Electrostatic charge image developing toner, electrostatic charge image developer, and toner cartridge

By using core-shell structure toner masterbatches and hydrophobizing agent-modified inorganic particles in electrostatic image developer, the problems of poor storage and insufficient fluidity in the prior art are solved, and a higher image is achieved Quality and long-term preservation in multiple environments.

CN119087758APending Publication Date: 2024-12-06HUBEI DINGLONG CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411363663.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-28
Publication Date
2024-12-06

Smart Images

  • Figure BDA0005065548870000141
    Figure BDA0005065548870000141
Patent Text Reader

Abstract

The invention provides a toner for developing an electrostatic image, an electrostatic image developer and a toner cartridge, and relates to the technical field of toners. The electrostatic image developing toner includes a toner base particle having a core-shell structure composed of a core particle and a shell layer covering the core particle, the shell layer including a hydrophobizing treatment agent modified inorganic particle and a shell resin, the shell resin being a binder resin, the adhesive resin is a combination of high-molecular-weight amorphous adhesive resin, low-molecular-weight amorphous adhesive resin and crystalline resin; the external additive includes hydrophobizing treatment agent modified inorganic particles. According to the toner, the inorganic particles modified by the hydrophobization treatment agent are added into the toner, so that the toner has higher charge uniformity, and the requirement for higher image quality is met; meanwhile, the storage property and the flowability of the toner are improved, so that the toner is prevented from being influenced in a high-temperature and high-humidity environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of toners, and in particular to a toner for electrostatic image development, an electrostatic image developer and a toner box. Background Art

[0002] Methods for visualizing image information by electrostatic charge images, such as electrophotography, are currently being used in various fields. In electrophotography, an electrostatic charge image (electrostatic latent image) is formed on a photoreceptor (image holder) by charging and exposure, and the electrostatic latent image is visualized by developing it with a developer containing a toner, and then transferring and fixing the image. The developer used in this development process includes a two-component developer containing a toner and a carrier, and a single-component developer using a magnetic toner or a non-magnetic toner.

[0003] As the requirements for printing quality, speed and life of printers continue to increase, toners are required to have higher fluidity and charge uniformity to meet the demand for image quality. At the same time, toners are required to have higher preservation properties to achieve longer preservation of toners in a variety of environments. Summary of the invention

[0004] The present application provides a colorant for electrostatic image development, an electrostatic image developer and a colorant box. The colorant for electrostatic image development has stronger charge uniformity, preservation and fluidity, can meet the demand for higher image quality, and the colorant is less affected by high temperature and high humidity environments, so as to achieve longer preservation in a variety of environments.

[0005] In the first aspect, the present application provides a colorant for electrostatic image development, comprising a colorant masterbatch and an external additive, wherein the colorant masterbatch has a core-shell structure consisting of a core particle and a shell layer covering the core particle, wherein the shell layer comprises inorganic particles modified by a hydrophobic treatment agent and a shell resin, the shell resin is a binder resin, and the binder resin is a combination of a high molecular weight amorphous binder resin, a low molecular weight amorphous binder resin and a crystalline resin, the high molecular weight amorphous binder resin has a number average molecular weight between 10000-80000 g / mol, and the low molecular weight amorphous binder resin has a number average molecular weight between 1000-40000 g / mol; the external additive comprises the inorganic particles modified by the hydrophobic treatment agent.

[0006] In the above technical scheme, inorganic particles are modified by a hydrophobic treatment agent to obtain modified inorganic particles having excellent thermal stability and the ability to inhibit spatial charge accumulation, and the inorganic particles modified by the hydrophobic treatment agent are doped into the shell resin to form the shell layer of the colorant masterbatch. At the same time, the inorganic particles modified by the hydrophobic treatment agent are used as external additives to give the colorant good charge uniformity, fluidity and preservation properties, thereby being able to meet higher image quality requirements, and avoiding the toner from being affected by high temperature and high humidity environments, thereby achieving longer preservation of the toner in a variety of environments.

[0007] In some possible implementations, the inorganic particles are selected from one or more of silicon dioxide, titanium dioxide, aluminum oxide, copper oxide, zinc oxide, iron oxide, magnesium oxide, tin oxide, and cerium oxide.

[0008] In some possible implementations, the inorganic particles are magnesium oxide, and the particle size of the magnesium oxide is between 5-100 nm.

[0009] In some possible implementations, the hydrophobic treatment agent is selected from one or more of a fluorine-containing silane coupling agent, a titanate coupling agent, and an aluminum coupling agent.

[0010] In some possible implementations, the hydrophobic treatment agent is a fluorine-containing silane coupling agent, and the fluorine-containing silane coupling agent is selected from one or more of perfluorodecyltriethoxysilane, perfluorooctyltriethoxysilane, difluoromethyltrimethylsilane, trifluoromethyltrimethylsilane, and triethyltrifluoromethylsilane.

[0011] In some possible implementations, the inorganic particles are magnesium oxide, and the hydrophobic treatment agent is perfluorooctyltriethoxysilane.

[0012] In some possible implementations, the sphericity of the toner master particles is greater than 0.98, and the particle size of the toner master particles is between 1 μm and 20 μm.

