Method for analyzing thermal runaway gas production time sequence of lithium ion battery
The method combines thermal analysis, infrared spectroscopy, and mass spectrometry to comprehensively analyze gas production timing and composition in lithium-ion batteries, addressing the limitations of existing methods and enhancing safety through detailed thermal runaway mechanism understanding.
Patent Information
- Application Number
- CN202411262591.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-12-06
AI Technical Summary
Existing methods for analyzing gas production during lithium-ion battery thermal runaway are inadequate, as they cannot provide comprehensive and real-time detection, particularly failing to identify diatomic substances and being interfered by electrolyte fragments.
A method involving synchronous thermal analysis, Fourier transform infrared spectroscopy, and gas chromatography-mass spectrometry to determine the timing and composition of gas production in lithium-ion batteries, by analyzing the mass and heat generation of battery components and identifying functional groups and compositions of gaseous substances.
Enables comprehensive and real-time detection of thermal runaway gas production, providing insights into the mechanisms and aiding in safety design and protection of lithium-ion batteries.
Smart Images

Figure CN119086478A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-ion batteries, and in particular relates to a method for analyzing the timing of thermal runaway gas production in lithium-ion batteries. Background Art
[0002] Lithium-ion batteries are considered the most promising power source for electric vehicles due to their high energy density, long cycle life and wide range of working conditions. However, explosion accidents in energy storage systems caused by thermal runaway of lithium-ion batteries pose a great threat to people's lives and property safety, and also limit the commercial application of lithium-ion batteries. In order to improve the safety of lithium-ion battery energy storage systems, it is necessary to study the thermal runaway mechanism in essence, so as to guide battery safety design and other work.
[0003] When lithium-ion batteries are subjected to thermal abuse, electrical abuse, mechanical abuse, and electrochemical abuse, the internal temperature of the battery will rise, resulting in various reactions between the internal materials of the battery. Generally, the internal temperature of the battery will go from low temperature to high temperature: SEI film decomposition, negative electrode-electrolyte reaction to produce reducing gas, reducing gas crosstalk to the positive electrode and attack, positive electrode release of active oxygen (ternary lithium-ion battery), diaphragm melting, positive and negative electrode redox reaction, adhesive reaction, etc. It should be noted that these reactions contribute differently to the heat release and gas production of thermal runaway, and they are not carried out independently in sequence. At certain moments, multiple reactions may occur simultaneously.
[0004] Reactions inside the battery will produce flammable, explosive and toxic gases such as hydrogen, methane, ethylene, carbon monoxide, carbon dioxide and hydrofluoric acid. Among the existing gas production analysis technologies, GC-MS takes a long time to detect and will destroy the gas sample, so it is impossible to achieve in-situ observation of thermal runaway gas production. FTIR cannot analyze non-polar diatomic components, and mass spectrometers are limited by the influence of electrolyte fragments.
[0005] Therefore, there is an urgent need for a method that can realize comprehensive and real-time detection of gas production of lithium-ion battery component materials, so as to provide support for the study of lithium-ion thermal runaway mechanism. Summary of the invention
[0006] The purpose of the present invention is to provide a method for analyzing the gas production timing of a lithium-ion battery during thermal runaway. The method provided by the present invention can achieve comprehensive detection of the gas production timing of each component material of a lithium-ion battery during thermal runaway.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] The present invention provides a method for analyzing the gas generation time sequence of thermal runaway of a lithium-ion battery, comprising the following steps:
[0009] Step 1: Determine the mass of the positive electrode material, negative electrode material and electrolyte in the lithium-ion battery respectively;
[0010] Step 2: Prepare any one, any two or three combinations of the positive electrode material, the negative electrode material and the electrolyte in step 1 to obtain a test sample; when the test sample is a combination of any two or three of the above materials, the mass ratio between the materials is the same as the mass ratio of the materials in step 1;
[0011] Step 3: Perform a synchronous thermal analyzer test on each test sample to obtain a TG curve and a DSC curve of each test sample; determine the temperature point at which the mass loss of each test sample is the fastest according to the TG curve; determine the temperature point at which the heat generation of each test sample is the highest according to the DSC curve, and determine the thermal runaway reaction sequence according to the DSC curves of all test samples;
[0012] Step 4: Perform Fourier transform infrared spectroscopy on the gaseous substances generated during the test of the synchronous thermal analyzer in step 3 to determine the functional groups of the gaseous substances;
[0013] At the same time, the gaseous substances corresponding to the temperature point with the fastest mass loss and the temperature point with the highest heat generation determined in step 3 are tested by gas chromatography-mass spectrometry to determine the composition of the gaseous substances;
[0014] Step 5: According to the thermal runaway reaction sequence determined in step 3 and the composition of the gaseous substance determined in step 4, determine the thermal runaway gas generation sequence of the lithium-ion battery.
