Negative active material as well as preparation method and application thereof

The inner hydrophobic and outer hydrophilic double-layer protective structure covers the silicon-based material, which solves the problem of volume expansion and gas production during charging and discharging of silicon-based materials, significantly improves the stability and safety of the battery and extends the length of the battery. The service life of the battery.

CN119092660AActive Publication Date: 2024-12-06ZHEJIANG UNIV +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410994660.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-12-06
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Silicon-based materials have serious volume expansion problems during charging and discharging, resulting in deterioration of electrochemical properties and increasing instability and safety risks. The existing modification methods may cause gas production surges and electrode manufacturing defects.

Method used

Using an negative electrode active material with a hydrophobic and outer layer hydrophilic two-layer protective structure, the silicon-based material is coated with water-soluble polymer and surfactant to form a polymer cladding layer, inhibit volume expansion and gas production, and improve battery Stability and safety.

Benefits of technology

It effectively inhibits the volume expansion and gas production of silicon-based materials, improves the stability and safety of the battery, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004962070800000032
    Figure BDA0004962070800000032
  • Figure BDA0004962070800000081
    Figure BDA0004962070800000081
  • Figure BDA0004962070800000123
    Figure BDA0004962070800000123
Patent Text Reader

Abstract

The invention relates to a negative electrode active material and a preparation method and application thereof. The negative active material comprises a silicon-based material and a polymer coating layer coating the surface of the silicon-based material, the polymer coating layer comprises a water-soluble polymer and a surfactant, and the water contact angle of the polymer coating layer is 65-85 degrees; the chemical formula of the surfactant is A1-R-A2, A1 and A2 are independently selected from polar groups containing at least one element of N, O, P and S, r is selected from a substituted or unsubstituted aliphatic hydrocarbon chain segment of C8-C50, a substituted or unsubstituted aliphatic hydrocarbon chain segment of C8-C50 containing heteroatoms, a substituted or unsubstituted alicyclic hydrocarbon chain segment of C8-C50, a substituted or unsubstituted alicyclic hydrocarbon chain segment of C8-C50 containing heteroatoms, a substituted or unsubstituted aromatic hydrocarbon chain segment of C8-C50, and a substituted or unsubstituted aromatic hydrocarbon chain segment of C8-C50 containing heteroatoms. The negative electrode active material has a double-layer protection structure with a hydrophobic inner layer and a hydrophilic outer layer, and is excellent in dispersity and low in gas production rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a negative electrode active material and a preparation method and application thereof. Background Art

[0002] With the growing demand for high-energy-density batteries, silicon-based materials with relatively high theoretical specific capacity (about 4200 mAh / g) have become a hot research direction for battery negative electrode materials. However, silicon-based materials have a serious volume expansion problem (up to 300%) during the charge and discharge process, causing the silicon-based materials to pulverize and peel off from the current collector, resulting in the loss of electrical contact between active materials and active materials, and between active materials and current collectors. At the same time, a new solid electrolyte layer (SEI) is continuously formed, which ultimately leads to the deterioration of electrochemical performance and limits the practical application of batteries.

[0003] Although surface modification, element doping, and pre-lithiation of silicon-based negative electrode materials can help inhibit the volume expansion of silicon-based negative electrode materials and improve their performance, these treatment methods also increase the instability of silicon-based negative electrode materials, causing the gas production of silicon-based negative electrode materials with gas production defects to surge during the electrode manufacturing process, which not only brings safety risks to the slurry process, but also may cause defects such as pinholes, pores, particles, scratches, and material loss during electrode coating and drying, thereby reducing the overall performance of the electrode sheet. In particular, coating the surface of the silicon-based negative electrode material with a hydrophilic polymer helps to improve the dispersibility of silicon-carbon during the slurry process, but it exacerbates the gas production of the side reaction between silicon and water, resulting in battery capacity loss and reduced life. Summary of the invention

[0004] Based on this, it is necessary to provide a negative electrode active material and a preparation method and application thereof to address the above problems; the negative electrode active material has a unique double-layer protective structure of inner hydrophobic layer and outer hydrophilic layer, which not only has excellent dispersibility, but also can effectively inhibit gas production and volume expansion, which is beneficial to improving the stability and safety of the battery.

