Famiable forming method of milling groove type thrust chamber

Through laser printing and thermal isostatic pressure processing combined with ultrasonic rolling technology, the complexity of indoor and outdoor wall forming of rocket engine thrust is solved, the density and performance improvement of copper alloys are achieved, the process flow is simplified and the delivery cycle is shortened.

CN119084186APending Publication Date: 2024-12-06SHAANXI SIRUI ADVANCED MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411117573.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The interlayer regeneration cooling forming method of the thrust chamber of the existing rocket engine is complex and has a high process difficulty. The additive manufacturing technology is not yet mature, so it is impossible to achieve simultaneous forming with zero defects in the inner and outer walls.

Method used

Laser printing is used to prepare the inner wall structural parts of the copper alloy thrust chamber, and the coordinated thermal isostatic pressure treatment of the copper alloy interlayer and the stainless steel cover, combined with ultrasonic rolling technology, the inner and outer walls are densified and connected.

Benefits of technology

The process flow is simplified, the overall performance strength and yield of the thrust chamber are improved, the product delivery cycle is shortened, and the density and oxygen content control of copper alloys are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119084186A_ABST
    Figure CN119084186A_ABST
Patent Text Reader

Abstract

The invention discloses a feasible forming method of a milling groove type thrust chamber. The feasible forming method comprises the following steps that S1, a thrust chamber inner wall structural part is printed; s2, assembling a copper alloy interlayer; s3, assembling the mold; s4, assembling a stainless steel sheath; s4, hot isostatic pressing treatment; and S5, post-processing. According to the method, the forming mode that hot isostatic pressing is conducted on the inner wall of the thrust chamber through laser printing and the stainless steel sheath is adopted, densification of the copper alloy can be achieved, it can be guaranteed that the oxygen content is not increased in the machining process, the synergism between addition of the copper alloy interlayer and the inner wall of the thrust chamber and the stainless steel sheath is high, near-net forming can be directly conducted, and the machining efficiency is improved. A new thought is developed, outer wall forming and inner and outer wall diffusion connection can be achieved at the same time in cooperation with cold spraying and hot isostatic pressing treatment, and the method has the advantages that the process is simple, connection reliability is high, and the product delivery period is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rocket engine manufacturing, and in particular to a feasible molding method for a milling groove type thrust chamber. Background Art

[0002] The thrust chamber is an important part of the rocket engine. It accelerates the expansion of the propellant combustion products by changing the geometric shape of the inner wall of the tube section, so that the engine can obtain propulsion power. At the same time, the combustion of propellant will increase the gas temperature inside the thrust chamber. In the extremely harsh environment of up to 3500K, basically no material can withstand such a high temperature for a long time. Therefore, most thrust chambers use interlayer regenerative cooling technology. The propellant flows through the grooves between the inner and outer walls of the thrust chamber to take away the heat transferred to the chamber wall by the combustion gas, ensuring the normal operation of the rocket launch process.

[0003] At present, the commonly used forming methods of sandwich regenerative cooling thrust chambers mainly include electroforming, vacuum pressure brazing and isostatic diffusion welding. Electroforming has low efficiency, high process difficulty and long manufacturing cycle; vacuum pressure brazing and isostatic diffusion welding processes both weld the outer wall and the inner wall by combining positive and negative pressure, which requires high dimensional accuracy of the inner and outer walls. The inner and outer walls need to be electroplated separately during the process, and a high vacuum state must be ensured in the sealed space between the inner and outer walls. Overall, the process is very complicated. At the same time, high temperature during welding can easily cause the copper alloy material of the inner wall to soften.

[0004] New technologies for connecting and forming inner and outer walls through additive manufacturing, such as laser cladding and cold spraying, can eliminate the tedious process of welding. The process is relatively simplified, but it is subject to other problems brought about by the development of current technology. Various additive manufacturing technologies in China, including laser printing technology, are not yet mature, and they all need to be hot isostatic pressing to improve common defects inside printed samples. There are defects on the inner wall and the outer wall. We want to achieve zero defects on the inner and outer walls at the same time through a hot isostatic pressing treatment. Many factors need to be considered, such as shrinkage deformation, interface bonding strength, etc., which are basically impossible to achieve with current technology. Summary of the invention

[0005] In view of the above-mentioned problems, the present invention provides a feasible forming method of a milling groove thrust chamber.