[0015] Preferably, the process of determining the mass of the positive electrode material includes: punching and sampling the disassembled positive electrode sheet, scraping off the positive electrode material on the obtained sample, and calculating the mass of the positive electrode material on the entire positive electrode sheet and the mass of the positive electrode current collector based on the mass of the positive electrode material on the sample.
[0016] Preferably, the process of determining the mass of the negative electrode material includes: soaking the disassembled negative electrode sheet in water, drying the negative electrode current collector from which the negative electrode material has been removed and weighing it, and subtracting the mass of the negative electrode current collector from the mass of the negative electrode sheet to obtain the mass of the negative electrode material.
[0017] Preferably, the process of determining the mass of the electrolyte includes: cleaning the disassembled diaphragm with an organic solvent, and then drying and weighing it in sequence to obtain the mass of the diaphragm; subtracting the mass of the positive electrode material, the positive electrode collector, the negative electrode material, the negative electrode collector and the diaphragm from the total mass of the disassembled battery cell to obtain the mass of the electrolyte; the battery cell includes a positive electrode sheet, a negative electrode sheet, a diaphragm and an electrolyte.
[0018] Preferably, the mass of the test sample in step 2 does not exceed 10 mg.
[0019] Preferably, in step 2, when the test sample is any one of a positive electrode material, a negative electrode material and an electrolyte, the sample preparation process of the positive electrode material or the negative electrode material, except for the electrolyte, includes: grinding the positive electrode material or the negative electrode material and placing it in an aluminum crucible, and using a tablet press to compact and seal the aluminum cover sheet and the aluminum crucible.
[0020] Preferably, in step 2, when the test samples are positive electrode materials and negative electrode materials, the sample preparation process includes: mixing and grinding the positive electrode material and the negative electrode material, placing them in an aluminum crucible, and using a tablet press to compact and seal the aluminum cover sheet and the aluminum crucible.
[0021] Preferably, in step 2, when the test sample is a positive electrode material and an electrolyte, or a negative electrode material and an electrolyte, the sample preparation process includes: grinding the positive electrode material or the negative electrode material, mixing it with the electrolyte, placing the obtained mixture in an aluminum crucible, and using a tablet press to compact and seal the aluminum cover sheet and the aluminum crucible.
[0022] Preferably, when the test sample is a combination of a positive electrode material, a negative electrode material and an electrolyte, the sample preparation process includes: mixing and grinding the positive electrode material and the negative electrode material, mixing them with the electrolyte, placing the resulting mixture in an aluminum crucible, and using a tablet press to compact and seal the aluminum cover sheet and the aluminum crucible.
[0023] Preferably, the test conditions of the synchronous thermal analyzer test include: an initial temperature of 35°C, a final temperature of 600°C, a heating rate of 10K / min, and a nitrogen atmosphere.
[0024] The invention provides a method for analyzing the timing of thermal runaway gas production of a lithium-ion battery.
