Solid state battery

By using a combined design of active materials, sulfide cathode electrolyte, conducting single ion buffer and borohydride adhesive layer in solid-state batteries, the cost, mechanical strength and conductivity challenges of solid-state batteries are solved, achieving efficient Lithium ion conduction and battery stability.

CN119092792APending Publication Date: 2024-12-06QUANTUMSPACE BATTERY INC

Patent Information

Application Number
CN202411404235.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2018-06-06
Filing Date
2019-06-06
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the commercialization process, existing solid-state batteries face problems of high cost, low mechanical strength and ionic conductivity, and conducting single-ion solid-state electrolytes are difficult to remain stable in the 0-5V voltage range in Li+ batteries.

Method used

Design of solid electrochemical cell with active material, sulfide cathode electrolyte, solid buffering agent that conducts single ions and borohydride adhesive layer, by mixing buffering agents in the positive electrode layer and filling lithium with garnet layer with the positive electrode. A borohydride adhesive layer is used between the layers to form an efficient ion conduction path.

Benefits of technology

The efficient conduction of lithium ions and the mechanical strength of the battery are achieved at an area specific resistance (ASR) of less than 50Ω-cm2, reducing the cost of the battery and maintaining dynamic stability within the 2.7-4.2V voltage window.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092792A_ABST
    Figure CN119092792A_ABST
Patent Text Reader

Abstract

A solid state battery structure includes an oxide electrolyte in contact with an anode of an electrochemical cell and a sulfide electrolyte in contact with a cathode of the electrochemical cell.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to the following patent application: Application date June 6, 2018, entitled "HYBRIDSOLID-STATE BATTERY", Provisional Patent Application No. 62 / 681,576, the entire contents of which are incorporated herein by reference for all purposes. Technical Field

[0003] The present invention relates to solid-state rechargeable batteries, also known as secondary batteries. Background Art

[0004] When there is a solid electrolyte separator between the positive and negative electrodes of a battery cell, the battery is called a solid-state battery. Solid electrolytes do not contain flammable organic solvents and have good application prospects in consideration of safety factors.

[0005] Solid-state batteries can operate over a wider range of temperatures, voltages, and pressures than liquid electrolyte batteries. Solid-state batteries can also include solid-state positive and negative electrodes. For example, a solid-state battery can include a lithium metal negative electrode. The lithium metal negative electrode can maximize the voltage difference between the positive and negative electrodes, thus making Li + Maximizing energy density in batteries. Solid-state rechargeable batteries are expected to be safer (e.g., less flammable) and have higher energy and power densities than liquid electrolyte batteries currently on the market. However, a number of unresolved difficulties remain that prevent solid-state batteries from achieving commercialization.

[0006] Some solid-state battery researchers have used monolithically integrated single-ion conductors as the electrolyte separator between the positive and negative electrodes. There are many problems with this approach. For example, to date, no single-ion conducting solid electrolyte has both high enough ionic conductivity and high enough mechanical strength, is commercially cost-effective, lightweight enough for certain uses, and is stable to Li in the 0-5V voltage range. To date, solid-state batteries have inevitably made design trade-offs to address these issues.

[0007] Some researchers have tried to add more than one type of solid electrolyte to a solid-state electrochemical cell. For example, some researchers have prepared an oxide-sulfide composite material of a lithium superion conductor. See J. Mater. Chem. A, 2014, 2, 4111-4116 DOI: 10.1039 / C3TA15223E, which proposes an oxide-sulfide composite including a mixture of lithium-filled garnet powder and lithium phosphide sulfide (LPS) powder. See also the abstract section of http: / / ma.ecsdl.org / content / MA2016-01 / 2 / 264, which describes a lithium metal anode, a solid oxide electrolyte (LLZO) and a 75Li superion conductor. 2 S:25P 2 S 5 Sulfide electrolytes and TiS 2 See also Y.Kato et al., DOI: 10.1038 / NENERGY.2016.30, which reported the electrochemical effect of a composite cathode composed of LiNbO 3 Coated LiCoO 2 Positive electrode active materials and certain sulfide solid electrolytes (Li 9.6 P 3 S 12 , Li 10 G 2 S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 ) electrochemical cycle data of electrochemical cells. See also Suzuki et al., Journal of Power Sources 359 (2017) 97-103, which proposed a solid-state battery. The results of these reports have multiple drawbacks, including low capacity and capacity decay over time.

[0008] Since the above problems and other problems in related fields still have a series of unresolved difficulties, it is necessary to propose corresponding solutions. This patent provides compositions, processes and methods that overcome various difficulties and problems. Summary of the invention

[0009] In one embodiment, a solid-state electrochemical cell (SSEC) is provided, which includes (a) a positive electrode layer containing an active material and a sulfide cathode electrolyte; (b) a solid buffer that conducts a single ion; (c) a borohydride bonding layer; (d) a lithium-filled garnet layer. The buffer is mixed in the positive electrode layer, or as a layer in contact with the positive electrode layer, or the buffer is mixed in the positive electrode layer and the buffer is as a layer in contact with the positive electrode layer. The borohydride bonding layer is between the lithium-filled garnet layer and (i) the positive electrode layer in which the buffer is mixed or (ii) the buffer layer in contact with the positive electrode, and is in contact with them.

[0010] In a second embodiment, a method for manufacturing an electrochemical cell is proposed, the method comprising the following steps: (a) providing a first slurry comprising an active material, a cathode electrolyte and a solvent; (b) depositing the first slurry onto a current collector; (c) drying the first slurry; (e) providing a second slurry containing a solid buffer that conducts a single ion; (f) depositing the second slurry onto a substrate; (g) drying the deposited second slurry to form a buffer layer; (h) transferring the buffer layer to the first slurry after drying to form a stack; (i) pressurizing and heating the stack; (j) providing a solid separator; (k) depositing a borohydride layer onto the solid separator; (l) combining the stack with the solid separator having the borohydride layer thereon to form an electrochemical cell stack; and (m) pressurizing and heating the electrochemical cell stack.

[0011] In one aspect, a solid-state electrochemical stack is provided, comprising: (a) a positive electrode layer comprising a positive electrode active material, a binder and a sulfide cathode electrolyte, the positive electrode layer having a porosity of less than 15% v / v; (b) a buffer layer comprising a sulfide electrolyte in contact with the positive electrode layer, the buffer layer having a porosity of less than 15% v / v; (c) a separator layer comprising a material selected from the group consisting of lithium-filled garnet and LPSX, the separator layer having a porosity of less than 10% v / v; and the buffer layer is between the positive electrode layer and the separator layer.

[0012] On the other hand, a method for manufacturing a solid-state electrochemical stack is provided, comprising: (a) pouring a first slurry containing a sulfide solid electrolyte powder onto a first substrate to form a first layer; (b) pouring a second slurry containing a sulfide solid electrolyte powder and a positive electrode active powder onto a second substrate to form a second layer; (c) calendering the first layer and the second layer, wherein the first layer and the second layer are in direct contact with each other. On the other hand, the present patent provides a double-layer stack, comprising: (a) a positive electrode layer containing an active material and a sulfide cathode electrolyte; and (b) a solid buffer that conducts a single ion, the buffer being mixed in the positive electrode layer, or being a layer in contact with the positive electrode layer, or being mixed in the positive electrode layer and in contact with the positive electrode layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 Schematic diagram of an electrochemical cell.

[0014] Figure 2 A cross-sectional scanning electron microscope image (cross-section generated by a focused ion beam) of a solid state cathode (SSC), a buffer layer, an adhesive layer, and a garnet film in the electrochemical cell fabricated in Example 1 is shown. Figure 2 The scale bar in the figure is 50 μm. The imaging conditions are: working distance 4.4 mm, high voltage 5.00 kV, high frequency resistance welded pipe (HFW) 207 μm, magnification 2000x, function TLD, tilt 52°, BSE mode.

[0015] Figure 3 This is a curve diagram of the change in voltage versus active mass specific capacity (mAh / g) within 50 cycles described in Example 2.

[0016] Figure 4 is a graph of the active mass specific discharge capacity (mAh / g) described in Example 2 as a function of cycle number.

[0017] Figure 5 3 is a graph showing the relationship between the ASR and the static voltage described in Example 2.

[0018] Figure 6 is a schematic diagram of an electrochemical cell including a separator, a buffer layer and a positive electrode layer.

[0019] Figure 7 is a schematic diagram of an electrochemical cell including a separator, a bonding layer and a positive electrode layer.

[0020] Figure 8 The lithium ion conductivity (Log (S / cm)) of a series of LBHI compositions and LBHI compositions doped with amide at 60°C is shown. As shown in the figure, (A) is LiBH 4 :LiI(3:1), (B) is LiNH 2 :LiBH 4 :LiI(3:3:2), (C) is LiNH 2 :LiBH 4 :LiI(9:3:4) and (D) are LiNH 2 :LiBH 4 :LiI(9:3:2).