[0005] A negative electrode active material, comprising a silicon-based material and a polymer coating layer coated on the surface of the silicon-based material, wherein the polymer coating layer comprises a water-soluble polymer and a surfactant, and the water contact angle of the polymer coating layer is 65°-85°;

[0006] The chemical formula of the surfactant is A1-R-A2, wherein A1 and A2 are independently selected from polar groups containing at least one element of N, O, P, and S, and R is selected from substituted or unsubstituted C8-C 50 Aliphatic hydrocarbon chain segments, substituted or unsubstituted C8-C 50 Aliphatic hydrocarbon chain segments containing heteroatoms, substituted or unsubstituted C8-C 50Alicyclic hydrocarbon segments, substituted or unsubstituted C8-C 50 Alicyclic hydrocarbon segments containing heteroatoms, substituted or unsubstituted C8-C 50 Aromatic hydrocarbon segments, substituted or unsubstituted C8-C 50 Aromatic hydrocarbon chain containing heteroatoms, the substituents are selected from C1-C 20 branched or straight chain hydrocarbon group, C1-C 20 Branched or straight chain alkoxy, C3-C 20 Branched or straight chain cycloalkyl, C6-C 30 Aromatic groups, C5-C 30 At least one of the heteroaromatic groups.

[0007] In one embodiment, A1 and A2 are each independently selected from at least one of a carboxylic acid group, a carboxylate group, a sulfonic acid group, a sulfonate group, a sulfuric acid group, a sulfate group, a phosphoric acid group, a phosphate group, an amino group, an amide group, a urea group, a thiourea group, a hydroxyl group, a thiol group, an ammonium salt group, a quaternary ammonium salt group, a phosphonium salt group, a quaternary phosphonium salt group, an imidazolium salt group, a pyridinium salt group, an ammonium oxide group, a polyether group, an alkyl glycoside group or a polysaccharide group.

[0008] In one embodiment, A1 and A2 are each independently selected from at least one of a quaternary ammonium salt group, a carboxylic acid group, an amino group, an amide group, an alkyl glycoside group, a thiourea group, and a hydroxyl group.

[0009] In one embodiment, when the heteroatom is selected from silicon atoms, the number of carbon atoms or silicon atoms in R is independently selected from 8-1000;

[0010] And / or, the molecular weight of R is 100-10000.

[0011] In one embodiment, the surfactant is selected from

[0012] At least one of .

[0013] In one embodiment, the water-soluble polymer is selected from at least one of polysaccharide polymers, polyether polymers, polyamide polymers, polysulfone polymers, polysulfide polymers, polyacrylic acid polymers, polyacrylate polymers, polyacrylamide polymers, polyacrylonitrile polymers, polyvinyl acetate polymers, polyvinyl alcohol polymers, polyvinyl alkyl ether polymers, polyepoxide polymers, polyethyleneimine polymers, and polyionic liquid polymers.

[0014] In one embodiment, the mass of the polymer coating layer is 0.2%-80% of the mass of the silicon-based material;

[0015] And / or, the mass ratio of the water-soluble polymer to the surfactant is 0.1:50-30:0.1;

[0016] And / or, the polymer coating layer further includes at least one of a lithium salt additive, a conductive agent, and a cross-linking agent.

[0017] In one embodiment, the silicon-based material is selected from at least one of silicon microparticles, silicon nanoparticles, silicon-carbon materials, silicon-oxygen materials, and silicon alloy materials.

[0018] A method for preparing the negative electrode active material as described above comprises: dispersing a silicon-based material, a water-soluble polymer, and a surfactant in a solvent to obtain a first mixture, and drying the first mixture to obtain the negative electrode active material;

[0019] Alternatively, the silicon-based material and the water-soluble polymer are dispersed in a solvent to obtain a second mixture, the second mixture is dried to obtain a composite, the composite and a surfactant are dispersed in a solvent to obtain a third mixture, and the third mixture is dried to obtain the negative electrode active material.

[0020] In one embodiment, the mass ratio of the silicon-based material to the water-soluble polymer and the surfactant is 100:(0.1-30):(0.1-50);

[0021] and / or, the dispersion speed is 100 rpm-5000 rpm;

[0022] and / or, the drying temperature is 25°C-200°C;

[0023] And / or, the first mixture further includes at least one of a lithium salt additive, a conductive agent, and a cross-linking agent;

[0024] And / or, the second mixture further includes at least one of a lithium salt additive, a conductive agent, and a cross-linking agent.