[0025] Compared with the prior art, the advantages of the present invention are:
[0026] Compared with the existing single STA-FTIR, the analytical method provided by the present invention solves the shortcomings of not being able to detect diatomic substances and not being able to determine specific components; compared with STA-MS, it solves the interference of electrolyte fragments; the present invention complements the advantages of mass spectrometer and Fourier transform infrared spectroscopy testing, thereby realizing in-situ observation and full component analysis of thermal runaway gas production reactions, providing ideas for in-depth tracing of thermal runaway and gas production mechanisms of lithium-ion batteries. On this basis, new thermal runaway mechanisms and gas production analysis research methods can be derived, which can help improve the understanding of lithium-ion battery mechanisms and provide ideas for lithium-ion battery safety design and thermal runaway protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the process involved in step 1 and step 2 of the present invention;
[0028] Figure 2is the DSC curve of each test sample in Example 1;
[0029] Figure 3 FTIR curves of various test samples in Example 1;
[0030] Figure 4 GC-MS curves of various test samples in Example 1;
[0031] Figure 5 This is a timing diagram of thermal runaway gas production of the lithium-ion battery obtained in Example 1;
[0032] Figure 6 A schematic diagram of the flow chart of the analytical method provided by the present invention. DETAILED DESCRIPTION
[0033] The present invention provides a method for analyzing the gas generation time sequence of thermal runaway of a lithium-ion battery, comprising the following steps:
[0034] Step 1: Determine the mass of the positive electrode material, negative electrode material and electrolyte in the lithium-ion battery respectively;
[0035] Step 2: Prepare any one, any two or three combinations of the positive electrode material, the negative electrode material and the electrolyte in step 1 to obtain a test sample; when the test sample is a combination of any two or three of the above materials, the mass ratio between the materials is the same as the mass ratio of the materials in step 1;
[0036] Step 3: Perform a synchronous thermal analyzer test on each test sample to obtain a TG curve and a DSC curve of each test sample; determine the temperature point at which the mass loss of each test sample is the fastest according to the TG curve; determine the temperature point at which the heat generation of each test sample is the highest according to the DSC curve, and determine the thermal runaway reaction sequence according to the DSC curves of all test samples;
[0037] Step 4: Perform Fourier transform infrared spectroscopy on the gaseous substances generated during the test of the synchronous thermal analyzer in step 3 to determine the functional groups of the gaseous substances;
[0038] At the same time, the gaseous substances corresponding to the temperature point with the fastest mass loss and the temperature point with the highest heat generation determined in step 3 are tested by gas chromatography-mass spectrometry to determine the composition of the gaseous substances;
[0039] Step 5: According to the thermal runaway reaction sequence determined in step 3 and the composition of the gaseous substance determined in step 4, determine the thermal runaway gas generation sequence of the lithium-ion battery.
[0040] In the present invention, the lithium ion battery is preferably a lithium ion battery that has passed a 100% SOC test. The present invention has no particular limitation on the type of the lithium ion battery, and any lithium ion battery may be used.
[0041] The present invention determines the masses of positive electrode material, negative electrode material and electrolyte in a lithium ion battery respectively.
[0042] In the present invention, the process of determining the mass of the positive electrode material preferably includes: punching and sampling the disassembled positive electrode sheet, scraping off the positive electrode material on the obtained sample, and calculating the mass of the positive electrode material on the entire positive electrode sheet and the mass of the positive electrode current collector based on the mass of the positive electrode material on the sample.
[0043] In the present invention, the process of determining the mass of the negative electrode material preferably includes: soaking the disassembled negative electrode sheet in water, drying the negative electrode current collector from which the negative electrode material has been removed and weighing it, and subtracting the mass of the negative electrode current collector from the mass of the negative electrode sheet to obtain the mass of the negative electrode material.
[0044] In the present invention, the process of determining the mass of the electrolyte preferably includes: washing the disassembled diaphragm with an organic solvent, drying and weighing in sequence to obtain the mass of the diaphragm; subtracting the mass of the positive electrode material, positive electrode collector, negative electrode material, negative electrode collector and diaphragm from the total mass of the disassembled battery cell to obtain the mass of the electrolyte; the battery cell preferably includes a positive electrode sheet, a negative electrode sheet, a diaphragm and an electrolyte. In the present invention, the organic solvent preferably includes dimethyl carbonate (DMC).
