Bio-based polyurethane waterproof moisture-permeable film and preparation method thereof
By using bio-based polyurethane resin and additives to prepare waterproof and moisture-permeable films, the environmental and sustainability problems of traditional petroleum-based materials are solved, and the production of high-strength and environmentally friendly bio-based polyurethane waterproof and moisture-permeable films is achieved, satisfying sustainability Development requirements.
Patent Information
- Application Number
- CN202411221295.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-06-27
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-02
AI Technical Summary
Traditional petroleum-based waterproof and moisture-permeable membrane materials consume a lot of energy during production and use, pose a threat to the environment and the human body, and are difficult to recycle and degrade, and cannot meet the needs of sustainable development.
The waterproof and moisture-permeable film is prepared by using bio-based polyurethane resin and bio-based additives. The membrane pore structure is adjusted by wet synthesis method. The polyether-type aliphatic polyurethane resin with high biomass content and solvent extracted from natural ingredients are added. The strength and environmental protection of the material.
The large-scale production of environmentally friendly bio-based polyurethane waterproof and moisture-permeable films has been achieved, which reduces carbon emissions, improves the hydrostatic pressure and toughness of the materials, and solves the pollution problem of traditional materials through biodegradable materials.
Smart Images

Figure CN119083195A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of functional textiles, in particular to a bio-based polyurethane waterproof and breathable membrane and a preparation method thereof. Background Art
[0002] Bio-based materials are environmentally friendly polymer materials made from renewable biomass (such as soybeans, corn, wheat, etc.). They have the characteristics of wide range of raw materials and green environmental protection. Nowadays, most waterproof and breathable membrane materials on the market are petroleum-based materials, which will threaten the environment during their production and use. Therefore, it is urgent to develop a bio-based waterproof and breathable membrane to overcome the shortcomings of traditional petroleum-based materials, such as high energy consumption in processing and difficulty in recycling.
[0003] Nowadays, with the rapid development of the times, the demand for fabrics in the market is increasing. In addition to the most basic protection and decorative functions, there are higher demands for clothing protection and comfort in some special working environments and daily life, and waterproof and breathable membrane materials have come into being. Waterproof and breathable membrane is a functional membrane material with excellent water permeability and moisture permeability. It is usually compounded with natural fiber fabrics or synthetic fiber fabrics to manufacture functional clothing with unique protection and comfort, such as: mountaineering clothes, ski suits, assault jackets, field military uniforms, chemical protection clothing, shoes, socks and gloves, etc. Clothing made with waterproof and breathable membrane as the core material can block rain and snow from penetrating into the interior and prevent damage from harsh external conditions, while transmitting the sweat produced by the human body in the form of moisture, thereby ensuring the safety and comfort of the human body. Therefore, it is becoming more and more important in people's production activities and daily life.
[0004] The polyurethane porous membrane has good waterproof and breathable properties, and its elasticity is excellent. It can adapt to different bonding processes during the bonding process with the fabric. At the same time, during high-intensity outdoor sports, the fabric at the joints will be stretched to varying degrees. This film material gives the clothing good elasticity and adaptability, preventing the film from tearing during intense exercise. Therefore, polyurethane waterproof and breathable membrane is a more preferred material. The PU membrane using phase separation pores has a simple production process, adjustable pore structure and low cost, which is conducive to large-scale production. So far, there are few reports on its use in the field of waterproof and breathable membranes.
[0005] In addition, traditional petroleum-based waterproof and breathable membrane materials consume a lot of energy during processing, pose a threat to the human body and the environment, are prone to produce volatile organic compounds during use, and are difficult to recycle and degrade after use. The use of bio-based materials, converting renewable raw materials into biopolymer materials or monomers, and then developing various products to obtain environmentally friendly functional materials is a new research and development direction. Therefore, it is urgent to develop a fully bio-based polyurethane waterproof and breathable porous membrane to achieve clean and pollution-free throughout the entire process - the solvent is recyclable and the raw materials are degradable to meet the current requirements of sustainable development. Summary of the invention
[0006] The purpose of the present invention is to provide a bio-based polyurethane waterproof and breathable membrane and a preparation method thereof in order to overcome the defects of the above-mentioned prior art. The polyurethane and additives of the waterproof and breathable membrane casting liquid provided by the present invention are all bio-based materials, and at the same time have good waterproof and breathable properties and can be produced on a large scale.
