Method for synchronously recovering metal and ammonia through direct electrochemistry of alkaline etching solution

Through the combination of one-step electrodeposition and electrolytic reaction, the synchronous recovery of metal and ammonia in the alkaline etching liquid is achieved, the problems of complex separation processes in the prior art are solved, and resource utilization and production efficiency are improved.

CN119082802APending Publication Date: 2024-12-06CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411484472.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, when dealing with alkaline etching waste liquid, the separation and recycling process of metal and ammonia is complex, the resource utilization rate is low, and conventional methods consume high energy, making it impossible to achieve simplified and efficient recycling.

Method used

A one-step electrodeposition method is used to recover valuable metals in an alkaline environment, and the metal-ammonia complex ions are driven to move to the cathode surface through an electric field, and the pH value is increased by the reduction reaction of electrolytic water, which promotes the recovery of ammonia, combined with stripping. The membrane achieves high purity recovery of ammonia, skipping the acidification pretreatment step.

Benefits of technology

The synchronous recovery of metal and ammonia in the alkaline etching liquid is achieved, with a purity of 99.55%, simplifying the process flow, reducing processing cycles, improving production efficiency and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082802A_ABST
    Figure CN119082802A_ABST
Patent Text Reader

Abstract

The invention provides a method for synchronously recovering metal and ammonia through direct electrochemistry of alkaline etching liquid. Parameter fitting is carried out on a model curve graph obtained through multiple sets of calculation data through MATLAB software to obtain a function relation. According to the research, the influence of the ratio of the metal ion concentration to the ammonia concentration on the recovery effect is as follows: under the condition of low ammonia, if a large amount of copper hydroxide appears in the solution, the part of copper cannot be recovered in an electrolysis form, and if the ammonia concentration is relatively high, copper ammonia complex ions in the solution are increased, and the copper hydroxide is reduced, the part of copper cannot be recovered in an electrolysis form. The copper ammonia complex ions can be recycled in an electrolysis mode. The ratio of metal to ammonia affects the recovery effect, and copper loss is caused mainly based on whether copper hydroxide is generated or not and the amount of generated copper hydroxide. The solution is directly regulated to the copper ammonia complex to inhibit copper hydroxide, so that the loss of an additional reagent is directly regulated and reduced, and the cost is reduced. The recovery purity of the method is as high as 99.55%, and the process flow is greatly simplified.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of wastewater treatment technology and resource recovery, and in particular to a method for directly electrochemically and synchronously recovering metal and ammonia using an alkaline etching solution. Background Art

[0002] The etching process is a key step in the manufacturing process of printed circuit boards. During the etching process, a large amount of copper, nickel, cobalt and other metals are dissolved. When the solution reaches saturation, it is unstable and easily forms muddy precipitation, which loses the etching function and becomes waste liquid. The main components of alkaline etching waste liquid include metal ions, ammonium salts, ammonia water and a small amount of metal salts used to improve etching performance. If it is directly discharged into the environment, it will not only cause a waste of resources, but also pollute the environment. The metal-ammine complex formed by high concentrations of metal ions and ammonia is the main pollutant in this type of wastewater. Its high toxicity, high strength and strong stability pose a serious threat to aquatic ecosystems and human health.

[0003] At present, the conventional idea for the treatment of metal-ammonia wastewater is to first perform a pretreatment of the broken complex, and then treat the metal and ammonia separately by traditional methods after the metal and ammonia are separated. Common methods of breaking complexes include magnesium ammonium phosphate precipitation, sulfide precipitation, breakpoint chlorination or acid-base neutralization, the principle of which is to attack the metal-ammonia coordination bond by electrophilic reaction or nucleophilic reaction to break it. The metal ions after decomplexation are recovered by precipitation, adsorption or electrolysis, but the product has many impurities and low resource utilization. When the free ammonia in the solution is at a low concentration, biological metabolism, breakpoint chlorination and other methods are used to remove it, the treatment cycle is long and it cannot be recycled. When the concentration is high, three-phase evaporation, stripping and other methods are used for recovery, which has high energy consumption and low production capacity. The whole process requires a combination of multiple processes, complex procedures, long processing time and unstable effect. Therefore, how to efficiently and easily recover metals and ammonia while simplifying the treatment process has become one of the difficult problems that need to be solved and overcome in the current field of alkaline etching waste liquid treatment.