[0025] A negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer, wherein the negative electrode active material layer comprises the negative electrode active material as described above.

[0026] A battery comprises the negative electrode sheet as described above.

[0027] In the negative electrode active material described in the present invention, a water-soluble polymer cooperates with a surfactant with a special structure to be coated on the surface of a silicon-based material to form a polymer coating layer. In the polymer coating layer, both the R hydrophobic chain of the surfactant and the water-soluble polymer can act on the surface of the silicon-based material, and there is a hydrophobic interaction force between the R hydrophobic chain of the surfactant and the hydrophobic group in the water-soluble polymer, thereby forming a hydrophobic protective layer coated on the surface of the silicon-based material. At the same time, the hydrophilic double-headed structure in the surfactant is mainly distributed in a U-shape on the surface of the hydrophobic protective layer to form a hydrophilic outer layer, thereby forming a double-layer protective structure of inner layer hydrophobic-outer layer hydrophilic with a special water contact angle, which can not only utilize the hydrophobic effect of the inner layer to reduce the side reaction between silicon and water and effectively inhibit the gas production, but also can improve the dispersion effect of the negative electrode active material in the aqueous slurry through the hydrophilic effect of the outer layer.

[0028] In addition, when the silicon-based material expands in volume, the surfactant with a special structure can release stress by being stretched, thereby effectively inhibiting the volume expansion of the negative electrode active material and thereby improving the stability and safety of the battery. DETAILED DESCRIPTION

[0029] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.

[0031] In traditional technology, considering that the carbon structure on the surface of silicon-based materials is a hydrophobic layer, which is not conducive to the dispersion of silicon-based materials in water, it is usually preferred to coat the surface of silicon-based materials with hydrophilic polymers to improve their dispersibility during the homogenization process. However, the hydrophilic polymers on the surface will also cause more serious side reactions between silicon-based materials and water, thereby aggravating the gas production problem during the homogenization process.

[0032] Based on this, the present invention provides a negative electrode active material, including a silicon-based material and a polymer coating layer coated on the surface of the silicon-based material, the polymer coating layer includes a water-soluble polymer and a surfactant, and the water contact angle of the polymer coating layer is 65°-85°.

[0033] The chemical formula of the surfactant is A1-R-A2, wherein A1 and A2 are independently selected from polar groups containing at least one element of N, O, P, and S, and R is selected from substituted or unsubstituted C8-C 50 Aliphatic hydrocarbon chain segments, substituted or unsubstituted C8-C 50 Aliphatic hydrocarbon chain segments containing heteroatoms, substituted or unsubstituted C8-C 50 Alicyclic hydrocarbon segments, substituted or unsubstituted C8-C 50 Alicyclic hydrocarbon segments containing heteroatoms, substituted or unsubstituted C8-C 50 Aromatic hydrocarbon segments, substituted or unsubstituted C8-C 50 Aromatic hydrocarbon chain containing heteroatoms, the substituents are selected from C1-C 20 branched or straight chain hydrocarbon group, C1-C 20 Branched or straight chain alkoxy, C3-C 20 Branched or straight chain cycloalkyl, C6-C 30 Aromatic groups, C5-C 30 At least one of the heteroaromatic groups.

[0034] In the negative electrode active material described in the present invention, a water-soluble polymer cooperates with a surfactant with a special structure to be coated on the surface of a silicon-based material to form a polymer coating layer. In the polymer coating layer, both the R hydrophobic chain of the surfactant and the water-soluble polymer can act on the surface of the silicon-based material, and there is a hydrophobic interaction force between the R hydrophobic chain of the surfactant and the hydrophobic group in the water-soluble polymer, thereby forming a hydrophobic protective layer coated on the surface of the silicon-based material. At the same time, the hydrophilic double-headed structure in the surfactant is mainly distributed in a U-shape on the surface of the hydrophobic protective layer to form a hydrophilic outer layer, thereby forming a double-layer protective structure of inner hydrophobic layer-outer hydrophilic layer with a special water contact angle, which can not only utilize the inner layer hydrophobic effect to reduce the side reaction between silicon and water and effectively inhibit the gas production, but also can improve the dispersion effect of the negative electrode active material in the aqueous slurry through the outer layer hydrophilic effect and the non-covalent bond interaction formed by the hydrophilic double-headed structure in the surfactant and the hydrophilic group in the water-soluble polymer.