[0007] The purpose of the present invention can be achieved by the following technical solutions: A method for preparing a bio-based polyurethane waterproof and breathable membrane comprises the following steps: Add bio-based polyurethane resin to an organic solvent, stir until the polyurethane resin is evenly mixed, then add other additives, continue to stir evenly to obtain a mixed solution; pour the mixed solution onto a substrate, use a scraping tool to scrape it into a thin film, then immerse it in a coagulation bath, and after solidification, wash and dry it to obtain a bio-based polyurethane waterproof and breathable membrane.
[0008] Furthermore, the components, by weight, include: 40-55 parts of bio-based polyurethane resin; 30-55 parts of bio-based organic solvent; 0.5~3 parts of bio-based penetrant; 2~3 parts of bio-based surfactant; 3~12 parts of porogen.
[0009] Furthermore, the bio-based polyurethane resin solution selects a polyether-type aliphatic polyurethane having a biomass content greater than or equal to 50%, and selects: a bio-based polyurethane containing isosorbide polyether, wherein the isosorbide polyether accounts for 10% of the total volume of the bio-based polyurethane liquid.
[0010] Furthermore, the bio-based permeabilizer includes fatty acid methyl ester sulfonate or alkyl betaine; the bio-based surfactant includes one or more of sarcosine lipopeptide, dodecyl glucoside, polyethyleneimine lipopolysaccharide or dodecyl polyethoxylated alcohol amine; the porogen includes one or more of walnut shell particles, bamboo fiber particles, hawthorn seed particles or koizsa apricot kernel shell particles.
[0011] Furthermore, the substrate is selected from one of non-woven fabric, spunbond fabric, release paper, kraft paper, wood pulp fabric, and cotton fabric.
[0012] Furthermore, the coagulation bath is a mixed solution of water and N,N-dimethylformamide, and the volume ratio of water to N,N-dimethylformamide is (8-8.2):2.
[0013] Furthermore, the duration of the coagulation bath is 2 min to 5 min.
[0014] Furthermore, the water washing temperature is 25-40°C, and the water washing time is 20min~40min.
[0015] Furthermore, the drying temperature is 80-120° C., and the drying time is 10-20 minutes.
[0016] A bio-based polyurethane waterproof and breathable membrane is prepared by adopting the above-mentioned preparation method.
[0017] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) The polyurethane waterproof and breathable membrane of the present invention adopts the phase separation pore-forming method of wet synthetic leather, and the pore structure of the membrane obtained is adjustable, and it has both high elasticity and good waterproof and breathable properties.
[0018] (2) The polyurethane resin in the raw material of the waterproof and breathable membrane of the present invention is renewable and can replace traditional petroleum-based raw materials, which can effectively reduce carbon emissions and is an environmentally friendly membrane material.
[0019] (3) The conventional high-biobased polyurethane waterproof and breathable membrane has a low hydrostatic pressure because its molecular chain is too soft and difficult to form a dense structure. The polyurethane waterproof and breathable composite membrane of the present invention contains isosorbide as a component, which increases the strength and toughness of the material and can effectively improve its hydrostatic pressure.
[0020] (4) The solvents used in the present invention are all environmentally friendly bio-based solvents extracted from natural ingredients such as plants and animals. They not only have low volatility and toxicity, but also have good biodegradability and will not cause pollution to the environment.
[0021] (5) The surfactant of the present invention is a bio-based surfactant, which has a wide source and is renewable.
[0022] (6) The penetrant of the present invention is a bio-based penetrant, which overcomes the difficulties of traditional penetrants such as being acid- and alkali-resistant, difficult to degrade, and not environmentally friendly.