[0045] After obtaining the masses of the positive electrode material, the negative electrode material and the electrolyte, the present invention prepares a sample by using any one, any two or a combination of three of the positive electrode material, the negative electrode material and the electrolyte in step 1 to obtain a test sample; when the test sample is a combination of any two or three of the above materials, the mass ratio between the materials is the same as the mass ratio of the materials in step 1.
[0046] In the present invention, the electrolyte used in the sample preparation process is preferably prepared by re-preparing the disassembled electrolyte according to the component types and contents obtained after component analysis. The present invention has no special limitation on the component analysis and re-preparation process, and those familiar to those skilled in the art can be used.
[0047] In the present invention, the mass of the test sample is preferably no more than 10 mg.
[0048] In the present invention, when the test sample is any one of a positive electrode material, a negative electrode material and an electrolyte, in addition to the electrolyte, the sample preparation process of the positive electrode material or the negative electrode material preferably includes: grinding the positive electrode material or the negative electrode material and placing it in an aluminum crucible, and using a tablet press to compact and seal the aluminum cover sheet and the aluminum crucible. In the present invention, when the test sample is an electrolyte, the sample preparation process preferably includes: placing the electrolyte in an aluminum crucible, and using a tablet press to compact and seal the aluminum cover sheet and the aluminum crucible.
[0049] In the present invention, when the test samples are positive electrode materials and negative electrode materials, the sample preparation process preferably includes: mixing and grinding the positive electrode materials and the negative electrode materials, placing them in an aluminum crucible, and using a tablet press to compact and seal the aluminum cover sheet and the aluminum crucible.
[0050] In the present invention, when the test sample is a positive electrode material and an electrolyte, or a negative electrode material and an electrolyte, the sample preparation process preferably includes: grinding the positive electrode material or the negative electrode material, mixing it with the electrolyte, placing the obtained mixture in an aluminum crucible, and using a tablet press to compact and seal the aluminum cover sheet and the aluminum crucible.
[0051] In the present invention, when the test sample is a combination of a positive electrode material, a negative electrode material and an electrolyte, the sample preparation process preferably includes: mixing and grinding the positive electrode material and the negative electrode material, mixing them with the electrolyte, placing the obtained mixture in an aluminum crucible, and using a tablet press to compact and seal the aluminum cover sheet and the aluminum crucible.
[0052] The present invention has no special limitation on the grinding and compacting and sealing process in the above scheme, and the process well known to those skilled in the art can be adopted.
[0053] In the present invention, the test samples are preferably recorded as positive electrode, negative electrode, positive electrode-negative electrode, negative electrode-electrolyte, positive electrode-electrolyte, electrolyte, positive electrode-negative electrode-electrolyte.
[0054] In the present invention, the processes involved in step 1 and step 2 are as follows Figure 1 shown.
[0055] After obtaining the test sample, the present invention performs a synchronous thermal analyzer test (STA) on each test sample to obtain a TG curve and a DSC curve of each test sample, respectively; determines the temperature point at which the mass loss of each test sample is the fastest according to the TG curve; determines the temperature point at which the heat generation of each test sample is the highest according to the DSC curve, and determines the thermal runaway reaction timing according to the DSC curves of all test samples.
[0056] In the present invention, the test conditions of the synchronous thermal analyzer test preferably include: an initial temperature of 35°C, a final temperature of 600°C, a heating rate of 10K / min, and a nitrogen atmosphere. The present invention has no special limitation on the process of the synchronous thermal analyzer test, and those familiar to those skilled in the art can be used.
[0057] After the synchronous thermal analyzer test, the present invention performs Fourier transform infrared spectroscopy (FTIR) detection on the gaseous substances generated during the synchronous thermal analyzer test to determine the functional groups of the gaseous substances; at the same time, the gaseous substances corresponding to the temperature points with the fastest mass loss and the highest heat generation determined in step 3 are subjected to gas chromatography-mass spectrometry (GC-MS) detection to determine the composition of the gaseous substances.