[0035] In addition, on the one hand, when the silicon-based material expands in volume, the surfactant with a special structure can release stress by being stretched, thereby effectively inhibiting the volume expansion of the negative electrode active material; on the other hand, the surfactant also has a role similar to that of a cross-linking agent, and is cross-linked with the water-soluble polymer through non-covalent bonds and coated on the surface of the silicon-based material, thereby improving the mechanical properties of the coating layer.

[0036] Therefore, using the negative electrode active material of the present invention in a battery is beneficial to improving the stability and safety of the battery and extending its service life.

[0037] It should be noted that the surfactant can form a composite coating layer outside the water-soluble polymer, or can be blended with the water-soluble polymer to form a cross-linked coating layer. The present invention does not limit the positional relationship between the surfactant and the water-soluble polymer.

[0038] In one embodiment, the surfactant includes but is not limited to at least one of anionic surfactants, cationic surfactants, zwitterionic surfactants and nonionic surfactants.

[0039] Specifically, A1 and A2 are each independently selected from at least one of a carboxylic acid group, a carboxylate group, a sulfonic acid group, a sulfonate group, a sulfuric acid group, a sulfate group, a phosphoric acid group, a phosphate group, an amino group, an amide group, a urea group, a thiourea group, a hydroxyl group, a sulfhydryl group, an ammonium salt group, a quaternary ammonium salt group, a phosphonium salt group, a quaternary phosphonium salt group, an imidazolium salt group, a pyridinium salt group, an ammonium oxide group, a polyether group, an alkyl glycoside group or a polysaccharide group, and are preferably at least one of a quaternary ammonium salt group, a carboxylic acid group, an amino group, an amide group, an alkyl glycoside group, a thiourea group or a hydroxyl group.

[0040] The heteroatom in R includes but is not limited to at least one of an oxygen atom, a sulfur atom, a nitrogen atom, a silicon atom and a phosphorus atom. When the heteroatom is selected from a silicon atom, it can be understood that R is an organic silane segment. Preferably, the number of carbon atoms or silicon atoms in R is independently selected from 8-1000, preferably 8-40.

[0041] In one embodiment, the molecular weight of R is 100-10000, preferably 100-700.

[0042] In one embodiment, R is preferably an unsubstituted C8-C 50 of aliphatic hydrocarbon chains.

[0043] In one embodiment, the surfactant is preferably

[0044] At least one of .

[0045] In one embodiment, the water-soluble polymer is selected from at least one of polysaccharide polymers, polyether polymers, polyamide polymers, polysulfone polymers, polysulfide polymers, polyacrylic acid polymers, polyacrylate polymers, polyacrylamide polymers, polyacrylonitrile polymers, polyvinyl acetate polymers, polyvinyl alcohol polymers, polyvinyl alkyl ether polymers, polyepoxide polymers, polyethyleneimine polymers, and polyionic liquid polymers.

[0046] Preferably, the water-soluble polymer is selected from at least one of polyvinyl alcohol (PVA), polyethylene glycol (PEG), polyacrylamide (PAM), polyacrylic acid (PAA) and its salts, polyethyleneimine (PEI), sodium polyvinyl sulfate (PVS), sodium carboxymethyl cellulose (CMC-Na), polyimidazole salts, polyquaternary ammonium salts, polyquaternary phosphonium salts, gelatin, sodium alginate, sodium xylan polysulfate, chitosan, and polyvidone (PVP).

[0047] It is understandable that the above-mentioned water-soluble polymers also include their corresponding physically or chemically modified polymers, and the monomers corresponding to any two or more polymers can be copolymerized to form one or more forms of random copolymers, alternating copolymers, block copolymers, and graft copolymers, and the present invention is not limited to this.

[0048] In one embodiment, the molecular weight of the water-soluble polymer is 1,000-1,000,000.

[0049] In one embodiment, the mass of the polymer coating layer is 0.2%-80% of the mass of the silicon-based material, preferably 2%-20%.