[0023] (7) The porogen of the present invention is a bio-based porogen. Traditional porogens mainly include SiO2 and Ca2CO3. These porogens are prone to cause pollution to the human body and the environment during production and use. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The following is a SEM image of the bio-based polyurethane waterproof and breathable membrane prepared in Example 1; a schematic diagram of the structure of a fully bio-based waterproof and breathable fabric preparation device used; Figure 2 This is a SEM image of the bio-based polyurethane waterproof and breathable membrane prepared in Example 3; Figure 3 This is the SEM image of the bio-based polyurethane waterproof and breathable membrane prepared in Example 7. DETAILED DESCRIPTION
[0025] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0026] A method for preparing a bio-based polyurethane waterproof and breathable membrane comprises the following steps: Add bio-based polyurethane resin to an organic solvent, stir until the polyurethane resin is evenly mixed, then add other additives, continue to stir evenly to obtain a mixed solution; pour the mixed solution onto a substrate, use a scraping tool to scrape it into a thin film, then immerse it in a coagulation bath, and after solidification, wash and dry it to obtain a bio-based polyurethane waterproof and breathable membrane.
[0027] Furthermore, the components, by weight, include: 40-55 parts of bio-based polyurethane resin; 30-55 parts of bio-based organic solvent; 0.5~3 parts of bio-based penetrant; 2~3 parts of bio-based surfactant; 3~12 parts of porogen.
[0028] Furthermore, the bio-based polyurethane resin solution selects a polyether-type aliphatic polyurethane having a biomass content greater than or equal to 50%, and selects: a bio-based polyurethane containing isosorbide polyether, wherein the isosorbide polyether accounts for 10% of the total volume of the bio-based polyurethane liquid.
[0029] The structure of the bio-based polyether containing isosorbide is as follows:
[0030] Furthermore, the bio-based penetrant includes fatty acid methyl ester sulfonate or alkyl betaine, and the added content is 0.5%~3% of the total mass of the solvent and polyurethane; the bio-based surfactant includes one or more of sarcosine lipopeptide, dodecyl glucoside, polyethyleneimine lipopolysaccharide or dodecylpolyethoxyl alcoholamine, and the added content is 1%~3% of the total mass of the solvent and polyurethane; the porogen includes one or more of walnut shell particles, bamboo fiber particles, hawthorn seed particles or koizsa apricot shell particles, and the added content is 3%~12%.
[0031] Furthermore, the substrate is selected from one of non-woven fabric, spunbond fabric, release paper, kraft paper, wood pulp fabric, and cotton fabric.
[0032] Furthermore, the coagulation bath is a mixed solution of water and N,N-dimethylformamide, the volume ratio of water to N,N-dimethylformamide is (8-8.2):2, and the substrate is immersed in the coagulation bath device quickly and continuously.
[0033] Furthermore, the duration of the coagulation bath is 2 min to 5 min.
[0034] Furthermore, the water washing temperature is 25-40°C, and the water washing time is 20min~40min.
[0035] Furthermore, the drying temperature is 80-120° C., and the drying time is 10-20 minutes.
[0036] A bio-based polyurethane waterproof and breathable membrane is prepared by adopting the above-mentioned preparation method.
[0037] The mechanism of the present invention is described as follows: (1) Regulation mechanism of surfactants during the solidification of bio-based waterproof and breathable membranes The purpose of adding surfactants to the casting solution of bio-based waterproof and breathable membranes is to adjust the pore structure. The molecular structure of surfactants has a common feature. Its molecules are composed of two parts, one is solvent-philic (polar part) and the other is solvent-phobic (non-polar part). The surface activity of surfactants comes from the amphiphilic structure of surfactant molecules.
[0038] When the surfactant is dissolved in the bio-based polyurethane solution, according to the rule of "like attracts like", the polar groups make the molecules tend to enter the solvent, that is, the strongly polar solvent is friendly to the polar groups in the surfactant, while the non-polar long hydrocarbon chains try their best to prevent them from dissolving in the solvent and migrate from the inside of the solvent, tending to escape from the solvent.