[0013] In some possible embodiments, the colorant also includes a charge control agent, which is uniformly dispersed in the binder resin, and the charge control agent is selected from one or more of azo dyes, salicylic acid metal complexes, aniline black dyes, quaternary ammonium salts, triphenylmethane control agents and oil black, cyclohexane acid, salicylic acid, octanoic acid and its metal salts, and alkyl salicylic acid metal chelates.

[0014] In a second aspect, the present application provides an electrostatic image developer, comprising a carrier and the electrostatic image developing colorant described in any one embodiment of the first aspect.

[0015] In a third aspect, the present application provides a toner cartridge that contains the toner for developing an electrostatic image as described in any one of the embodiments of the first aspect and is detachable from an imaging device. DETAILED DESCRIPTION

[0016] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0017] It should be noted that the following embodiments are examples of the present application and are only used to illustrate the present application, but not to limit the present application. Other combinations and various improvements within the concept of the present application may be made without departing from the subject matter or scope of the present application.

[0018] The electrostatic image developing toner, electrostatic image developer and toner cartridge provided in the present application are described in detail below.

[0019] The colorant for developing electrostatic images in an embodiment of the present application (hereinafter referred to as "colorant") includes a colorant masterbatch and an external additive, the colorant masterbatch has a core-shell structure consisting of a core particle and a shell layer covering the core particle, wherein the shell layer includes inorganic particles modified by a hydrophobic treatment agent and a shell resin, the core particles include a core resin, a colorant and a release agent, and the external additive includes inorganic particles modified by a hydrophobic treatment agent.

[0020] The present application uses a hydrophobic treatment agent to modify inorganic particles to obtain modified inorganic particles having excellent thermal stability and space charge accumulation inhibition performance. The inorganic particles modified by the hydrophobic treatment agent are doped into a shell resin to form a shell layer of a toner masterbatch. At the same time, the inorganic particles modified by the hydrophobic treatment agent are used as an external additive to provide a toner. The toner has good charge uniformity, fluidity and preservation, so that the toner can meet the requirements of higher image quality, and avoids the toner being affected in a high temperature and high humidity environment, so as to achieve a longer preservation of the toner in a more diverse environment.

[0021] Each component will be described below in sequence.

[0022] <Binder Resin>

[0023] The shell resin and the core resin are independent of each other and are binder resins. The number average molecular weight of the binder resin is

[0024] 1000-80000 g / mol, preferably, in the range of 10000-50000 g / mol. Examples of binder resins include, but are not limited to, styrene resins, acrylic resins, vinyl resins or polyolefin resins, polyether-based polyol resins, phenolic resins, silicone resins, polyester resins, epoxy resins, polyimide resins, polyurethane resins, polybutadiene resins, and the binder resin can be selected from one or more of the above resins.

[0025] Preferably, the binder resin is a polyester resin. Polyester resins can be prepared by direct esterification or transesterification between aliphatic, alicyclic or aromatic polycarboxylic acids or their alkyl esters and polyols. Examples of polycarboxylic acids may include isophthalic acid, phthalic acid, terephthalic acid, chlorophthalic acid, tetrachlorophthalic acid, nitrophthalic acid, p-carboxyphenylacetic acid, isophthalic acid, terephthalic acid, phthalic acid, diphenylacetic acid. In addition to dicarboxylic acids, polycarboxylic acids such as trimellitic acid, pyromellitic acid, naphthalenetricarboxylic acid, naphthalenetetracarboxylic acid, pyrenetricarboxylic acid, and pyrenetetracarboxylic acid may also be used; carboxyl groups may also be used to react to form carboxylic acid derivatives of anhydrides, chlorinated oxides or ester groups, such as terephthalic acid or its low esters, diphenylacetic acid, cyclohexanedicarboxylic acid, etc. Examples of polyols may include aromatic diols, aliphatic diols, and alicyclic diols. The polyol may be selected from one or more of ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol glycerol, cyclohexanediol, cyclohexanedimethanol or hydrogen. In addition, polyols having three or more -OH groups, such as glycerol, trimethylolpropane or pentaerythritol, may also be used, which may be used together with the diol to have a cross-linked structure or a branched structure to increase the fixability or fusibility of the toner.

[0026] The binder resin is a combination of a high molecular weight amorphous binder resin, a low molecular weight amorphous binder resin and a crystalline resin. The number average molecular weight of the high molecular weight amorphous binder resin is between 10000-80000 g / mol, and the number average molecular weight of the low molecular weight amorphous binder resin is between 1000-40000 g / mol.

[0027] In some possible embodiments, the proportion of high molecular weight amorphous binder resin is between 30-50wt%, preferably between 40-45wt%; the proportion of low molecular weight amorphous binder resin is between 20-40wt%, preferably between 30-35wt%; the proportion of crystalline resin is between 1-25wt%, preferably between 5-10wt%. Two binder resins with different molecular weights can have independent functions. The low molecular weight binder resin has very few molecular chain entanglements, so it can help improve the solubility and gloss of the toner; the high molecular weight binder resin has a certain degree of elasticity even at high temperatures due to many molecular chain entanglements, which helps to improve the mechanical properties of the toner. Therefore, by adjusting the ratio between the high molecular weight amorphous binder resin, the low molecular weight amorphous binder resin and the crystalline resin, the performance of the toner can be adjusted, so that the toner can meet more diverse application scenarios.

[0028] <Colorant>

[0029] The colorant may be a pigment, and the pigment may be selected from one or more of a black pigment, a magenta pigment, a yellow pigment, and a cyan pigment.

