Large-size nano-diamond film as well as preparation method and application thereof

The hot wire chemical vapor deposition method under medium-pressure conditions addresses the challenges of low deposition rates and large-area deposition in nanodiamond film production, achieving rapid growth of high-quality films with uniform grain size and low surface roughness for durable applications.

CN119082698APending Publication Date: 2024-12-06ZHEJIANG TIANDI ENVIRONMENTAL PROTECTION TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975215.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing methods for preparing nanodiamond films face challenges such as low deposition rates, high energy consumption, and difficulty in achieving large-area deposition under controlled conditions, while maintaining high film quality and uniform distribution.

Method used

A method using hot wire chemical vapor deposition with a mixed gas of methane and hydrogen under medium-pressure conditions (3-6 kPa) and controlled parameters to produce a large-sized nanodiamond film with a high degree of nanonization, characterized by a growth rate exceeding 500 nm/h and uniform distribution.

Benefits of technology

The method achieves rapid and large-area growth of high-quality nanodiamond films with uniform grain size and low surface roughness, suitable for applications requiring smooth and durable surfaces, such as electrochemical electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082698A_ABST
    Figure CN119082698A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a nano-diamond film by adopting a hot filament chemical vapor deposition method. According to the method, only methane and hydrogen are used as reaction precursors, other inert gases do not need to be added, the content of methane is larger than 6%, and the hot filament temperature is controlled to be 2000 DEG C or above; the reaction pressure is controlled in a medium-low pressure condition, and the maximum pressure can reach 6kPa; and the surface temperature of the substrate is in a range of 750-850 DEG C. The grain size of the nano-diamond film prepared by the method is about several nanometers to dozens of nanometers, and the growth rate of the film is greater than 500nm / h. The preparation method is simple, a reaction gas source is single, other inert gases do not need to be added, the deposition rate is high and is far higher than that of methods such as microwave plasma chemical vapor deposition, the prepared nano-diamond film is high in quality and uniform in distribution, and the method is very suitable for large-area diamond films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material preparation, and in particular to the preparation of a large-size nano diamond film. Background Art

[0002] Diamond has many excellent properties, such as high hardness, high Young's modulus, good stability and chemical inertness. When the grain size of diamond is reduced to the nanometer level (generally from a few nanometers to hundreds of nanometers), its properties will also change accordingly. When its grain size is reduced, the sp 2 The content of bond carbon will increase accordingly, and the surface roughness of the diamond film will be significantly reduced, and its friction coefficient will also be greatly reduced. It is these unique properties of nanodiamond that make it widely used in micro-electromechanical systems, electron field emission devices, electrochemical anode materials and other fields.

[0003] Both micron-scale diamond films and nano-scale diamond films are prepared under hydrogen-rich conditions. x (x=1, 2, 3) to form diamond film, but the two have different requirements in specific process control. The formation of micron-scale diamond film needs to suppress the re-nucleation rate of diamond, while the formation of nano-scale diamond film needs to increase the re-nucleation rate of diamond. Compared with micron-scale diamond film, nano-scale diamond film has a much smaller grain size than micron-scale diamond film, and its film composition is also very different. Common micron-scale diamond film usually contains only sp 3 Bond carbon, sp 2 The content of bond carbon is extremely low; however, in nano-scale diamond films, the grains are mainly sp 3 Diamond phase, but in addition to sp 3 In addition to the bond carbon, it also contains a considerable amount of sp 2 Bonded carbon, hydrocarbons, graphite, amorphous carbon (aC), etc.

[0004] Nanodiamond films are prepared mainly by microwave plasma chemical vapor deposition (MPCVD) and hot wire chemical vapor deposition (HFCVD). Regardless of the method used, the most common method for preparing nanodiamond films is to add inert gas (Ar, He, etc.) to the reaction precursor to form methane, hydrogen, inert gas or a mixture of methane and inert gas to participate in the reaction. In addition, there are reports on the preparation of nanodiamond films using only methane and hydrogen as precursors. This method is more common in reports using MPCVD technology, and requires the methane ratio to be maintained at around 10%. Zeng et al. (Carbon 84 (2014) 103–117) used HFCVD technology to prepare nanodiamond films under the conditions of a methane ratio of 10%, a reaction pressure of 5 Torr (less than 1 KPa, 1 KPa is equivalent to 7.6 torr), and a substrate temperature of 750°C. However, this method generally requires the reaction pressure to be maintained at a low level, less than 15 Torr (about 2 kPa). Under this pressure condition, the reaction rate of the growing film is low, the nucleation rate is slow, and the energy consumption of maintaining low pressure is high.

[0005] In summary, it is particularly important to study a method for manufacturing nanodiamond films with a simple method, a single reaction gas source, a fast deposition rate, and relatively mild reaction conditions. This method can meet the characteristics of high film quality, uniform distribution, and suitability for large-area deposition. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a large-sized nanodiamond film and a preparation method thereof. The preparation method provided by the present invention can prepare a large-sized nanodiamond film with a high degree of nanonization or even completely nanonization under easily controllable process conditions.