[0039] When the non-solvent enters, the polarity of the non-solvent molecule is weak, which is not enough to make the polar group of the surfactant break away from the action of the solvent and combine with the non-solvent. Therefore, one end of the polar group in the surfactant extends to the solvent with stronger polarity and the non-polar group extends to the non-solvent with weaker polarity. It is precisely because of this state of existence of the surfactant that the surfactant can change the bidirectional diffusion rate of the solvent and the non-solvent when the bio-based polyurethane solidifies. The results of the action are different for different surfactants.
[0040] The following embodiments are implemented based on the above technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.
[0041] The following are more detailed implementation cases, which further illustrate the technical solutions of the present invention and the technical effects that can be obtained. Example 1
[0042] A phase separation pore forming method for a bio-based polyurethane waterproof and breathable membrane, the specific steps are as follows: Step 1: Add ethanol and acetone in a mixing ratio of 1:3 into a reactor and stir, then add a bio-based polyurethane resin solution, where the bio-based resin accounts for 55% of the total content of the solution, and stir for 50 minutes to obtain a uniform and clear mixed solution; Step 2: Add a series of additives to the above reactor, including 2% bio-based penetrant fatty acid methyl ester sulfonate, 3% surfactant dodecyl glucoside, and 10% porogen walnut shell particles, and stir for 5 minutes; Step 3: Scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free release paper, immerse the above release paper in a 20% DMF aqueous solution coagulation bath for 2 minutes, and induce non-solvent phase separation to form a polyurethane microporous membrane; Step 4: Wash the microporous membrane with water at room temperature for 30 minutes to remove the residual solvent; Step 5: Bake the washed polyurethane microporous membrane at 80°C for 10 minutes to remove moisture, and finally roll up the dried polyurethane microporous membrane. Example 2
[0043] A phase separation pore forming method for a bio-based polyurethane waterproof and breathable membrane, the specific steps are as follows: Step 1: Add ethanol and acetone in a mixing ratio of 1.5:2 into a reactor and stir, then add a bio-based polyurethane resin solution, where the bio-based resin accounts for 50% of the total content of the solution, and stir for 40 minutes to obtain a uniform and clear mixed solution; Step 2: Add a series of additives to the above reactor, including 1% of bio-based penetrant alkyl betaine, 3% of bio-based surfactant dodecyl glucoside, and 10% of bio-based porogen walnut shell particles, and stir for 10 minutes; Step 3: Scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free release paper, immerse the above release paper in a 17% DMF coagulation bath for 5 minutes, and induce non-solvent phase separation to form a polyurethane microporous membrane; Step 4: Wash the microporous membrane with water at room temperature for 40 minutes to remove the residual solvent; Step 5: Bake the washed polyurethane microporous membrane at 120° C. for 20 minutes to remove moisture, and finally roll up the dried polyurethane microporous membrane. Example 3
[0044] A phase separation pore forming method for a bio-based polyurethane waterproof and breathable membrane, the specific steps are as follows: Step 1: Add ethanol and acetone in a mixing ratio of 1.2:3 into a reactor and stir, then add a bio-based polyurethane resin solution, where the bio-based resin accounts for 45% of the total content of the solution, and stir for 30 minutes to obtain a uniform and clear mixed solution; Step 2: Add a series of additives into the above reactor, including 1% bio-based penetrant fatty acid methyl ester sulfonate, 1% bio-based surfactant sarcosine lipopeptide, and 3% bio-based porogen walnut shell particles, and stir evenly; Step 3: Scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free release paper, immerse the above release paper in a 22% DMF coagulation bath for 3 minutes, and induce non-solvent phase separation to form a polyurethane microporous membrane; Step 4: Wash the microporous membrane with water at 40°C for 20 minutes to remove the residual solvent; Step 5: Bake the washed polyurethane microporous membrane at 100° C. for 15 minutes to remove moisture, and finally roll up the dried polyurethane microporous membrane. Example 4
