problem faced by the present invention; by using the technical solution provided by the present invention to prepare the hardened layer, the obtained hardened layer will essentially be divided into two sub-layers, the upper (near the surface) sub-layer is the second sub-layer formed by the secondary remelting, and the lower part is the first sub-layer formed by the primary laser remelting. The hardness and density of the second sub-layer are higher than those of the first sub-layer.
[0046] In some embodiments, a metal substrate and a hardened layer formed on the surface of the metal substrate are included; the material of the metal substrate includes low alloy steel or stainless steel. Of course, this is not limited to this. Other metals that can be laser remelted and strengthened, such as titanium alloys, aluminum alloys, etc., can adopt the technical solution provided by the present invention, but it is necessary to adjust the basic conditions such as appropriate heat input to match the metal material.
[0047] The technical solution of the present invention is further described in detail below through several embodiments and in conjunction with the accompanying drawings. However, the selected embodiments are only used to illustrate the present invention, and do not limit the scope of the present invention.
[0048] Comparative Example 1-1:
[0049] The surface of the H13 hot working die steel plate with a thickness of 10 mm was mechanically polished to remove surface stains and oxide layer, and then rinsed with water and alcohol in turn and then blown dry;
[0050] The laser remelting current was 50A, the scanning rate was 108mm / min, the spot diameter was 0.6mm, the frequency used was 10Hz, and the pulse width was 8ms to achieve an overlap rate of 70%; the overlap rate between passes was 60%, and the last spot ended outside the workpiece.
[0051] The surface hardness of the remelted spot was measured using a micro Vickers hardness tester, with a load of 50g and a holding time of 10s. The surface hardness was measured along the diameter of the remelted spot, with an interval of 0.03mm, and 20 points were punched to calculate the average hardness. The sample was cut and polished so that the cross section passed through the center of the spot, and the hardness from the surface to the inside of the molten pool was measured. Starting from 0.03mm from the center surface, 10 points were punched at an interval of 0.03mm to calculate the hardness, and 10 groups were measured to calculate the average value.
[0052] Embodiment 1:
[0053] The surface of the H13 hot working die steel plate with a thickness of 10 mm was mechanically polished to remove surface stains and oxide layer, and then rinsed with water and alcohol in turn and then blown dry;
[0054] The laser remelting current was 50A, the scanning rate was 216mm / min, the spot diameter was 0.6mm, the frequency used was 10Hz, and the pulse width was 8ms to achieve a 40% overlap rate; the overlap rate between passes was 40%, and the last spot ended outside the workpiece.
[0055] The secondary remelting current is 30A, and the other parameters and scanning paths are the same as the primary remelting;
[0056] The microhardness test method is the same as above.
[0057] The average hardness from the surface to the inside of the molten pool center of Comparative Example 1 and Example 1 is as follows: Figure 1 shown.
[0058] It can be seen from the figure that compared with the control sample that has not undergone secondary laser remelting, the hardness at the center of the spot has been significantly improved after the secondary laser remelting.
[0059] Comparative Example 1-2
[0060] This comparative example is substantially the same as Example 1, except that:
[0061] The current of the secondary remelting was set to be equal to that of the primary laser remelting, and other conditions remained unchanged.
[0062] The average hardness of the obtained sample at the center of the spot did not change much from the surface to the inside.
[0063] Comparative Examples 1-3
[0064] This comparative example is substantially the same as Example 1, except that:
[0065] The center of the spot of the secondary laser remelting is shifted along the pass direction so that the spot of the secondary remelting is located at 1 / 2 of the line connecting the center points of two adjacent primary remelting spots, and other conditions remain unchanged.
[0066] In the obtained samples, part of the central loose area was not completely eliminated and the hardness was relatively low.
[0067] Comparative Examples 1-4
[0068] This comparative example is substantially the same as Example 1, except that:
[0069] The spot diameter of the second laser remelting was adjusted to 2 / 3 of that of the first remelting, and other conditions remained unchanged.
[0070] In the obtained sample, the hardness of the area that was not remelted for the second time decreased significantly.
[0071] Comparative Example 2:
[0072] The surface of the H13 hot working die steel plate with a thickness of 10 mm was mechanically polished to remove surface stains and oxide layer, and then rinsed with water and alcohol in turn and then blown dry;
[0073] The laser remelting current was 50A, the scanning rate was 144mm / min, the spot diameter was 0.6mm, the frequency used was 10Hz, and the pulse width was 10ms to achieve a 60% overlap rate; the overlap rate between passes was 70%, and the last spot ended outside the workpiece.
[0074] The microhardness test method is the same as above.
[0075] Embodiment 2:
[0076] The surface of the H13 hot working die steel plate with a thickness of 10 mm was mechanically polished to remove surface stains and oxide layer, and then rinsed with water and alcohol in turn and then blown dry;
[0077] The laser remelting current was 50A, the scanning rate was 234mm / min, the spot diameter was 0.6mm, the frequency used was 10Hz, and the pulse width was 10ms to achieve an overlap rate of 35%; the overlap rate between passes was 40%, and the last spot ended outside the workpiece.
[0078] The secondary remelting current is 25A, and the other parameters and scanning paths are the same as the primary remelting;
[0079] The microhardness test method is the same as above.
[0080] The average hardness from the surface to the inside of the molten pool center of Comparative Example 2 and Example 2 is as follows: Figure 2 shown.