[0021] Fig. 9 Cycling data is shown for a solid-state electrochemical cell in Example 13 comprising a lithium-filled garnet electrolyte membrane bonded to a solid cathode membrane with LPSI. Detailed description

[0022] General Notes

[0023] In some embodiments, the present invention discloses a material that exhibits a thermal conductivity of less than 50 Ω-cm at room temperature. 2 An electrochemical cell of an ASR. The electrochemical cell disclosed in this patent includes an oxide electrolyte membrane and a sulfide electrolyte membrane. The electrochemical cell described in this patent includes a sulfide-oxide solid electrolyte interface. An adhesive layer comprising borohydride is used to bond the oxide electrolyte membrane and the sulfide electrolyte membrane. The oxide electrolyte membrane is kinetically stable to metallic Li and has suitable mechanical strength to conduct Li ions at high current density. The sulfide cathode electrolyte in the solid cathode and / or the sulfide buffer layer adjacent to the solid cathode provides a conductive path for lithium ions, which is suitable for use when the positive electrode is loaded with highly active substances. In some embodiments, the sulfide cathode electrolyte is kinetically stable to coated active materials (e.g., LZO-coated NCA or LZO-coated NMC). In some instances, the sulfide cathode electrolyte is kinetically stable to coated active materials (e.g., LZO-coated NCA) at a voltage window of 2.7-4.2V relative to Li. The borohydride bonding layer bonds the oxide electrolyte membrane and the sulfide (buffer) electrolyte membrane and provides an ion conducting path between the two electrolyte membranes.

[0024] In some embodiments, the electrochemical cell disclosed in the present patent includes an oxide solid separator in contact with the negative electrode side of the electrochemical cell and a sulfide solid separator in contact with the positive electrode side of the electrochemical cell. In some embodiments, both the sulfide and oxide solid separators have high lithium ion conductivity, for example, greater than 1*10 -3 S / cm 2 In some embodiments, between the oxide solid membrane and the sulfide solid membrane is an adhesive layer made of borohydride. In some embodiments, on the side of the oxide solid membrane opposite to the borohydride adhesive layer is a lithium metal negative electrode. In some embodiments, on the side of the sulfide solid membrane opposite to the borohydride adhesive layer is a positive electrode.

[0025] definition

[0026] If a definition in any material incorporated by reference into this patent conflicts with a definition in this patent, the definition in this patent shall control.

[0027] The term "about" as used in this patent, when used to define a number, such as about 15% w / w, refers to the stated value and optionally includes a value within the range of ±10% of the stated value. For example, about 15% w / w includes 15% w / w and 13.5% w / w, 14% w / w, 14.5% w / w, 15.5% w / w, 16% w / w or 16.5% w / w. For example, "about 75°C" includes 75°C and 68°C, 69°C, 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C or 83°C.

[0028] The term "active material" as used in this patent refers to a material that intercalates or converts to lithium in a reversible reaction, making the active material suitable for use in a rechargeable battery. Active materials may include intercalating materials such as NCA or NMC. Active materials may include, for example, materials that convert to FeF 3 For example, the active material may include, but is not limited to, all active materials described in U.S. Patent No. US20160211517A1, entitled “LITHIUM RICH NICKEL MANGANESE COBALT OXIDE”, published on July 21, 2016.

[0029] The term "amorphous body" used in this patent refers to a material that is non-crystalline or does not contain a crystalline phase as the main phase. "Amorphous body" refers to a material that does not exhibit crystalline characteristics, for example, clear X-ray diffraction peaks measured by X-ray diffraction. Amorphous materials are at least mainly amorphous, and are characterized by more amorphous components than crystals. Basically amorphous bodies refer to materials that do not include clear X-ray diffraction peaks or X-ray diffraction patterns characterized by broad reflections, and the broad reflections are interpreted by those skilled in the art as the main components being amorphous phases. In fact, amorphous materials can have nanoscale crystalline domains, but are still characterized by x-ray diffraction images as being mainly amorphous phases. In amorphous materials, certain transmission electron microscope (TEM) area diffraction patterns (SADP) can be displayed as crystalline domains, but the main component of the material is still displayed as an amorphous body.

[0030] The terms "semi-amorphous" or "semi-crystalline" as used in this patent refer to compositions having both crystalline and amorphous domains. In addition to an amorphous component, a semi-crystalline material also includes nanocrystalline and / or microcrystalline components. A semi-crystalline material is a partially crystalline material, or a material that includes some crystalline blocks and some amorphous blocks. For example, a material heated to a crystallization temperature but then cooled before all of the material is completely crystallized is a semi-crystalline material as described in this patent. An XRD powder pattern can characterize a semi-crystalline material as described in this patent, wherein the main peak of highest intensity has a full width at half maximum at at least 1° (2θ) or at least 2° (2θ), or at least 3° (2θ).

[0031] The term "anolyte" as used in this patent refers to an ionically conductive material that is mixed, layered or laminated to the anode material or anode current collector.

[0032] The term "applying pressure" as used in this patent refers to the process by which an external device, such as a calender, applies pressure to another material.

[0033] The term "at least one selected from the group" described in this patent includes selecting one or more items or combinations thereof from the group. Selected from the group consisting of A, B, and C, including, for example, only A, only B, or only C, and any combination of A and B, A and C, B and C, and A, B, C, or A, B, C.

[0034] The term "ASR" as used in this patent refers to area specific resistance. ASR is measured using electrochemical impedance spectroscopy (EIS). EIS can be measured on a VMP3 instrument produced by Biologic or an equivalent instrument. In the ASR measurement, lithium contacts are deposited on both sides of the sample. While measuring the current, an AC voltage of 25mV rms is applied at a frequency of 300kHz-0.1mHz. EIS divides the ASR into bulk contribution and boundary ASR contribution by resolving the two semicircular patterns in the Nyquist plot.

[0035] The term "borohydride bonding layer" as used in this patent refers to a layer comprising a borohydride and bonding the lithium-filled garnet layer to the sulfide electrolyte layer or the sulfide containing buffer. Non-limiting examples of borohydrides include, but are not limited to, 3LiBH 4 2LiI 3LiNH 2 or 3LiBH 4 ·4LiI·9LiNH 2. Boron hydride is described in a patent application entitled “ELECTROLYTE SEPARATORS INCLUDING LITHIUM BOROHYDRIDE AND COMPOSITEELECTROLYTE SEPARATORS OF LITHIUM-STUFFED GARNET AND LITHIUM BOROHYDRIDE”, International PCT Patent Application No. PCT / US2017 / 057735, published on April 26, 2018, and published as WO2018 / 075972, the entire contents of which are incorporated herein by reference in their entirety for all purposes. Borohydride is mentioned in the patent application entitled “BOROHYDRIDE-SULFIDE INTERFACIAL LAYER IN ALL SOLID STATE BATTERY”, the international PCT patent application number is PCT / US2017 / 057739, the application date is October 20, 2017, the publication date is April 25, 2019, and the publication number is WO2019078897A1, and the entire content of which is incorporated by reference into this application for all purposes.

[0036] The term "binder" as used in this patent refers to a polymer having the ability to increase the adhesion and / or bonding of the electrode. Suitable binders include, but are not limited to, PVDF, PVDF-HFP, SBR, and ethylene α-olefin copolymers.

[0037] The term "buffer" as used in this patent refers to a solid electrolyte that conducts a single ion, which is fully mixed or combined with the positive electrode portion, or is a layer in direct contact with the positive electrode, for example, the solid electrolyte is an electrolyte layer laminated on the positive electrode layer. Conducting a single ion means that the material conducts only one type of ion, such as Li ions with a migration number greater than 0.9. Solid means that the buffer exists in a solid phase at ambient temperature and pressure.

[0038] The term "buffering agent mixed in the positive electrode layer" used in this patent means that when forming the positive electrode layer, the buffering material is ground, for example, milled, and then mixed with other positive electrode layer compounds such as active materials and conductive carbon.

[0039] The term "cast film" as used in this patent refers to the process of transferring or transferring a liquid or slurry into a mold or onto a substrate so that the liquid or slurry forms or becomes a film. Casting can be performed by doctor blade, metering rod, comma coater, gravure coater, micro gravure coating, reverse comma coater, coating die, slide mold and / or tape casting, among other methods.

[0040] As used herein, the term "characterized by a formula" refers to a description of the chemical composition of a compound.

[0041] The term "current collector" used in this patent refers to a component or layer in direct contact with an electrode in a secondary battery, and electrons are conducted to the electrode or leave from the electrode through the current collector to complete an external circuit. In some instances, the current collector is a metal (e.g., Al, Cu or Ni, steel, and alloys or combinations thereof) layer laminated to the positive or negative electrode. In some instances, the current collector is Al. In some instances, the current collector is Cu. In some instances, the current collector is Ni. In some instances, the current collector is steel. In some instances, the current collector is an alloy of Al. In some instances, the current collector is an alloy of Cu. In some instances, the current collector is an alloy of steel. In some instances, the current collector is Al. In some instances, the current collector is coated with carbon. In some instances, the current collector includes a combination of the above metals. During charge and discharge, electrons are conducted in the direction opposite to the Li ion flow and pass through the current collector when entering or leaving the electrode.