[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions.

[0008] First of all, the present invention provides a large-sized nano-diamond film (NCD), which is a fully nano-thin film formed by the accumulation of a large number of fine and dense small diamond grains, and the size of the small diamond grains is about 1 to 99 nanometers; the surface roughness of the nano-diamond film is as low as 12.2nm; the large size means that the uniform growth diameter of the nano-diamond film can reach 10mm to 100mm.

[0009] Again, the present invention also provides a method for preparing the above-mentioned large-size nano-diamond film, using a mixed gas of methane and hydrogen as a reaction precursor, and using a hot wire chemical vapor deposition method to prepare a nano-diamond film on the surface of a substrate, using an HFCVD growth system. The specific preparation includes the following steps:

[0010] (1) Pretreatment of the substrate: The substrate is a tantalum sheet, and the pretreatment is to polish and clean the coated surface of the tantalum sheet. More specifically, the pretreatment process is: polish the tantalum sheet with sandpaper, and then ultrasonically clean it in an acetone solution; then ultrasonically clean the tantalum sheet in an acetone solution of diamond paste with a particle size of 1 μm; finally, ultrasonically clean the tantalum sheet in ultrapure water and blow dry it with nitrogen.

[0011] (2) Vacuum the reaction chamber: Vacuum the reaction chamber until the pressure inside the reaction chamber reaches 10 -3 Pa order of magnitude.

[0012] (3) Tantalum wire carbonization: A mixed gas of methane and hydrogen is introduced to maintain the pressure of the chamber at the pressure value required for the thin film deposition reaction process, wherein the pressure value required for the thin film deposition reaction process is preferably 3kPa to 6kPa; the hot wire (i.e., tantalum wire) is heated, and the heating power is gradually increased to make the hot wire reach the required temperature. When the hot wire reaches the required temperature, the heating power is stabilized to maintain the hot wire at this temperature, and the surface of the hot wire is carbonized. The carbonized tantalum wire is not easily deformed, which facilitates the generation of a stable temperature field.

[0013] The required temperature of the hot wire is preferably 2000-2500° C. The temperature of the hot wire needs to ensure the complete dissociation of hydrogen. At this temperature, the hot wire can dissociate hydrogen well.

[0014] (4) Deposition of nano-diamond film: Continue to stabilize the heating power and maintain the temperature of the hot wire at the required temperature described in step 3), i.e., within the range of 2000-2500°C; adjust the distance between the substrate and the hot wire so that the substrate surface temperature is between 750-850°C; and at the same time adjust the ratio of the reaction precursor, i.e., methane and hydrogen, so that the volume ratio of methane to the reaction precursor gas is 6%-10%, and then start to deposit the nano-diamond film. During the deposition of the nano-diamond film, the pressure of the reaction chamber continues to be maintained within the range of 3kPa-6kPa.

[0015] (5) Cooling: After the deposition reaction is completed, turn off the methane and cool down under the condition of only hydrogen. Gradually and slowly reduce the heating power. After the reaction chamber is cooled to room temperature, release the gas, open the chamber and take out the sample.

[0016] The present invention adopts the technology of hot wire chemical vapor deposition, takes methane and hydrogen as reaction precursors, and controls experimental parameters such as methane ratio, reaction pressure, substrate surface temperature, etc., to achieve the growth of high-quality nano-diamond film on the surface of tantalum sheet under hydrogen-rich conditions and medium-low pressure conditions, and realizes the rapid and large-area growth of diamond film.

[0017] In the process of preparing the nano-diamond film of the present invention using the above method, the inventors adjusted the control of various process parameters and analyzed the various performance indicators of the prepared diamond film, and found that parameters such as the proportion of methane in the reaction precursor, the chamber gas pressure during the deposition process, the hot wire temperature and the substrate surface temperature are key factors affecting whether a nano-diamond film can be prepared and its quality.

[0018] The reaction precursor is a mixed gas of methane and hydrogen. In the preparation process of the present invention, the content of methane in the precursor is the main factor affecting the size of diamond grains. When the volume percentage of methane in the precursor is less than 5%, the size of the diamond grains obtained is mainly micron-sized, and the crystal form is regular. When the methane ratio is 5.5%, the polyhedral diamond begins to break, and there are many long strips of fragments on the surface of the film, and a transformation process between micron-sized diamond and nano-sized diamond occurs. When the methane ratio reaches 6%, a nano-diamond film is obtained, and the grain size ranges from a few nanometers to tens of nanometers. And as the volume percentage of methane increases between 6% and 10%, I D / I G It fluctuates with the methane concentration, decreases with the increase of methane concentration, reaches the minimum value between 9-10%, and then gradually increases, but the overall difference is not obvious. However, when the methane concentration is higher than 10%, the value increases significantly, indicating that the degree of amorphization of the grain boundary increases and the film quality begins to decline. The change trend of H is similar to that of I t-PA / I G The change of is similar to that of , and its value reaches the minimum when the methane concentration reaches about 10%.