[0006] The technical solution of the present invention is:

[0007] A feasible forming method of a milling groove thrust chamber comprises the following steps:

[0008] S1. Printing of thrust chamber inner wall structural parts: A thrust chamber inner wall structural part with a hollow interior is prepared by laser printing. A plurality of grooves are arranged at equal intervals on the outer wall of the thrust chamber inner wall structural part. A convex rib is formed between two adjacent grooves. The convex rib gradually decreases in width when extending from the end of the thrust chamber inner wall structural part with a larger inner diameter to the end of the thrust chamber inner wall structural part with a smaller inner diameter. The inner and outer surfaces of the thrust chamber inner wall structural part are subjected to surface sandblasting, grinding, polishing and cleaning. The material of the thrust chamber inner wall is CuCr alloy, CuCrZr alloy or CuCrNb alloy;

[0009] S2. Copper alloy interlayer assembly: assemble the copper alloy interlayer on the outside of the thrust chamber inner wall structure, so that the copper alloy interlayer is closely fitted with the convex ribs of the outer wall of the thrust chamber inner wall structure, and the fit degree is ensured to be greater than 95%. The material of the copper alloy interlayer is CuCr alloy, CuCrZr alloy or CuCrNb alloy, and a pure nickel layer is sprayed on the outer wall surface of the copper alloy interlayer;

[0010] S3, mold assembly: assemble the inner middle part of the thrust chamber inner wall structure with the mold, and the outer wall of the mold is tightly fitted with the inner wall of the thrust chamber inner wall structure, ensuring that the fit degree is greater than 95%;

[0011] S4, stainless steel sheath assembly: a prefabricated stainless steel sheath is assembled outside the copper alloy interlayer, and an annular prefabricated manifold is welded to the upper and lower ends of the prefabricated stainless steel sheath respectively. The prefabricated manifold is also connected to the inner wall structure of the thrust chamber by welding. The two prefabricated manifolds are respectively connected to the two ends of each rib and the groove. A vacuum tube is provided on the prefabricated manifold at the end with the larger inner diameter of the inner wall structure of the thrust chamber. The prefabricated manifold and the groove are evacuated by the vacuum tube to ensure that the vacuum degree of the groove is within 1×10 -2 ~1×10 - 3 Pa, then weld and seal the vacuum tube;

[0012] S4, hot isostatic pressing treatment: placing the prefabricated stainless steel sheath in a hot isostatic pressing furnace for hot isostatic pressing treatment, the temperature of the hot isostatic pressing treatment is 800-1000° C., the pressure of the hot isostatic pressing treatment is 1-15 MPa, and the duration of the hot isostatic pressing treatment is 2-8 hours, and a thrust chamber assembly with a sheath is obtained after being taken out of the furnace;

[0013] S5, post-processing: removing the mold and the prefabricated manifolds at the upper and lower ends of the thrust chamber assembly with the sleeve, and then performing ultrasonic rolling treatment on the inner wall of the thrust chamber assembly to obtain a milled groove thrust chamber structural component.

[0014] Furthermore, in step S1, the specific steps of the laser printing are: passing the atomized powder of CuCr alloy, CuCrZr alloy or CuCrNb alloy through a 270-300 mesh sieve, importing the drawn 3D model diagram into the laser printer, filling the atomized powder, placing the base plate, installing the scraper, and then evacuating the laser selective melting equipment to a vacuum degree of 3-5 Pa, and then introducing argon as a protective gas, and spreading the atomized powder evenly to the laser processing area through the scraper, and printing layer by layer according to the set printing parameters, the atomized powder printing single layer thickness is 0.03-0.06 mm, the scanning interval is 0.05-0.2 mm, the printing power is 380-460 W, and the scanning speed is 400-1600 mm / s to obtain the thrust chamber inner wall structure.

[0015] Description: The copper alloy of the thrust chamber inner wall structural parts is printed by laser, which has high strength and fast preparation speed.

[0016] Furthermore, in the step S1, the roughness of the rib tops of the convex ribs of the outer wall of the thrust chamber inner wall structure is Ra≤3.2 μm.

[0017] Note: By keeping the roughness of the rib top within a reasonable range, the fit between the thrust chamber inner wall and the copper alloy interlayer can be ensured to meet the requirements.

[0018] Furthermore, in step S2, the copper alloy interlayer is provided as two mutually symmetrical half-shell structures, and during assembly, the two copper alloy interlayer half-shells are butt-fitted with the thrust chamber inner wall structure and then electron beam butt-welded.