[0030] Among them, the black pigment can be carbon black, aniline black or any mixture thereof. The magenta pigment can be a condensed nitrogen compound, anthraquinone compound, quinacridone compound, basic dye lake, naphthol compound, benzimidazole compound, thioindigo compound, perylene compound, or any mixture thereof. The yellow pigment can be a condensed nitrogen compound, isoindole compound, anthraquinone compound, azo metal complex, allyl imide compound or any mixture thereof. The cyan pigment can be a copper phthalocyanine compound or its derivative, anthraquinone compound, basic dye lake or any mixture thereof.

[0031] <Release Agent>

[0032] The melting point of the release agent is 50-150° C. Examples of the release agent include, but are not limited to, polyethylene wax, polypropylene wax, silicone wax, paraffin wax, microcrystalline wax, carnauba wax, rice bran wax, candelilla wax, beeswax, montan wax, ozokerite wax, and Fischer-Tropsch wax, and the release agent is selected from one or more of the above waxes.

[0033] The amount of the release agent contained in the core particles may be 1-20 parts by weight based on 100 parts by weight of the core particles, and preferably, 5-10 parts by weight. The release agent can prevent the toner particles from adhering to the heating roller of the fixing device.

[0034] <Charge Control Agent>

[0035] In some possible implementations, the toner masterbatch further includes a charge control agent, and the charge control agent is uniformly dispersed in the binder resin. It is understandable that the toner masterbatch may not include the charge control agent, or may include the charge control agent; when the toner masterbatch includes the charge control agent, the charge control agent may be uniformly dispersed in the core resin, may be uniformly dispersed in the shell resin, or may be uniformly dispersed in both the core resin and the shell resin.

[0036] The charge control agent is selected from one or more of azo dyes, salicylic acid metal complexes, nigrosine dyes, quaternary ammonium salts, triphenylmethane control agents and oil black, cyclohexane acid, salicylic acid, octanoic acid and its metal salts, and alkyl salicylic acid metal chelates. Among them, the metal salts of octanoic acid can include manganese salts, cobalt salts, iron salts, zinc salts, aluminum salts, and lead salts.

[0037] Preferably, the charge control agent is a salicylic acid metal complex, including but not limited to magnesium salicylate, zinc salicylate, calcium salicylate, iron salicylate, etc. More preferably, the charge control agent is zinc salicylate.

[0038] <Curing Agent>

[0039] Examples of curing agents include compounds containing active hydrogen groups, examples of which include hydroxyl, amino, carboxyl and mercapto groups. These active hydrogen groups can be used alone or in combination. Preferably, they are amines, more preferably diamines, trivalent or higher amines, amino alcohols, amino mercaptan, amino acids, and compounds in which the amino groups in the above-listed amines are blocked.

[0040] <Accelerator>

[0041] Examples of promoters include metal salts, organic compounds and mixtures of two or more thereof, such as vanadium octoate, cobalt naphthalene dicarboxylate, iron octoate, manganese naphthalene dicarboxylate, dimethylaniline and mixtures thereof. Preferably, the peroxy promoter compound is a metal salt, more preferably vanadium octoate.

[0042] <Inorganic particles modified with a hydrophobic treatment agent>

[0043] The inorganic particles are selected from one or more of silicon dioxide, titanium dioxide, aluminum oxide, copper oxide, zinc oxide, iron oxide, magnesium oxide, tin oxide, and cerium oxide. Preferably, the inorganic particles are magnesium oxide. The particle size of magnesium oxide is between 5-100 nm, preferably between 10-50 nm, and more preferably between 15-30 nm, which is conducive to avoiding the magnesium oxide particles being too small to be buried in the toner masterbatch, resulting in the magnesium oxide particles being unable to function, and also avoiding the magnesium oxide particles being too large to affect the quality of the electrostatic charge image.

[0044] The hydrophobic treatment agent is selected from one or more of a fluorinated silane coupling agent, a titanate coupling agent, and an aluminum coupling agent, for example, vinyl triethoxysilane, perfluorodecyl triethoxysilane, perfluorooctyl triethoxysilane, difluoromethyl trimethyl silane, trifluoromethyl trimethyl silane, triethyl trifluoromethyl silane, dioctyl pyrophosphate acyloxy titanate, distearoyloxy isopropoxy aluminate, etc. Preferably, the fluorinated polymer is a fluorinated silane coupling agent, and the fluorinated silane coupling agent is selected from one or more of perfluorodecyl triethoxy silane, perfluorooctyl triethoxy silane, difluoromethyl trimethyl silane, trifluoromethyl trimethyl silane, and triethyl trifluoromethyl silane.

[0045] Since nano magnesium oxide has the advantages of high thermal conductivity, excellent thermal stability and inhibition of space charge accumulation, a material with a rough structure and low surface energy is obtained by hybridizing fluorine-containing polymers and magnesium oxide to achieve hydrophobic surface construction of inorganic particles. The present application makes the toner have stronger charge uniformity by doping the modified magnesium oxide into the shell resin to meet the demand for higher image quality; at the same time, the preservation and fluidity of the toner are improved, thereby avoiding the toner being affected by high temperature and high humidity environments, and obtaining a toner that can be stored longer in more diverse environments.

