Device and method for measuring high-temperature electrical and mechanical resistance characteristics of components of ceramic matrix composite material
The device and method for measuring high-temperature resistance characteristics of CMC components address the lack of suitable methods by using a sample plate, electrodes, and vacuum chamber to accurately measure resistance and mechanical properties, overcoming thermal expansion interference.
Patent Information
- Application Number
- CN202411169252.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-06
AI Technical Summary
Current methods fail to measure the high-temperature electrical and mechanical resistance characteristics of ceramic matrix composite (CMC) components, particularly interfaces and matrices, due to the lack of suitable devices and the interference caused by thermal expansion.
A device and method involving a sample plate, high-temperature electrodes, a high-temperature furnace, and a vacuum environment chamber, along with specific sample preparation and measurement steps, to accurately measure the resistance characteristics of CMC components while accounting for thermal expansion effects.
Accurately measures high-temperature resistance and mechanical resistance of CMC components, accounting for thermal expansion, providing precise electrical and mechanical resistance data under high-temperature conditions.
Smart Images

Figure CN119086268A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of composite material damage self-sensing health monitoring, and specifically relates to a device and method for measuring high-temperature electrical and mechanical resistance characteristics of ceramic-based composite material components. Background Art
[0002] Ceramic Matrix Composites (CMCs) have outstanding advantages such as high temperature resistance and oxidation resistance, and have great potential in the future aerospace field. At present, CMCs have been initially applied to the hot end components of aircraft engines, and hot end components such as flame tubes and high-pressure turbines serve in extremely complex working environments, which leads to more complex damage and failure modes of CMCs hot end components. After the damage occurs, if it cannot be detected and the impact cannot be evaluated in time, it will cause more serious consequences. Therefore, it is extremely important to monitor the health status of CMCs components and predict their health status. CMCs are conductive, and their resistance is sensitive to temperature, load and various damage modes, so their own resistance characteristics such as temperature resistance and mechanical resistance can be used to implement health monitoring and life assessment.
[0003] Fiber-reinforced ceramic matrix composites are composed of reinforcing fibers, interfaces and ceramic matrices. The resistance characteristics of different components are also different, so the resistance characteristics of different components of CMCs at high temperatures are extremely important for the study of the macroscopic resistance characteristics of CMCs. The premise for measuring the resistance characteristics of different components at high temperatures is the preparation of high-temperature samples and the elimination of errors caused by thermal expansion under high-temperature environments. However, in the prior art, there are currently only methods for measuring the force resistance response of fiber monofilaments at room temperature and high temperatures (an online test device and test method for the force resistance response of fiber monofilaments, CN114486525A; a high-temperature high-throughput measurement device and method for the force resistance response of fiber monofilaments, 202410204310.9). There are no public reports of related prior art for measuring the resistance characteristics of components such as interfaces and matrices at high temperatures.
[0004] Therefore, it is necessary to invent a device and method for testing the resistance characteristics of a single component of CMCs in a high temperature environment, solve the problem of preparing high-temperature samples and eliminate the interference caused by thermal expansion, and obtain the resistance characteristics of a single component in a high temperature environment. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a device and method for measuring the high-temperature electrical and mechanical resistance characteristics of ceramic-based composite materials in view of the deficiencies of the above-mentioned prior art.
[0006] In order to achieve the above technical purpose, the technical solution adopted by the present invention is:
[0007] The device for measuring high-temperature electrical and mechanical resistance characteristics of ceramic-based composite material components includes a sample plate, a high-temperature electrode, a sample, a high-temperature furnace and a vacuum environment chamber. Both ends of the sample are fixed on the sample plate. At the same time, both ends of the sample are also connected to the high-temperature electrodes. The sample plate is placed in the high-temperature furnace, and both ends of the sample plate extend out of the high-temperature furnace. The sample is located in the uniform temperature section of the high-temperature furnace. The sample plate, the high-temperature electrode, the sample and the high-temperature furnace are all located in the vacuum environment chamber, and the high-temperature electrode is connected to a digital multimeter outside the vacuum environment chamber.
[0008] To optimize the technical solution, the present invention further adopts the following measures:
[0009] The above-mentioned sample plate is cut into two sample plate sections from the middle, so that the two ends of the sample are respectively located on the two sample plate sections, and the two sample plate sections are bonded together by paper tape, and the two ends of the sample plate or the two ends of the sample are connected to the tensile testing machine.
[0010] The above-mentioned specimens include fiber monofilaments and monofilament composite materials.
