Artificial leather treating agent, artificial leather preparation method and artificial leather
By using specific composition treatment agents and preparation methods in automotive artificial leather, a high weather resistance and light resistance automotive leather is formed, and the problems of multi-color artificial leather in the prior art in weather resistance and color stability are solved, and the problem of multi-color artificial leather in the prior art is realized. The effect of meeting strict automotive standards.
Patent Information
- Application Number
- CN202411261471.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-12-06
AI Technical Summary
The existing automotive artificial leather is difficult to meet the performance requirements of weather resistance, stain resistance and detergent resistance in multi-color design, and the color is prone to discoloration or disappearing under long-term sunlight, and the detergent dissolves and destroys the pattern.
Using an artificial leather treatment agent, including a top layer and a bottom layer treatment agent, the top layer treatment agent consists of an aqueous polyurethane dispersion, an aqueous polyacrylate dispersion, a crosslinking agent, a leveling agent, a defoaming agent, a thickening agent and a light stabilizer, The dense layer and pattern layer are formed through steps such as vacuum defoaming, coating and high-temperature decapsulation, thereby enhancing the interfacial adhesion and weather resistance of the material.
It improves the binding and weather resistance of artificial leather, avoids color fading under light conditions, enhances resistance to chemical and physical stimulation, and meets the strict standards of automotive leather.
Smart Images

Figure CN119083196A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of standard artificial leather for vehicles, in particular to an artificial leather treating agent, an artificial leather preparation method and artificial leather. Background Art
[0002] In recent years, with the improvement of people's living standards, the requirements for car interiors have become higher and higher, and the design style of car interiors has changed greatly, becoming more and more rich and novel. Many models targeting young people have also broken through the traditional use of colors and become very rich.
[0003] Conventional automotive leather has a single color. If you want to achieve a colorful design effect, you have to use the splicing method, which greatly increases the cost and has poor quality.
[0004] Although other leather-making industries such as home furnishing, advertising, and luggage leather have used multi-color printers to produce multi-color leather, they cannot meet the stringent testing standards for automotive leather. Their weather resistance, stain resistance, detergent and ethanol resistance, etc. cannot meet the performance requirements of automotive leather.
[0005] During use, these multi-color leathers that do not meet the standards for automotive leather will have their patterns worn out, and their colors will change color or even disappear under long-term sunlight exposure. They are easily contaminated during use and difficult to clean. The existence of the pattern layer makes it possible for detergents or solvents such as anhydrous ethanol to dissolve and destroy the pattern when using detergents.
[0006] Therefore, there is still a need for an artificial leather treating agent, an artificial leather preparation method and an artificial leather to solve the above problems. Summary of the invention
[0007] The invention provides an artificial leather treating agent, an artificial leather preparation method and artificial leather for solving the above problems.
[0008] The purpose of the present invention is achieved by the following technical solutions:
[0009] An artificial leather treating agent, comprising: a top treating agent, wherein the top treating agent comprises, by weight:
[0010] 80-90 parts by weight of aqueous polyurethane dispersion, 5-20 parts by weight of aqueous polyacrylate dispersion, 2-5 parts by weight of high molecular weight polydimethylsiloxane, crosslinking agent, 0.3-2 parts by weight of leveling agent, 0.1-1 parts by weight of defoaming agent, 0.1-2 parts by weight of thickener, 0.5-2 parts by weight of light stabilizer;
[0011] The cross-linking agent comprises 1-4 parts by weight of a first cross-linking agent and 1-4 parts by weight of a blocked isocyanate cross-linking agent that is deblocked at high temperature.
[0012] In one embodiment, a bottom layer treatment agent is further included, which includes, by weight: 90-95 parts by weight of an aqueous polyurethane dispersion, 2-8 parts by weight of a cross-linking agent, 0.3-2 parts by weight of a leveling agent, 0.1-1 parts by weight of a defoaming agent, and 0.1-2 parts by weight of a thickener.
[0013] In one embodiment, the aqueous polyurethane dispersion is composed of one or more of polyether or polyester in aliphatic polyurethane or aromatic polyurethane, and the solid content is 30-50%;
[0014] The solid content of the aqueous polyacrylate dispersion is 30-50%.
[0015] In one embodiment, the high molecular weight polydimethylsiloxane is a mixture of water-based silicone oil and high molecular weight polydimethylsiloxane, with a solid content of 70-90% and a viscosity of about 450,000 cps.
[0016] In one embodiment, the leveling agent is one or more of polydimethylsilane, polymethylphenylsiloxane, polydimethylsiloxane, polyether polyester modified organic siloxane, and alkyl modified organic siloxane.