[0042] The term "diameter (d 90 )” refers to the size under the size distribution measured by microscopy or other particle size analysis techniques, including but not limited to scanning electron microscopy or dynamic light scattering. 90 Including a characteristic dimension, i.e., the particle size, means the total particle area (e.g., for 2D sampling methods such as microscopy) or volume (e.g., for 3D sampling methods such as light scattering) representing 90% of the particles is smaller than the stated dimension. In other words, in a particle mixture, d 90 In other words, the term "diameter (d 50 )” means a particle size (or volume) smaller than the stated size representing 50% of the total particle area (or volume). Similarly, the term “diameter (d 10 )" means that 10% of the total particle area (or volume) of the particles is smaller than the stated size. These figures can be calculated per unit volume or per unit area. If not explicitly stated, the unit volume shall be the standard.

[0043] The term "adhesive" used in this patent refers to a material that helps to adhere to another material. For example, as used in this patent, polyvinyl butyral is an adhesive because it can be used to bond garnet materials. Other adhesives may include polycarbonate. Other adhesives may include polyacrylates and polymethacrylates. These examples of adhesives are not limited to the scope of the adhesive described in this patent, and are only used as examples. Adhesives that can be used for the present disclosure include but are not limited to polypropylene (PP), polyethylene, atactic polypropylene (aPP), isotactic polypropylene (iPP), ethylene-propylene rubber (EPR), ethylene-pentene copolymer (EPC), polyisobutylene (PIB), styrene-butadiene rubber (SBR), polyolefins, polyethylene-co-1-octene (PE-co-PO), polyethylene-co-(methylene cyclopentane) (PE-co-PMCP), poly(methyl methacrylate) (and other acrylic acid), acrylic acid, polyvinyl acetal resin, polyvinyl butyral resin, PVB, polyvinyl acetal resin, three-dimensional block polypropylene, polypropylene polymethylpentene copolymer, polyethylene oxide (PEO), PEO block copolymer, silicone, etc. In some examples, including any of the foregoing, the binder is selected from polyacrylonitrile (PAN), polypropylene, polyethylene, polyethylene oxide (PEO), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyethylene oxide poly (allyl glycidyl ether) PEO-AGE, polyethylene oxide 2-methoxyethoxyethyl glycidyl ether (PEO-MEEGE), polyethylene oxide 2-methoxyethoxyethyl glycidyl poly (allyl glycidyl ether) (PEO The term "selected from the group consisting of" used in this patent includes selecting one or more items or combinations thereof from the group. Selected from the group consisting of A, B, and C, including, for example, only A, only B, or only C, as well as any combination of A and B, A and C, B and C, and A, B, C or A, B, C.

[0044] Unless otherwise specified, the term "contact" as used in this patent refers to direct contact. For conductive materials, contact means contact between the contacting materials sufficient to produce electrical conduction. For ion conductive materials, contact means contact between the contacting materials sufficient to produce ion conduction. Two materials in direct contact means that there are no interleaving layers between the two materials. The term "electrical contact" as used in this patent means contact sufficient to produce electrical conduction between the contacting materials.

[0045] The term "direct contact" as used in this patent, for conductive materials or ion conductive materials, means that the physical contact between the two materials is sufficient to allow electronic or ionic current to be conducted between them; for materials where one of the materials is electrically insulating or ion insulating, direct contact between the two materials means that the two materials share an interface that can transmit external force or pressure.

[0046] The term "electrical contact" as used in this patent means that two materials are in direct contact and can conduct electric current through the direct contact point.

[0047] The terms "cathode" and "anode" used in this patent refer to the electrodes of a battery. During the charge cycle of a lithium secondary battery, lithium ions leave the cathode and move to the anode through the electrolyte. During the charge cycle, electrons leave the cathode and move to the anode through an external circuit. During the discharge cycle of a lithium secondary battery, lithium ions migrate from the anode to the cathode through the electrolyte. During the discharge cycle, electrons leave the anode and move to the cathode through an external circuit.

[0048] The term "green film" or "green tape" as used in this patent refers to an unsintered tape or film comprising a lithium-filled garnet or a precursor of a lithium-filled garnet, and at least one binder, plasticizer, carbon, dispersant, solvent, or combination thereof. As used in this patent, "green film tape" refers to a cast roll, continuous layer, or cut portion of a dried or non-dried green film.

[0049] The term "electrochemical cell" or "cell" used in this patent refers to a single battery including a positive electrode and a negative electrode, which are ionically connected through an electrolyte. In some embodiments, the same cell includes multiple positive electrodes and / or multiple negative electrodes encapsulated in a container.

[0050] The term "electrochemical device" as used in this patent refers to an energy storage device, such as but not limited to a lithium secondary battery that operates or generates electricity or current through an electrochemical reaction, e.g. conversion chemical reaction.

[0051] The term "electrolyte" as used in this patent refers to an electrolyte that allows ions (such as Li +) in a secondary battery but does not allow ions (such as Li) to migrate through it. The ionic conductivity is at least 1000 times greater than the electronic conductivity. Electrolytes can be used to electrically insulate between the cathode and anode of a secondary battery, but allow ions (such as Li) to migrate through it. + ) through the electrolyte. In some examples, solid electrolytes rely on ion hopping and / or diffusion through a rigid structure. Solid electrolytes may also be referred to as fast ion conductors or superionic conductors. In this case, the solid electrolyte layer may also be referred to as a solid electrolyte membrane or a solid electrolyte membrane.

[0052] The term "energy storage electrode" used in this patent refers to an electrode suitable for use in an energy storage device such as a lithium rechargeable battery or a lithium secondary battery. Such an electrode can conduct electrons and lithium ions required for charging and discharging of a rechargeable battery.

[0053] The term "film thickness" as used in this patent refers to the distance or median measured distance between the top and bottom surfaces of a film. The term "thickness" as used in this patent refers to the distance or median measured distance between the top and bottom surfaces of each layer. As used in this patent, the top and bottom surfaces refer to the sides of the film having the largest surface area. Unless otherwise expressly stated, scanning electron microscopy is used to measure thickness.

[0054] The term "flat" surface as used in this patent refers to the maximum normal distance between the lowest point on a surface and the plane containing the three highest points on the surface, and also refers to the maximum normal distance between the highest point on a surface and the plane containing the three lowest points on the surface. It can be measured using an atomic force microscope (AFM), a high-precision optical microscope, or a laser interferometer to measure the height map of the surface.

[0055] The term "film" used herein refers to a film containing the components, components or materials described in this patent, and its average thickness is about 10nm to about 100μm. In some examples, "film" refers to a film with a thickness less than about 1μm, 10μm, or 50μm.

[0056] The "lithium interface impedance" used here refers to the interface impedance of the material to the incorporation of Li ions. The lithium interface ASR (ASR) is calculated from the interface impedance (Rinterface) by the following formula: interface ), ASR interface =R interface *A / 2, where: A represents the area of ​​contact between the electrode and the separator, the coefficient 2 represents two interfaces (in a symmetrical single cell), R interface =R total -R bulk , where R total is the total impedance, R bulk is the volume impedance.