[0011] The above-mentioned monofilament composite material is a fiber monofilament with a single component of a predetermined thickness deposited on the surface.
[0012] The above-mentioned bending setting of the high-temperature electrode prevents the high-temperature electrode from being close to the two ends of the sample plate, and the bending part of the high-temperature electrode is wrapped with a high-temperature resistant insulating tape.
[0013] The method for measuring the high temperature electrical resistance characteristics of a ceramic matrix composite material component uses the above-mentioned high temperature electrical and mechanical resistance characteristics measuring device of the ceramic matrix composite material component, and specifically comprises the following steps:
[0014] Step 1: Cut the sample plate so that its center can be placed in the high-temperature furnace while both ends can extend out of the high-temperature furnace;
[0015] Step 2, take a fiber monofilament of a predetermined size and place it in the center of the sample plate;
[0016] Step 3, cut two sections of high-temperature electrodes and place them at both ends of the fiber monofilament respectively;
[0017] Step 4, take high temperature conductive glue, bond the end face of the fiber monofilament to one end of the high temperature electrode, and after curing, measure the exposed length of the fiber monofilament to be l;
[0018] Step 5, placing the middle part of the sample plate and the fiber monofilament into a high temperature furnace, so that the fiber monofilament is in the uniform temperature section of the high temperature furnace;
[0019] Step 6. Place the high temperature furnace inside the vacuum environment box, connect the high temperature electrode to the wire inside the vacuum environment box, and connect the internal wire to the digital multimeter. Turn on the digital multimeter to observe whether the resistance value is normal. Close the vacuum environment box and evacuate the inside to vacuum. Record the temperature T1 and the fiber single filament resistance value R at this time. f(T1), subscript f represents fiber monofilament;
[0020] Step 7: Turn on the high temperature furnace and heat it up in a step-by-step manner. After reaching the target temperature, keep it warm for a predetermined time, then turn off the high temperature furnace. During the cooling process, record the temperature T and the corresponding single fiber resistance value R. f (T),
[0021] Step 8: Replace the fiber monofilament with the monofilament composite material, repeat steps 2-7, and record the resistance R of the monofilament composite material at temperature T. c (T), subscript c represents a single-filament composite;
[0022] Step 9: Calculate the resistivity of the components in the single-filament composite material at temperature T:
[0023] In the monofilament composite material, the fiber monofilament and the single component are regarded as a parallel circuit, and the resistance of the fiber monofilament in the monofilament composite material is corrected. The resistance of the fiber monofilament in the monofilament composite material is recorded as The diameter of the fiber single filament is d, and the thermal expansion coefficient of the fiber single filament is α f , when the temperature is T, the temperature difference ΔT=T-T1, at this time
[0024]
[0025] Δl is the size change of the fiber filament in the monofilament composite material, Δd is the diameter change of the fiber filament in the monofilament composite material,
[0026] Then the resistivity of the fiber single fiber in the single fiber composite material at T is:
[0027]
[0028] The diameter of the single-filament composite material is D, and the thermal expansion coefficient of the single-filament composite material is α c , according to the thermal stress balance, then:
[0029] α c E c =V f E f α f +V m E m α m (3)
[0030] Where the subscript c represents the monofilament composite material, f represents the fiber monofilament, m represents the deposited component, α is the thermal expansion coefficient, E is the modulus, V represents the volume fraction, and the specimen is a cylinder, then:
[0031]
[0032] Substituting formula (4) into formula (3), the thermal expansion coefficient of the single-filament composite material is calculated as:
[0033]
[0034] Dimensional changes of fiber filaments in monofilament composites:
[0035] Δl=ΔD=Δd=α c ΔT (6)
[0036] The resistance of a single fiber in a monofilament composite is:
[0037]
[0038] in:
[0039]
[0040] Substituting equations (2) and (8) into equation (7), we can obtain the resistance of a single fiber in a single-fiber composite material:
[0041]
[0042] The component resistance in the monofilament composite material is:
[0043]
[0044] Substituting equation (9) into equation (10), we can obtain the component resistance in the single-filament composite material:
[0045]
[0046] The resistivity of the component in the single-filament composite material at temperature T is:
[0047]
[0048] Substituting equations (8) and (11) into equation (12), the resistivity of the component in the single-filament composite material at temperature T is obtained as follows:
[0049]
[0050] The method for measuring the high temperature mechanical resistance characteristics of a ceramic matrix composite material component uses the above-mentioned high temperature electrical and mechanical resistance characteristics measuring device of the ceramic matrix composite material component, and comprises the following steps:
