Positive electrode active material, nickel electrode, and alkaline storage battery
By adopting a positive electrode active material with a multi-layer coated structure, using the gradient-reduced Al and Mg content and cobalt oxide and other elements, the problems of nickel hydroxide in terms of cycle stability and electrochemical capacity are solved, and high-temperature discharge recovery is achieved and stable improvement in circulation reduces preparation costs.
Patent Information
- Application Number
- CN202410975413.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Nickel hydroxide cathode material has instability during repeated charging and discharge cycles, and although the addition of cationic substitutes such as aluminum and magnesium increases the voltage and suppresses self-discharge, it also leads to a decrease in electrochemical capacity and crystal structure expansion, affecting the battery. cycle stability and capacity.
The positive electrode active material adopts a multi-layer clad structure, wherein the core is nickel hydroxide, the first and second clad layers contain solid-soluble aluminum and magnesium, respectively, and reduce the content of Al and Mg through a gradient, and combine cobalt oxide. and other elements form a tightly coated and porous structure, enhancing the tap density and Coulomb efficiency of the material.
The discharge recovery and cycle stability at high temperatures are achieved, the battery capacity, discharge voltage and charge and discharge cycle characteristics are improved, the preparation cost is reduced, and the battery cycle life is extended.
Smart Images

Figure CN119092658A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of chemical batteries, in particular to a positive electrode active material applicable to alkaline storage batteries, a nickel electrode prepared by using the positive electrode active material, and an alkaline storage battery having the nickel electrode. Background Art
[0002] This section provides background information related to the present disclosure which does not necessarily constitute prior art.
[0003] Active materials containing nickel hydroxide have long been used in the positive electrode of rechargeable batteries or secondary batteries, especially for alkaline rechargeable batteries. Typical batteries using this type of active material include nickel metal hydride batteries, nickel cadmium batteries, nickel hydrogen batteries, nickel iron batteries and nickel zinc batteries. The molecular structure of nickel hydroxide active materials has two phases, namely α and β phases. The β phase material is usually oxidized and reduced between the +2 and +3 oxidation states, and the α phase nickel hydroxide can be prepared by bringing the nickel valence to the +4 oxidation state. Each nickel atom in the α phase nickel hydroxide can exchange up to 1.67 electrons, which can increase the electrode storage capacity by 85% compared to electrodes using β phase nickel hydroxide. However, the α phase nickel hydroxide material is unstable during repeated charge and discharge cycles (the α phase material slowly generates undesirable secondary β phase materials during repeated charge and discharge cycles).
[0004] Studies have shown that partial replacement of nickel cations with greater than 20wt% cations such as aluminum, cobalt, iron or magnesium can stabilize the α-phase structure of nickel hydroxide materials. Although the addition of these cations can increase the discharge voltage of nickel hydroxide materials and inhibit the self-discharge of nickel hydroxide materials, the addition of these cations also acts as impurities that are not conducive to the performance of nickel hydroxide materials. For example, the addition of magnesium and aluminum will cause the electrochemical capacity of nickel hydroxide materials to decrease, and the addition of magnesium and aluminum will cause the crystal structure of nickel hydroxide materials to change, resulting in significant expansion during the charge and discharge cycle. Summary of the invention
[0005] The object of the present invention is to provide a positive electrode active material and a method for producing the positive electrode active material, a nickel electrode comprising the positive electrode active material, and an alkaline storage battery comprising the nickel electrode. The positive electrode active material is excellent in discharge recovery after overdischarge, discharge recovery after long-term storage at high temperature, and high temperature characteristics. The alkaline storage battery has high capacity, high discharge voltage, high open circuit voltage, and excellent charge and discharge cycle stability characteristics.
[0006] To achieve the above object, the present invention adopts the following technical solution: a positive electrode active material, the positive electrode active material comprising:
[0007] A core, wherein the core is mainly composed of nickel hydroxide or a nickel hydroxide solid solution containing two or more other elements;
[0008] A first coating layer coated on the surface of the core, wherein the first coating layer is mainly composed of nickel hydroxide or a nickel hydroxide solid solution containing one or more other elements;
[0009] A second coating layer coated on the surface of the first coating layer, wherein the second coating layer has a nickel hydroxide solid solution containing two or more other elements dissolved therein as a main component.
[0010] The core comprises a 1-x (Al,Mg) x (OH)2 material; the first coating layer includes a material having the general formula Ni 1-x1- y1 Al x1 Mg y1 (OH)2 material; the second coating layer includes a material having the general formula Ni 1-x2-y2 Al x2 Mg y2 (OH)2 material. And the positive electrode active material satisfies:
[0011] 0.15 ≥ x ≥ 0;
[0012] x2>x1≥0, x2 is 0.01-0.1;
[0013] y2>y1≥0, y2 is 0.01-0.1.
[0014] From the second coating layer to the first coating layer, the content of Al element and Mg element decreases gradually. Among them, the "gradient decrease" can specifically be "gradually decreased". The core material of the positive electrode active material can play a synergistic role with the first coating layer material and the second coating layer, and with the higher mass proportion of the core material, the positive electrode active material can take into account high tap density, high coulomb efficiency, high specific capacity, good rate performance, etc. Furthermore, the positive electrode active material provided by the present invention can be made without introducing any Co-containing material, which can help reduce the preparation cost of the positive electrode active material.