[0019] Note: The electron beam butt welding method can also further improve the fit between the inner wall of the thrust chamber and the copper alloy interlayer.

[0020] Furthermore, in step S2, the thickness of the pure nickel layer is 1 to 20 mm, cold spraying is adopted during spraying, the spraying temperature is 350 to 600° C., the spraying gas is nitrogen, the pressure is 3 to 7 MPa, the powder feeding amount of the pure nickel powder used during spraying is 150 to 350 g / min, and the distance from the nozzle to the surface of the substrate is 20 to 40 mm.

[0021] Note: The overall strength of the thrust chamber structure is further improved by optimizing the spraying thickness of the pure nickel layer.

[0022] Furthermore, in step S3, the prefabricated stainless steel sheath is provided as two mutually symmetrical half-shell structures, and during assembly, the two prefabricated stainless steel sheaths are butt-jointed with the copper alloy interlayer and then electron beam butt-welded.

[0023] Note: The electron beam butt welding method can also further improve the fit between the copper alloy interlayer and the stainless steel sheath.

[0024] Furthermore, in step S3, the mold is made of stainless steel, and the outer wall of the mold is sprayed with solder stop, and the thickness of the solder stop spray is 1 to 2 mm.

[0025] Note: Spray anti-solder to prevent adhesion between the mold and the inner wall of the thrust chamber.

[0026] Furthermore, in step S5, when ultrasonic rolling is performed on the inner wall of the thrust chamber assembly, a heating wire is first wrapped around the outside of the thrust chamber assembly to heat the thrust chamber assembly to 220-240°C, and then an ultrasonic rolling head is used to extend along the extension direction of the convex rib from the end with a larger inner diameter of the thrust chamber inner wall structural part to the end with a smaller inner diameter of the thrust chamber inner wall structural part, with an ultrasonic rolling pressure of 650-750N, an ultrasonic frequency of 20-30kHz, an amplitude of 5-10μm, a cooling lubricant is coated on the ultrasonic rolling head, the ultrasonic rolling temperature is maintained at 60-80°C, and the feed speed is 0.05-0.1mm / rev.

[0027] Description: Ultrasonic rolling is performed on the inner wall of the thrust chamber assembly so that the inner wall of the thrust chamber assembly has a better surface morphology and lower surface roughness. By optimizing the direction of ultrasonic rolling, the surface microhardness of the inner wall of the thrust chamber assembly and the overall hardness of the thrust chamber assembly are further improved.

[0028] The beneficial effects of the present invention are:

[0029] (1) A feasible forming method of a milled groove thrust chamber of the present invention adopts a forming method of hot isostatic pressing by laser printing the inner wall of the thrust chamber and adding a stainless steel sheath, which can realize the densification of the copper alloy and ensure that the oxygen content does not increase during the processing. Among them, the addition of the copper alloy interlayer and the synergy between the inner wall of the thrust chamber and the stainless steel sheath are high, and near-net forming can be directly performed, which opens up a new idea. In combination with cold spraying and hot isostatic pressing treatment, the outer wall forming and the diffusion connection of the inner and outer walls can be realized simultaneously, which has the advantages of simple process, high connection reliability, and shortened product delivery cycle.

[0030] (2) A feasible forming method of a milled groove thrust chamber of the present invention further adds ultrasonic rolling treatment to the inner wall of the thrust chamber after hot isostatic pressing, thereby further improving the performance of the inner wall of the thrust chamber, especially optimizing the direction of the ultrasonic rolling so that it cooperates with the ribs provided on the inner wall of the thrust chamber, thereby improving the overall performance strength of the thrust chamber assembly. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic diagram of the inner wall structural part of the thrust chamber in a feasible forming method of a milling groove thrust chamber of the present invention;

[0032] Figure 2 It is a schematic diagram of a copper alloy sandwich structure in a feasible forming method of a milling groove thrust chamber of the present invention;

[0033] Figure 3 It is a schematic diagram of the structure after the stainless steel package is assembled in step S4 of a feasible forming method of a milling groove thrust chamber of the present invention;

[0034] Figure 4 It is a cross-sectional view of a milling groove thrust chamber structural part in a feasible forming method of a milling groove thrust chamber of the present invention.