[0051] Step 1: Cut the sample board, divide it into two sections from the middle of the sample board, and stick the two sections of the sample board together with paper tape so that the center part can be put into the high-temperature furnace while the two ends extend out of the high-temperature furnace;
[0052] Step 2: Take a fiber monofilament of a predetermined size and place it in the center of the sample plate;
[0053] Step 3, cut two sections of high-temperature electrodes and place them at both ends of the fiber monofilament respectively;
[0054] Step 4: Take high-temperature conductive glue and bond the end face of the fiber monofilament to one end of the high-temperature electrode. After curing, measure the exposed length of the fiber monofilament as l';
[0055] Step 5: Place the middle of the sample plate and the fiber monofilament into a high-temperature furnace, so that the fiber monofilament is in the uniform temperature section of the high-temperature furnace; clamp the two ends of the sample plate on a tensile testing machine, and cut the paper tape to completely separate the two sample plate sections;
[0056] Step 6. Connect the high temperature electrode to the wire inside the vacuum environment box, lead out the internal wire and connect it to the multimeter. Turn on the multimeter to observe whether the resistance value is normal. Close the vacuum environment box and evacuate the inside to vacuum. Record the temperature T2 and the resistance R f (T2), subscript f represents fiber monofilament;
[0057] Step 7: Turn on the high temperature furnace, step by step heat up to the target temperature T' and keep it warm for a period of time. At this time, the temperature difference ΔT' = T'-T2, and the length of the fiber monofilament is l(T') = (1+α f ΔT')l', the diameter is d(T')=(1+α f ΔT')d',
[0058] d' is the diameter of the fiber monofilament at temperature T2, the diameter difference Δd'=d(T')-d', and the thermal expansion coefficient of the fiber monofilament is α f , a load F is applied to both ends of the fiber monofilament by a tensile testing machine, and the length deformation of the fiber monofilament under the load F is recorded as Δl(σ). At this time, the resistance of the fiber monofilament is R f (σ), Poisson's ratio is μ, and modulus is E p , then the axial strain ε of the fiber y and radial strain ε x They are:
[0059]
[0060] At this time, the stress on the fiber monofilament is σ=ε y ·E p , the size of the fiber monofilament is:
[0061]
[0062] l(σ) is the length of the fiber monofilament under load F, d(σ) is the diameter of the fiber monofilament under load F, then the stress is σ, and the resistivity of the fiber monofilament at temperature T' is:
[0063]
[0064] Step 8: Replace the fiber monofilament with a monofilament composite material having a single component, and repeat steps 2-6.
[0065] Step 9. Turn on the high temperature furnace, raise the temperature step by step to the target temperature T', keep it warm for a while, and record the resistance R c (T'), where the subscript c represents the sample; the geometric dimensions of the monofilament composite material are:
[0066]
[0067] α c is the thermal expansion coefficient of the single-filament composite material, D' is the diameter of the single-filament composite material at temperature T2, l(T') * d(T') * and D(T') * are the length of the single-filament composite material, the diameter of the fiber single filament and the diameter of the single-filament composite material at the target temperature T'; the modulus of the single-filament composite material is E q , a load F is applied to both ends of the monofilament composite material by a tensile testing machine. * , to ensure that the stress of the single-filament composite material is σ, then the axial strain of the single-filament composite material is Radial strain Length deformation of monofilament composites Record the resistance R of the single-filament composite material at this time c (σ), the geometric dimensions of the single-filament composite material are:
[0068]
[0069] l(σ) * d(σ) * and D(σ) * The target temperature T' and the load F applied to both ends of the single-filament composite material are * Next, the length of the monofilament composite material, the fiber monofilament diameter, and the monofilament composite material diameter;
[0070] At this time, the resistivity of the fiber single wire is the same as formula (16), so the resistance of the fiber single wire is for:
[0071]
[0072] According to the parallel circuit law, the component resistance R m (σ) is:
[0073]
[0074] Substituting formula (19) into formula (20), we have:
[0075]
[0076] At this time, the geometric dimensions of the single-filament composite material are shown in formula (18), and the resistivity of the component when the temperature is T' and the stress is σ is:
[0077]
[0078] Compared with the prior art, the present invention has the following beneficial effects:
[0079] 1. The present invention realizes the measurement of high-temperature resistance characteristics of components of ceramic-based composite materials. At the same time, based on the measurement of high-temperature resistance characteristics of components, the present invention realizes the measurement of mechanical resistance effect of components under high-temperature environment. In the calculation process, the influence of changes in geometric dimensions during heating and stretching on resistivity is simultaneously considered, and the relationship between resistivity and stress and temperature is obtained. The electrical and mechanical resistance characteristics of a single component under high-temperature environment are obtained more accurately, eliminating the interference caused by thermal expansion of the material.