[0004] The electrolysis method converts pollutants into harmless substances through oxidation and reduction reactions at the two electrodes. It has the advantages of simple process, convenient operation, and the ability to remove and recover multiple heavy metals at the same time. It has been widely used in engineering practice. Alkaline etching solution will produce hydroxide interference during the electrolysis process, and it is often necessary to add a large amount of acid in advance to adjust the pH to acidic. Studies have shown that metals and ammonia will undergo complexation under alkaline conditions to form metal-ammine complexes with a stability constant of 2*10 13, with a strong thermodynamic driving force. Under alkaline conditions, the formation of metal-ammine complexes is very favorable within a certain range of ammonia concentration, which can effectively inhibit the precipitation of hydroxides. During the electrochemical reaction, the pH of the cathode surface is much greater than the pH of the solution itself, reaching about 13. Combined with thermodynamic equilibrium calculation analysis, under this condition, ammonia nitrogen mainly exists in the form of NH3(g), and ammonia can be recovered using an ammonia stripping membrane. By controlling the ammonia concentration and the solution pH, using a one-step electrodeposition method to recover metals and coupling an ammonia stripping membrane to recover ammonia, it is expected to achieve direct electrochemical simultaneous recovery of metals and ammonia in alkaline etching solutions, simplify the process flow, and improve processing efficiency.

[0005] In view of this, the present invention provides a method for directly electrochemically recovering metal and ammonia from an alkaline etching solution, so as to simultaneously achieve the treatment and resource recovery of the alkaline etching waste liquid, thereby achieving the dual benefits of pollution control and resource utilization. Summary of the invention

[0006] The invention provides a method for directly electrochemically and synchronously recovering metal and ammonia from an alkaline etching solution, the purpose of which is to solve the above-mentioned problems existing in the background technology.

[0007] In order to achieve the above-mentioned purpose, an embodiment of the present invention provides a method for the direct electrochemical simultaneous recovery of metals and ammonia in an alkaline etching solution, wherein valuable metals are recovered by a one-step electrodeposition method in an alkaline environment, with a purity of 99.55%, skipping the acidification pretreatment step, and reducing the cost of adding reagents. Driven by the electric field, the metal-ammonia complex ions and ammonium ions in the solution are directed to the cathode surface, reducing the diffusion mass transfer limitation. At the same time, the electrolytic reduction of water near the cathode causes the pH value to increase, promoting the conversion of ammonium ions to ammonia, which is beneficial to the recycling of ammonia. This method recovers high-purity ammonia by stripping, without the need for additional energy consumption. While the metal is deposited at the cathode, the ammonia is absorbed by the acid solution through the stripping membrane, successfully realizing the simultaneous separation and recovery of metals and ammonia in the alkaline etching solution, simplifying the process flow, reducing the processing cycle, and improving production efficiency, which has great commercial prospects.

[0008] An embodiment of the present invention provides a method for directly electrochemically recovering metal and ammonia from an alkaline etching solution, comprising the following steps:

[0009] S1: Calculate the metal hydroxide content at a certain ratio of ammonia to metal ions based on chemical thermodynamics, and obtain a metal hydroxide percentage diagram;

[0010] S2: taking a plurality of boundary points in the metal hydroxide percentage diagram, performing nonlinear fitting using MATLAB software, and obtaining a functional relationship of the boundary conditions of the metal hydroxide;

[0011] S3: Based on the functional relationship of the boundary condition of metal hydroxide, the alkaline etching solution is regulated by adjusting the molar concentration ratio of metal ions to ammonia and the pH of the alkaline etching solution;

[0012] S4: pumping the regulated alkaline etching solution into an electrochemical reaction device to simultaneously recover metal and ammonia through electrochemical reaction.

[0013] Preferably, the molar concentration ratio of metal ions to ammonia is 1:2 to 1:64.

[0014] Preferably, the metal hydroxide boundary condition function relationship is Y=2.63X+29488.74e -X -1.94E - 31 e 6.27X -20.41, X is pH, Y is the ratio of ammonium to metal ions.

[0015] More preferably, R of the metal hydroxide boundary condition functional relationship 2 is 0.99.

[0016] Preferably, the alkali in the alkaline etching solution is at least one of copper, nickel, cobalt, zinc and molybdenum, and the concentration is 0.1-10 g / L.