[0017] In one embodiment, the first cross-linking agent is an aziridine or an unblocked isocyanate cross-linking agent;
[0018] The deblocking temperature of the high temperature deblocking cross-linking agent is above 130°C;
[0019] The thickener is one or more of methyl cellulose, hydroxypropyl methyl cellulose, sodium carboxymethyl cellulose and hydroxyethyl cellulose.
[0020] A method for preparing artificial leather, using any one of the artificial leather treating agents described above, comprising the following steps:
[0021] The raw materials of the dense layer are mixed into a paste according to a certain proportion, and after degassing using a vacuum degassing machine, the paste is coated on a release paper and dried and solidified to form a primary dense layer;
[0022] The primary dense layer is coated and foamed, dried and solidified to form a dense layer, and a glue layer is coated on the dense layer and then bonded to the base fabric, and then dried and solidified to form a prefabricated layer;
[0023] The prefabricated layer is fed into the printer so that the ink is coated on the surface of the dense layer and dried to form a pattern;
[0024] Coating the stirred bottom treatment agent on the pattern side of the prefabricated layer and drying it to form a bottom layer;
[0025] The stirred top layer treatment agent is coated on the bottom layer and dried to form a top layer, which is then unsealed in sections at high temperature.
[0026] An artificial leather with automotive leather standard is formed by adopting the artificial leather preparation method.
[0027] Compared with the prior art, the beneficial effects of the present invention include at least:
[0028] The aqueous polyurethane dispersion and aqueous polyacrylate dispersion in the top treatment agent can enhance the formation of a strong cross-linked network on the surface of the dense layer, thereby improving the binding force. The polar groups in the aqueous dispersion can form hydrogen bonds or van der Waals forces with the functional groups in the dense layer. The aqueous polyacrylate dispersion can enhance the interfacial effect between the materials when combined with other polymers. Through chemical or physical interactions, it can increase the interfacial adhesion between the top treatment agent and the dense layer. The top layer formed by the top treatment agent enhances the protection of the color, prevents the color from fading and fading under light conditions, and improves the weather resistance of the leather. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 is a schematic diagram of the cross-sectional structure of artificial leather according to Example 1 of the present invention;
[0030] Figure 2 Schematic diagram of the steps of the method for preparing artificial leather according to Example 1 of the present invention;
[0031] Figure 3 is a diagram showing the results of the Taber wear test of Example 1 of the present invention;
[0032] Figure 4 1 is a Taber wear test result diagram of Comparative Example 1 of the present invention;
[0033] Figure 5 1 is a diagram showing the Taber wear test results of Comparative Example 2 of the present invention;
[0034] Figure 6 This is a graph showing the test results of anhydrous ethanol resistance of Example 1 of the present invention;
[0035] Figure 7 This is a test result diagram of anhydrous ethanol resistance of Comparative Example 1 of the present invention;
[0036] Figure 8 This is a graph showing the test results of anhydrous ethanol resistance of Comparative Example 2 of the present invention;
[0037] Fig. 9 This is a graph showing the light aging test results of a solid color block according to Example 1 of the present invention;
[0038] Fig.10 This is a graph showing the light aging test results of a pure color block of Comparative Example 1 of the present invention;
[0039] Fig.11 This is a graph showing the light aging test results of a pure color block of Comparative Example 2 of the present invention;
[0040] In the figure: 1, top layer; 2, bottom layer; 3, pattern layer; 4, dense layer; 5, base fabric layer. DETAILED DESCRIPTION
[0041] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the embodiments set forth herein; rather, these embodiments are provided to make the present invention more comprehensive and complete and to fully convey the concepts of example embodiments to those skilled in the art. The same reference numerals in the figures represent the same or similar structures, and thus their repeated description will be omitted.
[0042] The words expressing positions and directions described in the present invention are all explained with reference to the accompanying drawings as examples, but they can be changed as needed, and all such changes are included in the protection scope of the present invention.
[0043] An artificial leather treating agent, comprising: a top treating agent, wherein the top treating agent comprises, by weight:
[0044] 80-90 parts by weight of waterborne polyurethane dispersion, wherein the waterborne polyurethane dispersion is selected from: Starr Fine Coating WF-3800. 5-20 parts by weight of waterborne polyacrylate dispersion, selected from: Dow Chemical, CR-17B. 2-5 parts by weight of high molecular weight polydimethylsiloxane, wherein the high molecular weight polydimethylsiloxane is selected from: Dow Corning emulsion, MEM-1352. Crosslinking agent, leveling agent 0.3-2 parts by weight, wherein the leveling agent is selected from: BYK Chemical, BYK-349. 0.1-1 parts by weight of defoamer, 0.1-2 parts by weight of thickener, 0.5-2 parts by weight of light stabilizer. The defoamer is selected from: BYK Chemical, BYK-024, the thickener is selected from: BYK Chemical, BYK-425; the light stabilizer is selected from: Lianlong New Materials, B7750W.