[0057] The term "lithium-filled garnet" as used in this patent refers to an oxide having crystal structure characteristics associated with the garnet crystal structure. The entire content of the U.S. patent application with a filing date of October 7, 2014, a publication date of April 9, 2015, a patent application publication number of 2015 / 0099190, and a patent application number of 14 / 509,029 is incorporated herein by reference. This application describes lithium-filled garnet solid electrolytes for solid-state lithium rechargeable batteries. These lithium-filled garnets typically contain the components represented by the following formula: Li A La B M′ C M″ D Zr E O F 、Li A La B M′ C Mv D Ta E O F 或Li A La B M′ C M″ D Nb E O F , where 4 < A < 8.5, 1.5 < B < 4, 0 ≤ C ≤ 2, 0 ≤ D ≤ 2, 0 ≤ E < 2.5, 10 < F < 13, and M′ and M″ are each independently selected from Ga, Al, Mo, W, Nb, Sb, Ca, Ba, Sr, Ce, Hf, Rb, and Ta in each case; or Li a La b Zr c Al d Me” e O f , where 5 < a < 8.5, 2 < b < 4, 0 < c ≤ 2.5, 0 ≤ d < 2, 0 ≤ e < 2, 10 < f < 13, and Me” is a metal selected from Ga, Nb, Ta, V, W, Mo, and Sb; and other components as described in the patent with a U.S. patent application publication number of US2015 / 0099190. The lithium-filled garnets and garnets described in this patent generally include, but are not limited to, Li 7.0 La 3 (Zr t1 +Nb t2 +Ta t3 )O 12 +0.35Al 2 O 3; wherein δ represents 0-3 and (t1+t2+t3=2), so that the La:(Zr / Nb / Ta) ratio is 3:2. For example, δ is 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9 or 3.0. In some embodiments, the lithium-filled garnet contains Li 7±δ Li 3 Zr 2 O 12 ·xAl 2 O 3 In another embodiment, the lithium-filled garnet contains Li 7±δ Li 3 Zr 2 O 12 0.22Al 2 O 3 In other embodiments, the lithium-filled garnet contains Li 7±δ Li 3 Zr 2 O 12 0.35Al 2 O 3 In one embodiment, the lithium-filled garnet contains Li 7±δ Li 3 Zr 2 O 12 0.5Al 2 O 3 In another embodiment, the lithium-filled garnet contains Li 7±δ Li 3 Zr 2 O 12 0.75Al 2 O 3 Similarly, the garnet described in this patent includes but is not limited to Li x La 3 Zr 2 O F +yAl 2 O 3, where x is in the range of 5.5 to 9 and y is in the range of 0.05 to 1. In these examples, the subscripts x, y, and F are selected so that the garnet is charge neutral. In some examples, x is 7 and y is 1.0. In some examples, x is 5 and y is 1.0. In some examples, x is 6 and y is 1.0. In some examples, x is 8 and y is 1.0. In some examples, x is 9 and y is 1.0. In some examples, x is 7 and y is 0.35. In some examples, x is 5 and y is 0.35. In some examples, x is 6 and y is 0.35. In some examples, x is 8 and y is 0.35. In some examples, x is 9 and y is 0.35. In some examples, x is 7 and y is 0.7. In some examples, x is 5 and y is 0.7. In some instances, x is 6 and y is 0.7. In some instances, x is 8 and y is 0.7. In some instances, x is 9 and y is 0.7. In some instances, x is 7 and y is 0.75. In some instances, x is 5 and y is 0.75. In some instances, x is 6 and y is 0.75. In some instances, x is 8 and y is 0.75. In some instances, x is 9 and y is 0.75. In some instances, x is 7 and y is 0.8. In some instances, x is 5 and y is 0.8. In some instances, x is 6 and y is 0.8. In some instances, x is 8 and y is 0.8. In some instances, x is 9 and y is 0.8. In some instances, x is 7 and y is 0.5. In some instances, x is 5 and y is 0.5. In some instances, x is 6 and y is 0.5. In some instances, x is 8 and y is 0.5. In some instances, x is 9 and y is 0.5. In some instances, x is 7 and y is 0.4. In some instances, x is 5 and y is 0.4. In some instances, x is 6 and y is 0.4. In some instances, x is 8 and y is 0.4. In some instances, x is 9 and y is 0.4. In some instances, x is 7 and y is 0.3. In some instances, x is 5 and y is 0.3. In some instances, x is 6 and y is 0.3. In some instances, x is 8 and y is 0.3. In some instances, x is 9 and y is 0.3. In some instances, x is 7 and y is 0.22. In some instances, x is 5 and y is 0.22. In some instances, x is 6 and y is 0.22. In some instances, x is 8 and y is 0.22. In some examples, x is 9 and y is 0.22. The lithium-filled garnets described in this patent also include but are not limited to Li x La 3 Zr 2 O 12 +yAl 2 O 3 , wherein y ranges from 0 to 1, including 0 and 1. In one embodiment, the lithium-filled garnet contains Li 7 Li3 Zr 2 O 12 ingredients.

[0058] The garnet described in this patent does not include YAG garnet (i.e. yttrium aluminum garnet, or Y 3 Al 5 O 12 ). The garnet used in this patent does not include silicate-based garnets, such as pyrope, almandine, spessartine, grossular, cinnamon stone or cinnabar garnet, tsavorite, grossular, andradite, pyrope-almandine-sponsartine solid solution and grossular-grossular-andradite solid solution. The garnet used in this patent does not include the general formula X 3 Y 2 (SiO 4 ) 3 Island silicates, wherein X is Ca, Mg, Fe and or Mn; Y is Al, Fe or Cr.

[0059] The terms "garnet chemical precursor", "garnet-type electrolyte chemical precursor", "garnet precursor" and "garnet precursor material" as used herein refer to chemical substances that can react to form lithium-filled garnet materials. The chemical precursors described in this patent include, but are not limited to, lithium hydroxide (e.g., LiOH), lithium oxide (e.g., Li 2 O), lithium carbonate (such as LiCO 3 ), zirconium oxide (such as ZrO 2 ), lanthanum oxide (such as La 2 O 3 ), lanthanum hydroxide (e.g. La(OH) 3 ), aluminum oxide (such as Al2O 3 ), aluminum hydroxide (such as Al(OH) 3 )), AlOOH, aluminum (such as Al), boehmite, magnesite, corundum, aluminum nitrate (such as Al(NO 3 ) 3 ), aluminum nitrate nonahydrate, niobium oxide (such as Nb 2 O 5 ), gallium oxide (Ga 2 O 3 ) and tantalum oxide (such as Ta 2 O 5 ). Other precursors of garnet materials can be applied to the method described in this patent.

[0060] The term "garnet-type electrolyte" as used in this patent refers to an electrolyte containing the lithium-filled garnet material described in this patent as a lithium-ion conductor. Solid-state lithium-filled garnet electrolytes have many advantages and can replace liquid, flammable electrolytes that are commonly used in lithium rechargeable batteries.

[0061] The term “LIRAP” used in this patent refers to lithium-rich antiperovskite, which is different from “LOC” or “Li 3 OCl" is synonymous. The composition of LIRAP is aLi 2 O+bLiX+cLiOH+dAl 2 O 3 , wherein X = Cl, Br and / or I, a / b = 7-9, c / a = 0.01-1, d / a = 0.001-0.1.

[0062] The term "LXPS" or "LPS+X" used in this patent refers to a lithium-conducting electrolyte comprising Li, P, S and X, wherein X = Cl, Br and / or I. For example, "LSPI" refers to a lithium-conducting electrolyte comprising Li, P, S and I. In general, it should be understood that a Li 2 S+b 2 S y +cLiX, wherein X = Cl, Br and / or I, and y = 3-5 and wherein a / b = 2.5-4.5, wherein (a+b) / c = 0.5-15.

[0063] The term "LBHPS" used in this patent refers to a lithium-conducting electrolyte having Li, B, H, P and S, such as A(LiBH 4 )(1-A)(P 2 S 5 ), where 0.05≤A≤0.95.

[0064] The term "LSS" used in this patent refers to the 2 S-SiS 2 、Li-SiS 2 , Li-S-Si lithium silicon sulfide and / or a cathode electrolyte mainly composed of Li, S and Si. LSS refers to a cathode electrolyte composed of the formula Li x Si y S z LSS refers to an electrolyte material comprising Li, Si, and S. In some examples, LSS is Li 2 S and SiS 2 In some embodiments, Li2 S :SiS 2 The molar ratio of is 90:10, 85:15, 80:20, 75:25, 70:30, 2:1, 65:35, 60:40, 55:45 or 50:50. LSS can be doped with, for example, Li xPO y 、LixBO y 、Li 4 SiO 4 、Li 3 MO 4 、Li 3 MO 3 、PS x (where 0 < x ≤ 5 and 0 < y ≤ 5) and / or lithium halides and other compounds, including but not limited to, for example, LiI, LiC, LiF or LiBr.

[0065] Unless otherwise specified, the "SLOPS" described in this patent contains Li with a molar ratio of 60:40 2 S:SiS 2 and 0.1 - 10 mol% of Li 3 PO 4 . In some instances, the "SLOPS" contains Li 10 Si 4 S 13 (50:50 Li 2 S:SiS 2 ) and 0.1 - 10 mol% Li 3 PO 4 . In some instances, the "SLOPS" contains Li 26 Si 7 S 27 (65:35 Li 2 S:SiS 2 ) and 0.1 - 10 mol% Li 3 PO 4 . In some instances, the "SLOPS" contains Li 4 SiS 4 (67:33 Li 2 S:SiS 2 ) and 0.1 - 5 mol% Li 3 PO 4 . In some instances, the "SLOPS" contains Li 14 Si 3 S 13 (70:30 Li 2 S:SiS 2 ) and 0.1 - 5 mol% Li 3 PO 4 . In some instances, the "SLOPS" consists of (1 - x)(60:40 Li 2 S:SiS 2 ) * (x)(Li 3 PO 4), where x is 0.01 to 0.99. The "LBS-POX" described in this patent refers to a Li 2 S:B 2 S 3 :Li 3 PO 4 :LiX electrolyte, wherein X is a halogen ((X = F, Cl, Br, I). The composition may include Li doped with 0-30% lithium halide 3 BS 3 or Li 5 B 7 S 13 For example, the lithium halide is LiI and / or 0-10% Li 3 PO 4 .