[0019] In the present invention, the diamond film deposition reaction can obtain nano-diamond film at a medium or low pressure of 3kPa to 6kPa, and it is not necessary to control the pressure to be less than 2kPa or even less than 1kPa to obtain nano-diamond as in conventional technology. In the present invention, when the deposition reaction pressure is higher than 3kPa, I d / I dnc Reduced to 0, indicating that the diamond film has been completely nanosized; at the same time, I D / I G As the reaction pressure increases, the amorphous carbon content in the grain boundaries of the nano-diamond film increases. However, when the pressure is higher than 4 kPa, its content is almost constant. t-PA / I GThe variation trend of H is similar to that of H. With the increase of pressure, it increases slightly at first, then decreases, reaches the minimum value at 5 kPa, and then increases slightly, which also shows that when the pressure is close to 5 kPa, the nano-diamond film has high quality. In short, when the pressure of the diamond film deposition reaction is within the range of 3 kPa to 6 kPa, the change of pressure does not have a particularly large effect on the growth of nano-diamonds, and high-quality nano-diamond films can be grown.

[0020] Among the indicators mentioned above, I D and I G There are two common peaks in Raman spectroscopy, corresponding to different carbon material structures and lattice vibration modes. D The peaks represent the defects and disorder in the carbon material, while the I G The peaks represent the lattice vibration and degree of order. D It indicates low defects and disorder, indicating that the structure of carbon materials is relatively complete and orderly. G It shows high lattice vibration and order, indicating that the structure of carbon material is relatively compact and stable. For the nano-scale diamond film prepared by the present invention, I D / I G Represents the degree of sp2 hybridization of nano-diamond grain boundaries. The larger the value, the higher the amorphization of the grain boundaries. The smaller the value, the higher the graphitization of the grain boundaries. For nano-diamonds, the smaller the value, the higher the quality of the nano-diamond film. d / I dnc Represents the degree of nano-crystallization of diamond. The smaller the value, the higher the degree of nano-crystallization. When the value is 0, it means complete nano-crystallization, that is, there is no amorphous carbon. t-PA / I G It represents the relative content of t-PA at the grain boundary. The larger the value, the higher the t-PA content at the grain boundary. t-PA can be regarded as one of the growth groups, so it indicates that the diamond quality is lower. H represents the concentration of hydrogen atoms at the grain boundary.

[0021] When the substrate surface temperature is within the preferred temperature range of 750-850°C, the quality of the diamond is almost the same, the particle morphology is clear, and they are relatively complete, while outside this range, the quality is slightly reduced. When the substrate temperature is 700°C or 900°C, the diamond grains obtained will be slightly larger.

[0022] The preparation method of the present invention, under the above process control, the growth rate of the nano diamond film is relatively fast. Under the above process conditions, the growth rate of the nano diamond film of the present invention is greater than 500nm / h, which is much higher than the growth rate of nano diamond by microwave plasma chemical vapor deposition. For example: under the conditions of 8% volume percentage of methane in the precursor, 800°C substrate temperature, and 4kPa reaction pressure, the growth rate of nano diamond can reach 660nm / h.

[0023] The preparation method of the present invention can be applied to the growth method of large-area nano-diamond thin film. It only needs to increase the number of hot wires so that the flat hot wires can completely cover the substrate surface to ensure uniform heat distribution on the substrate surface. By controlling the output power of the hot wire heating motor, the heating power of each hot wire is always maintained consistent to ensure that the hot wire temperature remains basically consistent. At the same time, the deposition substrate is enlarged to achieve a uniform growth diameter of the prepared nano-diamond thin film of 10 mm to 100 mm.

[0024] The present invention also provides a nano-diamond film growth kinetics model, which is expressed as follows:

[0025]

[0026] Wherein Rd is the growth rate of the nanodiamond film, in μm / h; x is the methane concentration ratio (%), i.e., the volume ratio of methane in the mixed gas of the reaction precursor methane and hydrogen; y is the gas pressure (Pa) of the reaction chamber during the nanodiamond film deposition reaction, and z is the substrate temperature (°C) of the deposited nanodiamond film. The above model is based on the preparation method of the nanodiamond film provided by the present invention, and under the control of the above growth process, the deposition of the nanodiamond film conforms to the above growth kinetics model.

[0027] The present invention proposes the above-mentioned nano-diamond film growth kinetic model, which is based on the diamond film growth kinetic model proposed by Ford, and mainly describes diamond growth as the following three processes: 1) disordered carbon is deposited on the substrate surface; 2) atomic hydrogen etches disordered carbon on the substrate surface; 3) disordered carbon is converted into diamond under the action of atomic hydrogen. The following kinetic equation is derived:

[0028]

[0029] in are the fluxes of atomic hydrogen and atomic carbon flowing into the substrate surface, respectively; K is the conversion coefficient of disordered carbon into diamond under the action of atomic hydrogen; A is the adhesion coefficient of carbon on the substrate surface; E C is the probability of disordered carbon etching on the substrate surface under the action of atomic hydrogen.