[0050] In one embodiment, the mass ratio of the water-soluble polymer to the surfactant is 0.1:50-30:0.1, preferably 0.1:1-10:1.

[0051] In one embodiment, the polymer coating layer further includes at least one of a lithium salt additive, a conductive agent, and a cross-linking agent.

[0052] Specifically, the conductive agent includes but is not limited to at least one of graphene, acetylene black, carbon black, single-walled carbon nanotubes, multi-walled carbon nanotubes, flake graphite, polyaniline, polypyrrole, polyacetylene, polythiophene, and poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid (PEDOT:PSS).

[0053] The lithium salt additive includes, but is not limited to, at least one of lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) and lithium bis(fluorosulfonyl)imide (LiFSI).

[0054] In one embodiment, the silicon-based material is selected from at least one of silicon microparticles, silicon nanoparticles, silicon-carbon materials, silicon-oxygen materials, and silicon alloy materials.

[0055] It should be noted that the present invention does not limit silicon-based materials. Silicon-based materials can be prepared by chemical vapor deposition, sol-gel method, high-temperature pyrolysis method, mechanical ball milling method, hydrothermal synthesis method and electrospinning method, and can also be made into composite silicon-based materials with other materials through physical or chemical methods.

[0056] The present invention also provides a method for preparing the negative electrode active material as described above, comprising: dispersing a silicon-based material, a water-soluble polymer, and a surfactant in a solvent to obtain a first mixture, and drying the first mixture to obtain the negative electrode active material; or dispersing a silicon-based material and a water-soluble polymer in a solvent to obtain a second mixture, and drying the second mixture to obtain a composite, and then dispersing the composite and a surfactant in a solvent to obtain a third mixture, and drying the third mixture to obtain the negative electrode active material.

[0057] In the preparation method described in the present invention, the hydrophilic groups in the water-soluble polymer are combined with the silicon atoms on the surface of the silicon-based material through hydrogen bonding, and the hydrophobic groups are combined with the carbon atoms on the surface of the silicon-based material through hydrophobic interactions. At the same time, the surfactant forms a U-shaped structure in the solvent, wherein the middle part of the U-shaped structure is a hydrophobic segment, which can be combined with the carbon atoms on the surface of the silicon-based material through hydrophobic interactions, and the two heads of the U-shaped structure are divided into polar hydrophilic ends, which can increase the dispersibility of the silicon-based material in water through hydrophilic interactions, and there is also a hydrophobic interaction force between the hydrophobic segments of the surfactant and the hydrophobic groups of the water-soluble polymer, so that the surfactant has an effect similar to that of a cross-linking agent, which is beneficial to improving the mechanical properties of the coating layer.

[0058] In one embodiment, the mass ratio of the silicon-based material to the water-soluble polymer and the surfactant is 100:(0.1-30):(0.1-50), preferably 100:(1-10):(1-10).

[0059] In one embodiment, the dispersion rotation speed is 100 rpm-5000 rpm, including but not limited to any point value of 100 rpm, 500 rpm, 1000 rpm, 1500 rpm, 2000 rpm, 2500 rpm, 3000 rpm, 3500 rpm, 4000 rpm, 4500 rpm, and 5000 rpm, or a range value between any two of them.

[0060] In one embodiment, the drying temperature is 25°C-200°C, including but not limited to any one of 25°C, 50°C, 60°C, 100°C, 120°C, 150°C, 180°C, 200°C or a range between any two of them.

[0061] In one embodiment, the drying method is selected from at least one of hot air drying, spray drying or vacuum drying.

[0062] It should be noted that the solvent includes but is not limited to water, preferably water; the dispersion speed, drying temperature and drying method for preparing the first mixture, the second mixture and the third mixture can be the same or different, and the present invention does not limit this.

[0063] In one embodiment, the first mixture and / or the second mixture further comprises at least one of a lithium salt additive, a conductive agent, and a cross-linking agent.

[0064] Specifically, the conductive agent includes but is not limited to at least one of graphene, acetylene black, carbon black, single-walled carbon nanotubes, multi-walled carbon nanotubes, flake graphite, polyaniline, polypyrrole, polyacetylene, polythiophene, and poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid (PEDOT:PSS).

[0065] The lithium salt additive includes, but is not limited to, at least one of lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) and lithium bis(fluorosulfonyl)imide (LiFSI).