[0017] Preferably, the pH value of the alkaline etching solution is 8-13.

[0018] Preferably, the electrochemical reaction device comprises a working electrode constructed by mesh metal and membrane, coupled with an acidic ammonia absorption chamber.

[0019] More preferably, the mesh metal is at least one of iron, copper, titanium and nickel, and has a mesh size of 50 to 400; the membrane is a porous polytetrafluoroethylene (PTFE) membrane; and the membrane and the mesh metal are combined by bonding or physical bonding.

[0020] More preferably, the acidic ammonia absorption chamber is at least one of sulfuric acid, hydrochloric acid and nitric acid.

[0021] Preferably, the electrochemical reaction is carried out under constant voltage or constant current, the constant voltage is -0.6V to -3V vs. Ag / AgCl, and the constant current is 2 to 200 mA / cm 2 .

[0022] The principle and reaction equation are described below.

[0023]

[0024] By adjusting the pH and ammonia concentration of the solution, the proportion of copper-containing species in the solution can be controlled so that the copper-ammine complex takes the dominant position, thereby recovering this part of the copper by electrolysis.

[0025] Specifically, as the pH increases, the amount of NH3 in the solution increases, resulting in more ammonia combining with copper, and the proportion of copper-ammine complexes formed also increases. Therefore, the present invention can suppress the generation of copper hydroxide by adjusting the pH and ammonia concentration to form a copper-ammine complex.

[0026] The above scheme of the present invention has the following beneficial effects:

[0027] (1) The present invention uses MATLAB software to perform parameter fitting on a model curve graph based on multiple sets of calculation data to obtain a functional relationship, and controls the molar concentration ratio of metal ions to ammonia and the pH of the alkaline etching solution to achieve the control of the alkaline etching solution, and then pumps the regulated alkaline etching solution into an electrochemical reaction device to simultaneously recover metal and ammonia through electrochemical reactions. The present invention not only utilizes the specificity of metal-ammonia complexation under alkaline conditions to effectively prevent the precipitation of metal ions under alkaline conditions, but also can simultaneously achieve the recovery of metal and ammonia through the mesh metal and the working electrode of the membrane.

[0028] (2) Through the above research, it was found that the ratio of metal ion concentration to ammonia concentration affects the recovery effect as follows: Under low ammonia conditions, if a large amount of copper hydroxide appears in the solution, this part of copper cannot be recovered by electrolysis. If the ammonia concentration is high, the copper-ammonia complex ions in the solution increase and the copper hydroxide decreases. The copper-ammonia complex ions can be recovered by electrolysis. The ratio of metal to ammonia affects the recovery effect, mainly based on whether copper hydroxide is produced and how much copper hydroxide is produced, resulting in copper loss.

[0029] (3) Compared with the alkaline copper ammonia solution recovery process using extraction-electrolysis or acidification-electrolysis, the present invention directly regulates the solution to copper ammonia complex to inhibit copper hydroxide, thereby directly regulating to reduce the loss of added reagents and reduce costs. In addition, with regard to the recovery purity, the current recovery purity of extraction-electrolysis and acidification-electrolysis is already the highest in the industry (about 99.99%), and the recovery purity of the present invention regulation-electrolysis is 99.55%, and the process flow is greatly simplified. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 This is a graph showing the percentage of copper hydroxide in Example 1 of the present invention.

[0032] Figure 2 This is the copper hydroxide distribution relationship model in Example 1 of the present invention.

[0033] Figure 3 It is the recovery rate of copper and ammonia in Example 2 of the present invention.

[0034] Figure 4 This is the SEM image of sample 1 in Example 2 of the present invention.

[0035] Figure 5 This is the XRD diagram of sample 1 in Example 2 of the present invention. DETAILED DESCRIPTION

[0036] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0037] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0038] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0039] In view of the existing problems, the present invention provides a method for directly electrochemically recovering metal and ammonia from an alkaline etching solution, comprising the following steps:

[0040] S1: Calculate the metal hydroxide content at a certain ratio of ammonia to metal ions based on chemical thermodynamics, and obtain a metal hydroxide percentage diagram;

[0041] S2: taking a plurality of boundary points in the metal hydroxide percentage diagram, performing nonlinear fitting using MATLAB software, and obtaining a functional relationship of the boundary conditions of the metal hydroxide;

[0042] S3: Based on the functional relationship of the boundary condition of metal hydroxide, the alkaline etching solution is regulated by adjusting the molar concentration ratio of metal ions to ammonia and the pH of the alkaline etching solution;

[0043] S4: pumping the regulated alkaline etching solution into an electrochemical reaction device to simultaneously recover metal and ammonia through electrochemical reaction.