[0058] The present invention has no special limitation on the process of Fourier transform infrared spectroscopy detection, and the process known to those skilled in the art can be adopted. In the present invention, FTIR is used to analyze the type of pyrolysis products and observe product changes in situ.
[0059] In the present invention, when no product produced by the synchronous thermal analyzer test is detected by Fourier transform infrared spectroscopy, the temperature point with the fastest mass loss and the temperature point with the highest heat generation of the corresponding test sample may not be determined in the above step 3.
[0060] The present invention has no special limitation on the process of gas chromatography-mass spectrometry detection, and those skilled in the art can adopt the method known to those skilled in the art. In the present invention, GC-MS can analyze the gaseous products at a certain key temperature node to obtain the full product analysis of the node.
[0061] After obtaining the thermal runaway reaction sequence and the composition of the gaseous substance, the present invention determines the thermal runaway gas generation sequence of the lithium ion battery according to the determined thermal runaway reaction sequence and the determined composition of the gaseous substance.
[0062] The schematic diagram of the analytical method provided by the present invention is as follows Figure 6 shown.
[0063] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.
[0064] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0065] Example 1
[0066] The lithium-ion battery of this embodiment is a lithium-ion battery that has passed the 100% SOC test. It uses a 340Ah lithium iron phosphate battery. The negative electrode is made of graphite, the negative electrode current collector is made of copper, the positive electrode is lithium iron phosphate, and the positive electrode current collector is made of aluminum. There are four battery cells inside, using a stacked structure, and the electrolyte includes the following mass percentage components: EMC 50%, EC 35%, PC 5%, LiPF 6 10%;
[0067] (1) Quantitative analysis of battery components:
[0068] The lithium-ion battery is disassembled, and a positive electrode sheet obtained by the disassembly is punched to obtain a sample, and the positive electrode material on the obtained sample is scraped off, and the mass of the positive electrode material on the entire positive electrode sheet and the mass of the positive electrode current collector are calculated according to the mass of the positive electrode material on the sample;
[0069] The disassembled negative electrode sheet is soaked in water, and the negative electrode current collector from which the negative electrode material is removed is dried and weighed. The mass of the negative electrode material is obtained by subtracting the mass of the negative electrode current collector from the mass of the negative electrode sheet;
[0070] The disassembled diaphragm is cleaned with dimethyl carbonate (DMC), dried and weighed in sequence to obtain the mass of the diaphragm; the mass of the electrolyte is obtained by subtracting the mass of the positive electrode material, the positive electrode current collector, the negative electrode material, the negative electrode current collector and the diaphragm from the total mass of the disassembled battery cell;
[0071] (2) Test sample preparation:
[0072] The electrolyte obtained by the above disassembly is subjected to component analysis, and the electrolyte is re-prepared according to the types and contents of the components obtained by the analysis for standby use; the test samples obtained by the preparation are recorded as positive electrode, negative electrode, positive electrode-negative electrode, negative electrode-electrolyte, positive electrode-electrolyte, electrolyte, positive electrode-negative electrode-electrolyte;
[0073] The sample preparation process of the electrolyte is as follows: the electrolyte is placed in an aluminum crucible, and an aluminum cover sheet and an aluminum crucible are compacted and sealed by a tablet press;
[0074] The sample preparation process of the positive electrode or negative electrode is as follows: the positive electrode material or the negative electrode material is ground and placed in an aluminum crucible, and the aluminum cover sheet and the aluminum crucible are compacted and sealed by a tablet press;
[0075] The positive electrode-negative electrode sample preparation process: the positive electrode material and the negative electrode material are mixed and ground, and then placed in an aluminum crucible, and the aluminum cover sheet and the aluminum crucible are compacted and sealed by a tablet press;