[0046] <External Additives>

[0047] The external additive includes the inorganic particles modified by the hydrophobic treatment agent. The proportion of the external additive in the toner is 0.01-10wt%, preferably 0.1-8wt%, and more preferably 0.5-3wt%. By making the proportion of the external additive in the toner above 0.01wt%, it is possible to avoid the increase of flying powder in the printing process due to the low charge of the toner; by making the proportion of the external additive in the toner below 10wt%, it is possible to avoid the accumulation of the toner due to the excessive charge of the toner and the impact on the image quality.

[0048] <Method for producing toner>

[0049] There is no particular limitation on the method for producing the toner masterbatch, and known methods such as the kneading and pulverization method and the wet production method can be used. The preferred method is the emulsification coagulation method, and the toner masterbatch obtained by the emulsification coagulation method has a uniform particle size, a controllable shape, and a core-shell structure. The emulsification coagulation method refers to a method of mixing a dispersion of binder resin particles dispersed by a surfactant and a dispersion of colorant particles used as needed, agglomerating them to form core particles of the toner, and further coating the binder resin particles outside the core particles to control the shape, thereby producing the toner masterbatch.

[0050] The binder resin dispersion contains a crystalline resin and an amorphous resin. According to the properties of the binder resin particles, the binder resin particles can be dispersed into a binder resin dispersion by a phase inversion emulsification method and a direct emulsification method, preferably a phase inversion emulsification method. The phase inversion emulsification method includes but is not limited to the following steps: dissolving the crystalline resin and the amorphous resin in a hydrophobic organic solvent capable of dissolving the resin, and continuously adding a certain amount of alkaline substances and hydrophobic organic solvents, and then adding a large amount of aqueous phase substances to convert the dispersion from W / O to O / W, and the continuous phase is converted to an aqueous phase substance. The volume average particle size of the dispersed binder resin particles in the binder resin dispersion is between 0.01-20 μm; preferably, between 0.05-10 μm; more preferably, between 0.3-5 μm; further preferably, between 0.5-2 μm.

[0051] In addition to the binder resin dispersion, a mixed particle dispersion of dispersed colorant particles and release agent particles is also required. The mixed particle dispersion of colorant particles and release agent particles can be dispersed by phase inversion emulsification and direct emulsification, preferably direct emulsification. The direct emulsification method is to directly add the colorant and release agent combination into deionized water, add a dispersion stabilizer, and obtain a mixed particle dispersion by mechanical stirring or the like. The average particle size of the mixed particle dispersion can be between 0.01-10 μm; preferably between 0.1-1 μm; more preferably between 0.3-0.8 μm.

[0052] The binder resin dispersion and the mixed particle dispersion can be dispersed separately or mixed, preferably mixed. The binder resin particle dispersion and the mixed particle dispersion are mixed with deionized water, and a coagulant is added to the mixed solution. The pH of the mixed solution is adjusted to an acidic value, such as pH 1-6, preferably pH 2-3, and a dispersion stabilizer is added if necessary. Then, the particles dispersed in the mixed solution are agglomerated by heating the mixed solution to a glass transition temperature close to the resin particles, thereby forming core particles. A resin dispersion containing modified nano magnesium oxide is further added to obtain a toner masterbatch.

[0053] The coagulants used in the present application include surfactants, inorganic metal salts, and metal complexes with a valence of more than 2 and polymers thereof, wherein the polarity of the surfactant is opposite to the polarity of the dispersion stabilizer contained in the mixed particle dispersion. Examples of coagulants may be magnesium chloride, calcium chloride, barium chloride, zinc chloride, aluminum chloride, aluminum sulfate, polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. The coagulant is preferably an inorganic metal salt, and more preferably calcium chloride. If necessary, the coagulant may be used together with a chelating agent, and the chelating agent may include citric acid, gluconic acid, iminodiacetic acid, ethylenediaminetetraacetic acid, and nitrilotriacetic acid. The amount of coagulant added is 0.01-0.8wt% of the toner masterbatch, preferably 0.05-0.4wt%, and more preferably 0.1-0.2wt%. If necessary, the amount of chelating agent added is 0.02-1.5wt% of the toner masterbatch, preferably 0.1-1.0wt%, and more preferably 2.0-5.0wt%.

[0054] The dispersion stabilizer and surfactant used in the present application are independently anionic surfactants and nonionic surfactants. Among them, the anionic surfactant is selected from one or more of alkyl aryl sulfonates, alkyl sulfates, alkyl ether sulfates, alkyl carboxylates, and alkyl alkoxylated carboxylates. For example, sodium dodecyl sulfate, sodium tetradecyl sulfate, sodium pentadecyl sulfate, sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium α-olefin sulfonate, sodium secondary alkyl sulfonate, lauryl alcohol ether phosphate, isooctyl alcohol phosphate, etc. The anionic surfactant is preferably an alkyl sulfate, more preferably sodium tetradecyl sulfate. The nonionic surfactant is selected from one or more of polyoxyethylene hexadecyl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene stearyl ether, nonylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, alkanolamide, polyoxyethylene alkanolamide alkyl ethoxylate, and alkyl propoxylate. Preferably, the nonionic surfactant is polyoxyethylene hexadecyl ether.

[0055] After the toner masterbatch is obtained, the toner masterbatch is washed, solid-liquid separated, and dried. The washing method is washing with deionized water. The solid-liquid separation method can be by suction filtration, natural sedimentation, etc., preferably suction filtration. The drying method can be selected from normal temperature drying and low temperature drying, preferably low temperature drying.