[0035] Among them, 1-thrust chamber inner wall structural parts, 2-copper alloy interlayer, 3-pure nickel layer, 4-prefabricated stainless steel sheath, 5-vacuum tube, 6-prefabricated manifold. DETAILED DESCRIPTION

[0036] Example 1

[0037] A feasible forming method of a milling groove thrust chamber comprises the following steps:

[0038] S1. Printing of thrust chamber inner wall structure 1: A thrust chamber inner wall structure 1 with a hollow interior is prepared by laser printing. A plurality of grooves are arranged at equal intervals on the outer wall of the thrust chamber inner wall structure 1. A convex rib is formed between two adjacent grooves. The width of the convex rib gradually decreases as it extends from the end with a larger inner diameter of the thrust chamber inner wall structure 1 to the end with a smaller inner diameter. The inner and outer surfaces of the thrust chamber inner wall structure 1 are subjected to surface sandblasting, grinding, polishing and cleaning. The roughness Ra of the rib top of the outer wall of the thrust chamber inner wall structure 1 is 2.5 μm. The material of the thrust chamber inner wall is CuCrZr alloy.

[0039] The specific steps of laser printing are as follows: passing the atomized powder of CuCrZr alloy through a 280-mesh sieve, importing the drawn 3D model into the laser printer, filling the atomized powder, placing the base plate, installing the scraper, and then evacuating the laser selective melting equipment to a vacuum degree of 4 Pa, and then introducing argon as a protective gas, and evenly spreading the atomized powder to the laser processing area through the scraper, and printing layer by layer according to the set printing parameters, the atomized powder printing single layer thickness is 0.05 mm, the scanning interval is 0.07 mm, the printing power is 420 W, and the scanning speed is 1000 mm / s, and the thrust chamber inner wall structure 1 is obtained;

[0040] S2, copper alloy interlayer 2 assembly: copper alloy interlayer 2 is assembled on the outside of thrust chamber inner wall structure 1, so that copper alloy interlayer 2 and the convex rib of the outer wall of thrust chamber inner wall structure 1 are closely fitted, and the fitting degree is ensured to be 96%. The copper alloy interlayer 2 is arranged as two mutually symmetrical half-shell structures. When assembling, the two copper alloy interlayer 2 half shells are butt-fitted with thrust chamber inner wall structure 1, and then electron beam butt welding is performed. The material of copper alloy interlayer 2 is CuCrNb alloy. Pure nickel layer 3 is sprayed on the outer wall surface of copper alloy interlayer 2. The thickness of pure nickel layer 3 is 10mm. Cold spraying is adopted during spraying. The spraying temperature is 500°C. The spraying gas is nitrogen. The pressure is 4MPa. The powder feeding amount of pure nickel powder used during spraying is 200g / min. The distance from the nozzle to the substrate surface is 30mm.

[0041] S3, mold assembly: Assemble the inner middle part of the thrust chamber inner wall structure 1 with the mold. The mold is made of stainless steel. The outer wall of the mold is sprayed with solder stop. The spray thickness of the solder stop is 1.5 mm. The outer wall of the mold is tightly fitted with the inner wall of the thrust chamber inner wall structure 1 to ensure that the fit is 98%. The solder stop is commercially available C80-2 high-purity boron nitride powder.

[0042] S4, stainless steel sheath 4 assembly: prefabricated stainless steel sheath 4 is assembled outside the copper alloy interlayer 2. The prefabricated stainless steel sheath 4 is arranged as two mutually symmetrical half-shell structures. During assembly, the two prefabricated stainless steel sheaths 4 are butt-jointed with the copper alloy interlayer 2, and then electron beam butt welding is performed. Annular prefabricated manifolds 6 are respectively welded at the upper and lower ends of the prefabricated stainless steel sheath 4. The prefabricated manifold 6 is also connected to the thrust chamber inner wall structure 1 by welding. The two prefabricated manifolds 6 are respectively connected to the two ends of each rib and the groove. A vacuum tube 5 is provided on the prefabricated manifold 6 at the end with a larger inner diameter of the thrust chamber inner wall structure 1. The prefabricated manifold 6 and the inside of the groove are evacuated by the vacuum tube 5 to ensure that the vacuum degree of the groove is within 1×10 -2 Pa, then weld and seal the vacuum tube 5;