[0080] 2. The present invention solves the problem that single-filament composite materials are brittle, easy to break, and difficult to prepare samples. The high-temperature electrode is combined with the high-temperature glue to keep the sample in a heat-equalizing section to avoid the influence of thermoelectric effect on the resistance data. The influence of the difference in the size change of the fiber single filament during the heating process on the resistivity of the component is taken into account, and the temperature resistance characteristics of the component are more accurately reflected. BRIEF DESCRIPTION OF THE DRAWINGS
[0081] Figure 1 It is a schematic diagram of a device for measuring high temperature resistance characteristics of a ceramic matrix composite material component of the present invention;
[0082] Figure 2 It is a schematic diagram of a device for measuring high-temperature electrical and mechanical resistance characteristics of a ceramic-based composite material component of the present invention;
[0083] Figure 3 It is the graph of the resistance change rate of the interface component (pyrolytic carbon) of the ceramic matrix composite material as a function of temperature;
[0084] Figure 4 It is the graph of the resistance change rate of the matrix component (SiC) of the ceramic matrix composite material as a function of temperature;
[0085] Figure 5 This is a graph showing the resistivity of the interface component (pyrolytic carbon) of a ceramic matrix composite material as a function of strain at 600°C.
[0086] The markings in the attached drawings are: 1. Sample; 2. Test sample; 3. High temperature electrode; 4. High temperature conductive adhesive; 5. High temperature resistant insulating tape; 6. Paper tape. DETAILED DESCRIPTION
[0087] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0088] Obviously, the drawings described below are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios based on these drawings without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in this field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.
[0089] Reference to "embodiments" in this application means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those of ordinary skill in the art that the embodiments described in this application may be combined with other embodiments without conflict.
[0090] like Figure 1 As shown, the device for measuring the high temperature resistance characteristics of the ceramic matrix composite material component of the present invention comprises a sample plate 1; a sample 2; a high temperature electrode 3; a high temperature conductive adhesive 4; and a high temperature resistant insulating adhesive tape 5.
[0091] Sample 1 is a zirconia ceramic plate with a size of 150*10*2mm.
[0092] Sample 2 includes fiber monofilaments and monofilament composite materials. In this embodiment, the monofilament composite material is a monofilament sample after the interface component (pyrolytic carbon) is deposited, and the length is 30 mm.
[0093] The high temperature electrode 3 is a niobium wire.
[0094] The high temperature conductive adhesive 4 is a two-component silver powder conductive adhesive.
[0095] The high temperature resistant insulating tape 5 is a high temperature insulating tape.
[0096] When preparing the monofilament composite material, a ceramic matrix composite material single component preparation tool is used, and the ceramic matrix composite material single component preparation tool includes a winding frame, bolts, and threaded gaskets.
[0097] The winding frame, bolts and threaded washers are all made of graphite.
[0098] Bolts can be installed on the winding frame, and threaded washers can cooperate with the bolts.
[0099] The bolts are installed on the winding frame, threaded washers can be installed on the bolts, and the washers can be fastened with the winding frame to clamp the monofilament.
[0100] A method for preparing a monofilament composite material comprises the following steps:
[0101] 1. Screw the bolts into the threaded holes corresponding to the winding frame, heat and remove the glue of the fiber bundle of appropriate length, extract the fiber monofilament of appropriate length, place the two ends of the fiber monofilament next to the corresponding bolts, and tighten the threaded gasket;
[0102] 2. Repeat the operation in step 1 until all the threaded gaskets are pressed with fiber monofilaments, and deposit corresponding components on the fiber monofilaments using corresponding processes. After the deposition is completed, a monofilament composite material with a single component can be obtained.