[0030] In order to further simplify the calculation, the present invention assumes that the rate at which atomic hydrogen etches disordered carbon is equal to the rate at which disordered carbon is converted into diamond under the action of atomic hydrogen, that is, K / E C =1. The formula can be simplified to:

[0031]

[0032] The model is relatively simple in form, but it is difficult to determine the variables, and its value cannot be directly measured through experiments. It is mainly related to the ratio and pressure of the carbon-hydrogen mixed gas flowing into the chamber. A is mainly affected by pressure, and EC and K are mainly affected by substrate temperature. It is expressed as a function of carbon-hydrogen ratio and pressure, A is expressed as a function of pressure, E C , K is expressed as a function of substrate temperature, and it is assumed that it can be expressed in the form of a power function. The formula is as follows:

[0033]

[0034] Where x is the methane concentration (%), y is the reaction pressure (Pa), z is the substrate temperature (°C), and a, b, c, d, e, α, and β are all parameters to be determined. In the above formula, a represents the carbon-hydrogen ratio of the inflow chamber. The influence index of b represents the pressure on and A, c represents the total influence index of substrate temperature on E C The influence index of d represents the carbon-hydrogen ratio of the inflow cavity. The influence index of pressure on and A, α represents the total influence index of carbon-hydrogen ratio, pressure and substrate temperature on The proportional coefficient of the total effect of β represents the carbon-hydrogen ratio and pressure on The following table 1 shows the experimental data collected by the inventors through experiments by adjusting various process parameters and the data fitted on the growth dynamics of nano-diamond films based on the experimental data.

[0035] Table 1: Data table and fitting data table of nanodiamond film growth experiments conducted by the inventors to establish a nanodiamond film growth kinetic model

[0036]

[0037]

[0038] The above experimental data were fitted using Matlab, and the fitting results are shown in Table 2. The corresponding fitting rate "Rd fit" is shown in the fifth column of Table 1 above.

[0039] Table 2: Fitting results of the nanodiamond film growth kinetics model

[0040]

[0041] According to the fitting results, the growth kinetic model of nanodiamond film can be expressed as:

[0042]

[0043] Wherein x is methane concentration (%), y is reaction pressure (Pa), and z is substrate temperature (°C). In addition to the experiments in Table 1 obtained by the above-mentioned model, the inventors also conducted a verification experiment on the above nanodiamond film growth kinetics model. The parameters of the verification experiment are shown in Table 3 below. The experimental verification was conducted in three groups. The deposition time is not a parameter that affects the deposition reaction rate of the nanodiamond film. The deposition time parameter is recorded in the experiment only for calculating the growth thickness of the film per unit time, that is, the growth rate, based on the thickness of the deposited film tested last.

[0044] Table 3: Parameters of the experimental verification of the nanodiamond film growth kinetics model conducted by the inventors

[0045]

[0046] The nanodiamond films obtained from the three verification experiments of Groups 1, 2, and 3 in Table 3 were characterized by SEM. Fig. 9 As shown, they are SEM cross-sectional images of nanodiamond films obtained from the three groups of experiments in Table 3, namely, Groups 1, 2, and 3 (Figure a is Group 1; Figure b is Group 2; Figure c is Group 3), and their corresponding SEM characterization thicknesses are 1.32, 1.24, and 2.06 μm, respectively. Therefore, their film growth rates are 0.440, 0.413, and 0.687 μm / h, respectively.

[0047] The growth rate of the nanodiamond film was calculated using the model formula obtained above, and the growth rates of the three groups of experiments in groups 1, 2, and 3 in Table 3 were calculated to be 0.487, 0.367, and 0.631 μm / h, respectively. The errors of the theoretical calculation values ​​were 10.6%, 10.9%, and 8.18%, respectively, relative to the actual measured values. The errors of the three values ​​were all within a reasonable range, indicating that the model can be used to calculate the growth rate of the nanodiamond film under the deposition conditions of the present invention.

[0048] In some practical application embodiments of the present invention, a boron-doped nano-diamond film with a diameter of 100 mm prepared by the present invention is used as an electrode, and 200 mL of simulated urine is electrochemically anodic oxidized. After 4 hours of degradation, the TOC removal rate is 93%, and after 8 hours of degradation, the TOC removal rate reaches 99%. The results are consistent with the pseudo-first-order kinetic model, and the degradation rate constant is 0.681h -1 Compared with micron-scale diamond film, nano-scale diamond film has smaller grain size, significantly improved film uniformity, and a large difference in surface roughness between the two. For example, the surface roughness of micron-scale diamond film is 239nm, while the surface roughness of the nano-scale diamond film of the present invention is only 12.2nm, which is 19.6 times different. The low surface roughness, combined with the high nano-diamond growth rate in the embodiment of the present invention, indicates that the high growth rate is mainly manifested in the fast re-nucleation rate of the nano-diamond film during the deposition process, and the grain size does not change significantly with the increase of the thickness of the deposition process, so the surface remains extremely smooth; therefore, in the process of electrochemical anodization degradation of TOC, the nano-diamond film has a smaller grain size and abundant grain interfaces, so that it exhibits a better TOC removal rate and degradation rate than the micron-scale diamond film.