[0045] A phase separation pore forming method for a bio-based polyurethane waterproof and breathable membrane, the specific steps are as follows: Step 1: Add ethanol and acetone in a mixing ratio of 1:2 into a reactor and stir, then add a bio-based polyurethane resin solution, where the bio-based resin accounts for 50% of the total content of the solution, and stir for 30 minutes to obtain a uniform and clear mixed solution; Step 2: Add a series of additives into the above reactor, including 0.5% of bio-based penetrant fatty acid methyl ester sulfonate, 1% of bio-based surfactant polyethyleneimine lipopolysaccharide, and 10% of bio-based porogen walnut shell particles, and stir evenly; Step 3: Scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free release paper, immerse the above release paper in a coagulation bath of 18% DMF for 3 minutes, and induce phase formation by non-solvent, and phase separation forms a polyurethane microporous membrane; Step 4: Wash the microporous membrane with water at 40°C for 20 minutes to remove the residual solvent; Step 5: Bake the washed polyurethane microporous membrane at 100° C. for 10 minutes to remove moisture, and finally roll up the dried polyurethane microporous membrane. Example 5
[0046] A phase separation pore forming method for a bio-based polyurethane waterproof and breathable membrane, the specific steps are as follows: Step 1: Add ethanol and acetone in a mixing ratio of 1.1:3 into a reactor and stir, then add the bio-based polyurethane solution, with the bio-based resin accounting for 50% of the total content of the solution, and stir for 40 minutes to obtain a uniform and clear mixed solution; Step 2: Add a series of additives into the above reactor, including 3% bio-based penetrant fatty acid methyl ester sulfonate, 3% bio-based surfactant polyethyleneimine lipopolysaccharide, and 12% bio-based porogen bamboo fiber particles, and stir evenly; Step 3: Scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free non-woven fabric, immerse the above non-woven fabric in a 25% DMF coagulation bath for 3 minutes, and induce phase formation by non-solvent, and phase separation to form a polyurethane microporous membrane; Step 4: Wash the microporous membrane with water at 40°C for 20 minutes to remove the residual solvent; Step 5: Bake the washed polyurethane microporous membrane at 100° C. for 10 minutes to remove moisture, and finally roll up the dried polyurethane microporous membrane. Example 6
[0047] A phase separation pore forming method for a bio-based polyurethane waterproof and breathable membrane, the specific steps are as follows: Step 1: Add ethanol and acetone in a mixing ratio of 1:3 into a reactor and stir, then add the bio-based polyurethane solution, with the bio-based resin accounting for 50% of the total content, and stir for 20 minutes to obtain a uniform and clear mixed solution; Step 2: Add a series of additives into the above reactor, including 2% of bio-based penetrant fatty acid methyl ester sulfonate, 3% of bio-based surfactant poly(ethyleneimine) lipopolysaccharide, and 10% of bio-based pore-forming agent hawthorn seed particles, and stir evenly; Step 3: Scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free spunbond fabric, immerse the spunbond fabric in a 20% DMF coagulation bath for 3 minutes, and induce non-solvent phase separation to form a polyurethane microporous membrane; Step 4: Wash the microporous membrane with water at 40°C for 20 minutes to remove the residual solvent; Step 5: Bake the washed polyurethane microporous membrane at 100° C. for 20 minutes to remove moisture, and finally roll up the dried polyurethane microporous membrane. Example 7