[0045] The crosslinking agent includes 1-4 parts by weight of a first crosslinking agent and 1-4 parts by weight of a blocked isocyanate crosslinking agent that is unblocked at high temperature. The aqueous polyurethane dispersion in the top layer treatment agent can enhance the bonding strength with the bottom structure, and the polar groups in the aqueous dispersion can form hydrogen bonds or van der Waals forces with the functional groups in the dense layer. The aqueous polyacrylate dispersion can enhance the interface between materials when combined with other polymers. It can enhance the protective effect on the leather color and improve the weather resistance of the leather.
[0046] In addition, during the formation, the heating temperature is divided into two stages. In the first stage, the first crosslinker in the crosslinker first takes effect in an oven at 120°C, causing the resin and crosslinker in the top treatment agent to begin crosslinking to form a stable chemical bond, thereby curing into a film. Then in the second stage, taking effect in an oven at 150°C, the blocked isocyanate groups in the high-temperature deblocking crosslinker are deblocked at high temperatures to release active isocyanate groups, which can react with other molecules such as hydroxyl or amino groups to form a crosslinked structure. The deblocked isocyanate groups undergo crosslinking reactions with other molecules in the coating to form a stable three-dimensional network structure, which helps to improve the hardness, chemical resistance, heat resistance and wear resistance of the coating.
[0047] In one embodiment, the artificial leather treatment agent further comprises a bottom layer treatment agent, which comprises, by weight, 90-95 parts by weight of an aqueous polyurethane dispersion, 2-8 parts by weight of a crosslinking agent, 0.3-2 parts by weight of a leveling agent, 0.1-1 parts by weight of a defoaming agent, and 0.1-2 parts by weight of a thickener. The bottom layer treatment agent is coated between the top of the pattern layer and the top layer treatment agent, and serves to increase the bonding force between the top layer and the pattern layer and the dense layer, and to enhance the adhesion after being connected with other structures, thereby enhancing the firmness of the leather formed.
[0048] The components of the bottom treatment agent are selected from the following manufacturers and models:
[0049]
[0050]
[0051] In one embodiment, the aqueous polyurethane dispersion is composed of one or more of polyether or polyester in aliphatic polyurethane or aromatic polyurethane, and has a solid content of 30-50%.
[0052] The solid content of the aqueous polyacrylate dispersion is 30-50%.
[0053] In one embodiment, the high molecular weight polydimethylsiloxane is a mixture of water-based silicone oil and high molecular weight polydimethylsiloxane, with a solid content of 70-90% and a viscosity of about 450,000 cps.
[0054] In one embodiment, the leveling agent is one or more of polydimethylsilane, polymethylphenylsiloxane, polydimethylsiloxane, polyether polyester modified organic siloxane, and alkyl modified organic siloxane. The leveling agent can promote the uniform spreading of the coating on the substrate and reduce the unevenness of the coating thickness.
[0055] In one embodiment, the first crosslinking agent is aziridine or an unblocked isocyanate crosslinking agent. Aziridine and isocyanate crosslinking agents can react with functional groups in the material to form stable chemical bonds, thereby constructing a three-dimensional network structure and enhancing the mechanical properties of the material.
[0056] The deblocking temperature of the high-temperature deblocking cross-linking agent is above 130°C; after the top treatment agent undergoes a drying reaction at 100-120°C in a conventional treatment agent processing process, it will undergo a secondary reaction at 140-150°C to deblock the high-temperature deblocking cross-linking agent, further react, and improve the performance of the top treatment agent layer. Improve the wet rubbing resistance, wear resistance, and high temperature resistance of the leather coating. The cross-linking agent forms a strong chemical bond with the molecules in the leather coating through chemical reaction, enhancing the stability and durability of the coating.
[0057] The thickener is one or more of methylcellulose, hydroxypropylmethylcellulose, sodium carboxymethylcellulose and hydroxyethylcellulose. The thickener helps to improve the suspension of solid particles in the liquid, prevent the particles from settling, and make the product more uniform.