[0066] The term "LSTPS" as used in this patent refers to an electrolyte material having the chemical composition of Li, Si, P, Sn and S. As used in this patent, "LSPSO" refers to a LSPS doped with or having O. In some instances, "LSPSO" is a LSPS material with an oxygen content between 0.01 and 10 at%. The "LATP" described in this patent refers to an electrolyte material having the chemical composition of Li, As, Sn and P. The "LAGP" described in this patent refers to an electrolyte material having the chemical composition of Li, As, Ge and P. The "LXPSO" described in this patent refers to an electrolyte material having the formula Li a MP b S c O d The cathode electrolyte material represented by wherein M represents Si, Ge, Sn and / or Al, wherein 2≤a≤8, 0.5≤b≤2.5, 4≤c≤12, d<3. LXPSO refers to LXPS as defined above and doped with 0.1 to about 10 at% oxygen. LPSO refers to LPS as defined above and doped with 0.1 to about 10 at% oxygen. In some examples, "SLOPS" contains Li 10 Si 4 S 13 (50:50Li 2 S:SiS 2 ) and 0.1-10 mol% Li 3 PO 4 In some instances, "SLOPS" contains Li 26 Si 7 S 27 (65:35Li 2 S:SiS 2 ) and 0.1-10 mol.% Li 3 PO 4In some instances, "SLOPS" contains Li 4 SiS 4 (67:33Li 2 S:SiS 2 ) and 0.1-5 mol% Li 3 PO 4 In some instances, "SLOPS" contains Li 14 Si 3 S 13 (70:30Li 2 S:SiS 2 ) and 0.1-5 mol% Li 3 PO 4 In some examples, "SLOPS" is given by the formula (1-x)(60:40Li 2 S:SiS 2 )*(x)(Li 3 PO 4 ), where x is 0.01 to 0.99. The "LBS-POX" described in this patent refers to a Li 2 S:B 2 S 3 :Li 3 PO 4 :LiX electrolyte, wherein X is a halogen ((X = F, Cl, Br, I). The composition may include Li doped with 0-30% lithium halide 3 BS 3 or Li 5 B 7 S 13 For example, the lithium halide is LiI and / or 0-10% Li 3 PO 4 .

[0067] The term "LPSC1" as used in this patent refers to an electrolyte material having a chemical composition of LiPS and Cl. The term "LPSBr" as used in this patent refers to an electrolyte material having a chemical composition of LiPS and Br. The term "LPSI" as used in this patent refers to an electrolyte material having a chemical composition of LiPS and I. LXPSO refers to LXPS as defined above, and is doped with 0.1at% to about 10at% oxygen. LPSO refers to LPS as described above, and is doped with 0.1at% to about 10at% oxygen.

[0068] The term "LAPS" used in this patent refers to an electrolyte material having a chemical composition of Li, As, P, and S. "LPSCl" refers to an electrolyte material having a chemical composition of Li, P, S, and Cl. The term "LTPS" used in this patent refers to an electrolyte material having a chemical composition of Li, P, Sn, and S. The term "LSPS" used in this patent refers to an electrolyte material having a chemical composition of Li, P, Si, and S. The term "LGPS" used in this patent refers to an electrolyte material having a chemical composition of Li, P, Ge, and S. The term "LPS" used in this patent refers to an electrolyte material having a chemical composition of Li, P, and S. The term "LSTPSCl" used in this patent refers to an electrolyte material having a chemical composition of Li, Si, P, Sn, S, and Cl. The term "LSPSCl" used in this patent refers to an electrolyte material having a chemical composition of Li, Si, P, S, and Cl. The term "LSPSBr" used in this patent refers to an electrolyte material having a chemical composition of Li, Si, P, S, and Br. The term "LTS" used in this patent refers to a lithium tin sulfide compound, which can be described as Li 2 S:SnS 2 :As 2 S 5 , Li 2 S-SnS 2 , Li 2 S-SnS, Li-S-Sn and / or a cathode electrolyte mainly composed of Li, S and Sn. The composition can be Li x Sn y S z , wherein 0.25≤x≤0.65, 0.05≤y≤0.2 and 0.25≤z≤0.65. In some examples, LTS is Li 2 S and SnS 2 A mixture in a molar ratio of 80:20, 75:25, 70:30, 2:1 or 1:1. LTS may contain up to 10 at% oxygen. LTS may be doped with Bi, Sb, As, P, B, Al, Ge, Ga and / or Indium and / or lithium halides, but not limited to, for example, LiI, LiCl, LiF or LiBr.

[0069] The term "LATS" as used in this patent refers to LTS further comprising arsenic: As 2 S 5 , Li 2 S-SnS 2 , Li 2 S-SnS, Li-S-Sn and / or a cathode electrolyte mainly composed of Li, S and Sn. The composition can be Li x Sn y S z, wherein 0.25≤x≤0.65, 0.05≤y≤0.2, and 0.25≤z≤0.65. In some examples, LTS is Li 2 S and SnS 2 A mixture in a molar ratio of 80:20, 75:25, 70:30, 2:1 or 1:1. LTS may contain up to 10 at% oxygen. LTS may be doped with Bi, Sb, As, P, B, Al, Ge, Ga and / or Indium and / or lithium halides, but not limited to, for example, LiI, LiCl, LiF or LiBr.

[0070] The term "LBHI" or "LiBHI" used in this patent refers to a lithium-conducting electrolyte containing Li, B, H and I. Generally, it should be understood that it contains aLiBH 4 + bLiX, where X = Cl, Br and / or I, where a:b = 7:1, 6:1, 5:1, 4:1, 3:1, 2:1, or in the range of a / b = 2-4. LBHI can also be aLiBH 4 +bLiX+cLiNH 2 The form contains nitrogen, wherein (a+c) / b=2-4 and c / a=0-10.

[0071] The term "LBHXN" as used in this patent refers to a 4 )·B·(LiX)·C·(LiNH 2 ), wherein X is fluorine (F), bromine (Br), chlorine (Cl), iodine (I) or a combination thereof, wherein 3≤A≤6, 2≤B≤5, 0≤C≤9. The term "LBHFN" used in this patent refers to a compound characterized by A·(LiBH 4 )·B·(LiF)·C·(LiNH 2 ) wherein 3≤A≤6, 2≤B≤5, 0≤C≤9. The term "LBHBrN" used in this patent refers to a compound characterized by A·(LiBH 4 )·B·(LiBr)·C·(LiNH 2 ) wherein 3≤A≤6, 2≤B≤5, 0≤C≤9. The term "LBHClN" used in this patent refers to a compound characterized by A·(LiBH 4 )·B·(LiCl)·C·(LiNH 2 ) wherein 3≤A≤6, 2≤B≤5, 0≤C≤9. The term "LBHIN" used in this patent refers to a compound characterized by A·(LiBH 4 )·B·(LiI)·C·(LiNH 2 ) wherein 3≤A≤6, 2≤B≤5, 0≤C≤9.

[0072] Unless otherwise specified, the "SLOBS" described in this patent contains Li 2 S:SiS 2 and 0.1-10 mol% LiBH 4 In some examples, "SLOBS" contain Li 10 Si 4 S 13 (50:50Li 2 S:SiS 2 ) and 0.1-10 mol% LiBH 4 In some examples, "SLOBS" contain Li 26 Si 7 S 27 (65:35Li 2 S:SiS 2 ) and 0.1-10 mol.% LiBH 4 In some examples, "SLOBS" contain Li 4 SiS 4 (67:33Li 2 S:SiS 2 ) and 0.1-5 mol% LiBH 4 In some examples, "SLOBS" contain Li 14 Si 3 S 13 (70:30Li 2 S:SiS 2 ) and 0.1-5 mol% LiBH 4 In some examples, "SLOBS" is represented by the formula (1-x)(60:40Li 2 S:SiS 2 )*(x)(Li 3 BO 4 ), where x is 0.01 to 0.99. The "LBS-BOX" described in this patent refers to a 2 S:B 2 S 3 :LiBH 4 : LiX electrolyte, wherein X is a halogen ((X = F, Cl, Br, I). The composition may include 0-30% lithium halide such as LiI and / or 0-10% LiPO 4 . 3 BS 3 or Li 5 B 7 S 13 .

[0073] The term "made of the same type of material" as used in this patent refers to two or more different physical forms of a material, but including the same components. For example, lithium-filled garnet powder and lithium-filled garnet film are made of the same type of material. For example, LSTPS powder and LSTPS film are made of the same type of material.

[0074] The term "manufacturing" as used in this patent refers to the process or method of forming or causing the formation of the manufactured object. For example, manufacturing an energy storage electrode includes a process, process operation, process step or method of forming or causing the formation of an electrode of an energy storage device. The end result of the operation of manufacturing an energy storage electrode is the production of a material that functions as an electrode.

[0075] The term "positive electrode" as used in this patent refers to an electrode in a secondary battery that releases positive ions such as Li during battery discharge. + Conduct, flow or move toward the electrode. The term "negative electrode" as used in this patent refers to an electrode in a secondary battery where positive ions such as Li + In the case of a cathode active material composed of a lithium metal electrode and a conversion chemistry, an intercalation chemistry, or a combination of conversion / intercalation chemistry (i.e., a cathode active material; e.g., NiF x 、NCA、LiNi x Mn y Co z O 2 [NMC] or LiNi x Al y Co z O 2 [NCA], where x+y+z=1) is a battery composed of electrodes, the electrode with conversion chemistry, intercalation chemistry or combined conversion / intercalation chemistry is called the positive electrode. In some common practices, the cathode replaces the positive electrode and the anode replaces the negative electrode. When charging a lithium secondary battery, lithium ions are transferred from the positive electrode (such as NiF x , NMC, NCA) to the negative electrode (such as lithium metal). When the lithium secondary battery is discharged, the lithium ions move from the negative electrode to the positive electrode.