[0103] The method of operating the device for measuring the high temperature electrical resistance characteristics of the ceramic matrix composite component shall include the following steps:
[0104] 1. Cut the sample 1 into a size of 150*10*2mm so that the center part can be placed in the high-temperature furnace while leaving a certain size at both ends for clamping;
[0105] 2. Take a 30mm fiber monofilament after degumming and place it in the center of the sample plate 1;
[0106] 3. Cut the high temperature electrodes 3 of appropriate length and place them at both ends of the fiber monofilament;
[0107] 4. Take two-component silver powder conductive glue and bond the end face of the fiber monofilament to the end of the high-temperature electrode 3 close to the fiber monofilament. After curing, measure the exposed length l = 20 mm;
[0108] 5. Place the prepared sample into a high temperature furnace, bend the high temperature electrode 3, protect the bend with a high temperature resistant insulating tape 5, and ensure that the fiber monofilament is in the soaking section of the high temperature furnace;
[0109] 6. Fix the sample 1 with the clamp, connect the high temperature electrode 3 to the wire inside the vacuum environment box, lead the internal wire to the digital source meter, turn on the digital source meter to observe whether the resistance data is normal, close the vacuum environment box and evacuate the inside to vacuum, record the temperature T1 = 20℃ and the resistance value R f (T1) = 86.29 MΩ;
[0110] 7. Turn on the high temperature furnace and use a step-by-step heating method. After reaching the target temperature, keep the temperature for a while. Turn off the high temperature furnace and record the resistance R corresponding to the temperature T = 600 °C during the cooling process. f (T) = 75 MΩ, subscript f represents the fiber monofilament;
[0111] 8. Replace the sample with the prepared single-filament composite material with a single interface component, repeat the above steps 2 to 7, and record the resistance R at T = 600 ° C c (T) = 116.3Ω, subscript c represents the sample;
[0112] 9. The fiber monofilament and the single component can be regarded as a simple parallel circuit. However, due to the different thermal expansion coefficients of the fiber monofilament and the monofilament composite sample, the dimensional changes after heating are also different. Therefore, it is necessary to correct the resistance of the fiber monofilament in the monofilament composite, which is recorded as The fiber monofilament diameter is d = 13 μm, and the thermal expansion coefficient is α f =4.7ppm / K, when the temperature is T=600℃, the temperature difference ΔT=T-T1=580℃, at this time:
[0113]
[0114] The fiber monofilament is at T i The resistivity is:
[0115]
[0116] The diameter of the single-filament composite material is D = 15 μm, and the thermal expansion coefficient is α c , thermal stress balance, then:
[0117] α c E c =V f E f α f +V m E m α m (3)
[0118] Where the subscript c represents the sample, f represents the fiber monofilament, m represents the corresponding deposited component, here PyC, α is the thermal expansion coefficient, E is the modulus, V represents the volume fraction, and the sample is a cylinder, then the relevant parameters are:
[0119]
[0120] Substituting formula (4) into formula (3), the thermal expansion coefficient of the single-filament composite material is calculated as:
[0121]
[0122] Size changes:
[0123] Δl=ΔD=Δd=α c ΔT=1.74×10 -6 (6)
[0124] At this time, the resistance of the fiber monofilament is:
[0125]
[0126] in:
[0127]
[0128] Substituting equations (2) and (8) into equation (7), we can obtain the resistance of a single fiber in a single-fiber composite material:
[0129]
[0130] The component resistance is:
[0131]
[0132] Substituting equation (9) into equation (10) yields the interface component resistance:
[0133]
[0134] The resistivity of the components is:
[0135]
[0136] Substituting equations (8) and (11) into equation (12), the resistivity of the component in the single-filament composite material at temperature T is obtained as follows:
[0137] ρ m (T) = 2.55 × 10 -5 Ω·cm (13)
[0138] Repeat the above operation to obtain the resistivity-temperature curve, such as Figure 3 , Figure 4 shown.
[0139] like Figure 2 The device for measuring the high temperature mechanical resistance characteristics of the ceramic matrix composite material components of the present invention is similar in structure to the device for measuring the high temperature electrical resistance characteristics of the ceramic matrix composite material components, except that there is an additional paper tape 6, which is used to fix the two sample plates.
[0140] A method for operating a high temperature force resistance test device for ceramic matrix composite components, which should include the following steps:
[0141] Step 1: Cut the sample to a size of 150*10*2mm, divide it into two halves, and use tape on one side to bond them together for sample placement;
[0142] Step 2: Take a fiber monofilament of a predetermined size and place it in the center of the sample plate;
[0143] Step 3, cut two sections of high-temperature electrodes and place them at both ends of the fiber monofilament respectively;
[0144] Step 4: Take high-temperature conductive glue and bond the end face of the fiber monofilament to one end of the high-temperature electrode. After curing, measure the exposed length of the fiber monofilament to be l'=18.6 mm.