[0043] S4, hot isostatic pressing treatment: placing the prefabricated stainless steel sheath 4 in a hot isostatic pressing furnace for hot isostatic pressing treatment, the temperature of the hot isostatic pressing treatment is 900° C., the pressure of the hot isostatic pressing treatment is 3 MPa, and the duration of the hot isostatic pressing treatment is 6 hours, and after being taken out of the furnace, a thrust chamber assembly with a sheath is obtained;

[0044] S5, post-processing: removing the mold and the prefabricated manifolds 6 at the upper and lower ends of the thrust chamber assembly with the sleeve, and then performing ultrasonic rolling treatment on the inner wall of the thrust chamber assembly to obtain a milled groove thrust chamber structural component;

[0045] When ultrasonic rolling is performed on the inner wall of the thrust chamber assembly, the heating wire is first wrapped around the outside of the thrust chamber assembly to heat the thrust chamber assembly to 230°C, and then an ultrasonic rolling head is used to extend along the extension direction of the convex rib from the end with a larger inner diameter of the thrust chamber inner wall structural part 1 to the end with a smaller inner diameter of the thrust chamber inner wall structural part 1. The ultrasonic rolling pressure is 700N, the ultrasonic frequency is 25kHz, and the amplitude is 6μm. The ultrasonic rolling head is coated with a cooling lubricant, which is a commercially available FOSS water-soluble grinding fluid ECOCOOLGLOBAL 1000 10 aerospace cutting coolant. The ultrasonic rolling temperature is maintained at 75°C and the feed speed is 0.08mm / rev.

[0046] Example 2

[0047] The difference between this embodiment and embodiment 1 is that:

[0048] S1. Printing of thrust chamber inner wall structural part 1: The roughness Ra of the rib top of the outer wall of the thrust chamber inner wall structural part 1 is 2 μm, and the material of the thrust chamber inner wall is CuCr alloy;

[0049] The specific steps of laser printing are as follows: passing the atomized powder of CuCr alloy through a 270-mesh sieve, importing the drawn 3D model into the laser printer, filling the atomized powder, placing the base plate, installing the scraper, and then evacuating the laser selective melting equipment to a vacuum degree of 3Pa, and then introducing argon as a protective gas, and spreading the atomized powder evenly to the laser processing area through the scraper, and printing layer by layer according to the set printing parameters. The atomized powder printing single layer thickness is 0.03mm, the scanning interval is 0.05mm, the printing power is 380W, and the scanning speed is 400mm / s, and the thrust chamber inner wall structure 1 is obtained.

[0050] Example 3

[0051] The difference between this embodiment and embodiment 1 is that:

[0052] S1. Printing of thrust chamber inner wall structure 1: A thrust chamber inner wall structure 1 with a hollow interior is prepared by laser printing. A plurality of grooves are arranged at equal intervals on the outer wall of the thrust chamber inner wall structure 1. A convex rib is formed between two adjacent grooves. The width of the convex rib gradually decreases as it extends from the end with a larger inner diameter of the thrust chamber inner wall structure 1 to the end with a smaller inner diameter. The inner and outer surfaces of the thrust chamber inner wall structure 1 are subjected to surface sandblasting, grinding, polishing and cleaning. The roughness Ra of the rib top of the outer wall of the thrust chamber inner wall structure 1 is 3 μm. The material of the thrust chamber inner wall is CuCrNb alloy.

[0053] The specific steps of laser printing are as follows: passing the atomized powder of CuCrNb alloy through a 300-mesh sieve, importing the drawn 3D model into the laser printer, filling the atomized powder, placing the base plate, installing the scraper, and then evacuating the laser selective melting equipment to a vacuum degree of 5 Pa, and then introducing argon as a protective gas, and spreading the atomized powder evenly to the laser processing area through the scraper, and printing layer by layer according to the set printing parameters. The thickness of a single layer of atomized powder printing is 0.06 mm, the scanning interval is 0.2 mm, the printing power is 460 W, and the scanning speed is 1600 mm / s, and the thrust chamber inner wall structure 1 is obtained.