[0076] The sample preparation process of positive electrode-electrolyte or negative electrode-electrolyte is as follows: the positive electrode material or the negative electrode material is ground and mixed with the electrolyte, the obtained mixture is placed in an aluminum crucible, and the aluminum cover sheet and the aluminum crucible are compacted and sealed by a tablet press;
[0077] The sample preparation process of positive electrode-negative electrode-electrolyte: the positive electrode material and the negative electrode material are mixed and ground, and then mixed with the electrolyte. The obtained mixture is placed in an aluminum crucible, and the aluminum cover sheet and the aluminum crucible are compacted and sealed by a tablet press;
[0078] (3) Synchronous Thermal Analyzer Test (STA)
[0079] Each test sample is tested by a synchronous thermal analyzer to obtain a TG curve and a DSC curve of each test sample; the temperature point T at which the mass loss of each test sample is fastest is determined according to the TG curve. 质量 ; Determine the temperature point T with the highest heat generation of each test sample according to the DSC curve 产热 , and the thermal runaway reaction sequence was determined based on the DSC curves of all the test samples; the temperature point with the fastest mass loss and the temperature point with the highest heat generation for each test sample are shown in Table 1;
[0080] Table 1 The temperature point where the mass loss is fastest and the temperature point where the heat generation is highest for each test sample
[0081]
[0082] Since no product was detected in the subsequent Fourier transform infrared spectroscopy test of the three test samples of positive electrode, negative electrode and positive electrode-negative electrode, the temperature points with the fastest mass loss and the highest heat generation of the three test samples were not counted;
[0083] in, Figure 2 From the DSC curves obtained for each test sample, it can be seen that through the DSC data of all component materials (i.e. positive electrode-negative electrode-electrolyte), there are four exothermic peaks. The first three exothermic peaks correspond to the temperature range of the exothermic peak of the "negative electrode-electrolyte" material reaction, and the fourth exothermic peak corresponds to the decomposition exotherm of the positive electrode material. By comparing the tests between different component materials, it was found that compared with other reactions, the negative electrode-electrolyte exothermic peak appeared at the earliest temperature and released the highest amount of heat. It can be determined that the negative electrode-electrolyte is the triggering reaction and main exothermic reaction of thermal runaway. The exothermic reactions between the component materials in the process of battery thermal runaway can find the corresponding temperature range in the DSC results, so the timing of the thermal runaway reaction inside the battery can be determined. For details, please refer to Figure 5 Description of
[0084] (4) Fourier transform infrared spectroscopy (FTIR) and gas chromatography-mass spectrometry (GC-MS):
[0085] Perform Fourier transform infrared spectroscopy on the gaseous substances generated during the test of the synchronous thermal analyzer to determine the functional groups of the gaseous substances;
[0086] in, Figure 3 To obtain the FTIR curve, FTIR can realize the in-situ observation of the product. The temperature point with the fastest mass loss is also the temperature point with the most abundant product. Draw the FTIR spectra of these temperature points and analyze the functional groups of the product.
[0087] Depend on Figure 3 It can be seen that the electrolyte begins to have infrared absorption peaks at 71.9℃, among which 1019cm -1 The in-plane bending vibration absorption peak of CH is 1279 cm -1 The stretching vibration absorption peak of COC is 1786cm -1 The absorption peak at 2369cm is the C=O stretching vibration absorption peak. -1 The absorption peak at 767cm represents CO2. -1 and 971cm -1 The out-of-plane bending vibration absorption peak of CH appears at 2924 cm -1 and 2999cm -1 The stretching vibration absorption peak of CH appeared at 220 °C, and no substance was detected after 220 °C.
[0088] The negative electrode-electrolyte reaction starts at 669 cm-1 at 170 °C. -1 There is an absorption peak at 767cm -1 and 971cm -1 The absorption peaks appearing at 767cm-1 represent the vibration of the CH bond in low-carbon alkanes, indicating the generation of low-carbon alkanes. In addition, at high temperatures above 300°C, the negative electrode and the electrolyte still react to generate low-carbon alkanes and CO2. -1 and 971cm -1 The CH vibration absorption peak appears at , while no product is generated at higher temperatures. As for the infrared absorption peak of the anode-cathode-electrolyte reaction, it is almost the same as that of the anode-electrolyte reaction, which indicates that the anode-electrolyte reaction is the dominant reaction for the generation of thermal runaway gas products.