[0015] When y1 and y2 are in the above-mentioned range, it is found that when (x1+x2)≥0.03, the slope of the discharge characteristic curve of the battery prepared by the positive electrode active material will change at the end of discharge, which makes it possible to accurately detect the SOC through the battery voltage, thereby detecting the remaining capacity of the battery, but when (x1+x2)<0.01, it is difficult to fully obtain this effect. Preferably, (x1+x2) is not less than 0.05; more preferably, (x1+x2) is not less than 0.06. On the other hand, when (x1+x2)≥0.2, the nickel content in the positive electrode active material will decrease accordingly, resulting in a decrease in capacity, and the advantage of the voltage characteristics of the positive electrode active material will become less obvious (the difference between the equilibrium potential and the oxygen generation potential becomes smaller), while causing the cycle life characteristics of the positive electrode active material to decrease. Preferably, x2 is not greater than 0.1; more preferably, x2 is not greater than 0.07.
[0016] When x1 and x2 are in the above-mentioned range, it is found that when (y1+y2)≥0.03, the slope of the discharge characteristic curve of the battery prepared by the positive electrode active material will change at the end of discharge, which makes it possible to accurately detect the SOC through the battery voltage, thereby detecting the remaining capacity of the battery, but when (y1+y2)<0.01, it is difficult to fully obtain this effect. Preferably, (y1+y2) is not less than 0.05; more preferably, (y1+y2) is not less than 0.06. On the other hand, when (y1+y2)≥0.2, the nickel content in the positive electrode active material will decrease accordingly, resulting in a decrease in capacity, and the advantage of the voltage characteristics of the positive electrode active material will become less obvious (the difference between the equilibrium potential and the oxygen generation potential becomes smaller), while causing the cycle life characteristics of the positive electrode active material to decrease. Preferably, y2 is not greater than 0.1; more preferably, y2 is not greater than 0.07.
[0017] The second coating layer contains magnesium, but the first coating layer does not necessarily contain magnesium. However, when the first coating layer contains magnesium, the amount of magnesium contained in the first coating layer should be less than the amount of magnesium contained in the second coating layer. The positive electrode active material provided by the present invention includes a case where the second coating layer contains magnesium and the first coating layer does not contain magnesium at all. The equilibrium potential of nickel hydroxide will increase due to the solid solution of magnesium in nickel hydroxide. Since the magnesium content and the equilibrium potential are related, different magnesium contents will cause the discharge curve to change.
[0018] The second coating layer contains aluminum, and the first coating layer does not necessarily contain aluminum. However, when the first coating layer contains aluminum, the amount of aluminum contained in the first coating layer should be less than the amount of aluminum contained in the second coating layer. The positive electrode active material provided by the present invention includes a case where the second coating layer contains aluminum and the first coating layer does not contain aluminum at all. The equilibrium potential of nickel hydroxide will increase due to the solid solution of aluminum in nickel hydroxide. In addition, the solid solution of aluminum in nickel hydroxide can also promote the formation of α-phase nickel hydroxide, thereby improving the charge and discharge utilization rate of the positive electrode active material.
[0019] It was unexpectedly discovered that by stacking a first coating layer and a second coating layer with different aluminum solid solutions and different magnesium solid solutions, the volume expansion of the positive electrode active material during the charge and discharge process can be reduced, and the decrease in unit volume capacity caused by the volume expansion can be suppressed. It is speculated that this is the result of a synergistic effect between the aluminum solid solution and the magnesium solid solution.
[0020] In one or more embodiments, for the positive electrode active material, in addition to magnesium and aluminum, at least one element of zinc and cobalt is solid-dissolved in the nickel hydroxide of the inner core and / or the nickel hydroxide of the first coating layer and / or the nickel hydroxide of the second coating layer.
[0021] In one or more embodiments, the positive electrode active material further comprises a third coating layer. Preferably, the third coating layer comprises cobalt oxyhydroxide (CoOOH) and / or cobalt oxide (CoO).
[0022] The ratio of the inner core in the positive electrode active material is preferably 85 wt % to 97 wt %, within which the conductivity and electrode capacity of the positive electrode active material become better. When the ratio is lower than 80 wt %, this may result in a decrease in the capacity of the positive electrode active material; when the ratio exceeds 97 wt %, the conductivity and charge-discharge cycle stability of the positive electrode active material may not be sufficiently improved. The nickel hydroxide in the inner core is preferably α-phase nickel hydroxide because it can improve the conductivity of the positive electrode active material.
[0023] The proportion of nickel hydroxide in the first coating layer is preferably not less than 50 wt % based on the total mass of the first coating layer; the proportion of nickel hydroxide in the second coating layer is preferably not less than 50 wt % based on the total mass of the second coating layer.
[0024] In one or more embodiments, the powder resistance of the positive electrode active material is less than 200Ω·cm, and such a low powder resistance provides high conductivity. Therefore, in the electrode using the positive electrode active material, a higher active material utilization factor is obtained. For the purpose of further reducing the powder resistance of the positive electrode active material, the core and / or the first coating layer and / or the second coating layer include yttrium oxide, tungsten oxide, titanium oxide, zinc oxide or a combination thereof, and the above additives can improve the conductivity of the positive electrode active material and can inhibit the expansion of the positive electrode active material during charging and discharging.
[0025] In one or more embodiments, the specific surface area S of the positive electrode active material is less than or equal to 30 m 2 / g. The specific surface area S can be measured by nitrogen adsorption method (BET method). The specific surface area of the positive electrode active material will not be too high to significantly reduce the tap density. In addition, the present invention controls the total mass of the first coating layer and the second coating layer to account for a small proportion, which can make the tap density of the positive electrode active material higher. The specific surface area of the positive electrode active material is preferably 1-30m 2 / g, more preferably 5-25m 2 / g, at this time, the specific area of the positive electrode active material is more suitable, which can better take into account both high tap density and high rate output capability.