[0145] Step 5: Place the middle of the sample plate and the fiber monofilament into a high-temperature furnace, so that the fiber monofilament is in the uniform temperature section of the high-temperature furnace; clamp the two ends of the sample plate on a tensile testing machine, and cut the paper tape to completely separate the two sample plate sections;
[0146] Step 6. Connect the high temperature electrode to the wire inside the vacuum environment box, lead out the internal wire and connect it to the multimeter. Turn on the multimeter to observe whether the resistance value is normal. Close the vacuum environment box and evacuate the inside to vacuum. Note that the temperature T2 = 20 ° C and the resistance R f (T2) = 153.3 MΩ, subscript f represents the fiber monofilament;
[0147] Step 7: Turn on the high temperature furnace, step by step heat up to the target temperature T' = 600 ° C and keep it warm for a period of time. At this time, the temperature difference ΔT' = T'-T2 = 580 ° C, d(T') = 13 μm is the diameter of the fiber monofilament at temperature T2, and the length of the fiber monofilament is l(T') = (1 + α f ΔT')l'=18.55mm, diameter is d(T')=(1+α f ΔT')d'=13.04μm, Diameter difference Δd'=d(T')-d', thermal expansion coefficient of fiber monofilament is α f =4.7ppm / K, a load F=3CN is applied to both ends of the fiber monofilament by a tensile testing machine, and the deformation of the fiber monofilament length under the load F is recorded as Δl(σ)=0.08mm. At this time, the resistance of the fiber monofilament is R f (σ)=73.5MΩ, Poisson's ratio is μ=0.19, and modulus is E p =423GPa, then the axial strain of the fiber single wire ε y and radial strain ε x They are:
[0148]
[0149] At this time, the stress on the fiber monofilament is σ=εy ·E p =1.823GPa, the size of the fiber monofilament is:
[0150]
[0151] l(σ) is the length of the fiber monofilament under load F, d(σ) is the diameter of the fiber monofilament under load F, then the stress is σ, and the resistivity of the fiber monofilament at temperature T' is:
[0152]
[0153] Step 8: Replace the fiber monofilament with a monofilament composite material having a single interface component and repeat steps 2-6.
[0154] Step 9: Turn on the high temperature furnace, step by step heat up to the target temperature T' = 600 ° C, keep it warm for a while, record the sample length l' = 17.9 mm, resistance R c (T') = 213Ω, where the subscript c represents the sample; at this time, the geometric dimensions of the monofilament composite material are:
[0155]
[0156] α c =3.13ppm / K is the thermal expansion coefficient of the single-filament composite material, D'=15μm is the diameter of the single-filament composite material at temperature T2=20°C, l(T') * d(T') * and D(T') * are the length of the single-filament composite material, the diameter of the fiber single filament, and the diameter of the single-filament composite material at the target temperature T'=600℃; the modulus of the single-filament composite material is E q = 412GPa, a load F is applied to both ends of the monofilament composite material by a tensile testing machine. * , to ensure that the stress of the single-filament composite material is σ=1.823GPa, then the axial strain of the single-filament composite material is Radial strain Length deformation of monofilament composites Record the resistance R of the single-filament composite material at this time c (σ)=302Ω, at this time the geometric dimensions of the monofilament composite material are:
[0158]
[0159] l(σ) * d(σ) * and D(σ) * are the target temperature T', the stress σ applied at both ends of the single-filament composite material, the length of the single-filament composite material, the diameter of the fiber single-filament, and the diameter of the single-filament composite material;
[0160] At this time, the resistivity of the fiber single wire is the same as formula (16), so the resistance of the fiber single wire is for:
[0161]
[0162] According to the parallel circuit law, the component resistance R m (σ) is:
[0163]
[0164] Substituting formula (19) into formula (20), we have:
[0165]
[0166] At this time, the geometric dimensions of the single-filament composite material are shown in formula (18), and the resistivity of the component when the temperature is T' and the stress is σ is:
[0167]
[0168] By repeating the above operation, the relationship between the resistivity and stress of the component at the same temperature can be obtained.
[0169] The above are only preferred embodiments of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should be regarded as the protection scope of the present invention.
Claims
1. A device for measuring high-temperature electrical and mechanical resistance characteristics of ceramic matrix composite materials, characterized in that: It includes a sample plate, a high-temperature electrode, a sample, a high-temperature furnace and a vacuum environment box. The two ends of the sample are fixed on the sample plate. At the same time, the two ends of the sample are also connected to the high-temperature electrode. The sample plate is placed in the high-temperature furnace, and the two ends of the sample plate extend out of the high-temperature furnace. The sample is located in the uniform temperature section of the high-temperature furnace. The sample plate, the high-temperature electrode, the sample and the high-temperature furnace are all located in the vacuum environment box. The high-temperature electrode is connected to a digital multimeter outside the vacuum environment box.