[0066] The present invention also provides a negative electrode plate. The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer, and the negative electrode active material layer includes the negative electrode active material as described above. It is understandable that the negative electrode active material layer may also include materials such as a binder, and the present invention does not limit this.

[0067] The present invention also provides a battery. The battery includes the negative electrode plate as described above. It is understandable that the battery also includes a positive electrode plate, a separator and an electrolyte, and the present invention does not limit the positive electrode plate, the separator and the electrolyte.

[0068] The negative electrode active material, preparation method and application thereof will be further described below through the following specific examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, the conventional conditions or the conditions recommended by the manufacturer are followed. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0069] It should be noted that the silicon-based materials used in the examples and comparative examples were purchased from Zhejiang Lichen New Material Technology Co., Ltd., model C ONE-SC 1800, with a particle size of about 3 μm-7 μm and a specific surface area of ​​about 3 m 2 / g, the carbon content is about 51.23%, and the resistivity is about 4.63Ω·cm.

[0070] The surfactants used in the embodiments and comparative examples include: surfactant a (CAS: 1420-40-2), the chemical formula of which is Surfactant b (CAS: 821-38-5), chemical formula is Surfactant c (CAS: 946602-82-0), chemical formula is Surfactant d (CAS: 710311-41-4), chemical formula is Surfactant e (CAS: 19101-02-1), chemical formula is

[0071] Example 1

[0072] 50 g of silicon-based material, 1 g of polyvinyl alcohol, 1 g of surfactant a and 0.5 g of graphene were added to 500 mL of water, and the mixture was mechanically stirred at 1000 rpm for 30 minutes at room temperature to obtain a mixture. The mixture was spray-dried at 200° C., and the dried product was then dried at 130° C. under vacuum conditions for 3 hours to obtain a negative electrode active material.

[0073] Example 2

[0074] 50 g of silicon-based material, 1 g of polyacrylamide, 1 g of surfactant b, 0.5 g of LiTFSI and 0.5 g of acetylene black were added to 500 mL of water, and the mixture was mechanically stirred at 200 rpm for 60 minutes at room temperature to obtain a mixture. The mixture was spray-dried at 150° C., and the dried product was then dried at 130° C. under vacuum conditions for 3 hours to obtain a negative electrode active material.

[0075] Example 3

[0076] 50 g of silicon-based material, 1 g of modified hydroxymethyl cellulose, 0.5 g of surfactant c, 0.5 g of LiFSI and 0.5 g of carbon black were added to 500 mL of water, and the mixture was mechanically stirred at 1000 rpm at room temperature for 30 minutes to obtain the mixture. The mixture was spray dried at 140°C, and the dried product was then dried under vacuum conditions at 150°C for 3 hours to obtain the negative electrode active material.

[0077] Example 4

[0078] 50 g of silicon-based material, 1 g of polyacrylamide, 0.2 g of surfactant d and 0.5 g of single-walled carbon nanotubes were added to 500 mL of water, and the mixture was mechanically stirred at 1500 rpm for 30 minutes at room temperature to obtain a mixture. The mixture was spray-dried at 150° C., and the dried product was then dried at 130° C. under vacuum conditions for 3 hours to obtain a negative electrode active material.

[0079] Example 5

[0080] 50 g of silicon-based material, 1 g of polyacrylic acid, 0.4 g of surfactant e and 0.5 g of single-walled carbon nanotubes were added to 500 mL of water, and the mixture was mechanically stirred at 1300 rpm for 30 minutes at room temperature to obtain a mixture. The mixture was spray-dried at 120° C., and the dried product was then dried at 130° C. under vacuum conditions for 3 hours to obtain a negative electrode active material.

[0081] Comparative Example 1

[0082] The difference between Comparative Example 1 and Example 1 is that surfactant a is not added.

[0083] Comparative Example 2

[0084] The difference between Comparative Example 2 and Example 1 is that no polyvinyl alcohol is added.

[0085] According to the ratio of water-soluble polymer and surfactant provided in Examples 1-5, a corresponding mixture was prepared, and the mixture was dropped onto a silicon wafer and spin-coated to form a film. Water was used as the test solvent, and the water contact angle was measured by a contact angle meter. The water contact angles of the polyvinyl alcohol used in Comparative Example 1 and the surfactant a used in Comparative Example 2 were tested in the same manner. The results are shown in Table 1.