[0026] In one or more embodiments, the coverage rate of the coating layer composed of the first coating layer and the second coating layer on the surface of the inner core is greater than or equal to 90%, such as ≥92%, ≥95% or ≥98%, etc. This parameter can reflect that the coating degree of the coating layer on the surface of the inner core is relatively high and its distribution is relatively uniform, greatly avoiding the problem of uneven coating caused by the conventional secondary deposition technology, and the coating layer has a good effect of inhibiting oxygen evolution of the inner core. The coating layer has a pore structure, and the average pore diameter of the pores is 1 nm - 50 nm. This average pore diameter is much lower than the pore diameter in the loose coating layer obtained by the conventional coprecipitation method. The smaller average pore diameter can also reflect the close packing of the above-mentioned coating layer on the surface of the inner core from the side, which is beneficial to both high tap density and high Coulomb efficiency of the positive electrode active material; at the same time, it is also beneficial to increase the porosity of the coating layer, and then increase the porosity of the overall positive electrode active material, which can better relieve the stress change of the positive electrode active material during the charge and discharge cycle, and then reduce the phenomenon of particle pulverization of the positive electrode active material, which is beneficial to the improvement of the battery cycle life. Therefore, it can be understood that the coating layer of the present invention is closely packed / wrapped and porous. Among them, the close wrapping of the coating layer can inhibit the particle pulverization phenomenon of the inner core during the cycle and improve the cycle stability, and the existence of the porous structure in the coating layer can further facilitate the stress release of the inner core during the charge and discharge process, so that the positive electrode active material can have both high tap density, high Coulomb efficiency, high specific capacity, good rate performance, long cycle life, etc. The average pore diameter of the pores can be obtained by characterizing the cross-sectional electron microscope of the positive electrode active material, or by the nitrogen adsorption method.
[0027] In one or more embodiments, the porosity of the positive electrode active material can be 5 - 40%. The porosity can be obtained by characterizing the cross-sectional electron microscope of the positive electrode active material, or by the nitrogen adsorption method. The porosity at different positions of the positive electrode active material can be different, and the porosity can be lower closer to the inner core. The overall pore volume of the positive electrode active material is less than or equal to 0.2 cm 3 / g (measured by the nitrogen adsorption method), and the smaller pore volume is beneficial to making the tap density of the positive electrode active material higher and the electrochemical performance better.
[0028] In one or more embodiments, the particle diameter of the positive electrode active material is D0, the thickness of the first coating layer is D1, and the thickness of the second coating is D2, satisfying: 0 < D1 ≤ D2 ≤ 0.08D0. Among them, D0, D1 and D2 can be obtained from the electron microscope photograph of the positive electrode active material. The thickness of the coating layer composed of the first coating layer and the second coating layer is relatively thin, which is beneficial to ensuring a relatively tight coating. Among them, D0 can be in the range of 2 μm - 25 μm, and D1 and D2 can both be in the range of 10 nm - 800 nm.
[0029] In one or more embodiments, the average secondary particle size of the positive electrode active material is 5μm-15μm, which is the average particle size of the particles of the positive electrode active material in its dispersion measured by dynamic light scattering (DLS method). The appropriate average secondary particle size can regulate the transport channels of electrons, ions, etc. of the positive electrode active material during the electrochemical reaction, ensure its high electrochemical activity, and achieve its high specific capacity and high rate performance.
[0030] The preparation process of the positive electrode active material of the present invention includes the following steps (a) to (c).
[0031] Step (a): preparing core particles.
[0032] Step (b): forming a first coating layer on the surface of the inner core.
[0033] Step (c): forming a second coating layer on the surface of the first coating layer.
[0034] The positive electrode active material provided by the present invention can be prepared by a coprecipitation method or by an ion permeation self-exchange reaction.
[0035] In one or more embodiments, step (a) comprises the following steps: configuring an aqueous solution containing a given amount of a soluble salt containing nickel, a soluble salt containing Al, and a soluble salt containing Mg, configuring an aqueous solution containing a given amount of ammonium sulfate and sodium hydroxide, mixing the two aqueous solutions, stirring, and heating in a water bath, and during the entire operation, maintaining the pH value of the reaction system at 8-12 (using an alkaline aqueous solution to adjust the pH value of the reaction system), the reaction temperature at 50°C-90°C (for example, 50°C, 60°C, 70°C, 80°C, 85°C, 90°C, etc.), and the reaction time at 1-10 hours (for example, 1h, 2h, 3h, 4h, 5h, 6h, 8h, 10h, etc.), thereby obtaining a core particle including nickel hydroxide particles, the nickel hydroxide particles comprising aluminum hydroxide and magnesium hydroxide solid-dissolved in the form of ammine complex ions. Adjusting the pH value of the reaction system to 8 to 10 obtains α-phase Ni(OH)2, and adjusting its pH value to 10 to 12 obtains β-phase Ni(OH)2. When the soluble salt containing Al and the soluble salt containing Mg are omitted in step (a), core particles consisting of nickel hydroxide particles can be obtained.