[0056] After the toner masterbatch is obtained, an external additive is added to the toner masterbatch and mixed to prepare a finished product. The mixing can be performed by, for example, a V-blender, a Henschel mixer, or a Lodige mixer, preferably a Henschel mixer. In addition, if necessary, large toner masterbatch can be removed by using a vibrating sifter or a wind sifter, preferably a vibrating sifter.

[0057] In some possible implementations, the particle sphericity of the toner master particles reaches 0.98 or more, preferably 0.99 or more, and more preferably between 0.990 and 0.995. By making the particle sphericity of the toner master particles above 0.98, the shape of the toner master particles is more regular, which is beneficial to improve the glossiness of the toner, thereby improving the image quality; by making the particle sphericity of the toner master particles below 0.995, the shape of the toner master particles is avoided from being too regular, thereby avoiding the difficulty in scraping off the remaining toner powder after transfer, thereby ensuring the image quality.

[0058] In some possible implementations, the particle size of the toner master particle is between 1-20 μm, preferably between 10-15 μm. By making the particle size of the toner master particle larger than 1 μm, it is avoided that the toner master particle is too small and causes too high a waste powder rate; by making the particle size of the toner master particle smaller than 20 μm, the toner master particle is smaller, which is conducive to improving the image resolution.

[0059] <Electrostatic Image Developer>

[0060] The electrostatic image developer of the exemplary embodiment includes at least the toner of the exemplary embodiment described above. The electrostatic image developer of this exemplary embodiment may be a single-component developer including only the toner of the exemplary embodiment described above, or may be a two-component developer including a mixture of the toner and a carrier.

[0061] There is no particular limitation on the carrier, and a known carrier can be used. Examples of the carrier include: a coated carrier prepared by coating the surface of a core material formed of magnetic powder with a resin; a magnetic powder dispersion carrier, which is formed by dispersing magnetic powder in a matrix resin; and a resin impregnated carrier, which is formed by impregnating a porous magnetic powder with a resin. In each of the magnetic powder dispersion carrier and the resin impregnated carrier, the particles contained in the carrier can be used as cores, and their surfaces can be coated with a resin.

[0062] <Toner Cartridge>

[0063] The toner cartridge of the present embodiment is a toner cartridge that contains the toner of the present embodiment and is detachable from the image forming apparatus. The toner cartridge contains replenishment toner to be supplied to a developing device provided in the image forming apparatus.

[0064] <Example>

[0065] The present embodiment is specifically described below by way of examples, but the present embodiment is not limited thereto. The evaluation methods of the examples and comparative examples are as follows:

[0066] The particle size, peak width and sphericity of the toner were analyzed using a Mastersizer laser particle size analyzer.

[0067] 10 g of colorant is placed in an open round container and placed in a 50°C, 60% humidity environment for 72 hours to observe whether the colorant has lumps. If there are no lumps, the toner has excellent shelf life. If there are lumps but there is no obvious effect on the printing results, the shelf life is good. If there are lumps and there is a significant effect on the printing results, the shelf life is poor.

[0068] The image quality was evaluated using a modified machine of Docu Centre IV C5575 (manufactured by Fuji Xerox Co., Ltd.) and a modified machine of Color1000Press (manufactured by Fuji Xerox Co., Ltd.), and the print quality was evaluated according to the relevant requirements of GB / T21199-2007. Excellent means that the image density is ≥1.35, the bottom gray is ≤0.01, the level is ≥10, the fixing fastness is ≥90%, the density unevenness is ≤10%, and there is no image abnormality; good means that there are some problems with the image, but there is no obvious problem with the image; poor means that the image density is ≤1.35, or the bottom gray is ≥0.01, or the level is ≤10, or the fixing fastness is ≤90%, or the density unevenness is ≥10%, or there is an image abnormality.

[0069] Example 1

[0070] Take 10 parts of magnesium oxide powder (inorganic particles) and add them to 150 parts of anhydrous ethanol, and add vinyl triethoxy silane (silane coupling agent) at a mass ratio of 10:1, stir magnetically for 5 hours, then centrifuge the obtained solution at 8000r / min for 5 minutes, take the lower precipitate, add anhydrous ethanol and stir evenly, and repeat the centrifugation operation 4 times to remove excess vinyl triethoxy silane. The last precipitate obtained is placed in a vacuum environment at 60°C for 72 hours and dried to obtain modified nano magnesium oxide 1.

[0071] 10 parts of modified nano magnesium oxide 1 were added to 50 parts of acetone for ultrasonic dispersion for 30 minutes, and then added to 100 parts of polystyrene resin (high molecular weight amorphous resin with a molecular weight of 65,000: low molecular weight amorphous resin with a molecular weight of 10,000: crystalline resin = 50:25:25) (shell resin), and mechanically stirred at 800 r / min in an 80°C oil bath until the acetone was completely volatilized, and then the curing agent and the accelerator were added in a ratio of 100:50:1 to the mass ratio of polystyrene resin (shell resin), curing agent, and accelerator, and mechanically stirred at 800 r / min for 30 minutes to mix the resin composite system evenly, poured into a vacuum bottle, evacuated for 1 hour, and then heated at 120°C for 2 hours to complete curing. The resin composite material 1 doped with modified nano magnesium oxide 1 was obtained. And the toner S1 was obtained by this.