[0058] The present invention also discloses a method for preparing artificial leather, using any one of the artificial leather treating agents described above, comprising the following steps:
[0059] The raw materials of the dense layer are mixed into a paste according to the proportion, and after degassing using a vacuum degassing machine, they are coated on release paper and dried and solidified to form a primary dense layer. The solvent is dried to remove the solvent, so that the dense layer solvent is completely solidified.
[0060] The primary dense layer is coated and foamed, dried and solidified to form a dense layer, and a glue layer is coated on the dense layer and then bonded to the base cloth, and then dried and solidified to form a prefabricated layer.
[0061] The prefabricated layer is fed into the printer so that the ink is coated onto the surface of the dense layer and dried to form a pattern.
[0062] The stirred bottom treatment agent is coated on the pattern side of the prefabricated layer and dried to form a bottom layer.
[0063] The stirred top layer treatment agent is coated on the bottom layer and dried to form a top layer, which is then unsealed in sections at high temperature.
[0064] The high-temperature segmented unblocking is divided into two stages. After coating the top treatment agent on the bottom layer, the coated product is first placed in a 120°C oven to take effect, so that the resin and cross-linking agent in the top treatment agent begin to cross-link and form a stable chemical bond, thereby curing into a film. Then in the second stage, in a 150°C oven, the blocked isocyanate groups in the high-temperature unblocking cross-linking agent are unblocked at high temperature, releasing active isocyanate groups, forming a cross-linking structure, and a stable three-dimensional network structure, which improves the hardness, chemical resistance, heat resistance and wear resistance of the coating.
[0065] The invention also discloses an artificial leather of automotive leather standard, which is formed by the above method. The artificial leather formed by the above method has good wear resistance and strong bonding force after experimental inspection, avoids color fading and fading under light conditions, and improves the weather resistance of the leather.
[0066] Embodiment 1:
[0067] Prepare interior leather semi-finished products according to the dense layer formula in Table 1-1
[0068]
[0069] After the dense layer raw materials are mixed evenly into coating using a high-speed mixer, the bubbles are removed using a vacuum degasser; the coating is then applied on the release paper and then put into the first oven for drying and curing; the foaming layer coating is then applied and then put into the second oven for drying and curing; the glue layer coating is then applied and the base cloth is attached and then put into the third oven with a higher temperature to cure the glue and allow the foaming agent of the foaming layer to take effect and foam; the semi-finished product is then peeled off the release paper and rolled up for the next process. The temperature of the first oven is 160-180℃, the temperature of the second oven is 160-180℃, and the temperature of the third oven is 200-220℃.
[0070] The semi-finished product is sent to a multi-color printer, a color pattern is printed on the dense layer, and the multi-color semi-finished product is obtained after the pattern is dried by infrared heating.
[0071] According to the bottom treatment agent formula in Table 1-2 and the top treatment agent formula in Table 1-3, artificial leather with patterns meeting the automotive leather standards was prepared. The units are parts by weight.
[0072] After the ingredients in the treatment agent formula are configured in proportion, a mechanical stirrer is used at a speed of 1000-1500 rpm for 40-60 minutes to obtain a surface treatment agent. The bottom treatment agent is first printed on the surface of the multi-color semi-finished product by gravure printing, and then dried at 120°C; then the top treatment agent is printed and dried at 120°C; then heated at 150°C to activate the high-temperature unblocked end-blocking cross-linking agent; finally, high-temperature embossing is performed to obtain an artificial leather with a pattern that meets the automotive leather standards.
[0073]
[0074]
[0075] Comparative Example 1:
[0076] 1. Using the same method as above, prepare a semi-finished product according to the dense layer formula in Table 2-1.
[0077]
[0078]
[0079] 2. Produce multi-color patterns to obtain multi-color semi-finished products.
[0080] 3. Prepare automotive leather with color patterns according to the treatment agent formula in Table 2-2
[0081]
[0082] Comparative Example 2: It is a generally commercially available artificial leather with multi-color patterns.
[0083] Performance Testing:
[0084] 1. Taber wear resistance test
[0085] The products in the above embodiments and comparative examples were cut into the same size and placed on a Taber abrasion tester for testing. The samples were graded, with the highest grade being 5 and the standard passing requirement being 4.
[0086] 2. Bending resistance test
[0087] The products in the above-mentioned embodiments and comparative examples were cut into the same size and placed on a folding endurance tester for testing. The samples were graded, with the highest grade being 5 and the standard passing requirement being 4.