[0048] A phase separation pore forming method for a bio-based polyurethane waterproof and breathable membrane, the specific steps are as follows: Step 1: Add ethanol and acetone in a mixing ratio of 1:1.4 into a reactor and stir, then add the bio-based polyurethane solution, with the bio-based resin accounting for 50% of the total content of the solution, and stir for 30 minutes to obtain a uniform and clear mixed solution; Step 2: Add a series of additives into the above reactor, including 2% of bio-based penetrant fatty acid methyl ester sulfonate, 3% of bio-based surfactant polyethyleneimine lipopolysaccharide, and 6% of bio-based pore-forming agent apricot kernel shell particles, and stir evenly; Step 3: Scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free non-woven fabric, immerse the non-woven fabric in a coagulation bath of 18% DMF for 3 minutes, and induce phase formation by non-solvent, and phase separation to form a polyurethane microporous membrane; Step 4: Wash the microporous membrane with water at 40°C for 20 minutes to remove the residual solvent; Step 5: Bake the washed polyurethane microporous membrane at 120° C. for 10 minutes to remove moisture, and finally roll up the dried polyurethane microporous membrane. Example 8
[0049] A phase separation pore forming method for a bio-based polyurethane waterproof and breathable membrane, the specific steps are as follows: Step 1: Add ethanol and acetone with a mixing ratio of 1.3:2 into a 60°C reactor and stir, then add the bio-based polyurethane solution, with the bio-based accounting for 50% of the total content of the solution, and stir for 40 minutes to obtain a uniform and clear mixed solution; Step 2: Add a series of additives to the above reactor, including 1% bio-based penetrant fatty acid methyl ester sulfonate, 2% surfactant dodecyl glucoside, and 10% porogen walnut shell particles, and stir for 5 minutes; Step 3: Scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free spunbond fabric, immerse the spunbond fabric in a 17% DMF coagulation bath for 2 minutes, and induce non-solvent phase separation to form a polyurethane microporous membrane; Step 4: Wash the microporous membrane with water at room temperature for 30 minutes to remove the residual solvent; Step 5: Bake the washed polyurethane microporous membrane at 80°C for 20 minutes to remove moisture, and finally roll up the dried polyurethane microporous membrane. Example 9
[0050] A phase separation pore forming method for a bio-based polyurethane waterproof and breathable membrane, the specific steps are as follows: Step 1: Add ethanol and acetone in a mixing ratio of 1:1 into a 60°C reactor and stir, then add the bio-based polyurethane solution, with the bio-based accounting for 50% of the total content of the solution, and stir for 40 minutes to obtain a uniform and clear mixed solution; Step 2: Add a series of additives to the above reactor, including 2% bio-based penetrant fatty acid methyl ester sulfonate, 2% surfactant dodecyl glucoside, and 10% porogen walnut shell particles, and stir for 5 minutes; Step 3: Smear the mixed solution in the above reaction kettle on a flat, clean and water-free kraft paper, immerse the above kraft paper in a coagulation bath of 15% DMF for 2 minutes, and non-solvent induced phase formation occurs, and phase separation forms a polyurethane microporous membrane; Step 4: Wash the microporous membrane with water at room temperature for 30 minutes to remove the residual solvent; Step 5: Bake the washed polyurethane microporous membrane at 80° C. for 25 minutes to remove moisture, and finally roll up the dried polyurethane microporous membrane.
[0051] Comparative Example A method for phase separation and pore formation of a non-biobased polyurethane waterproof and breathable membrane, the specific steps are as follows: Step 1: Add DMF into the reactor and stir, then add the bio-based polyurethane solution, with the bio-based accounting for 50% of the total content of the solution, stir for 30 minutes to obtain a uniform and clear mixed solution; Step 2: Add a series of additives, including 2% surfactant sorbitan fatty acid ester (S80) and 10% porogen CaCO3, into the above reactor and stir evenly; Step 3: Scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free release paper, immerse the above release paper in a 22% DMF coagulation bath for 3 minutes, and induce non-solvent phase separation to form a polyurethane microporous membrane; Step 4: Wash the microporous membrane with water at 40°C for 20 minutes to remove the residual solvent; Step 5: Bake the washed polyurethane microporous membrane at 100° C. for 10 minutes to remove moisture, and finally roll up the dried polyurethane microporous membrane.