[0086] Table 1

[0087]

[0088]

[0089] According to Table 1, Comparative Example 1 is the water contact angle of the polyvinyl alcohol-coated silicon-based material. Compared with Comparative Example 1, with the addition of surfactant a, the water contact angle of Example 1 is increased from 60° to 78°, which proves that the addition of surfactant effectively improves the overall hydrophilic and hydrophobic properties of the system and is conducive to maintaining dispersibility.

[0090] The negative electrode active materials prepared in Examples 1-5 and Comparative Examples 1-2 were subjected to gas generation tests and soft-pack battery tests.

[0091] (1) The gas production test method includes: taking 5 g of negative electrode active material and 50 g of water into a sealed bottle, fully dissolving them by centrifugal stirring, and then standing in a constant temperature room at 25°C, and testing the gas production (H2) in the bottle on the 1st day, the 3rd day, the 5th day and the 7th day respectively. The test results are shown in Table 2.

[0092] (2) The soft pack battery test method includes: doping the negative electrode active material with artificial graphite at a mass ratio of 2:8 and adding 0.5% carbon nanotubes (CNT) as the negative electrode, using NCM811 ternary material as the positive electrode material, using a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) with a volume ratio of 1:1 as the electrolyte solvent, using Celgard2400 membrane as the separator, preparing a soft pack lithium ion battery, and performing a cycle test (200 cycles of capacity retention rate), the test conditions are: voltage range: 2.5V-4.2V, charge and discharge 1C / 1C. The cycle test results are shown in Table 3.

[0093] Table 2

[0094]

[0095] According to the data in Table 2, it can be seen that Comparative Example 1 is a silicon-based material coated with polyvinyl alcohol, and the average daily gas production is about 4.23CC / kg / day; Example 1 is a silicon-based material co-coated with polyvinyl alcohol and a surfactant, and the average daily gas production is about 1.55CC / kg / day. Obviously, the silicon-based material co-coated with a water-soluble polymer and a surfactant provided in Examples 1-5 can effectively reduce the gas production of the silicon-based material.

[0096] Table 3

[0097]

[0098] According to the data in Table 3, it can be seen that the silicon-based material co-coated with the water-soluble polymer and the surfactant provided in Examples 1-5 effectively improves the first efficiency (about 1%) and cycle stability of the battery. In addition, it can be seen from Tables 1-3 that the comparative example 2 also reduces the gas production to a certain extent due to the absence of the hydrophilic polyvinyl alcohol, but at the same time, due to the absence of the polyvinyl alcohol, its dispersibility is poor, resulting in the negative electrode material being easily agglomerated or precipitated after the battery is cycled 200 times, thereby reducing the cycle stability. The silicon-based material co-coated with the water-soluble polymer and the surfactant provided by the present invention not only has excellent dispersibility, but can also effectively inhibit the gas production and volume expansion, significantly improving the stability and safety of the battery.

[0099] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0100] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A negative electrode active material, characterized in that: The negative electrode active material comprises a silicon-based material and a polymer coating layer coated on the surface of the silicon-based material, wherein the polymer coating layer comprises a water-soluble polymer and a surfactant, and the water contact angle of the polymer coating layer is 65°-85°; The chemical formula of the surfactant is A1-R-A2, wherein A1 and A2 are independently selected from polar groups containing at least one element of N, O, P, and S, and R is selected from substituted or unsubstituted C8-C 50 Aliphatic hydrocarbon chain segments, substituted or unsubstituted C8-C 50 Aliphatic hydrocarbon chain segments containing heteroatoms, substituted or unsubstituted C8-C 50 Alicyclic hydrocarbon segments, substituted or unsubstituted C8-C 50 Alicyclic hydrocarbon segments containing heteroatoms, substituted or unsubstituted C8-C 50 Aromatic hydrocarbon segments, substituted or unsubstituted C8-C 50 Aromatic hydrocarbon chain containing heteroatoms, the substituents are selected from C1-C 20 branched or straight chain hydrocarbon group, C1-C 20 Branched or straight chain alkoxy, C3-C 20 Branched or straight chain cycloalkyl, C6-C 30 Aromatic groups, C5-C 30 At least one of the heteroaromatic groups.