[0054] Example 4

[0055] The difference between this embodiment and embodiment 1 is that:

[0056] S2. Assembly of copper alloy interlayer 2: assemble copper alloy interlayer 2 on the outside of thrust chamber inner wall structure 1, so that copper alloy interlayer 2 and convex rib of outer wall of thrust chamber inner wall structure 1 are closely fitted, and the fitting degree is ensured to be 96%. Copper alloy interlayer 2 is arranged as two symmetrical half-shell structures. When assembling, two half shells of copper alloy interlayer 2 are butt-fitted with thrust chamber inner wall structure 1, and then electron beam butt welding is performed. The material of copper alloy interlayer 2 is CuCr alloy. Pure nickel layer 3 is sprayed on the outer wall surface of copper alloy interlayer 2. The thickness of pure nickel layer 3 is 1 mm. Cold spraying is adopted during spraying. The spraying temperature is 350°C. The spraying gas is nitrogen. The pressure is 3MPa. The powder feeding amount of pure nickel powder used during spraying is 150g / min. The distance from the nozzle to the substrate surface is 20mm.

[0057] S3, mold assembly: Assemble the inner middle part of the thrust chamber inner wall structure 1 with the mold. The mold is made of stainless steel. The outer wall of the mold is sprayed with solder stop. The thickness of the solder stop is 1mm. The outer wall of the mold is tightly fitted with the inner wall of the thrust chamber inner wall structure 1 to ensure that the fit is 98%;

[0058] Example 5

[0059] The difference between this embodiment and embodiment 1 is that:

[0060] S2. Assembly of copper alloy interlayer 2: assemble copper alloy interlayer 2 on the outside of thrust chamber inner wall structure 1, so that copper alloy interlayer 2 and convex rib of outer wall of thrust chamber inner wall structure 1 are closely fitted, and the fitting degree is ensured to be 97%. Copper alloy interlayer 2 is arranged as two mutually symmetrical half-shell structures. When assembling, two half shells of copper alloy interlayer 2 are butt-fitted with thrust chamber inner wall structure 1, and then electron beam butt welding is performed. The material of copper alloy interlayer 2 is CuCrZr alloy. Pure nickel layer 3 is sprayed on the outer wall surface of copper alloy interlayer 2. The thickness of pure nickel layer 3 is 20 mm. Cold spraying is adopted during spraying. The spraying temperature is 600°C. The spraying gas is nitrogen. The pressure is 7 MPa. The powder feeding amount of pure nickel powder used during spraying is 350 g / min. The distance from nozzle to substrate surface is 40 mm.

[0061] S3, mold assembly: Assemble the middle part of the thrust chamber inner wall structure 1 with the mold. The mold is made of stainless steel. The outer wall of the mold is sprayed with solder stop. The thickness of the solder stop is 2 mm. The outer wall of the mold is tightly fitted with the inner wall of the thrust chamber inner wall structure 1 to ensure that the fit is 99%;

[0062] Example 6

[0063] The difference between this embodiment and embodiment 1 is that:

[0064] S4, stainless steel jacket 4 assembly: the vacuum degree of the groove is 1×10 -2 Pa;

[0065] S4, hot isostatic pressing treatment: the prefabricated stainless steel sheath 4 is placed in a hot isostatic pressing furnace for hot isostatic pressing treatment. The temperature of the hot isostatic pressing treatment is 800°C, the pressure of the hot isostatic pressing treatment is 1 MPa, and the duration of the hot isostatic pressing treatment is 2 hours. After taking out of the furnace, a thrust chamber assembly with a sheath is obtained.

[0066] Example 6

[0067] The difference between this embodiment and embodiment 1 is that:

[0068] S4, stainless steel jacket 4 assembly: the vacuum degree of the groove is 1×10 -3 Pa;

[0069] S4, hot isostatic pressing treatment: the prefabricated stainless steel sheath 4 is placed in a hot isostatic pressing furnace for hot isostatic pressing treatment. The temperature of the hot isostatic pressing treatment is 1000°C, the pressure of the hot isostatic pressing treatment is 15 MPa, and the duration of the hot isostatic pressing treatment is 8 hours. After taking out of the furnace, a thrust chamber assembly with a sheath is obtained.

[0070] Example 7

[0071] The difference between this embodiment and embodiment 1 is that:

[0072] When ultrasonic rolling is performed on the inner wall of the thrust chamber assembly, the heating wire is first wrapped around the outside of the thrust chamber assembly to heat the thrust chamber assembly to 220°C, and then an ultrasonic rolling head is used to extend along the extension direction of the convex rib from the end of the thrust chamber inner wall structural part 1 with a larger inner diameter to the end of the thrust chamber inner wall structural part 1 with a smaller inner diameter. The ultrasonic rolling pressure is 650N, the ultrasonic frequency is 20kHz, the amplitude is 5μm, and a cooling lubricant is coated on the ultrasonic rolling head. The ultrasonic rolling temperature is maintained at 60°C and the feed speed is 0.05mm / rev.