[0036] In one or more embodiments, step (b) comprises the following steps: mixing the core particles with a first reaction solution containing a given amount of a soluble salt containing nickel, the first reaction solution also containing a given amount of a soluble salt containing Al and a soluble salt containing Mg, stirring the core particles and the first reaction solution after mixing and heating in a water bath, and then adding an alkaline aqueous solution to adjust the pH value of the reaction system to 10 to 13, thereby precipitating and forming a first coating layer on the surface of the core particles, the reaction temperature of the process is 50°C-90°C, and the reaction time is 1-24 hours. Preferably, the mass ratio of the core particles to the first reaction solution is 1:5-100, and a suitable solid-liquid ratio can ensure that the coating thickness and coating compactness of the first coating layer are appropriate, and improve the preparation efficiency of the first coating layer. The concentrations of the soluble salt containing Al and the soluble salt containing Mg in the first reaction solution do not exceed 3.0 mol / L, which is conducive to ensuring that the first coating layer has a suitable generation rate and can regulate the content of Al and Mg in the first coating layer. When the soluble salt containing Mg is omitted in step (b), a first coating layer consisting of no magnesium solid solution can be obtained; when the soluble salt containing Al is omitted in step (b), a first coating layer consisting of no aluminum solid solution can be obtained; when the soluble salt containing Al and the soluble salt containing Mg are omitted in step (b), a first coating layer composed of nickel hydroxide particles can be obtained.
[0037] In one or more embodiments, step (c) includes the following steps: mixing the particles having a first coating layer with a second reaction solution containing a given amount of a soluble salt containing nickel, the first reaction solution also containing a given amount of a soluble salt containing Al and a soluble salt containing Mg, stirring and heating in a water bath after mixing, and then adding an alkaline aqueous solution to adjust the pH value of the reaction system to 10 to 13, thereby precipitating the second coating layer on the surface of the first coating layer, the reaction temperature of the process is 50°C-90°C, and the reaction time is 1-24 hours.
[0038] In one or more embodiments, the preparation process of the positive electrode active material further includes step (d), which includes the following steps: mixing the particles having the second coating layer, the cobalt sulfate aqueous solution and the sodium hydroxide aqueous solution, stirring and heating in a water bath, and adjusting the pH value of the reaction system to 11 to 13 using an alkaline aqueous solution, thereby forming a third coating layer containing cobalt hydroxide on the surface of the second coating layer. In water or in an alkaline aqueous solution with a concentration of 20 wt% or less, at a temperature of 60°C or less, an oxidant (such as potassium persulfate, sodium persulfate, ammonium persulfate, sodium hypochlorite, etc.) is used to oxidize the particles having the third coating layer (i.e., an oxidation treatment process), and then the particles are placed at a temperature of 80°C or higher and heated in an alkaline aqueous solution with a concentration of 30 wt% or higher (i.e., a heating treatment process). Through the "oxidation treatment process", the cobalt and a portion of the nickel in the positive electrode active material are oxidized, and the self-discharge of the positive electrode active material is suppressed, so that the battery using the positive electrode active material will have excellent internal pressure characteristics and charge / discharge cycle characteristics. The positive electrode active material obtained by the oxidation treatment process has a high powder resistance. However, since 30% by weight or more of an alkaline aqueous solution is added thereto and the material is heated at 80°C or more, the positive electrode active material will have a sufficiently low powder resistance after the heat treatment. If the heat treatment is performed using an alkaline aqueous solution with a concentration of less than 30% by weight or a temperature of less than 80°C, a sufficiently low powder resistance will not be obtained.
[0039] It should be noted that the alkaline aqueous solution described in the present invention is preferably a sodium hydroxide aqueous solution, but the alkaline aqueous solution is not limited thereto. The alkaline aqueous solution can be an aqueous solution of one or more of lithium hydroxide, sodium hydroxide and potassium hydroxide.
[0040] It should be noted that the "soluble salt" described in the present invention specifically refers to a salt that is soluble in water. For example, the soluble salt of Al may specifically include one or more of Al sulfate, nitrate or chloride, and the soluble salt of Mg may specifically include one or more of Mg sulfate, nitrate or chloride. Preferably, the soluble salt containing nickel is nickel sulfate, the soluble salt of Al is aluminum sulfate, and the soluble salt of Mg is magnesium sulfate.
[0041] The nickel electrode of the present invention is characterized in that the nickel electrode is obtained by filling a porous substrate with the positive electrode active material. The porous substrate can be a nickel-plated mesh, sponge or fiber-shaped metal body or foamed nickel. The nickel electrode containing the positive electrode active material significantly increases the potential difference between the oxygen evolution potential and the oxidation potential in the nickel electrode, thereby further improving the charging efficiency.
[0042] In one or more embodiments, the preparation process of the nickel electrode is specifically as follows: the positive electrode active material is mixed with a conductive material, an additive, water and an aqueous binder (the aqueous binder can be, for example, carboxymethyl cellulose, methyl cellulose, polytetrafluoroethylene dispersion, hydroxypropyl cellulose, etc.) to prepare a slurry; the obtained slurry is filled into the nickel foam and dried, and then rolled and cut in sequence to obtain a nickel electrode. The additive is preferably a compound containing one or more rare earth elements, and the oxygen evolution potential of the nickel electrode during charging will be positively shifted due to the rare earth compound, thereby inhibiting the oxygen evolution reaction and enhancing the oxidation reaction of nickel. Therefore, its charging efficiency is further improved.