[0076] The term "organic content (10%)" used in this patent refers to the weight percentage of organic matter in the main body. For example, if the buffer layer includes LSTPS and polymer, but the organic content (10%) means that the total amount of polymer in the mixture of LSTPS and polymer is 10% by weight, and the remaining 90% is inorganic, such as LSTPS.

[0077] The term "porosity determined by SEM" as used in this patent refers to a measurement of the density of a scanning electron micrograph analyzed by using image analysis software. For example, first, the user or the software assigns pixels and / or areas of the image as porosity. Then, the area fractions of those areas are added together. Finally, the porosity determined by SEM is equal to the area fraction of the porous area of ​​the image.

[0078] The term "providing" as used in this patent refers to the providing, generating, presenting or delivering of a provided object.

[0079] Unless otherwise specified, the terms "separator" and "Li-ion conductive separator" used in this patent are used interchangeably, wherein separator is an abbreviation of Li-ion conductive separator. Separator refers to a solid electrolyte that can conduct Li ions and is basically insulated from electrons and is suitable for use as a physical barrier or separator between positive and negative electrodes in an electrochemical cell or rechargeable battery. When the lithium ion conductivity of the separator is at least 10 greater than the electronic conductivity of the separator, the separator is used as a solid electrolyte. 3 times (usually 10 6 The separator used in this patent is essentially insulating when the lithium metal is in contact with the lithium metal. The separator can be a film, a monolith or a particle. Unless otherwise explicitly stated, the separator used in this patent is stable when in contact with lithium metal.

[0080] The term "sintered lithium-filled garnet film" as used in this patent refers to a film formed by sintering and compacting a green film containing lithium-filled garnet.

[0081] The term "solid cathode" or "solid positive electrode" used in this patent refers to a type of "positive electrode" defined in this patent. In some instances, all components in the solid cathode film are in solid form. The solid cathode includes an active cathode material as defined in this patent, a solid cathode electrolyte as defined in this patent, optionally a conductive additive and optionally a binder. In some instances, the solid cathode is a compacted film.

[0082] The term "solid electrolyte" used in this patent is interchangeable with the term "solid separator" and refers to a solid electrolyte that does not contain carbon and conducts ions (such as Li +) but does not conduct electrons. Inorganic solid electrolytes are solid materials suitable for electrical isolation between the positive and negative electrodes of lithium secondary batteries, while providing lithium ion conduction paths. Exemplary inorganic solid electrolytes include oxide electrolytes and sulfide electrolytes, which will be further described below. Non-limiting example sulfide electrolytes can be found in, for example, U.S. Patent No. 9,172,114, issued on October 27, 2015, and U.S. Patent Application No. 2017-0162901A1, issued on June 8, 2017, and U.S. Patent Application No. 15 / 367,103, filed on December 1, 2016, all of which are incorporated by reference into this patent for all purposes. Non-limiting example oxide electrolytes can be found in U.S. Patent Application No. 2015-0200420A1, published on July 16, 2015, all of which are incorporated by reference into this patent for all purposes. In some examples, the inorganic solid electrolyte further includes a polymer.

[0083] Unless otherwise specified, the term "subscripts and molar coefficients in the empirical formula are derived from the bulk raw materials processed to make the examples described" as used herein means, for example, Li 7 La 3 Zr 2 O 12 The subscripts 7, 3, 2, 12 and 0.35Al 2 O 3 The coefficient 0.35 in the formula refers to the 7 La 3 Zr 2 O 12 0.35Al 2 O 3 ) chemical precursors (e.g. LiOH, La 2 O 3 、ZrO 2 、Al 2 O 3 ) is the ratio of each element in .

[0084] The term "slot casting" or "slot die coating" as used herein refers to a deposition process in which a solution, liquid, slurry, or the like is passed through a slot or die having a fixed size, the slot or die being adjacent to, in contact with, or located on the substrate, thereby coating or depositing the solution, liquid, slurry, or the like on the substrate. In some examples, the slot casting method includes a slot opening of approximately 1 to 100 μm.

[0085] The term "oxide" as used in this patent refers to a compound that includes at least one oxygen atom and one other element in the chemical formula of the compound. For example, "oxide" can be interchanged with "oxide electrolyte". Non-limiting examples of oxide electrolytes can be found in U.S. Patent Application Publication No. 2015 / 0200420, published on July 16, 2015, the entire contents of which are incorporated into this patent by reference.

[0086] The term "sulfide" as used in this patent refers to a compound that includes at least one sulfur atom and one other element in the chemical formula of the compound. For example, "sulfide" can be interchangeable with "sulfide electrolyte".

[0087] Non-limiting examples of sulfide electrolytes can be found in, for example, U.S. Patent No. 9,172,114, issued on October 27, 2015, and U.S. Patent Application No. 2017-0162901A1, published on June 8, 2017, and U.S. Patent Application No. 15 / 367,103, filed on December 1, 2016, the entire contents of which are incorporated herein by reference for all purposes. A sulfide cathode electrolyte as used in this patent is a cathode electrolyte comprising or consisting primarily of a sulfide.

[0088] The term "sulfide electrolyte" or "lithium sulfide" used in this patent includes but is not limited to the electrolytes referred to in this patent as LSS, LTS, LXPS or LXPSO, where X is Si, Ge, Sn, As, Al or Li-Sn-Si-PS or Li-As-Sn-S. In these acronyms (LSS, LTS, LXPS or LXPSO), S represents the element S, Si or a combination thereof, and T represents the element Sn. "Sulfide electrolyte" may also include Li a P b S c X d , Li a B b S c X d , Li a Sn b S c X d or Li a Si b S c X d , wherein X = F, Cl, Br, I, and 10%≤a≤50%, 10%≤b≤44%, 24%≤c≤70%, 0≤d≤18%; the sulfide electrolyte may contain up to 10% of oxygen, either intentionally added or present as impurities.

[0089] The term "sulfide-halide" as used in this patent refers to a compound including at least one sulfur atom, at least one halogen atom and one other element in the chemical formula of the compound.

[0090] Unless otherwise stated, the voltages used in this patent are relative to lithium (ie, voltage to lithium) metal.

[0091] Electrochemical Cell

[0092] Figure 1 is a schematic diagram of an example of an electrochemical cell. Figure 1As shown, layer 101 represents an evaporated lithium metal anode. Layer 102 represents a lithium filled garnet layer. Layer 103 represents an adhesive layer. Layer 104 represents a buffer layer. Layer 105 represents a positive electrode layer. In some examples, layer 102 has a thickness of about 100 μm. In some examples, layer 101 has a thickness of about 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, or 40 μm. In some examples, layer 102 has a thickness of about 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100, 101, 102, 103, 104, 105, 106, 107, 108, 109, 110, 111, 112, 113, 114, 115, 116, 117, 118, 119, 120, 121, 122, 123, 124, or 125 μm. In some examples, layer 103 has a thickness of about 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 μm. In some examples, layer 104 has a thickness of about 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 μm. In some examples, layer 105 has a thickness of about 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100, 101, 102, 103, 104, 105, 106, 107, 108, 109, 110, 111, 112, 113, 114, 115, 116, 117, 118, 119, 120, 121, 122, 123, 1 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, or 170 μm.

[0093] In some examples, the present patent discloses a solid-state electrochemical cell (SSEC) comprising (a) a positive electrode layer comprising an active material and a sulfide cathode electrolyte; (b) a solid buffer that conducts a single ion; (c) a borohydride bonding layer; and (d) a lithium-filled garnet layer. The buffer is mixed into the positive electrode layer, or the buffer is used as a layer in contact with the positive electrode layer, or in some examples, the buffer is mixed into the positive electrode layer and is also used as a layer in contact with the positive electrode layer. The borohydride bonding layer is between and in contact with the lithium-filled garnet layer and (i) the positive electrode layer mixed with the buffer or (ii) the buffer layer in contact with the positive electrode. In some examples, the borohydride bonding layer is between and in contact with the lithium-filled garnet layer and the positive electrode layer mixed with the buffer. In some examples, the buffer is mixed into the positive electrode layer. In some examples, the buffer is used as a layer in contact with the positive electrode layer. In some examples, the buffer is mixed within the positive electrode layer and the buffer also serves as a layer in contact with the positive electrode layer. In some examples, the borohydride bonding layer is between and in contact with the lithium filled garnet layer and the buffer layer in contact with the positive electrode.

[0094] In some examples, including any of the above, the active material comprises a coating. In some examples, the active material comprises a coating selected from LLZO materials.