[0049] Compared with the prior art, the beneficial effects of the present invention are embodied in the following aspects: first, the preparation method of the present invention is simple, the reaction gas source is single, and no other inert gas needs to be added; second, the present invention prepares a nano-diamond film under medium pressure conditions, with a fast deposition rate and a fast nucleation rate, which are much higher than methods such as microwave plasma chemical vapor deposition, and the prepared nano-diamond film has high quality and uniform distribution, and because it does not need to maintain low-pressure growth, high energy consumption is avoided; in addition, the method of the present invention is very suitable for large-area nano-diamond film deposition, such as the nano-diamond film with a diameter of 100 mm prepared in Example 3 of the present invention.

[0050] Compared with the nano-diamond film (NCD) prepared by the present invention, the micro-diamond film (MCD) is a typical columnar crystal structure. Although the material has high phase purity, high hardness and thermal conductivity, it will correspondingly lead to large surface roughness and friction coefficient of the film material, poor bonding force between grains, relatively low strength, and quasi-isotropy. Ultimately, it is easy to break along the grain boundaries of the film material under large impact loads (such as wire drawing and high-speed cutting) in the application of tool and die materials, or small grains at the grain boundaries fall off and are destroyed. When used as a window or heat sink material, it is difficult to ensure the strength when the thickness is small. The NCD film prepared by the present invention is completely nano-sized, and is formed by the accumulation of a large number of fine diamond small grains. The preparation method of the present invention prepares NCD under process control such as high deposition pressure. The nano-diamond exhibits a high-speed deposition rate dominated by a fast re-nucleation rate, and the grain size does not change with the growth thickness. The surface is extremely smooth. Therefore, in addition to having almost the same overall properties as MCD, NCD also has outstanding advantages such as high elastic modulus, high fracture toughness, lower friction coefficient and resistivity, and high infrared transmittance. Therefore, the use of many specific occasions in mechanics, microelectronics, optics, etc. can well make up for the shortcomings of MCD, and has better application prospects in the fields of quantum optics, electrochemical coatings, friction-reducing coatings, antibacterial / antifungal coatings, lubricants and fuels, drug delivery, catalyst carriers, water cleaning processes, etc. For example, in Application Example 1 of the present invention, the nano-diamond film prepared by the present invention exhibits a very excellent TOC removal rate and degradation rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 Schematic diagram of the hot-wire chemical vapor deposition system used to prepare nanodiamond films.

[0052] Figure 2 This is a surface scanning electron microscope image of the nano-diamond film prepared in Example 2 of the present invention.

[0053] Figure 3 This is a scanning electron microscope image of the cross section of the nano-diamond film prepared in Example 2 of the present invention.

[0054] Figure 4 This is a Raman spectrum of the nano-diamond film prepared in Example 2 of the present invention.

[0055] Figure 5 This is a surface scanning electron microscope image of the micron diamond film prepared in Comparative Example 1 of the present invention.

[0056] Figure 6 This is a Raman spectrum of the micron diamond film prepared in Comparative Example 1 of the present invention.

[0057] Figure 7 This is a curve diagram of TOC removal rate of simulated urine by BD NCD anodization in Application Example 1 of the present invention.

[0058] Figure 8 AFM images of the diamond films prepared in Example 2 of the present invention and Comparative Example 1.

[0059] Figure a shows the micron-scale diamond film prepared in comparative example 1; and Figure b shows the nano-scale diamond film prepared in example 2.

[0060] Fig. 9 The SEM cross-sectional images of diamond films obtained by the present invention in the experiment of verifying the growth dynamics model of nano-diamond films. Figure a is the nano-diamond film of group 1 in Table 3; Figure b is the nano-diamond film of group 2 in Table 3; and Figure c is the nano-diamond film of group 3 in Table 3. DETAILED DESCRIPTION

[0061] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, but the implementation method of the present invention is not limited thereto.

[0062] The structural schematic diagram of the hot wire chemical vapor deposition system for preparing nano diamond film in various embodiments of the present invention is as follows Figure 1 As shown, the hot wire chemical vapor deposition system includes a gas volume flow meter 1, an inlet pipe stop valve 2, a vacuum system 3, a reaction chamber 4, an inlet ring 5, a hot wire 6, a substrate material tantalum sheet 7, a rotating substrate stage 8, an outlet ring 9, a water cooling device 10, a control panel 11, an external heating motor 12, an industrial chiller 13, and a maintenance pump 14. The gas volume flow meter and the inlet valve are used to control the inlet of the reaction precursor mixed gas methane and hydrogen; the rotating substrate stage can rotate and move up and down to adjust the distance between the substrate and the hot wire, thereby controlling the temperature of the substrate surface; during the deposition process, the stable gas pressure of the gas in the deposition system is maintained by the maintenance pump.