[0043] The alkaline storage battery of the present invention is an alkaline storage battery using a nickel electrode, characterized in that: the positive electrode of the alkaline storage battery includes the nickel electrode. The alkaline storage battery refers to a battery system based on the positive electrode active material provided by the present invention, an alkaline aqueous electrolyte and different negative electrodes. According to the different negative electrodes, the alkaline storage battery can be divided into different types, for example, the alkaline storage battery can be specifically a nickel-metal hydride battery, a nickel-zinc battery, a nickel-iron battery or a nickel-cadmium battery. Correspondingly, the negative electrode of the alkaline storage battery is a metal hydride negative electrode, a zinc negative electrode, an iron negative electrode or a cadmium negative electrode. Taking the zinc negative electrode as an example, it specifically refers to that the negative electrode includes a negative electrode active material containing a Zn element, such as ZnO. Among them, the electrolyte of the alkaline storage battery can contain an alkaline electrolyte and water, and the alkaline electrolyte can include one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide. Preferably, the concentration of the alkaline electrolyte in the electrolyte can be 0.5-10 mol / L.
[0044] The positive electrode active material provided by the present invention has good electrochemical properties. The nickel electrode provided by the present invention can take into account both high capacity and good charge-discharge cycle stability. The alkaline storage battery provided by the present invention has high volume energy density, high coulomb efficiency and specific capacity, and good cycle performance.
[0045] The following describes the invention in conjunction with specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] The accompanying drawings further illustrate the present invention, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention.
[0047] Figure 1 This is a schematic diagram of the structure of the positive electrode active material provided in Example 1 of the present invention.
[0048] The reference numerals are: a core 10 , a first coating layer 11 , a second coating layer 12 , and a third coating layer 13 . DETAILED DESCRIPTION
[0049] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.
[0050] [Example 1]
[0051] This embodiment provides a positive electrode active material, Figure 1 : is a schematic diagram of the structure of the positive electrode active material. The positive electrode active material provided in this embodiment is a shell structure, and the stacking degree of the shell material is higher. The positive electrode active material includes a core 10, a first coating layer 11 coated on the surface of the core 10, a second coating layer 12 coated on the surface of the first coating layer 11, and a third coating layer 13 coated on the surface of the second coating layer 12.
[0052] The core 10 is a spherical or quasi-spherical particle of the positive electrode active material. After being coated, the core 10 still maintains its spherical or quasi-spherical morphology, which is conducive to ensuring that the positive electrode active material has a higher tap density (the tap density of the positive electrode active material is greater than or equal to 1.8 g / cm 3 ) and specific area, which is beneficial to the improvement of its ion transport and the wettability of the electrolyte, etc., improving the kinetic characteristics and increasing its rate output capacity.
[0053] The core 10 is an α-phase nickel hydroxide material, which can be obtained by an in-situ phase transformation reaction of a β-phase nickel hydroxide raw material. The first coating layer 11 is a β-phase nickel hydroxide. The second coating layer 12 is a β-phase nickel hydroxide material in which Al and Mg are solid-dissolved. The chemical formula of the material of the second coating layer 12 is Ni 0.9 Al 0.05 Mg 0.05 (OH)2. The third coating layer is cobalt hydroxide oxide. Compared with a simple α-phase nickel hydroxide material, the positive electrode active material of the present invention is advantageous in ensuring the good structural stability of the α-phase nickel hydroxide material by coating three layers of coating layers, inhibiting its transformation back to the β-phase during the charge and discharge cycle, and improving the cycle stability of the positive electrode active material; at the same time, the β-phase nickel hydroxide of the first coating layer 11 can generate α-phase nickel hydroxide through an in-situ reaction, and realize the in-situ coating of the α-phase nickel hydroxide material of the inner core 10, and as mentioned above, the Al element and the Mg element in the second coating layer 12 enter the bulk phase of the β-phase nickel hydroxide material to further inhibit the oxygen evolution side reaction of the positive electrode active material. When the Al element and the Mg element exist in the β-phase nickel hydroxide material at the same time, it helps to improve its oxygen evolution overpotential, thereby improving the coulomb efficiency of the positive electrode active material and improving the comprehensive electrochemical performance of the positive electrode active material. The third coating layer is more conducive to improving the structural stability and ion conductivity of the positive electrode active material.
[0054] This embodiment also provides a nickel electrode for an alkaline storage battery, the nickel electrode includes the positive electrode active material provided in this embodiment, the nickel electrode provided in this embodiment includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, the positive electrode active material layer includes the positive electrode active material provided in this embodiment, and the positive electrode active material layer is disposed on one side surface or on two opposite sides of the positive electrode current collector. The positive electrode current collector can be a conventional choice in the battery field, for example, it can be nickel foam, porous nickel foil, nickel-plated perforated steel belt, perforated steel belt, etc. The positive electrode active material layer can also include a binder, a conductive agent, other positive electrode active components, etc.
[0055] This embodiment also provides an alkaline storage battery, which includes the nickel electrode provided in this embodiment. The alkaline storage battery provided in this embodiment includes a nickel electrode, a negative electrode, an electrolyte and a diaphragm, as well as corresponding connecting accessories and circuits. The diaphragm is located between the nickel electrode and the negative electrode, and the nickel electrode, the negative electrode and the diaphragm are immersed in the electrolyte.