[0088] 3. Heat resistance and tensile resistance test
[0089] The products in the above-mentioned embodiment and comparative example were cut into the same size, stretched by 160% and fixed in size, and placed in an oven at 100° C. for 24 hours. The samples were rated to observe whether the patterns were broken or cracked.
[0090] 4. Light aging performance test
[0091] The products in the above examples and comparative examples were cut into the same size and placed in a xenon lamp aging box for testing. The appearance of the samples and the color change of the patterns were rated, with the highest rating being 5 and the standard passing requirement being 4.
[0092] 5. Anhydrous ethanol resistance performance test
[0093] The products in the above examples and comparative examples were cut into the same size, placed on a rubbing color fastness tester, and tested using a standard cotton cloth soaked in anhydrous ethanol. The appearance of the samples and the color change of the patterns were rated, with the highest being 5 and the standard passing requirement being 4.
[0094] The test results are as follows:
[0095] Test items Wear-resistant Bending resistance Heat-resistant stretch light aging resistance Resistant to anhydrous ethanol Example 4.5 5 5 4 4.5 Comparative Example 1 3.5 5 5 3 3 Comparative Example 2 2 3 3 1 2
[0096] Experimental tests have shown that the leather prepared by the method of the present application has strong weather resistance, is not easy to fall off, and the pattern and color are not easy to fade or disappear with the extension of use time.
[0097] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, substitute and modify the above embodiments within the scope of the invention without departing from the principles and purpose of the present invention. All such changes should fall within the scope of protection of the claims of the present invention.
Claims
1. An artificial leather treating agent, characterized in that include: The top treatment agent comprises, by weight: 80-90 parts by weight of aqueous polyurethane dispersion, 5-20 parts by weight of aqueous polyacrylate dispersion, 2-5 parts by weight of high molecular weight polydimethylsiloxane, crosslinking agent, 0.3-2 parts by weight of leveling agent, 0.1-1 parts by weight of defoaming agent, 0.1-2 parts by weight of thickener, 0.5-2 parts by weight of light stabilizer; The cross-linking agent comprises 1-4 parts by weight of a first cross-linking agent and 1-4 parts by weight of a blocked isocyanate cross-linking agent that is deblocked at high temperature.
2. The artificial leather treating agent according to claim 1, characterized in that It also includes a bottom layer treatment agent, which includes, by weight: 90-95 parts by weight of an aqueous polyurethane dispersion, 2-8 parts by weight of a crosslinking agent, 0.3-2 parts by weight of a leveling agent, 0.1-1 parts by weight of a defoaming agent, and 0.1-2 parts by weight of a thickener.
3. The artificial leather treating agent according to claim 2, characterized in that The aqueous polyurethane dispersion is composed of one or more polyethers or polyesters in aliphatic polyurethane or aromatic polyurethane, and has a solid content of 30-50%; The solid content of the aqueous polyacrylate dispersion is 30-50%.
4. The artificial leather treating agent according to claim 1, characterized in that The high molecular weight polydimethylsiloxane is a mixture of water-based organic silicone oil and high molecular weight polydimethylsiloxane, with a solid content of 70-90% and a viscosity of about 450,000 cps.
5. The artificial leather treating agent according to claim 4, characterized in that The leveling agent is one or more of polydimethylsilane, polymethylphenylsiloxane, polydimethylsiloxane, polyether polyester modified organic siloxane, and alkyl modified organic siloxane.
6. The artificial leather treating agent according to claim 1, characterized in that The first cross-linking agent is aziridine or an unblocked isocyanate cross-linking agent; The deblocking temperature of the high temperature deblocking cross-linking agent is above 130°C; The thickener is one or more of methyl cellulose, hydroxypropyl methyl cellulose, sodium carboxymethyl cellulose and hydroxyethyl cellulose.
7. A method for preparing artificial leather, characterized in that: Using the artificial leather treating agent as described in any one of claims 1 to 6 comprises the following steps: The raw materials of the dense layer are mixed into a paste according to a certain proportion, and after degassing using a vacuum degassing machine, the paste is coated on a release paper and dried and solidified to form a primary dense layer; The primary dense layer is coated and foamed, dried and solidified to form a dense layer, and a glue layer is coated on the dense layer and then bonded to the base fabric, and then dried and solidified to form a prefabricated layer; The prefabricated layer is fed into the printer so that the ink is coated on the surface of the dense layer and dried to form a pattern; Coating the stirred bottom treatment agent on the pattern side of the prefabricated layer and drying it to form a bottom layer; The stirred top layer treatment agent is coated on the bottom layer and dried to form a top layer, which is then unsealed in sections at high temperature.