2. The negative electrode active material according to claim 1, characterized in that A1 and A2 are each independently selected from at least one of a carboxylic acid group, a carboxylate group, a sulfonic acid group, a sulfonate group, a sulfuric acid group, a sulfate group, a phosphoric acid group, a phosphate group, an amino group, an amide group, a urea group, a thiourea group, a hydroxyl group, a mercapto group, an ammonium salt group, a quaternary ammonium salt group, a phosphonium salt group, a quaternary phosphonium salt group, an imidazolium salt group, a pyridinium salt group, an ammonium oxide group, a polyether group, an alkyl glycoside group or a polysaccharide group.

3. The negative electrode active material according to claim 2, characterized in that: A1 and A2 are each independently selected from at least one of a quaternary ammonium salt group, a carboxylic acid group, an amino group, an amide group, an alkyl glycoside group, a thiourea group, and a hydroxyl group.

4. The negative electrode active material according to claim 1, characterized in that When the heteroatom is selected from silicon atoms, the number of carbon atoms or silicon atoms in R is independently selected from 8 to 1000; And / or, the molecular weight of R is 100-10000.

5. The negative electrode active material according to claim 1, characterized in that The surfactant is selected from At least one of .

6. The negative electrode active material according to claim 1, characterized in that The water-soluble polymer is selected from at least one of polysaccharide polymers, polyether polymers, polyamide polymers, polysulfone polymers, polysulfide polymers, polyacrylic acid polymers, polyacrylate polymers, polyacrylamide polymers, polyacrylonitrile polymers, polyvinyl acetate polymers, polyvinyl alcohol polymers, polyvinyl alkyl ether polymers, polyepoxide polymers, polyethyleneimine polymers, and polyionic liquid polymers.

7. The negative electrode active material according to claim 1, characterized in that The mass of the polymer coating layer is 0.2%-80% of the mass of the silicon-based material; And / or, the mass ratio of the water-soluble polymer to the surfactant is 0.1:50-30:0.1; And / or, the polymer coating layer further includes at least one of a lithium salt additive, a conductive agent, and a cross-linking agent.

8. The negative electrode active material according to claim 1, characterized in that The silicon-based material is selected from at least one of silicon microparticles, silicon nanoparticles, silicon-carbon materials, silicon-oxygen materials, and silicon alloy materials.

9. A method for preparing a negative electrode active material according to any one of claims 1 to 8, characterized in that: include: Dispersing a silicon-based material, a water-soluble polymer, and a surfactant in a solvent to obtain a first mixture, and drying the first mixture to obtain the negative electrode active material; Alternatively, the silicon-based material and the water-soluble polymer are dispersed in a solvent to obtain a second mixture, the second mixture is dried to obtain a composite, the composite and a surfactant are dispersed in a solvent to obtain a third mixture, and the third mixture is dried to obtain the negative electrode active material.

10. The method for preparing the negative electrode active material according to claim 9, characterized in that: The mass ratio of the silicon-based material to the water-soluble polymer and the surfactant is 100:(0.1-30):(0.1-50); and / or, the dispersion speed is 100 rpm-5000 rpm; and / or, the drying temperature is 25°C-200°C; And / or, the first mixture further includes at least one of a lithium salt additive, a conductive agent, and a cross-linking agent; And / or, the second mixture further includes at least one of a lithium salt additive, a conductive agent, and a cross-linking agent.

11. A negative electrode plate, characterized in that: The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer, and the negative electrode active material layer comprises the negative electrode active material according to any one of claims 1 to 8.

12. A battery, characterized in that: Comprising the negative electrode sheet as claimed in claim 11.

Citation Information

Patent Citations

  • Composite anode active material, method of preparing the same, and anode and lithium secondary battery

    CN105742584A

  • Micron silicon-carbon composite material for negative electrode of lithium ion battery and preparation method of micron silicon-carbon composite material

    CN115241426A

  • Silicon-carbon composite negative electrode material and preparation method and application thereof

    CN116259725A

  • Pretreatment method for physical dispersion of silicon nanowires and application of pretreatment method

    CN116936785A

  • Modified silicon-based negative electrode active material as well as preparation method and application thereof

    CN118335919A