[0095] In these examples, lithium ions are conducted through the inorganic single ion conductor, rather than through the polymer or organic component (10%).

[0096] In some examples, the solid-state electrochemical cell (SSEC) described in the present patent includes: (a) a positive electrode layer comprising an active material and a sulfide cathode electrolyte; (b) a solid buffer that conducts a single ion; (c) a borohydride bonding layer; (d) a lithium-filled garnet layer; wherein the buffer is mixed in the positive electrode layer, or is a layer in contact with the positive electrode layer, or both. Wherein, the borohydride bonding layer is between the lithium-filled garnet layer and (i) the positive electrode layer mixed with the buffer or (ii) the buffer layer in contact with the positive electrode and in contact with it.

[0097] In some examples, including any of the foregoing, a solid buffer that conducts a single ion is mixed in the positive electrode layer. In some embodiments, the buffer is mixed in the positive electrode layer in a gradient manner with the active material and the buffer material.

[0098] In some examples, including any of the foregoing, the single-ion conducting solid buffer is a layer in contact with the positive electrode layer.

[0099] In some examples, including any of the foregoing, a single ion conducting solid buffer is mixed within the positive electrode layer and serves as a layer in contact with the positive electrode layer.

[0100] In some examples, including any of the foregoing, a solid buffer layer that conducts a single ion prevents the borohydride bonding layer from contacting the positive electrode layer. In some examples, the borohydride bonding layer adheres the lithium-filled garnet layer to the buffer layer. In some examples, the borohydride bonding layer adheres the lithium-filled garnet layer to the buffer as a component of the positive electrode layer.

[0101] In some examples, including any of the foregoing, the negative electrode layer is between and in contact with the lithium-filled garnet layer and the negative electrode current collector layer. In some examples, including any of the foregoing, the buffer layer potential is shielded from the potential of the Li metal negative electrode. In some examples, including any of the foregoing, the borohydride bonding layer potential is shielded from the potential of the positive electrode. In some examples, including any of the foregoing, the ASR of the SSEC is 50Ωcm 2 or smaller.

[0102] In some examples, the present patent discloses a solid-state electrochemical cell (SSEC) comprising (a) a positive electrode layer comprising an active material and a sulfide cathode electrolyte; (b) a buffer, the buffer comprising a solid electrolyte that conducts a single ion, and the buffer is mixed in the positive electrode layer or in direct contact with the positive electrode layer; (c) a binding layer comprising a borohydride; and (d) a layer comprising a lithium-filled garnet. In this embodiment, the borohydride binding layer is between and in contact with the layer containing the lithium-filled garnet and the positive electrode layer, or between the layer containing the lithium-filled garnet and the buffer layer, and the buffer layer is in direct contact with the positive electrode.

[0103] In some examples, including any of the foregoing, the solid-state electrochemical stack further comprises (d) a negative electrode current collector in direct contact with the separator layer. In another example, any of the foregoing solid-state electrochemical stacks further comprises (e) a positive electrode current collector in direct contact with the positive electrode layer. In a further example, any of the foregoing solid-state electrochemical stacks further comprises (d) a negative electrode current collector and (e) a negative electrode, wherein the (e) negative electrode is between the separator layer and the negative electrode current collector and in direct contact with them.

[0104] In certain embodiments, the present patent discloses a composite material having a lithium-filled garnet and a LBHI, wherein the LBHI fills at least 90% of the through pores and / or surface pores of the lithium-filled garnet, and wherein the LBHI is A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ) wherein X represents a halide, and 3≤A≤6, 2≤B≤5 and 0≤C≤9.

[0105] In some examples, the borohydride bonding layer described in this patent is LBHI (lithium borohydride and lithium iodide). The buffer layer is LSTPS. The buffer layer seals (ie shields) the high voltage positive electrode.

[0106] Buffer component

[0107] In some examples, the sulfide in the buffer layer can be any sulfide described in the U.S. patent application with a publication date of January 5, 2017, publication number 2017-0005367A1, and title "COMPOSITE ELECTROLYTES". For various purposes, the entire content thereof is incorporated herein by reference.

[0108] In some examples, the sulfide in the buffer layer can be any sulfide proposed in the patent WO2017096088A1, with a publication date of June 8, 2017, international PCT patent application number PCT / US2016 / 064492, filing date of December 1, 2016, and title "LITHIUM,PHOSPHORUS,SULFUR,AND IODINE CONTAINING ELECTROLYTEAND CATHOLYTE COMPOSITIONS,ELECTROLYTE MEMBRANES FOR ELECTROCHEMICAL DEVICES,AND ANNEALING METHODS OF MAKING THESE ELECTROLYTES AND CATHOLYTES", published as WO 2017 / 096088 on June 8, 2017. For various purposes, the entire content thereof is incorporated herein by reference.

[0109] In some examples, including any of the foregoing, the buffer layer, the sulfide cathode electrolyte, or the single-ion-conducting solid buffer, or all of them, can be characterized by one of the following formulas: Li a Si b Sn c P d S e O f , where 2 ≤ a ≤ 8, 0 ≤ b ≤ 1, 0 ≤ c ≤ 1, b + c = 1, 0.5 ≤ d ≤ 2.5, 4 ≤ e ≤ 12, and 0 ≤ f ≤ 10; Li a Si b P c S d X e , where 8 < a < 12, 1 < b < 3, 1 < c < 3, 8 < d < 14, and 0 < e < 1, where X is F, Cl, Br, or I; Li g As h Sn j S k O l , where 2 ≤ g ≤ 6, 0 ≤ h ≤ 1, 0 ≤ j ≤ 1, 2 ≤ k ≤ 6, and 0 ≤ l ≤ 10; Lim P n S p I q , wherein 2≤m≤6, 0≤n≤1, 0≤p≤1, 2≤q≤6; (Li 2 S):(P 2 S 5 ) and LiI, wherein [(Li 2 S):(P 2 S 5 )]:LiI ratio is 95:5 to 50:50; LPS + X, wherein X is selected from Cl, I or Br; vLi 2 S+P 2 S 5 +yLiX or vLi 2 S+W 2 +yLiX. In some examples, including any of the foregoing, the sulfide cathode electrolyte comprises LSTPS. 2 S+B 2 S 3 +yLiX.

[0110] In some examples, the buffer comprises Li a Si b Sn c P d S e , wherein 2≤a≤8, 0≤b≤1, 0≤c≤1, 0.5≤d≤2.5 and 4≤e≤12. In some examples, the buffer comprises Li a Si b Sn c P d S e , wherein 2≤a≤8, 0≤b≤1, 0≤c≤1, b+c=1, 0.5≤d≤2.5 and 4≤e≤12. In some examples, the buffer comprises Li a Si b Sn c P d S e , wherein 3≤a≤7, 0≤b≤1, 0≤c≤1, b+c=1, 0.5≤d≤1.5 and 8≤e≤12. In some examples, the buffer comprises Li a Si b Sn c P d S e , wherein 3≤a≤5, 0≤b≤1, 0≤c≤1, b+c=1, 0.5≤d≤1 and 5≤e≤9. In some examples, the buffer comprises Li a Sib Sn c P d S e , wherein 3≤a≤5, 0≤b≤1, 0≤c≤1, b+c=1, 0.5≤d≤1 and 5≤e≤9. In some examples, the buffer comprises Li a Si b Sn c P d S e , wherein 2≤a≤8, 0≤b≤1, 0≤c≤1, b+c=1, 0.5≤d≤2.5 and 4≤e≤12. In some examples, the buffer comprises Li a Si b Sn c P d S e , wherein 3≤a≤5, 0≤b≤0.5, 0≤c≤0.5, 0≤d≤2, and 2≤e≤10. In some examples, the buffer comprises Li a Si b Sn c P d S e , wherein 3≤a≤5, 0≤b≤0.25, 0≤c≤1, 0≤d≤1 and 2≤e≤14. In some examples, the buffer comprises Li a Si b Sn c P d S e , where 3≤a≤5, 0≤b≤0.25, 0≤c≤1, 0≤d≤1 and 2≤e≤8.

[0111] In some examples, including any of the foregoing, the single-ion conducting solid buffer comprises LSTPS.

[0112] The buffer layer does not conduct electrons, thus protecting the positive electrode potential from the potential of the borohydride bonding layer.

[0113] The buffer layer does not conduct electrons, and thus the positive electrode potential is not affected by the negative electrode potential.

[0114] In some examples, the buffer layer is susceptible to deformation.

[0115] In some examples, the buffer layer is chemically stable when in contact with the sulfide cathode electrolyte disclosed herein and / or the coated active material disclosed herein.

[0116] In some examples, the buffer layer includes LSTPS.

[0117] In some examples, the buffer layer includes D50 The buffer layer includes particles having a diameter of about 10 nm to 1000 nm, about 100 nm to 500 nm, or about 150 nm to 300 nm. 50 The buffer layer includes D 90 The particles are about 500nm to 2000nm, 750nm to 1000nm or about 1000nm. In some examples, the buffer layer includes D 90 The particles are about 800 nm, 900 nm, 1000 nm or 1100 nm. In some examples, the buffer layer includes D 90 In some embodiments, the buffer layer includes D 90 The particles are at least about 900 nm.