[0044] Preferably, the molar concentration ratio of metal ions to ammonia is 1:2 to 1:64.

[0045] Preferably, the metal hydroxide boundary condition function relationship is Y=2.63X+29488.74e -X -1.94E - 31 e 6.27X-20.41, X is pH, Y is the ratio of ammonium to metal ions.

[0046] More preferably, R of the metal hydroxide boundary condition functional relationship 2 is 0.99.

[0047] Preferably, the alkali in the alkaline etching solution is at least one of copper, nickel, cobalt, zinc and molybdenum, and the concentration is 0.1-10 g / L.

[0048] Preferably, the pH value of the alkaline etching solution is 8-13.

[0049] Preferably, the electrochemical reaction device comprises a working electrode constructed by mesh metal and membrane, coupled with an acidic ammonia absorption chamber.

[0050] More preferably, the mesh metal is at least one of iron, copper, titanium and nickel, and has a mesh size of 50 to 400; the membrane is a porous polytetrafluoroethylene (PTFE) membrane; and the membrane and the mesh metal are combined by bonding or physical bonding.

[0051] More preferably, the acidic ammonia absorption chamber is at least one of sulfuric acid, hydrochloric acid and nitric acid.

[0052] Preferably, the electrochemical reaction is carried out under constant voltage or constant current, the constant voltage is -0.6V to -3V vs. Ag / AgCl, and the constant current is 2 to 200 mA / cm 2 .

[0053] To further illustrate the method proposed in this specific embodiment, relevant examples are listed below for illustration. In the following text, metal refers to copper, and metal hydroxide refers to copper hydroxide. The "ammonia" mentioned herein usually refers to ammonia gas, such as the "ammonia" in the copper ammonia complex refers to ammonia gas. It should be noted that the "ammonia metal ion ratio" refers to the ratio of the total ammonia and metal ion molar concentrations. Total ammonia can be understood as the total ammonia nitrogen concentration, which consists of two parts: ammonium ions and ammonia gas.

[0054] Example 1

[0055] The metal-ammonia-pH-hydroxide relationship model is established, including the following steps:

[0056] (1) Based on chemical thermodynamics, the copper hydroxide content at a copper concentration of 1000 mg / L and an ammonia copper ion molar concentration ratio of 2-10 was calculated. The results are as follows: Figure 1 The percentage of copper hydroxide is shown in the figure. In chemistry, the ion concentration in the solution is generally less than 1*10 -4 mol / L, it can be considered that the phase does not exist.

[0057] (2) Take multiple Figure 1The boundary point values ​​of the copper hydroxide percentage diagram are nonlinearly fitted by MATLAB software to obtain the copper hydroxide boundary condition function relationship, as shown in Figure 2 As shown, Y = 2.63X + 29488.74e -X -1.94E -31 e 6.27X -20.41(R 2 =0.99), X is pH, Y is the ratio of ammonia to copper ions. For example, when the copper concentration is 1000 mg / L, the pH is 9.5, and the ammonia concentration is 1501.42 mg / L, the copper hydroxide boundary condition is met.

[0058] To further verify the relationship model, a solution with a copper concentration of 1000 mg / L, an ammonia nitrogen concentration of 1500 mg / L, and a pH of 9.5 was prepared. The test found that the concentration of copper hydroxide in the solution was 8.7 mg / L, which was within the allowable error range, indicating that the metal-ammonia-pH-hydroxide relationship model is applicable.

[0059] Example 2

[0060] A method for directly electrochemically recovering metal and ammonia from an alkaline etching solution comprises the following steps:

[0061] An alkaline etching solution with a copper ion concentration of 1000 mg / L, an ammonia nitrogen concentration of 2204 mg / L, and a pH of 9.5 was used for electrochemical recovery of metals and ammonia.