[0089] The gaseous substances corresponding to the determined temperature points with the fastest mass loss and the highest heat generation are tested by gas chromatography-mass spectrometry (GC-MS) to determine the composition of the gaseous substances;
[0090] in, Figure 4 In order to obtain the GC-MS curve, it should be noted that the fragments of the electrolyte components broken into pieces by the mass spectrometer contain parts with the same molecular weight as the target product. Therefore, it is necessary to conduct electrolyte experiments at corresponding temperature points as a control. If the product peak is significantly increased compared with the control group, it can be determined that the product has been generated. Figure 4As shown, the product peaks in the electrolyte are the peaks of the electrolyte component fragments. The results of the single electrolyte are used as a comparison. The new peaks that appear after adding other component materials can be considered to be the generation of thermal runaway gases. It can be seen that the gases emitted by thermal runaway lithium-ion batteries are mainly H2, CH4, CO, CO2, C2H4, C2H6 and C3H6, and their relative molecular masses are 2, 16, 28, 44, 28, 30 and 42 respectively. These mass-to-charge ratios are searched in the results to obtain ion chromatograms of different samples (such as Figure 4 As shown), but due to the limitation of the chromatographic column, no molecular H2 component was detected. The peak time and relative abundance of the electrolyte ion fragment components can be used as a comparison chart for the analysis of other reaction target products. In the negative electrode-electrolyte reaction, the ion chromatographic curves with mass-to-charge ratios of 16, 28, 30, 42 and 44 all showed new chromatographic peaks compared with the electrolyte results, indicating the generation of CH4, CO, C2H4, C2H6, C3H6 and CO2. In the positive electrode-electrolyte reaction, the ion chromatographic curves with mass-to-charge ratios of 30, 42 and 44 all showed new chromatographic peaks compared with the electrolyte results, indicating the presence of C2H6, C3H6 and CO2. As for the product results of the full-component material, they are the same as the negative electrode-electrolyte results, which also shows that the negative electrode-electrolyte reaction is the main gas-producing reaction of thermal runaway.
[0091] The FTIR results obtained the temperature range of the generated products, which was then linked to the thermal runaway reaction and the gas production sequence of the thermal runaway reaction was determined. The GC-MS results analyzed the specific components in the key temperature range, thereby drawing a complete thermal runaway reaction mechanism and gas production sequence diagram. The obtained thermal runaway gas production sequence diagram of lithium-ion batteries is shown below: Figure 5 shown; from Figure 5 It can be seen that the electrolyte of the battery begins to evaporate at 110°C, and when the internal gas pressure reaches the upper limit of the eruption port, the battery erupts for the first time, erupting a large amount of electrolyte vapor. When the internal temperature reaches 165°C, the SEI film decomposition reaction occurs, and at 170°C, the positive electrode-electrolyte reaction occurs, generating C2H6, C3H8 and CO2. After that, the negative electrode-electrolyte reaction occurs at 225°C, generating CH4, CO, C2H4, C2H6, C3H6 and CO2, which generates most of the thermal runaway gas. At the same time, the negative electrode decomposition and the positive and negative electrode redox reactions occur at this temperature, among which the negative electrode decomposition contributes the most to heat generation. The positive electrode begins to decompose at 500°C, but the thermal runaway of lithium iron phosphate may not reach this temperature.