[0072] Example 2

[0073] Take 30 parts of magnesium oxide powder (inorganic particles) and add them to 100 parts of anhydrous ethanol, and add perfluorodecyl triethoxysilane (silane coupling agent) at a mass ratio of 10:3, stir magnetically for 3 hours, then centrifuge the obtained solution at 6000r / min for 10 minutes, take the lower precipitate, add anhydrous ethanol and stir evenly, and repeat the centrifugation operation 3 times to remove excess perfluorodecyl triethoxysilane. The last precipitate obtained is placed in a vacuum environment at 60°C and dried for 72 hours to obtain modified nano magnesium oxide 2.

[0074] 20 parts of modified nano magnesium oxide 2 were added to 50 parts of butanone for ultrasonic dispersion for 30 minutes, and then added to 50 parts of polyester resin (high molecular weight amorphous resin with a molecular weight of 70,000: low molecular weight amorphous resin with a molecular weight of 10,000: crystalline resin = 55:40:5) (shell resin), and mechanically stirred at 500 r / min in a 60°C oil bath until the butanone was completely volatilized, and then the curing agent and the accelerator were added in a ratio of 100:80:2 to the mass ratio of polyester resin (shell resin), curing agent, and accelerator, and mechanically stirred at 500 r / min for 40 minutes to mix the resin composite system evenly, poured into a vacuum bottle and vacuumed for 0.5 hours, and then heated at 130°C for 1.5 hours to complete curing. The resin composite material 2 doped with modified nano magnesium oxide 2 was obtained. And the toner S2 was obtained by this.

[0075] Example 3

[0076] Take 50 parts of magnesium oxide powder (inorganic particles) and add them to 100 parts of anhydrous ethanol, and add perfluorooctyl triethoxysilane (silane coupling agent) at a mass ratio of 10:5, stir magnetically for 4 hours, then centrifuge the obtained solution at 6000r / min for 20 minutes, take the lower precipitate, add anhydrous ethanol and stir evenly, and repeat the centrifugation operation 5 times to remove excess perfluorooctyl triethoxysilane. The last precipitate obtained is placed in a vacuum environment at 60°C for 72 hours and dried to obtain modified nano magnesium oxide 3.

[0077] 30 parts of modified nano magnesium oxide 3 were added to 100 parts of butanone for ultrasonic dispersion for 20 minutes, and then added to 150 parts of polyester resin (high molecular weight amorphous resin with a molecular weight of 65,000: low molecular weight amorphous resin with a molecular weight of 5,000: crystalline resin = 35:40:25) (shell resin), and mechanically stirred at 800 r / min in a 70°C oil bath until the butanone was completely volatilized, and then the curing agent and the accelerator were added in a ratio of 80:60:2 to the mass ratio of polyester resin (shell resin), curing agent, and accelerator, and mechanically stirred at 800 r / min for 20 minutes to mix the resin composite system evenly, poured into a vacuum bottle, vacuumed for 1.5 hours, and then heated at 110°C for 2.5 hours to complete curing. The resin composite material 3 doped with modified nano magnesium oxide 3 was obtained. And the toner S3 was obtained by this.

[0078] Example 4

[0079] Take 20 parts of magnesium oxide powder (inorganic particles) and add them to 130 parts of anhydrous ethanol, and add difluoromethyltrimethylsilane (silane coupling agent) at a mass ratio of 10:2, stir magnetically for 1 hour, then centrifuge the obtained solution at 4000r / min for 15 minutes, take the lower precipitate, add anhydrous ethanol and stir evenly, and repeat the centrifugation operation 4 times to remove excess difluoromethyltrimethylsilane. The last precipitate obtained is placed in a vacuum environment at 80°C for 72 hours and dried to obtain modified nano magnesium oxide 4.

[0080] 20 parts of modified nano magnesium oxide 4 were added to 80 parts of acetone for ultrasonic dispersion for 30 minutes, and then added to 100 parts of mixed resin (polystyrene resin: polyester resin = 70:30, polystyrene resin is the same as in Example 1, and polyester resin is the same as in Example 2) (shell resin), and mechanically stirred at 700 r / min in an 80°C oil bath until the acetone was completely volatilized, and then the curing agent and the accelerator were added in a ratio of 80:30:1 to the mixed resin (shell resin), curing agent, and accelerator, and mechanically stirred at 700 r / min for 20 minutes to mix the resin composite system evenly, poured into a vacuum bottle, vacuumed for 1.5 hours, and then heated at 120°C for 2 hours to complete curing. The resin composite material 4 doped with modified nano magnesium oxide 4 was obtained. And the toner S4 was obtained by this.

[0081] Example 5

[0082] Take 50 parts of magnesium oxide powder (inorganic particles) and add them to 180 parts of anhydrous ethanol, and add trifluoromethyltrimethylsilane (silane coupling agent) at a mass ratio of 10:4, stir magnetically for 1.5 hours, then centrifuge the obtained solution at 6000r / min for 10 minutes, take the lower precipitate, add anhydrous ethanol and stir evenly, and repeat the centrifugation operation 3 times to remove excess trifluoromethyltrimethylsilane. The last precipitate obtained is placed in a vacuum environment at 60°C for 72 hours and dried to obtain modified nano magnesium oxide 5.