[0081] Comparative Example 3*
[0082] The surface of the H13 hot working die steel plate with a thickness of 10 mm was mechanically polished to remove surface stains and oxide layer, and then rinsed with water and alcohol in turn and then blown dry;
[0083] The laser remelting current was 60A, the scanning rate was 108mm / min, the spot diameter was 0.6mm, the frequency used was 10Hz, and the pulse width was 8ms to achieve a 70% overlap rate; the overlap rate between passes was 60%, and the last spot ended outside the workpiece.
[0084] The microhardness test method is the same as above.
[0085] Embodiment 3:
[0086] The surface of the H13 hot working die steel plate with a thickness of 10 mm was mechanically polished to remove surface stains and oxide layer, and then rinsed with water and alcohol in turn and then blown dry;
[0087] The laser remelting current was 60A, the scanning rate was 216mm / min, the spot diameter was 0.6mm, the frequency used was 10Hz, and the pulse width was 8ms to achieve a 40% overlap rate; the overlap rate between passes was 40%, and the last spot ended outside the workpiece.
[0088] The secondary remelting current is 30A, and the other parameters and scanning paths are the same as the primary remelting;
[0089] The microhardness test method is the same as above.
[0090] The average hardness from the surface to the inside of the molten pool center of Comparative Example 3 and Example 3 is as follows: Figure 3 shown.
[0091] Comparative Example 4:
[0092] The surface of the H13 hot working die steel plate with a thickness of 10 mm was mechanically polished to remove surface stains and oxide layer, and then rinsed with water and alcohol in turn and then blown dry;
[0093] The laser remelting current was 60A, the scanning rate was 144mm / min, the spot diameter was 0.6mm, the frequency used was 10Hz, and the pulse width was 8ms to achieve a 60% overlap rate; the overlap rate between passes was 60%, and the last spot ended outside the workpiece.
[0094] The microhardness test method is the same as above.
[0095] Embodiment 4:
[0096] The surface of the H13 hot working die steel plate with a thickness of 10 mm was mechanically polished to remove surface stains and oxide layer, and then rinsed with water and alcohol in turn and then blown dry;
[0097] The laser remelting current was 60A, the scanning rate was 234mm / min, the spot diameter was 0.6mm, the frequency used was 10Hz, and the pulse width was 8ms to achieve an overlap rate of 35%; the overlap rate between passes was 40%, and the last spot ended outside the workpiece.
[0098] The secondary remelting current is 25A, and the other parameters and scanning paths are the same as the primary remelting;
[0099] The microhardness test method is the same as above.
[0100] The average hardness from the surface to the inside of the molten pool center of Comparative Example 4 and Example 4 is as follows: Figure 4 shown.
[0101] The average surface hardness of Comparative Examples 1-4 and Examples 1-4 is as follows Figure 5 shown.
[0102] from Figure 5 It can be seen that the technical solution provided by the present invention not only significantly improves the hardness level in the center of the spot, but also improves the overall average hardness level, compared with the traditional solution of increasing the overlap rate and the overlap rate to avoid central defects.
[0103] Based on the above embodiments and comparative examples, it can be clearly seen that the preparation method provided in the embodiments of the present invention utilizes a secondary laser remelting method, and further strengthening and adjustment of the remelted layer formed by the primary laser remelting is achieved by adjusting the light spot of the secondary laser remelting to completely overlap with the primary laser remelting and adjusting the heat input of the secondary laser remelting to be lower, thereby solving the problems of a large area of solidification loose area and severe solidification cracks in the center of the remelting area, and significantly reducing the hardness and wear and corrosion resistance of the remelted layer. A surface hardened layer with a large thickness, high hardness and good density can be obtained, while having high efficiency, a smooth surface and reduced energy consumption.
[0104] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a thick and dense hardened layer on the surface of a metal component, characterized in that: include: Performing a laser remelting on the surface of the metal component to form a remelting layer; A secondary laser remelting is continued on the surface of the remelting layer to form the hardened layer, the heat input of the secondary laser remelting is lower than that of the primary laser remelting, and all the light spots of the secondary laser remelting are concentric with the primary laser remelting, and the light spots of the secondary laser remelting completely cover the light spots of the primary laser remelting.
2. The preparation method according to claim 1, characterized in that: The first laser remelting and the second laser remelting are both performed in a combination of multiple passes, and the path of the first laser remelting is completely consistent with the path of the second laser remelting, and in any pass, the spot size and the spot center position of the first laser remelting are completely consistent with those of the second laser remelting.
3. The preparation method according to claim 2, characterized in that: In any pass of the laser remelting, the spot overlap rate is 30-50%, and the overlap rate between passes is 30-50%.
4. The preparation method according to claim 1, characterized in that: The heat input of the secondary laser remelting is 40-70% of that of the primary laser remelting.
5. The preparation method according to claim 4, characterized in that: The average heat input per unit area of the laser remelting spot is 70-200 J / mm 2 .
6. The preparation method according to claim 4, characterized in that: The pulse width of the laser remelting is 5 to 30 ms.
7. The preparation method according to claim 6, characterized in that: The average heat input per unit area of the secondary laser remelting spot is 10-40 J / mm 2 .
8. The preparation method according to claim 1, characterized in that: The last spot irradiation of the first laser remelting and the second laser remelting are both outside the preset strengthening area of the metal component.
9. A metal component having a thick and dense hardened layer obtained by the preparation method according to any one of claims 1 to 8.
10. The metal component according to claim 9, characterized in that It includes a metal substrate and a hardened layer formed on the surface of the metal substrate; The material of the metal matrix includes low alloy steel or stainless steel.