[0056] [Example 2-8]
[0057] Embodiments 2-8 all provide a positive electrode active material, and the preparation method of the positive electrode active material comprises the following steps:
[0058] Step 1: weigh 6 g of nickel sulfate and dissolve it in 50 mL of deionized water, then add aluminum sulfate and magnesium sulfate and stir to dissolve to obtain solution A, and dissolve 2 g of sodium hydroxide and 0.03 g of ammonium sulfate in 50 mL of deionized water to obtain solution B;
[0059] Step 2: Under the action of magnetic stirring, solution A and solution B are mixed and reacted in a reaction container, a 1 mol / L sodium hydroxide solution is used to control the pH value of the reaction system to 11-11.5, the reaction is carried out at 80° C. for 10 hours, the obtained reaction material is filtered, and then the solid is washed and dried to obtain a core material;
[0060] Step 3, dissolving 0.28g of nickel sulfate in 100mL of deionized water, adding aluminum sulfate and magnesium sulfate and stirring to dissolve to obtain the first reaction solution required for the coating reaction, mixing the core material prepared in step 2 with the first reaction solution in a reaction container under magnetic stirring, using 1mol / L sodium hydroxide solution to control the pH value of the reaction system to 11-11.5, reacting at 50°C for 3h, filtering the obtained reaction material, and then washing and drying the solid to obtain a material having a first coating layer;
[0061] Step 4, step 3, dissolving 0.56g of nickel sulfate in 100mL of deionized water, adding aluminum sulfate and magnesium sulfate and stirring to dissolve to obtain the second reaction solution required for the coating reaction, mixing the material prepared in step 3 with the second reaction solution in a reaction container under magnetic stirring, using 1mol / L sodium hydroxide solution to control the pH value of the reaction system to 11-11.5, reacting at 90°C for 5h, filtering the obtained reaction material, washing the solid and placing it in a 120°C oven for 2h and then taking it out, cooling it naturally to room temperature to obtain the positive electrode active material;
[0062] In the first reaction solution and the second reaction solution, the concentration of aluminum sulfate does not exceed 3.0 mol / L, and the concentration of magnesium sulfate does not exceed 3.0 mol / L. The content of aluminum and magnesium in the core material is regulated by adjusting the concentration of aluminum sulfate and magnesium sulfate in solution A. The content of aluminum and magnesium in the first coating material is regulated by adjusting the concentration of aluminum sulfate and magnesium sulfate in the first reaction solution. The content of aluminum and magnesium in the second coating material is regulated by adjusting the concentration of aluminum sulfate and magnesium sulfate in the second reaction solution.
[0063] The distribution range of the particle diameter of the positive electrode active material provided in Examples 1-8 is 8-22 μm, and the average secondary particle size of the positive electrode active material is 10-11 μm. The thickness of the first coating layer is about 400-500 nm, and the thickness of the second coating layer is about 500 nm-600 nm. The thickness of the third coating layer of the positive electrode active material provided in Example 1 is about 100 nm.
[0064] [Comparative Example 1]
[0065] Uncoated β-phase cobalt-free Ni 0.9 Al 0.05 Mg 0.05 (OH)2 is directly used as the positive electrode active material.
[0066] [Comparative Examples 2-7]
[0067] Comparative Examples 2-7 all adopt the same preparation method as Example 2 to obtain positive electrode active materials, the only difference being that the concentrations of aluminum sulfate and magnesium sulfate in solution A are different, or the concentrations of aluminum sulfate and magnesium sulfate in the first reaction solution are different, or the concentrations of aluminum sulfate and magnesium sulfate in the second reaction solution are different.
[0068] [Comparative Example 8]
[0069] Uncoated β-phase cobalt-free Ni(OH)2 is directly used as the positive electrode active material.
[0070] Table 1 shows the chemical formulas of the cores and coating layers of the positive electrode active materials provided in Examples 1-8 and the positive electrode active materials provided in Comparative Examples 1-8.
[0071] Table 1
[0072] Kernel First coating layer Second coating layer Example 1 <![CDATA[Ni(OH)2]]> <![CDATA[Ni(OH)2]]> <![CDATA[Ni 0.9 Al 0.05 Mg 0.05 (OH)2]]> Example 2 <![CDATA[Ni 0.9 Al 0.05 Mg 0.05 (OH)2]]> <![CDATA[Ni 0.96 Al 0.02 Mg 0.02 (OH)2]]> <![CDATA[Ni 0.88 Al 0.06 Mg 0.06 (OH)2]]> Example 3 <![CDATA[Ni 0.7 Al 0.15 Mg 0.15 (OH)5]]> <![CDATA[Ni 0.96 Al 0.02 Mg 0.02 (OH)2]]> <![CDATA[Ni 0.88 Al 0.06 Mg 0.06 (OH)2]]> Example 4 <![CDATA[Ni(OH)2]]> <![CDATA[Ni 0.96 Al 0.02 Mg 0.02 (OH)2]]> <![CDATA[Ni 0.88 Al 0.06 Mg 0.06 (OH)2]]> Example 5 <![CDATA[Ni 0.9 Al 0.05 Mg 0.05 (OH)2]]> <![CDATA[Ni(OH)2]]> <![CDATA[Ni 0.88 Al 0.06 Mg 0.06 (OH)2]]> Example 6 <![CDATA[Ni 0.9 Al 0.05 Mg 0.05 (OH)2]]> <![CDATA[Ni 0.96 Mg 0.02 (OH)2]]> <![CDATA[Ni 0.89 Al 0.1 Mg 0.01 (OH)2]]> Example 7 <![CDATA[Ni 0.9 Al 0.05 Mg 0.05 (OH)2]]> <h2 style=";text-align:left;direction:ltr"><![CDATA[Ni <h2 