[0073] Example 8

[0074] The difference between this embodiment and embodiment 1 is that:

[0075] When ultrasonic rolling is performed on the inner wall of the thrust chamber assembly, the heating wire is first wrapped around the outside of the thrust chamber assembly to heat the thrust chamber assembly to 240°C, and then an ultrasonic rolling head is used to extend along the extension direction of the convex rib from the end of the thrust chamber inner wall structural part 1 with a larger inner diameter to the end of the thrust chamber inner wall structural part 1 with a smaller inner diameter. The ultrasonic rolling pressure is 750N, the ultrasonic frequency is 30kHz, the amplitude is 10μm, and a cooling lubricant is coated on the ultrasonic rolling head. The ultrasonic rolling temperature is maintained at 80°C and the feed speed is 0.1mm / rev.

[0076] Experimental example

[0077] The performance of the milling groove thrust chamber structural component prepared by the feasibility molding method of a milling groove thrust chamber of the present invention is tested below. First, the performance parameters of various parts of the structural component after hot isostatic pressing are tested. The results of the multiple groups of structural components tested are shown in Table 1.

[0078] Table 1 Performance parameters of various parts of the structural parts after hot isostatic pressing

[0079]

[0080] It can be seen that the performance of each part of the milled groove thrust chamber structural component prepared by the method of the present invention is at an upper-middle level among the same type of structural components, and has a short production cycle, high reliability and high yield.

[0081] Then we tested the performance impact of ultrasonic rolling and compared them with structural parts without ultrasonic rolling. We found that the minimum surface roughness of the inner wall of the thrust chamber of the structural parts after ultrasonic rolling treatment can reach 0.15μm, and the maximum hardening depth is 320μm. Compared with the structural parts without ultrasonic rolling, the hardness of the inner wall of the thrust chamber is increased by 3-5%, and the hardness of the rib part is increased by 4-6%. Therefore, the special ultrasonic rolling method of the present invention is a good supplement to the hot isostatic pressing method of the present invention.

Claims

1. A feasible forming method of a milling groove thrust chamber, characterized in that: The following steps are involved: S1. Printing of thrust chamber inner wall structure (1): a thrust chamber inner wall structure (1) with a hollow interior is prepared by laser printing, a plurality of grooves are arranged at equal intervals on the outer wall of the thrust chamber inner wall structure (1), a convex rib is formed between two adjacent grooves, and the width of the convex rib gradually decreases when extending from the end of the thrust chamber inner wall structure (1) with a larger inner diameter to the end of the thrust chamber inner wall structure (1) with a smaller inner diameter. The inner and outer surfaces of the thrust chamber inner wall structure (1) are subjected to surface sandblasting, grinding, polishing and cleaning, and the material of the thrust chamber inner wall is CuCr alloy, CuCrZr alloy or CuCrNb alloy; S2, copper alloy interlayer (2) assembly: the copper alloy interlayer (2) is assembled on the outside of the thrust chamber inner wall structure (1), so that the copper alloy interlayer (2) is tightly fitted with the convex ribs of the outer wall of the thrust chamber inner wall structure (1), and the fit degree is ensured to be greater than 95%. The material of the copper alloy interlayer (2) is CuCr alloy, CuCrZr alloy or CuCrNb alloy, and a pure nickel layer (3) is sprayed on the outer wall surface of the copper alloy interlayer (2); S3, mold assembly: assemble the middle part of the thrust chamber inner wall structure (1) with the mold, and make the outer wall of the mold fit tightly with the inner wall of the thrust chamber inner wall structure (1), ensuring that the fit degree is greater than 95%; S4. Assembling the stainless steel sheath (4): Assemble the prefabricated stainless steel sheath (4) outside the copper alloy interlayer (2), weld annular prefabricated manifolds (6) at the upper and lower ends of the prefabricated stainless steel sheath (4), respectively, and connect the prefabricated manifold (6) and the thrust chamber inner wall structure (1) by welding. The two prefabricated manifolds (6) are respectively connected to the two ends of each rib and the groove. A vacuum tube (5) is provided on the prefabricated manifold (6) at the end with the larger inner diameter of the thrust chamber inner wall structure (1). The prefabricated manifold (6) and the inside of the groove are evacuated by the vacuum tube (5), and the vacuum degree of the groove is ensured to be within 1×10 -2 ~1×10 -3 Pa, and then weld and seal the vacuum tube (5); S4, hot isostatic pressing: placing the prefabricated stainless steel sheath (4) in a hot isostatic pressing furnace for hot isostatic pressing, wherein the temperature for hot isostatic pressing is 800-1000° C., the pressure for hot isostatic pressing is 1-15 MPa, and the duration for hot isostatic pressing is 2-8 hours, and after being taken out of the furnace, a thrust chamber assembly with a sheath is obtained; S5, post-processing: removing the mold and the prefabricated manifolds (6) at the upper and lower ends of the thrust chamber assembly with the sleeve, and then performing ultrasonic rolling treatment on the inner wall of the thrust chamber assembly to obtain a milled groove thrust chamber structural component.