[0063] Example 1

[0064] The specific steps of the nano-diamond film of this embodiment are as follows:

[0065] (1) Pretreatment of the substrate: The substrate is a tantalum sheet. The tantalum sheet is polished with metallographic sandpaper and then ultrasonically cleaned in an acetone solution for 30 minutes. The tantalum sheet is then ultrasonically cleaned in an acetone solution of diamond paste with a particle size of 1 μm for 1 hour. Finally, the tantalum sheet is ultrasonically cleaned in ultrapure water for 30 minutes, dried with nitrogen, and quickly placed in the reaction chamber of a hot wire chemical vapor deposition system and placed on a rotating substrate table.

[0066] (2) Vacuuming: Use the vacuum system of the HFCVD system to evacuate the reaction chamber until the pressure in the reaction chamber reaches 10 - 3 Pa order of magnitude.

[0067] (3) Tantalum wire carbonization: Tantalum wire is a hot wire. By heating the tantalum wire, the temperature required for the reaction is provided to the reaction chamber and the substrate. A mixed gas of methane and hydrogen is introduced, wherein the proportion of methane is 3%, and the pressure of the chamber is maintained at about 4KPa; the hot wire is heated by an external heating motor, and the motor current is gradually and slowly increased until the motor output power reaches the required value. When the HFCVD system used in this embodiment controls the heating power of a single hot wire to 600W, the temperature of the hot wire reaches 2200°C. When the hot wire reaches the required temperature, continue to maintain this condition and carbonize the tantalum wire for 30 minutes.

[0068] (4) Deposition of nano-diamond film: Raise the substrate stage to the required height so that the substrate surface temperature is between 750 and 800°C. At the same time, adjust the ratio of methane and hydrogen so that the volume percentage of methane is 8%. At this point, nano-diamond deposition begins. During the deposition process, it is necessary to control the output power of the heating so that the reaction temperature in the chamber is maintained within a relatively stable range; the reaction chamber pressure continues to be maintained at about 4 kPa; the deposition reaction time is 7 hours.

[0069] (5) Cooling: After the deposition reaction is completed, turn off the methane and cool down under the condition of only hydrogen. Gradually and slowly reduce the current of the heating motor. Finally, wait until the temperature in the chamber cools to room temperature before releasing the gas, opening the chamber and taking out the sample.

[0070] Example 2

[0071] In this embodiment, a nano-diamond film is deposited on the surface of a tantalum sheet (with a specification of 1cm*1cm*1mm), and the film is characterized. The deposition conditions used in this embodiment are: in the step of depositing the nano-diamond film, the volume ratio of methane in the methane and hydrogen mixed gas is 8%, the total gas flow rate is 400sccm, the chamber reaction pressure is 4kPa, the single heating wire power is 600W, the wire temperature is 2200℃, the deposition temperature on the surface of the tantalum sheet is 800℃, and the deposition time is 5h. Other conditions are in accordance with the method shown in Example 1, and the above reaction conditions are adopted to obtain a nano-diamond film.

[0072] Figure 2 The surface scanning electron microscope image of the nano-diamond film prepared in Example 2. As can be seen from the figure, the diamond nanoparticles are evenly distributed, the film quality is high, and the particle size is basically kept within 20nm. The surface of the prepared diamond film is mainly "cauliflower-shaped" or long strips of nano-particle diamonds. As the methane concentration increases, the nano-level of the diamond film increases. For example, in Example 2, the methane concentration ratio is 8%. It can be seen from the electron microscope scanning image that the nano-diamond film has been completely nano-leveled.

[0073] Figure 3This is a cross-sectional scanning electron microscope image of the nano-diamond film prepared in Example 2. As can be seen from the figure, the thickness of the nano-diamond film is about 3.3 μm, and the corresponding film growth rate is about 660 nm / h.

[0074] Figure 4 The Raman spectrum of the nanodiamond film prepared in Example 2 shows that the prepared nanodiamond film exhibits typical nanodiamond characteristics, mainly including four different peaks. The wave number is 1340cm -1 The peaks on the left and right are carbon D peaks with a wave number of 1580 cm -1 The peaks on the left and right are the G peaks of carbon. In addition, there are also peaks at wave numbers 1150 and 1480 cm -1 The peaks on the left and right are peaks of ethynyl groups.

[0075] Based on the process parameters of the above embodiment, the inventor adjusts the parameters in the nano-diamond film deposition step, mainly including the methane ratio, the reaction chamber pressure, the temperature of the deposition substrate, etc. When these parameters are controlled within a certain range, for example: the volume ratio of methane in the precursor gas mixed with methane and hydrogen is 6%-10%, the reaction chamber pressure is maintained at 3-6kPa during film deposition, the hot wire temperature is maintained in the range of 2000-2500°C, and the substrate surface temperature is controlled between 750-850°C. Under the control of these parameters, the obtained diamond film is equivalent to the nano-diamond film obtained in the above embodiment 1 and embodiment 2 in microscopic morphology, and the growth rate of the nano-diamond film in the preparation process can basically reach 500nm / h or more. Through the series of experiments adjusted by these parameters, the inventor has obtained a series of diamond films, as shown in Table 1 "Data table and fitting data table of nano-diamond film growth experiments conducted by the inventor for establishing a nano-diamond film growth kinetic model" in the above invention content, which will not be repeated here.