style=";text-align:left;direction:ltr"> 0.96 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.02 <h2 style=";text-align:left;direction:ltr"> (OH)2]]><h2 style=";text-align:left;direction:ltr"> <![CDATA[Ni 0.89 Al 0.01 Mg 0.1 (OH)2]]> Example 8 <![CDATA[Ni(OH)2]]> <![CDATA[Ni(OH)2]]> <![CDATA[Ni 0.8 Al 0.1 Mg 0.1 (OH)2]]> Comparative Example 1 <![CDATA[Ni 0.9 Al 0.05 Mg 0.05 (OH)1]]> / / Comparative Example 2 <![CDATA[Ni 0.9 Al 0.05 Mg 0.05 (OH)2]]> / <![CDATA[Ni 0.88 Al 0.06 Mg 0.06 (OH)2]]> Comparative Example 3 <![CDATA[Ni 0.9 Al 0.05 Mg 0.05 (OH)2]]> <![CDATA[Ni 0.96 Al 0.02 Mg 0.02 (OH)2]]> / Comparative Example 4 <![CDATA[Ni 0.9 Al 0.05 Mg 0.05 (OH)2]]> <![CDATA[Ni 0.88 Al 0.06 Mg 0.06 (OH)2]]> <![CDATA[Ni 0.96 Al 0.02 Mg 0.02 (OH)2]]> Comparative Example 5 <![CDATA[Ni 0.9 Al 0.05 Mg 0.05 (OH)2]]> <![CDATA[Ni 0.96 Al 0.02 Mg 0.02 (OH)2]]> <![CDATA[Ni(OH)2]]> Comparative Example 6 <![CDATA[Ni 0.9 Al 0.05 Mg 0.05 (OH)2]]> <![CDATA[Ni 0.6 Al 0.2 Mg 0.2 (OH)2]]> <![CDATA[Ni 0.88 Al 0.06 Mg 0.06 (OH)2]]> Comparative Example 7 <![CDATA[Ni 0.9 Al 0.05 Mg 0.05 (OH)2]]> <![CDATA[Ni 0.96 Al 0.02 Mg 0.02 (OH)2]]> <![CDATA[Ni 0.6 Al 0.2 Mg 0.2 (OH)2]]> Comparative Example 8 <![CDATA[Ni(OH)2]]> / /
[0073] [Preparation of nickel electrode]
[0074] Nickel electrodes were prepared using the positive electrode active materials provided in Examples 1-8 and the positive electrode active materials provided in Comparative Examples 1-8, respectively. The preparation process is as follows:
[0075] Step 1: 100 parts by mass of a positive electrode active material, 0.3 parts by mass of yttrium oxide, 0.6 parts by mass of tungsten oxide, 0.2 parts by mass of HPC (hydroxypropyl cellulose), 0.2 parts by mass of polytetrafluoroethylene dispersion and 30 parts by mass of water are mixed to prepare a composite slurry;
[0076] Step 2: Fill the composite slurry into the foamed nickel sheet as the positive electrode substrate, and then dry, roll and cut it in sequence to obtain a nickel electrode with a size of AA.
[0077] [Preparation of alkaline storage battery]
[0078] The above nickel electrodes are respectively used to prepare alkaline storage batteries, and the preparation process is as follows:
[0079] Step 1: weigh rare earth element compounds, magnesium, nickel, aluminum and cobalt in a molar ratio of 1.00:0.02:3.24:0.15:0.07, mix them evenly and place them in a furnace to melt. Pour the melted liquid into a mold and cool it to room temperature to make a hydrogen storage alloy ingot. The sample extracted from the ingot was analyzed by radio frequency plasma spectrometry (ICP). The composition of the hydrogen storage alloy is (La 0.32 Sm 0.55 ) 1.00 Mg 0.14 Ni 3.24 Al 0.15 Co 0.07 ;
[0080] Step 2: heat treating the hydrogen storage alloy ingot at 1050° C. for 8 hours in an argon atmosphere. After the heat treatment, the hydrogen storage alloy ingot cooled to room temperature is mechanically crushed in an argon environment to obtain hydrogen storage alloy powder. The particle size of the obtained hydrogen storage alloy powder is measured using a laser diffraction and scattering particle size distribution instrument. The volume average particle size (MV) of the hydrogen storage alloy particles is 40 μm.
[0081] Step 3, 100 parts by mass of hydrogen storage alloy powder, 0.4 parts by mass of sodium polyacrylate, 0.1 parts by mass of carboxymethyl cellulose, 1.0 parts by mass of styrene-butadiene rubber (SBR) dispersion, 1.0 parts by mass of carbon black and 30 parts by mass of water are mixed to form a paste;
[0082] Step 4: coating the paste on both sides of a steel perforated plate as a negative electrode substrate with a uniform coating thickness, wherein the thickness of the steel perforated plate is 60 μm and the surface of the steel perforated plate is nickel plated, and after coating, drying, rolling and cutting are performed in sequence to obtain a negative electrode of size AA;
[0083] Step 5, stacking the negative electrode, the separator (the separator is made of sulfonated polypropylene fiber non-woven fabric, with a thickness of 0.11 mm and a density of 48 g / m2) and the nickel electrode in sequence and winding them to obtain a battery core, placing the battery core in a cylindrical shell with a bottom, and injecting a prepared alkaline electrolyte according to a predetermined amount (using an aqueous solution containing potassium hydroxide, sodium hydroxide and lithium hydroxide as the alkaline electrolyte, the mass ratio of potassium hydroxide, sodium hydroxide and lithium hydroxide in the alkaline electrolyte is 1.3:6.4:0.85, and the concentration of hydroxide in the alkaline electrolyte is 5 mol / L), and then sealing the opening of the cylindrical shell with a cap, and assembling a nominal capacity (nominal capacity refers to the discharge capacity of the battery after charging at 0.1C for 16 hours at 20°C and discharging at 0.2C until the battery voltage reaches 1.0V) of 1450mAh AA size alkaline storage battery (i.e., nickel-hydrogen rechargeable battery);
[0084] Step 6: Charge the alkaline storage battery at 0.1C for 16 hours at 20°C and then discharge it at 0.2C. Repeat the charge and discharge operation five times until the voltage of the alkaline storage battery reaches 1.0V, thus completing the initial activation of the battery.