[0083] 10 parts of modified nano magnesium oxide 5 were added to 50 parts of acetone for ultrasonic dispersion for 30 minutes, and then added to 80 parts of polyester resin (high molecular weight amorphous resin with a molecular weight of 55,000: low molecular weight amorphous resin with a molecular weight of 8,000: crystalline resin = 50:40:10) (shell resin), and mechanically stirred at 800 r / min in an 80°C oil bath until the acetone was completely volatilized, and then the curing agent and the accelerator were added in a ratio of 130:50:2 to the mass ratio of polyester resin (shell resin), curing agent, and accelerator, and mechanically stirred at 800 r / min for 30 minutes to mix the resin composite system evenly, poured into a vacuum bottle and vacuumed for 1 hour, and then heated at 120°C for 2 hours to complete curing. The resin composite material 5 doped with modified nano magnesium oxide 5 was obtained. And the toner S5 was obtained by this.

[0084] Example 6

[0085] Take 50 parts of silica powder (inorganic particles) and add them to 180 parts of anhydrous ethanol, and add trifluoromethyltrimethylsilane (silane coupling agent) at a mass ratio of 10:2. Stir magnetically for 5 hours, then centrifuge the resulting solution at 8000r / min for 20 minutes, remove the lower precipitate, add anhydrous ethanol and stir evenly, and repeat the centrifugation operation 3 times to remove excess trifluoromethyltrimethylsilane. The last precipitate obtained is placed in a 60°C vacuum environment for 72 hours to dry, and modified nano-silica is obtained.

[0086] 15 parts of modified nano-silica were added to 60 parts of acetone for ultrasonic dispersion for 60 minutes, and then added to 130 parts of polyester resin (high molecular weight amorphous resin with a molecular weight of 65,000: low molecular weight amorphous resin with a molecular weight of 15,000: crystalline resin = 50:35:15) (shell resin), and mechanically stirred at 1000 r / min in an 85°C oil bath until the acetone was completely volatilized, and then the curing agent and the accelerator were added in a ratio of 130:40:4 to the polyester resin (shell resin), curing agent, and accelerator, and mechanically stirred at 800 r / min for 30 minutes to mix the resin composite system evenly, poured into a vacuum bottle, evacuated for 1.25 hours, and then heated at 120°C for 2.25 hours to complete curing. The modified nano-silica doped resin composite material 6 was obtained. And the toner S6 was obtained by this.

[0087] Example 7

[0088] Take 30 parts of magnesium oxide powder (inorganic particles) and add them to 140 parts of anhydrous ethanol, and add dioctyl pyrophosphate titanate (silane coupling agent) at a mass ratio of 20:3. Stir magnetically for 2 hours, then centrifuge the resulting solution at 6000r / min for 40 minutes, take the lower precipitate, add anhydrous ethanol and stir evenly, and repeat the centrifugation operation 3 times to remove excess dioctyl pyrophosphate titanate. The last precipitate obtained was placed in a 60°C vacuum environment and dried for 72 hours to obtain modified nano magnesium oxide 6.

[0089] According to the method of Example 3, the modified nano-magnesium oxide 6 doped resin composite material 7 is obtained, and the toner S7 is obtained therefrom.

[0090] Example 8

[0091] Take 18 parts of magnesium oxide powder (inorganic particles) and add them to 100 parts of anhydrous ethanol, and add distearoyloxyisopropoxyaluminate (silane coupling agent) at a mass ratio of 20:7. Stir magnetically for 1 hour, then centrifuge the resulting solution at 6000r / min for 30 minutes, take the lower precipitate, add anhydrous ethanol and stir evenly, and repeat the centrifugation operation 3 times to remove excess distearoyloxyisopropoxyaluminate. The last precipitate obtained was placed in a vacuum environment at 60°C for 72 hours and dried to obtain modified nano magnesium oxide 7.

[0092] According to the method of Example 3, the modified nano magnesium oxide 7 doped resin composite material 8 is obtained, and the toner S8 is obtained therefrom.

[0093] Example 9

[0094] According to Example 1, modified nano magnesium oxide 1 was obtained.

[0095] 10 parts of modified nano magnesium oxide 1 and 0.5 parts of zinc salicylate (charge control agent) were added to 50 parts of acetone for ultrasonic dispersion for 30 minutes, and then added to 100 parts of polystyrene resin (shell resin, the same as Example 1), and mechanically stirred at 800 r / min in an 80°C oil bath until the acetone was completely volatilized, and then the curing agent and the accelerator were added in a ratio of 100:50:1 of the mass ratio of polystyrene resin (shell resin), curing agent, and accelerator, and mechanically stirred at 800 r / min for 30 minutes to mix the resin composite system evenly, poured into a vacuum bottle, evacuated for 1 hour, and then heated at 120°C for 2 hours to complete curing. The modified nano magnesium oxide 1 doped resin composite material 9 was obtained. And the toner S9 was obtained by this.

[0096] Comparative Example 1

[0097] Toner D1 was obtained according to the method of Example 3 using unmodified magnesium oxide particles (inorganic particles) and polyester resin (shell resin).

[0098] Comparative Example 2

[0099] Toner D2 was obtained according to the method of Example 3 using unmodified silica particles (inorganic particles) and polyester resin (shell resin).

[0100] Comparative Example 3

[0101] According to Example 3, modified nano magnesium oxide particles 3 are obtained.