[0076] Example 3

[0077] This embodiment realizes the large-area preparation of nano-diamond thin film by adding hot wires. The details are as follows:

[0078] In this embodiment, a nano-diamond film is deposited on the surface of a large-sized tantalum sheet (specification: Φ10cm*thickness: 1mm), and the film is characterized. Except for the number of hot wires, the other deposition conditions adopted in this embodiment are the same as those in Example 2. The spacing between the hot wires is 7mm. On the basis of Example 2, hot wires with the same spacing are added. The distance between the surface of the tantalum sheet and the hot wire is 7cm higher than 1cm (the size of the tantalum sheet), ensuring that the surface temperature of the tantalum sheet is evenly distributed. For example, when the hot wire temperature is set to 2500K, the temperature of the central area of ​​the substrate is 1065K. At this time, the edge temperature of the 10cm tantalum sheet substrate is 1057K, and the difference between the two is only 0.75%. In this embodiment, the size of the substrate tantalum sheet is increased, and the same uniform temperature field is obtained on the surface of the substrate by increasing the number of hot wires. The nano-diamond film obtained under this condition is also evenly distributed on the entire surface of the large-sized tantalum sheet, and the nano-diamond film is of high quality.

[0079] Comparative Example 1

[0080] This example is to deposit a micron diamond film on the surface of a tantalum sheet (with a specification of 1cm*1cm*1mm) and characterize the film. Except for the methane concentration, the other deposition conditions used in this comparative example are the same as those in Example 2: the volume ratio of methane in the precursor gas is 2%, the total gas flow rate is 400sccm, the chamber reaction pressure is 4kPa, the power of a single heating wire is 600W, the deposition temperature on the surface of the tantalum sheet is 800℃, and the deposition time is 5h. According to the method shown in Example 1, using the above reaction conditions, the diamond film obtained is a micron diamond film.

[0081] Figure 5 The surface scanning electron microscope image of the micron diamond film prepared in this comparative example shows that the diamond particles have a very obvious grain structure, and their crystal forms are mainly hexahedron, octahedron, etc., and the particle size is basically maintained at about 1 μm.

[0082] Figure 6 This is the Raman spectrum of the micron diamond film prepared in this comparative example. The spectrum shows typical diamond characteristics, with a wave number of 1332cm -1 The peak is sp 3 The characteristic peak of diamond is very sharp, and apart from this, there are basically no other peaks.

[0083] Figure 8The following are AFM images of diamond films (a: micron-scale diamond film prepared in Comparative Example 1; b: nano-diamond film prepared in Example 2). Compared with micron-scale diamond film, nano-scale diamond film has smaller grain size, significantly improved film uniformity, and a large difference in surface roughness between the two. The surface roughness of micron-scale diamond film is 239nm, while the surface roughness of nano-scale diamond film is only 12.2nm, a difference of 19.6 times. It is this difference that leads to more holes and defects on the surface of micron-scale diamond film, and bubbles generated during the electrochemical process are more likely to enter the defects on the surface of the film, causing the film to fall off at the defective part, thereby causing electrode failure. On the contrary, nano-scale diamond film has fewer surface defects, and bubbles are not easy to cause damage to the local position of the film. Instead, the bubbles act on the entire film, delaying its failure time, and the area of ​​film shedding is larger when it fails.

[0084] Application Example 1

[0085] In this application example, under the process conditions of Example 3 of the present invention, a large-sized nano-scale diamond film with a diameter of 100 mm is prepared. The reaction precursor gases for depositing the diamond film are hydrogen and methane, both of which are high-purity gases with a purity of 99.99%. In order to make the nano-diamond film have semiconductor properties and realize the degradation function of organic matter, an extremely small amount of boron source is added during the deposition process. The boron source used for doping is gaseous diborane. The doping method adopts a conventional method, and a mixed gas of diborane and hydrogen is input into the reaction chamber for doping during the nano-diamond film deposition step; a boron-doped nano-scale diamond film electrode (BDNCD) is prepared. Since the amount of B doping is extremely small, it will not interfere with the various process parameters to affect the microscopic morphology, nano-level degree, etc. of the prepared nano-diamond film.