[0052] The following table shows the performance characterization results of Examples 1-9 and Comparative Examples Performance Indicator Implementation Case Thickness (μm) Porosity (%) Hydrostatic pressure (KPa) <![CDATA[Water vapor permeability (g / (m 2 *24 h))]]> Example 1 41.3 62.7 112 9041 Example 2 40.7 64.1 113 9148 Example 3 51.2 65.4 93 7534 Example 4 50.8 64.3 91 7661 Example 5 40.5 63.4 110 8867 Example 6 39.7 65.1 109 8453 Example 7 41.2 62.9 108 8913 Example 8 40.3 58.7 121 6131 Example 9 38.9 60.3 119 5003 Comparative Example 38.7 60.1 61 5029 It can be seen from the table that, compared with the comparative example, the performance of the film obtained by the method provided by the present invention is more excellent.
[0053] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing a bio-based polyurethane waterproof and breathable membrane, characterized in that: The following steps are involved: Add bio-based polyurethane resin to bio-based organic solvent, stir until the polyurethane resin is evenly mixed, then add other additives, continue to stir evenly to obtain a mixed solution; pour the mixed solution onto a substrate, use a scraping tool to scrape it into a thin film, then immerse it in a coagulation bath, and after solidification, wash with water and dry it to obtain a bio-based polyurethane waterproof and breathable membrane.
2. The method for preparing the bio-based polyurethane waterproof and breathable membrane according to claim 1, characterized in that: The components, by weight, include: 40-55 parts of bio-based polyurethane resin; 30-55 parts of bio-based organic solvent; 0.5~3 parts of bio-based penetrant; 2~3 parts of bio-based surfactant; 3~12 parts of porogen.
3. The method for preparing the bio-based polyurethane waterproof and breathable membrane according to claim 1, characterized in that: The bio-based polyurethane resin solution is selected from polyether-type aliphatic polyurethanes having a biomass content greater than or equal to 50%, and is selected from bio-based polyurethanes containing isosorbide polyether, wherein the isosorbide polyether accounts for 10% of the total volume of the bio-based polyurethane liquid.
4. The method for preparing the bio-based polyurethane waterproof and breathable membrane according to claim 2, characterized in that: The bio-based permeabilizer includes fatty acid methyl ester sulfonate or alkyl betaine; the bio-based surfactant includes one or more of sarcosine lipopeptide, dodecyl glucoside, polyethyleneimine lipopolysaccharide or dodecyl polyethoxy alcoholamine; the porogen includes one or more of walnut shell particles, bamboo fiber particles, hawthorn seed particles or koizsa apricot kernel shell particles.
5. The method for preparing the bio-based polyurethane waterproof and breathable membrane according to claim 1, characterized in that: The substrate is selected from one of non-woven fabric, spunbond fabric, release paper, kraft paper, wood pulp fabric and cotton fabric.
6. The method for preparing the bio-based polyurethane waterproof and breathable membrane according to claim 1, characterized in that: The coagulation bath is a mixed solution of water and N,N-dimethylformamide, and the volume ratio of water to N,N-dimethylformamide is (8-8.2):
2.
7. The method for preparing the bio-based polyurethane waterproof and breathable membrane according to claim 6, characterized in that: The duration of the coagulation bath is 2 min to 5 min.
8. The method for preparing the bio-based polyurethane waterproof and breathable membrane according to claim 6, characterized in that: The water washing temperature is 25-40°C, and the water washing time is 20min~40min.
9. The method for preparing a bio-based polyurethane waterproof and breathable membrane according to claim 1, characterized in that: The drying temperature is 80-120° C., and the drying time is 10-20 minutes.
10. A bio-based polyurethane waterproof and breathable membrane, characterized in that: The preparation is obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Electrostatic spinning / moisture-curing preparation method of fiber-based waterproof and moisture permeable film
CN106012303A
Preparation method of waterproof moisture-permeable composite cloth
CN114211848A
Compositions of eco-friendly nonswelling water-proof film, Nonswelling water-proof film having the same, and Manufacturing method thereof
KR101437399B1
Biological substance-based polyurethane formulation and waterproof moisture-permeable polyurethane film formed thereby
TW201329126A
Cited By
Preparation method of high-temperature-resistant and high-wear-resistant waterproof moisture-permeable film
CN120662154A
Preparation method of waterproof and moisture-permeable film with high temperature resistance and high wear resistance
CN120662154B