2. A feasible forming method of a milling groove thrust chamber according to claim 1, characterized in that: In step S1, the specific steps of laser printing are: passing the atomized powder of CuCr alloy, CuCrZr alloy or CuCrNb alloy through a 270-300 mesh sieve, importing the drawn 3D model diagram into a laser printer, filling the atomized powder, placing the base plate, installing a scraper, and then evacuating the laser selective melting equipment to a vacuum degree of 3-5 Pa, and then introducing argon as a protective gas, and evenly spreading the atomized powder to the laser processing area through the scraper, and printing layer by layer according to the set printing parameters, the atomized powder printing single layer thickness is 0.03-0.06 mm, the scanning interval is 0.05-0.2 mm, the printing power is 380-460 W, and the scanning speed is 400-1600 mm / s, so as to obtain the thrust chamber inner wall structure (1).

3. The feasibility forming method of a milling groove thrust chamber according to claim 1, characterized in that: In the step S1, the roughness of the rib tops of the convex ribs of the outer wall of the thrust chamber inner wall structure (1) is Ra≤3.2 μm.

4. The feasibility forming method of a milling groove thrust chamber according to claim 1, characterized in that: In the step S2, the copper alloy interlayer (2) is provided as two mutually symmetrical half-shell structures. During assembly, the two copper alloy interlayer (2) half-shells are butt-jointed with the thrust chamber inner wall structure (1) and then electron beam butt-welded.

5. The feasibility forming method of a milling groove thrust chamber according to claim 1, characterized in that: In the step S2, the thickness of the pure nickel layer (3) is 1 to 20 mm, cold spraying is adopted during spraying, the spraying temperature is 350 to 600° C., the spraying gas is nitrogen, the pressure is 3 to 7 MPa, the powder feeding amount of the pure nickel powder used during spraying is 150 to 350 g / min, and the distance from the nozzle to the surface of the substrate is 20 to 40 mm.

6. The feasibility forming method of a milling groove thrust chamber according to claim 1, characterized in that: In step S3, the prefabricated stainless steel sheath (4) is provided as two mutually symmetrical half-shell structures. During assembly, the two prefabricated stainless steel sheaths (4) are butt-jointed with the copper alloy interlayer (2) and then electron beam butt-welded.

7. The feasibility forming method of a milling groove thrust chamber according to claim 1, characterized in that: In step S3, the mold is made of stainless steel, and the outer wall of the mold is sprayed with solder stop, and the thickness of the solder stop spray is 1 to 2 mm.

8. The feasibility forming method of a milling groove thrust chamber according to claim 1, characterized in that: In the step S5, when ultrasonic rolling is performed on the inner wall of the thrust chamber assembly, a heating wire is firstly wrapped around the outside of the thrust chamber assembly to heat the thrust chamber assembly to 220-240° C., and then an ultrasonic rolling head is used to extend along the extension direction of the convex rib from the end of the thrust chamber inner wall structural component (1) with a larger inner diameter to the end of the thrust chamber inner wall structural component (1) with a smaller inner diameter, with an ultrasonic rolling pressure of 650-750N, an ultrasonic frequency of 20-30kHz, an amplitude of 5-10μm, a cooling lubricant is coated on the ultrasonic rolling head, the ultrasonic rolling temperature is maintained at 60-80° C., and the feed speed is 0.05-0.1mm / rev.

Citation Information

Cited By

  • Vacuum brazing method for chromium zirconium copper and stainless steel, brazing joint and application