[0086] Using the prepared boron-doped nano-diamond film with a diameter of 100 mm as an electrode (BDNCD), this application example carried out electrochemical anodization of 200 mL of simulated urine. After 4 hours of degradation, the TOC removal rate was 93%, and after 8 hours of degradation, the TOC removal rate reached 99%. Figure 7 As shown, Figure 7 This is the TOC removal rate curve of BDNCD anodic oxidation simulated urine in this application example, at 40mA / cm 2 Under constant current conditions, 200 mL of simulated urine was electrochemically anodized using a boron-doped nano-diamond film electrode with a diameter of 100 mm. After 4 hours of degradation, the TOC removal rate was 93%, and after 8 hours of degradation, the TOC removal rate reached 99%. Figure 7 The middle illustration shows the pseudo-first-order kinetic fitting of TOC removal. The result is consistent with the pseudo-first-order kinetic model, and its degradation rate constant is 0.681h -1 .

Claims

1. A large-size nanodiamond film, characterized in that: The nano-diamond film is a fully nano-thin film formed by the accumulation of a large number of fine and dense small diamond grains, and the average size of the small diamond grains is 1 to 99 nanometers.

2. The large-size nanodiamond film according to claim 1, characterized in that: The surface roughness of the nano-diamond film is as low as 12.2 nm; the large size means that the growth diameter of the nano-diamond film reaches 10 mm to 100 mm.

3. A method for preparing a large-size nanodiamond film according to any one of claims 1 to 2, characterized in that: The nano-diamond film is prepared on the substrate surface by hot wire chemical vapor deposition method using a hot wire chemical vapor deposition system and a mixed gas of methane and hydrogen as a reaction precursor, comprising the following steps: 1) Pre-treating the substrate: the substrate is a tantalum sheet, and the pre-treatment is to polish and clean the coating surface of the tantalum sheet; 2) Vacuuming the reaction chamber: Vacuuming the reaction chamber of the hot wire vapor deposition system; 3) Tantalum wire carbonization: A mixed gas of methane and hydrogen is introduced as a reaction precursor, and the pressure in the reaction chamber reaches the required value for the film deposition reaction process; the tantalum wire is heated, and the heating power is gradually increased to make the hot wire reach the required temperature, at which temperature, the surface of the hot wire is carbonized; 4) Depositing a nanodiamond film: maintaining the temperature of the hot wire within the desired temperature range described in step 3); The distance between the substrate and the hot wire is adjusted so that the substrate surface temperature reaches the deposition temperature; at the same time, the ratio of methane and hydrogen in the reaction precursor is adjusted to start depositing the nanodiamond film; During the deposition of the nanodiamond film, the pressure in the reaction chamber continues to be maintained within the pressure range required for the film deposition reaction process described in step 3); 5) Cooling: After the deposition reaction is completed, the methane is turned off, and the temperature is lowered under the condition of only hydrogen. The heating power is gradually and slowly reduced. After the reaction chamber is cooled to room temperature, the air is released and the chamber is opened to obtain the nano-diamond film.

4. The method for preparing a large-size nano-diamond film according to claim 3, characterized in that: The pressure value required for the thin film deposition reaction process in step 3) is 3kPa to 6kPa; the temperature required for the hot wire to reach is in the range of 2000 to 2500°C.

5. The method for preparing a large-size nano-diamond film according to claim 3, characterized in that: in, The step 4) of adjusting the ratio of methane to hydrogen in the reaction precursor means that the volume ratio of methane to the reaction precursor is 6% to 10%; the substrate reaches a deposition temperature between 750 and 850°C.

6. The method for preparing a large-size nano-diamond film according to claim 3, characterized in that: in, In step 4), the growth rate during the deposition of the nano-diamond film is greater than 500 nm / h.

7. A method for preparing a large-size nanodiamond film according to any one of claims 3 to 6, characterized in that: By increasing the number of hot wires, making the coverage of the flat hot wires exceed the substrate surface, controlling the output power of the hot wire heating motor, and maintaining the heating power of each hot wire consistent, large-area substrate deposition is achieved to obtain the large-size nano-diamond film; wherein the large size refers to the diameter of the nano-diamond film reaching 10mm to 100mm.

8. A nanodiamond film growth kinetics model, characterized in that: The model is expressed as: The nano-diamond film is prepared by hot wire chemical vapor deposition using a mixed gas of methane and hydrogen as a reaction precursor; Wherein Rd is the growth rate of the nano-diamond film during the chemical vapor deposition reaction, in μm / h; x is the methane concentration ratio, in volume percentage, that is, the volume proportion of methane in the mixed gas of the reaction precursors methane and hydrogen; y is the gas pressure of the reaction chamber during the chemical vapor deposition reaction of the nano-diamond film, in Pa; z is the temperature of the substrate on which the nano-diamond film is deposited during the chemical vapor deposition reaction of the nano-diamond film, in °C.

9. A nano-diamond film growth kinetics model according to claim 8, characterized in that: Wherein x is 6% to 10%; y is 3kPa to 6kPa; and z is between 750 and 850°C.

10. The use of a nano-diamond film according to claim 1 or 2, characterized in that: After the nano-diamond film is doped with boron to make it semiconductor, the semiconductor nano-diamond film is used as an electrode to simulate urine through electrochemical anodic oxidation, and the TOC removal rate reaches 99%.