2. The device for measuring high temperature electrical and mechanical resistance characteristics of ceramic matrix composite materials according to claim 1, characterized in that: The template is cut into two template sections from the middle, so that the two ends of the sample are respectively located on the two template sections, and the two template sections are bonded together by paper tape. The two ends of the template or the two ends of the sample are connected to the tensile testing machine.
3. The device for measuring high temperature electrical and mechanical resistance characteristics of ceramic matrix composite materials according to claim 2, characterized in that: The samples include fiber monofilaments and monofilament composite materials.
4. The device for measuring high temperature electrical and mechanical resistance characteristics of ceramic matrix composite materials according to claim 3, characterized in that: The monofilament composite material is a fiber monofilament with a single component of a predetermined thickness deposited on the surface.
5. The device for measuring high temperature electrical and mechanical resistance characteristics of ceramic matrix composite materials according to claim 4, characterized in that: The high temperature electrode is bent so that the high temperature electrode is not close to the two ends of the sample plate, and the bending part of the high temperature electrode is wrapped with a high temperature resistant insulating tape.
6. A method for measuring the high temperature electrical resistance characteristics of a ceramic matrix composite component, characterized by: The device for measuring high temperature electrical and mechanical resistance characteristics of ceramic matrix composite materials as claimed in claim 1 specifically comprises the following steps: Step 1: Cut the sample plate so that its center can be placed in the high-temperature furnace while both ends can extend out of the high-temperature furnace; Step 2, take a fiber monofilament of a predetermined size and place it in the center of the sample plate; Step 3, cut two sections of high-temperature electrodes and place them at both ends of the fiber monofilament respectively; Step 4, take high temperature conductive glue, bond the end face of the fiber monofilament to one end of the high temperature electrode, and after curing, measure the exposed length of the fiber monofilament to be l; Step 5, placing the middle part of the sample plate and the fiber monofilament into a high temperature furnace, so that the fiber monofilament is in the uniform temperature section of the high temperature furnace; Step 6. Place the high temperature furnace inside the vacuum environment box, connect the high temperature electrode to the wire inside the vacuum environment box, and connect the internal wire to the digital multimeter. Turn on the digital multimeter to observe whether the resistance value is normal. Close the vacuum environment box and evacuate the inside to vacuum. Record the temperature T1 and the fiber single filament resistance value R at this time. f (T1), subscript f represents fiber monofilament; Step 7: Turn on the high temperature furnace and heat it up in a step-by-step manner. After reaching the target temperature, keep it warm for a predetermined time, then turn off the high temperature furnace. During the cooling process, record the temperature T and the corresponding single fiber resistance value R. f (T), Step 8: Replace the fiber monofilament with the monofilament composite material, repeat steps 2-7, and record the resistance R of the monofilament composite material at temperature T. c (T), subscript c represents a single-filament composite; Step 9: Calculate the resistivity of the components in the single-filament composite material at temperature T: In the monofilament composite material, the fiber monofilament and the single component are regarded as a parallel circuit, and the resistance of the fiber monofilament in the monofilament composite material is corrected. The resistance of the fiber monofilament in the monofilament composite material is recorded as The diameter of the fiber single filament is d, and the thermal expansion coefficient of the fiber single filament is α f , when the temperature is T, the temperature difference ΔT=T-T1, at this time Δl is the size change of the fiber filament in the monofilament composite material, Δd is the diameter change of the fiber filament in the monofilament composite material, Then the resistivity of the fiber single fiber in the single fiber composite material at T is: The diameter of the single-filament composite material is D, and the thermal expansion coefficient of the single-filament composite material is α c , according to the thermal stress balance, then: a c E c =V f E f a f +V m E m a m (3) Where the subscript c represents the monofilament composite material, f represents the fiber monofilament, m represents the deposited component, α is the thermal expansion coefficient, E is the modulus, V represents the volume fraction, and the specimen is a cylinder, then: Substituting formula (4) into formula (3), the thermal expansion coefficient of the single-filament composite material is calculated as: Dimensional changes of fiber filaments in monofilament composites: Δl=ΔD=Δd=α c ΔT (6) The resistance of a single fiber in a monofilament composite is: in: Substituting equations (2) and (8) into equation (7), we can obtain the resistance of a single fiber in a single-fiber composite material: The component resistance in the monofilament composite material is: Substituting equation (9) into equation (10), we can obtain the component resistance in the single-filament composite material: The resistivity of the component in the single-filament composite material at temperature T is: Substituting equations (8) and (11) into equation (12), the resistivity of the component in the single-filament composite material at temperature T is obtained as follows:
7. A method for measuring the high temperature mechanical resistance properties of a ceramic matrix composite material component, characterized in that: The device for measuring high temperature electrical and mechanical resistance characteristics of ceramic matrix composite materials as claimed in claim 2 comprises the following steps: Step 1: Cut the sample board, divide it into two sections from the middle of the sample board, and stick the two sections of the sample board together with paper tape so that the center part can be put into the high-temperature furnace while the two ends extend out of the high-temperature furnace; Step 2: Take a fiber monofilament of a predetermined size and place it in the center of the sample plate; Step 3, cut two sections of high-temperature electrodes and place them at both ends of the fiber monofilament respectively; Step 4: Take high temperature conductive glue and bond the end face of the fiber monofilament to one end of the high temperature electrode. The exposed length of the fiber monofilament is l'; Step 5: Place the middle part of the sample plate and the fiber monofilament into a high temperature furnace, so that the fiber monofilament is in the uniform temperature section of the high temperature furnace; Clamp both ends of the sample plate on the tensile testing machine, and cut the paper tape to completely separate the two sample plate sections; Step 6. Connect the high temperature electrode to the wire inside the vacuum environment box, lead out the internal wire and connect it to the multimeter. Turn on the multimeter to observe whether the resistance value is normal. Close the vacuum environment box and evacuate the inside to vacuum. Record the temperature T2 and the resistance R f (T2), subscript f represents fiber monofilament; Step 7: Turn on the high temperature furnace, step by step heat up to the target temperature T' and keep it warm for a period of time. At this time, the temperature difference ΔT' = T'-T2, and the length of the fiber monofilament is l(T') = (1+Δ f ΔT')l', the diameter is d(T')=(1+α f ΔT')d', d' is the diameter of the fiber monofilament at temperature T2, the diameter difference Δd'=d(T')-d', and the thermal expansion coefficient of the fiber monofilament is α f , by pulling The tensile testing machine applies a load F to both ends of the fiber monofilament, and records the length deformation of the fiber monofilament under the load F as Δl(σ). At this time, the resistance of the fiber monofilament is R f (σ), Poisson's ratio is μ, and modulus is E p , then the axial strain of the fiber single wire ε y and radial strain ε x They are: At this time, the stress on the fiber monofilament is σ=ε y ·E p , the size of the fiber monofilament is: l(σ) is the length of the fiber monofilament under load F, d(σ) is the diameter of the fiber monofilament under load F, then the stress is σ, and the resistivity of the fiber monofilament at temperature T' is: Step 8: Replace the fiber monofilament with a monofilament composite material having a single component, and repeat steps 2-6. Step 9. Turn on the high temperature furnace, raise the temperature step by step to the target temperature T', keep it warm for a while, and record the resistance R c (T'), where the subscript c represents the sample; the geometric dimensions of the monofilament composite material are: α c is the thermal expansion coefficient of the single-filament composite material, D' is the diameter of the single-filament composite material at temperature T2, l(T') * d(T') * and D(T') * are the length of the single-filament composite material, the diameter of the fiber single filament and the diameter of the single-filament composite material at the target temperature T'; the modulus of the single-filament composite material is E q , a load F is applied to both ends of the monofilament composite material by a tensile testing machine. * , to ensure that the stress of the single-filament composite material is σ, then the axial strain of the single-filament composite material is Radial strain Length deformation of monofilament composites Record the resistance R of the single-filament composite material at this time c (σ), the geometric dimensions of the single-filament composite material are: l(σ) * d(σ) * and D(σ) * The target temperature T' and the load F applied to both ends of the single-filament composite material are * Next, the length of the monofilament composite material, the fiber monofilament diameter, and the monofilament composite material diameter; At this time, the resistivity of the fiber single wire is the same as formula (16), so the resistance of the fiber single wire is for: According to the parallel circuit law, the component resistance R m (σ) is: Substituting formula (19) into formula (20), we have: At this time, the geometric dimensions of the single-filament composite material are shown in formula (18), and the resistivity of the component when the temperature is T' and the stress is σ is:
Citation Information
Patent Citations
Online testing device and testing method for force resistance response of fiber monofilament
CN114486525A
High-temperature and high-flux measuring device and method for force resistance response of fiber monofilament
CN118258677A