[0062] The anode is a platinum sheet (4cm×4cm), the reference electrode is silver chloride, the cathode is a titanium mesh (4cm×4cm), and the ammonia stripping membrane (4cm×4cm) is a polytetrafluoroethylene membrane. A constant voltage of -1.2V vs. Ag / AgCl is applied to the titanium mesh using a Wantong electrochemical workstation. The reaction time is 10h. Samples are taken in the reaction chamber and the ammonia recovery chamber to detect the concentrations of copper ions and ammonia nitrogen. The results are as follows: Figure 3 The recovery rates of copper and ammonia were 99.79% and 75.92%, respectively.

[0063] The cathode copper on the titanium mesh was scraped off to obtain copper powder, which was named sample 1. Figure 4 As shown in the figure, the diameter of the copper particles is about 200 μm and their morphology is cauliflower-like. Figure 5 As shown, the XRD diffraction peaks of sample 1 mainly appear at 43.3°, 50.4°, 74.1° and 89.9°, indicating that the main component is elemental copper and contains a small amount of sodium sulfate. However, no diffraction peaks of copper oxide and hydroxide were found, further indicating that this method can effectively prevent the formation of copper hydroxide under alkaline conditions. In addition, the test shows that the purity of cathode copper is 99.55%.

[0064] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for directly electrochemically recovering metal and ammonia from an alkaline etching solution, characterized in that: The steps include: S1: Calculate the metal hydroxide content at a certain ratio of ammonia to metal ions based on chemical thermodynamics, and obtain a metal hydroxide percentage diagram; S2: taking a plurality of boundary points in the metal hydroxide percentage diagram, performing nonlinear fitting using MATLAB software, and obtaining a functional relationship of the boundary conditions of the metal hydroxide; S3: Based on the functional relationship of the boundary condition of metal hydroxide, the alkaline etching solution is regulated by adjusting the molar concentration ratio of metal ions to ammonia and the pH of the alkaline etching solution; S4: pumping the regulated alkaline etching solution into an electrochemical reaction device to simultaneously recover metal and ammonia through electrochemical reaction.

2. The method for direct electrochemical simultaneous recovery of metal and ammonia by alkaline etching solution according to claim 1, characterized in that: The molar concentration ratio of metal ions to ammonia is 1:2 to 1:

64.

3. The method for direct electrochemical simultaneous recovery of metal and ammonia by alkaline etching solution according to claim 1, characterized in that: The functional relationship of the boundary condition of metal hydroxide is Y = 2.63X + 29488.74e -X -1.94E -31 e 6.27X -20.41, X is pH, Y is the ratio of ammonium to metal ions.

4. The method for direct electrochemical simultaneous recovery of metal and ammonia by alkaline etching solution according to claim 3, characterized in that: The metal hydroxide boundary condition function relationship R 2 is 0.

99.

5. The method for direct electrochemical simultaneous recovery of metal and ammonia by alkaline etching solution according to claim 1, characterized in that: The alkali in the alkaline etching solution is at least one of copper, nickel, cobalt, zinc and molybdenum, and the concentration is 0.1-10 g / L.

6. The method for direct electrochemical simultaneous recovery of metal and ammonia by alkaline etching solution according to claim 1, characterized in that: The pH value of the alkaline etching solution is 8-13.

7. The method for direct electrochemical simultaneous recovery of metal and ammonia by alkaline etching solution according to claim 1, characterized in that: The electrochemical reaction device comprises a working electrode constructed by mesh metal and a membrane, and a coupled acidic ammonia absorption chamber.

8. The method for direct electrochemical simultaneous recovery of metal and ammonia by alkaline etching solution according to claim 7, characterized in that: The mesh metal is at least one of iron, copper, titanium and nickel, and has a mesh size of 50 to 400; the membrane is a porous polytetrafluoroethylene membrane; and the membrane and the mesh metal are combined by bonding or physical bonding.

9. The method for direct electrochemical simultaneous recovery of metal and ammonia by alkaline etching solution according to claim 7, characterized in that: The acidic ammonia absorption chamber is at least one of sulfuric acid, hydrochloric acid and nitric acid.

10. The method for direct electrochemical simultaneous recovery of metal and ammonia by alkaline etching solution according to claim 1, characterized in that: The electrochemical reaction is carried out under constant voltage or constant current, the constant voltage is -0.6V to -3V vs. Ag / AgCl, and the constant current is 2 to 200 mA / cm 2 .