[0102] 30 parts of modified nano magnesium oxide 3 were added to 100 parts of butanone for ultrasonic dispersion for 20 minutes, and then added to 150 parts of polyester resin (high molecular weight amorphous resin with a molecular weight of 70,000: low molecular weight amorphous resin with a molecular weight of 10,000 = 55:45) (shell resin), and mechanically stirred at 800 r / min in a 70°C oil bath until the butanone was completely volatilized, and then the curing agent and the accelerator were added in a ratio of 80:60:2 to the mass ratio of polyester resin (shell resin), curing agent, and accelerator, and mechanically stirred at 800 r / min for 20 minutes to mix the resin composite system evenly, poured into a vacuum bottle, vacuumed for 1.5 hours, and then heated at 110°C for 2.5 hours to complete curing. The resin composite material doped with modified magnesium oxide 3 was obtained, and the toner D3 was obtained by this.

[0103] Comparative Example 4

[0104] According to Example 3, modified nano magnesium oxide particles 3 are obtained.

[0105] 30 parts of modified nano magnesium oxide 3 were added to 100 parts of butanone for ultrasonic dispersion for 20 minutes, and then added to 150 parts of polyester resin (molecular weight 65000 high molecular weight amorphous resin: crystalline resin = 60:40) (shell resin), and mechanically stirred at 800r / min in a 70°C oil bath until the butanone was completely volatilized, and then the curing agent and the accelerator were added in a ratio of 80:60:2 to the mass ratio of polyester resin (shell resin), curing agent, and accelerator, and mechanically stirred at 800r / min for 20 minutes to mix the resin composite system evenly, poured into a vacuum bottle, vacuumed for 1.5 hours, and then heated at 110°C for 2.5 hours to complete curing. The resin composite material doped with modified magnesium oxide 3 was obtained, and the toner D4 was obtained from it.

[0106] Examples 1-9 and Comparative Examples 1-4 were evaluated using the above evaluation method. The results are shown in Table 1.

[0107] Table 1 Evaluation results of Examples 1-9 and Comparative Examples 1-4

[0108]

[0109] As can be seen from Table 1, among Examples 1-9, Examples 2-5 and Example 9 are preferred. The toners in the above Examples have good storage properties, and the image quality is excellent both initially and during use.

[0110] Although the implementation scheme of the present application has been disclosed as above, it is not limited to the applications listed in the specification and implementation scheme. It can be fully applicable to various fields suitable for the present application. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present application is not limited to the specific details and the implementation schemes shown and described herein.

Claims

1. A toner for electrostatic image development, characterized in that: A toner mother particle and an external additive, wherein the toner mother particle has a core-shell structure consisting of a core particle and a shell layer covering the core particle, Wherein, the shell layer comprises inorganic particles modified by a hydrophobizing agent and a shell resin, the shell resin is a binder resin, and the binder resin is a combination of a high molecular weight amorphous binder resin, a low molecular weight amorphous binder resin and a crystalline resin, the number average molecular weight of the high molecular weight amorphous binder resin is between 10000-80000 g / mol, and the number average molecular weight of the low molecular weight amorphous binder resin is between 1000-40000 g / mol; The external additive includes inorganic particles modified by the hydrophobizing agent.

2. The electrostatic image developing toner according to claim 1, wherein The inorganic particles are selected from one or more of silicon dioxide, titanium dioxide, aluminum oxide, copper oxide, zinc oxide, iron oxide, magnesium oxide, tin oxide, and cerium oxide.

3. The electrostatic image developing toner according to claim 2, wherein: The inorganic particles are magnesium oxide, and the particle size of the magnesium oxide is between 5-100 nm.

4. The electrostatic image developing toner according to claim 1, wherein The hydrophobic treatment agent is selected from one or more of a fluorine-containing silane coupling agent, a titanate coupling agent and an aluminum coupling agent.

5. The electrostatic image developing toner according to claim 4, wherein The hydrophobic treatment agent is a fluorine-containing silane coupling agent, and the fluorine-containing silane coupling agent is selected from one or more of perfluorodecyltriethoxysilane, perfluorooctyltriethoxysilane, difluoromethyltrimethylsilane, trifluoromethyltrimethylsilane, and triethyltrifluoromethylsilane.

6. The electrostatic image developing toner according to any one of claims 1 to 5, characterized in that The inorganic particles are magnesium oxide, and the hydrophobic treatment agent is perfluorooctyltriethoxysilane.

7. The electrostatic image developing toner according to any one of claims 1 to 5, characterized in that: The particle sphericity of the toner master particle reaches above 0.98, and the particle size of the toner master particle is between 1 μm and 20 μm.

8. The electrostatic image developing toner according to any one of claims 1 to 5, characterized in that: The colorant also includes a charge control agent, which is uniformly dispersed in the binder resin. The charge control agent is selected from one or more of azo dyes, salicylic acid metal complexes, aniline black dyes, quaternary ammonium salts, triphenylmethane control agents and oil black, cyclohexane acid, salicylic acid, octanoic acid and its metal salts, and alkyl salicylic acid metal chelates.

9. An electrostatic image developer, characterized in that: The invention comprises a carrier and the toner for developing an electrostatic image according to any one of claims 1 to 8.

10. A toner cartridge, characterized in that: The toner for developing an electrostatic image according to any one of claims 1 to 8 is accommodated and can be detached from an image forming apparatus.