[0092] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for analyzing the timing of thermal runaway gas production in lithium-ion batteries, characterized in that: The following steps are involved: Step 1: Determine the mass of the positive electrode material, negative electrode material and electrolyte in the lithium-ion battery respectively; Step 2: Prepare any one, any two or three combinations of the positive electrode material, the negative electrode material and the electrolyte in step 1 to obtain a test sample; when the test sample is a combination of any two or three of the above materials, the mass ratio between the materials is the same as the mass ratio of the materials in step 1; Step 3: Perform a synchronous thermal analyzer test on each test sample to obtain a TG curve and a DSC curve of each test sample; determine the temperature point at which the mass loss of each test sample is the fastest according to the TG curve; determine the temperature point at which the heat generation of each test sample is the highest according to the DSC curve, and determine the thermal runaway reaction sequence according to the DSC curves of all test samples; Step 4: Perform Fourier transform infrared spectroscopy on the gaseous substances generated during the test of the synchronous thermal analyzer in step 3 to determine the functional groups of the gaseous substances; At the same time, the gaseous substances corresponding to the temperature point with the fastest mass loss and the temperature point with the highest heat generation determined in step 3 are tested by gas chromatography-mass spectrometry to determine the composition of the gaseous substances; Step 5: According to the thermal runaway reaction sequence determined in step 3 and the composition of the gaseous substance determined in step 4, determine the thermal runaway gas generation sequence of the lithium-ion battery.
2. The analysis method according to claim 1, characterized in that: The process of determining the quality of the positive electrode material includes: punching holes in the disassembled positive electrode sheet to take samples, scraping off the positive electrode material on the obtained samples, and calculating the quality of the positive electrode material on the entire positive electrode sheet and the quality of the positive electrode current collector according to the quality of the positive electrode material on the samples.
3. The analysis method according to claim 2, characterized in that: The process of determining the mass of the negative electrode material includes: soaking the disassembled negative electrode sheet in water, drying the negative electrode current collector from which the negative electrode material is removed and weighing it, and subtracting the mass of the negative electrode current collector from the mass of the negative electrode sheet to obtain the mass of the negative electrode material.
4. The analysis method according to claim 3, characterized in that: The process of determining the mass of the electrolyte includes: cleaning the disassembled diaphragm with an organic solvent, and then drying and weighing the diaphragm in sequence to obtain the mass of the diaphragm; subtracting the mass of the positive electrode material, the positive electrode collector, the negative electrode material, the negative electrode collector and the diaphragm from the total mass of the disassembled battery cell to obtain the mass of the electrolyte; the battery cell includes a positive electrode sheet, a negative electrode sheet, a diaphragm and an electrolyte.
5. The analysis method according to claim 1, characterized in that: The mass of the test sample in step 2 does not exceed 10 mg.
6. The analysis method according to claim 1, characterized in that: In step 2, when the test sample is any one of the positive electrode material, the negative electrode material and the electrolyte, the sample preparation process of the positive electrode material or the negative electrode material, except for the electrolyte, includes: grinding the positive electrode material or the negative electrode material and placing it in an aluminum crucible, and using a tablet press to compact and seal the aluminum cover sheet and the aluminum crucible.
7. The analysis method according to claim 1, characterized in that: In step 2, when the test samples are positive electrode materials and negative electrode materials, the sample preparation process includes: mixing and grinding the positive electrode materials and the negative electrode materials, placing them in an aluminum crucible, and using a tablet press to compact and seal the aluminum cover sheet and the aluminum crucible.
8. The analysis method according to claim 1, characterized in that: In step 2, when the test sample is a positive electrode material and an electrolyte, or a negative electrode material and an electrolyte, the sample preparation process includes: grinding the positive electrode material or the negative electrode material, mixing it with the electrolyte, placing the resulting mixture in an aluminum crucible, and using a tablet press to compact and seal the aluminum cover sheet and the aluminum crucible.
9. The analysis method according to claim 1, characterized in that: When the test sample is a combination of positive electrode material, negative electrode material and electrolyte, the sample preparation process includes: mixing and grinding the positive electrode material and the negative electrode material, mixing them with the electrolyte, placing the obtained mixture in an aluminum crucible, and using a tablet press to compact and seal the aluminum cover sheet and the aluminum crucible.
10. The analysis method according to claim 1, characterized in that: The test conditions of the synchronous thermal analyzer test include: an initial temperature of 35° C., a final temperature of 600° C., a heating rate of 10 K / min, and a nitrogen atmosphere.