[0085] The following tests are performed on the alkaline storage batteries that have completed the initial activation process:
[0086] (1) Determination of the ratio of actual discharge capacity to theoretical capacity: At an ambient temperature of 20°C, charge the battery for 12 hours at a charging current of 0.1C (calculated based on the theoretical capacity), then let it stand for 1 hour, and then discharge it at a current of 0.2C (calculated based on the theoretical capacity). When the battery voltage reaches 1.0V, terminate the discharge. Measure the actual discharge capacity during this period.
[0087] The ratio of actual discharge capacity to theoretical capacity (%) = measured discharge capacity / 1450 × 100.
[0088] (2) Determination of the ratio of high-rate discharge capacity to theoretical capacity: At an ambient temperature of 20°C, charge the battery at a charging current of 0.1C (calculated based on the theoretical capacity) for 12 hours, then let it stand for 1 hour, and then discharge it at a current of 3C (calculated based on the theoretical capacity). When the battery voltage reaches 1.0V, the discharge is terminated. The actual discharge capacity during this period is measured.
[0089] Determination of the ratio of high rate discharge capacity to theoretical capacity (%) = measured discharge capacity ÷ 1450 × 100.
[0090] (3) Cycle performance test: At an ambient temperature of 20°C, the battery was charged at a current value of 0.5C for 2 hours, and then discharged at a current value of 0.5C until the voltage reached 1.0V. The charge and discharge cycle was repeated for a maximum of 500 cycles. The capacity retention rate (%) was calculated using the discharge capacity at the first charge and discharge cycle and the discharge capacity at the predetermined number of cycles.
[0091] Capacity retention rate (%) = discharge capacity at the 500th charge-discharge cycle ÷ discharge capacity at the 1st charge-discharge cycle × 100.
[0092] The above test results are shown in Table 2.
[0093] Table 2
[0094]
[0095] According to the results in Table 2, compared with Comparative Examples 1-8, the rate discharge capacity and cyclic charge and discharge stability of the alkaline storage battery prepared using the positive electrode active material provided in Examples 1-8 are improved, and the alkaline storage battery prepared using the positive electrode active material provided in Examples 1-8 can improve the utilization rate of the active material.
[0096] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0097] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A positive electrode active material, characterized in that: The positive electrode active material comprises: The core comprises a core having a general formula Ni 1-x (Al,Mg) x (OH)2 materials; The first coating layer coated on the surface of the core includes a general formula Ni 1-x1-y1 Al x1 Mg y1 (OH)2 materials; A second coating layer coated on the surface of the first coating layer, the second coating layer comprising a general formula Ni 1-x2-y2 Al x2 Mg y2 (OH)2 materials; The positive electrode active material satisfies: 0.15≥x≥0; x2>x1≥0, x2 is 0.01-0.1; y2>y1≥0, y2 is 0.01-0.
1.
2. The positive electrode active material according to claim 1, characterized in that The positive electrode active material satisfies: (x1+x2)≥0.03 and x2 is not greater than 0.
07.
3. The positive electrode active material according to claim 1, characterized in that The positive electrode active material satisfies: (y1+y2)≥0.03 and y2 is not greater than 0.
07.
4. The positive electrode active material according to claim 1, characterized in that The ratio of the core in the positive electrode active material is 85 wt % to 97 wt %.
5. The positive electrode active material according to claim 1, characterized in that Based on the total mass of the first coating layer, the proportion of nickel hydroxide in the first coating layer is not less than 50 weight %; based on the total mass of the second coating layer, the proportion of nickel hydroxide in the second coating layer is not less than 50 weight %.
6. The positive electrode active material according to claim 1, characterized in that The positive electrode active material further includes a third coating layer, and the third coating layer includes cobalt oxyhydroxide and / or cobalt oxide.
7. A nickel electrode, characterized in that The nickel electrode comprises the positive electrode active material as claimed in any one of claims 1 to 6.
8. An alkaline storage battery, characterized in that: The alkaline storage battery comprises a positive electrode, a negative electrode, an electrolyte and a separator located between the positive electrode and the negative electrode, and the positive electrode comprises the nickel electrode according to claim 7.
9. The alkaline storage battery according to claim 8, characterized in that The negative electrode of the alkaline storage battery includes a metal hydride negative electrode, a zinc negative electrode, an iron negative electrode or a cadmium negative electrode.
Citation Information
Patent Citations
Positive electrode material and preparation method and application thereof
CN118156435A
Alkaline secondary cell
CN1581541A
Non-sintered nickel electrode for sealed alkaline storage battery
JP1999144723A
Nickel metal hydride battery
JP2020009697A
Cited By
Nickel-based positive electrode material and preparation method thereof
CN120998981A