[0118] In some examples, the buffer layer is made of particles that are 1 / 10 of the thickness of the buffer layer. For example, in some examples, if the thickness of the buffer layer is 5 μm, the buffer layer contains buffer particles that are 0.5 μm. In some examples, if the buffer layer is 5 μm thick, the buffer layer contains d 50 The particle size of LSTPS particles is 0.5 μm in diameter.

[0119] In some examples, the interface impedance of the buffer layer to the positive electrode is negligible.

[0120] In some examples, the buffer layer is non-polymeric, meaning that the buffer layer includes less than 5 wt % polymer.

[0121] In some examples, the buffer layer is adhered to the positive electrode by a lamination and compaction process. This produces a bufferable positive electrode that blocks the entry of electrons so that other electrolyte layers are not affected by the positive electrode potential.

[0122] In some examples, the buffer layer is adhered to the positive electrode by a lamination and compaction process. This produces a bufferable positive electrode that blocks the entry of electrons so that other electrolyte layers are not affected by the positive electrode potential.

[0123] In some examples, the porosity of the buffer layer is less than about 20% v / v, 15% v / v, 12.5% ​​v / v, 10% v / v, 5% v / v, 1% v / v or less. In some examples, the porosity of the buffer layer is about 5% v / v to 20% v / v or about 10% v / v to 15% v / v.

[0124] Adhesive layer components

[0125] In some embodiments, the adhesive layer may include A·(LiBH4 )·B·(LiX)·C·(LiNH 2 ), wherein X can be fluorine, bromine, chlorine, iodine or a combination thereof, 3≤A≤6, 2≤B≤5 and 0≤C≤9. In some examples, the bonding layer includes A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein 3≤A≤6, 2≤B≤5 and 3≤C≤6. In some examples, the bonding layer comprises A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein 3≤A≤5, 2≤B≤5 and 3≤C≤5. In some examples, the bonding layer comprises A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein 3≤A≤4, 2≤B≤4 and 3≤C≤4. In some examples, the bonding layer includes A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein 4≤A≤5, 2≤B≤4 and 4≤C≤5. In some examples, the bonding layer comprises A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), where 4≤A≤5, 3≤B≤4 and 4≤C≤5.

[0126] In some embodiments, the adhesive layer may include A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ) wherein X can be fluorine, bromine, chlorine, iodine or a combination thereof, 0.1≤A≤3, 0.1≤B≤4.5 and 0≤C≤9.

[0127] In one embodiment, X can be bromine, chlorine, iodine, or a combination thereof. In another embodiment, X can be iodine. In some embodiments, A is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, or 3.0. In some embodiments, B is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, or 4.5. In some embodiments, C is 0.0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, or 9.0.

[0128] In some instances, the adhesive layer comprises a borohydride composition containing A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), where 2.5 < A < 4.5, 2.5 < B < 5.5, and 4 < C < 9. In some instances, including any of the foregoing, the borohydride adhesive layer comprises a borohydride composition containing A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ). In some instances, 2.5 < A < 3.5, 3.5 < B < 4.5, and 5 < C < 9.

[0129] In some examples, including any of the foregoing, the borohydride bonding layer comprises a borohydride composition, the composition being 3LiBH 4 2LiCl 3LiNH 2 or 3LiBH 4 ·4LiCl·9LiNH 2 In one embodiment, the composition may be 3LiBH 4 2LiI 3LiNH 2 In another embodiment, the composition may be 3LiBH 4 ·4LiI·9LiNH 2 In another embodiment, the composition may be 3LiBH 4 2LiCl 3LiNH 2 In another embodiment, the composition may be 3LiBH 4 ·4LiCl·9LiNH 2 In another embodiment, the composition may be 3LiBH 4 2LiBr 3LiNH 2 In another embodiment, the composition may be 3LiBH 4 ·4LiBr·9LiNH 2 .

[0130] In some examples, including any of the foregoing, the borohydride bonding layer comprises a borohydride composition, wherein the composition is 3LiBH 4 2LiCl 3LiNH 2 or 3LiBH 4 ·4LiCl·5LiNH 2 In one embodiment, the composition is 4LiBH 4 ·2LiI·4LiNH 2 In another embodiment, the composition is 4LiBH 4 ·3LiI·4LiNH 2 In another embodiment, the composition is 4LiBH 4 ·5LiCl·4LiNH 2 In another embodiment, the composition is 4LiBH 4 ·6LiCl·4LiNH 2 In some examples, including any of the foregoing, the borohydride bonding layer comprises a borohydride composition, wherein the composition is 3LiBH 4 ·3LiCl·4LiNH 2 or 3LiBH 4·3LiCl·5LiNH 2 。In one embodiment, the composition is 3LiBH 4 ·3LiI·6LiNH 2 。In another embodiment, the composition is 3LiBH 4 ·3LiI·7LiNH 2 。

[0131] In some instances, including any of the foregoing, the borohydride adhesive layer comprises a borohydride composition selected from LBHIN and LBHN. In some instances, including any of the foregoing, the borohydride adhesive layer comprises KBH 4 and LiNH 2 。

[0132] In some embodiments, the composition can exist in different physical states. For example, in one embodiment, the composition can be amorphous. As a further example, in one embodiment, the composition can be semi-crystalline. By controlling the sintering curve, for example by adjusting the cooling rate after sintering, the composition can be made amorphous or semi-crystalline.

[0133] In some embodiments, the LBHI composition can be in the form of a thin film, monolith, or pellet. For example, in one embodiment, the composition is a thin film. As a further example, in one embodiment, the composition is a monolith. As a further example, in one embodiment, the composition is a pressed pellet.

[0134] In some embodiments, the LBHI composition can further include an oxide, sulfide, sulfide-halide, or electrolyte. For example, in one embodiment, the oxide can be selected from lithium-filled garnets characterized as Li x La y- Zr z O t ·qAl 2 O 3 where 4 < x < 10, 1 < y < 4, 1 < z < 3, 6 < t < 14, and 0 ≤ q ≤ 1. As another example, in one embodiment, the composition includes an oxide having an LBHI coating, and the oxide can be selected from lithium-filled garnets characterized as having the formula Li x La y Zr z O t ·qAl 2 O 3 where 4 < x < 10, 1 < y < 4, 1 < z < 3, 6 < t < 14, 0 ≤ q ≤ 1. As another example, in one embodiment, the oxide can be selected from those characterized as having the formula Li aLa b Zr c Al d Me” e O f of lithium-filled garnet, where 5 < a < 8.5, 2 < b < 4, 0 < c ≤ 2.5, 0 ≤ d < 2, 0 ≤ e < 2, and 10 < f < 13, where Me” is a metal selected from Nb, Ga, Ta, or a combination thereof. As another example, in one embodiment, the composition includes an oxide having an LBHI coating, and the oxide can be selected from those characterized as Li a La b Zr c Al d Me” e O f of lithium-filled garnet, where 5 < a < 8.5, 2 < b < 4, 0 < c ≤ 2.5, 0 ≤ d < 2, 0 ≤ e < 2, and 10 < f < 13, where Me” is a metal selected from Nb, Ga, Ta, or a combination thereof. As another example, in one of the foregoing Li a La b Zr c Al d Me” e O f embodiments, Me” is Nb. As another example, in one of the foregoing Li a La b Zr c Al d Me” e O f embodiments, Me” is Ga. As another example, in one of the foregoing Li a La b Zr c Al d Me” e O f embodiments, Me” is Ta. As another example, in one of the foregoing Li a La b Zr c Al d Me” e O f embodiments, Me” is Nb and Ga. As another example, in one of the foregoing Li a La b Zr c Al d Me” e O f embodiments, Me” is Nb and Ta. As another example, in one of the foregoing Li a La b Zr cAl d Me” e O f In the embodiments, "Me" is Ga and Ta.

[0135] In some examples, the borohydride bonding layer is made of a borohydride compound. The borohydride compound can be any compound described in the patent application with a publication date of April 26, 2018, a publication number of WO2018 / 075972, an international PCT patent application number of PCT / US2017 / 057735, and a title of "ELECTROLYTE SEPARATORS INCLUDING LITHIUM BOROHYDRIDE AND COMPOSITE ELECTROLYTE SEPARATORS OF LITHIUM-STUFFED GARNET AND LITHIUMBOROHYDRIDE". The borohydride can be any compound described in the patent application with a publication date of April 25, 2019, a publication number of WO 2019 / 078897, an application date of October 20, 2017, an international PCT patent application number of PCT / US2017 / 057739, and a title of "BOROHYDRIDE-SULFIDE INTERFACIAL LAYER IN ALL SOLID STATEBATTERY".

[0136] In some embodiments, including any of the foregoing, the lithium salt is selected from LiTFSI, LiFSI, LiPF 6 、LiClO 4 、LiAsF 6 、LiBOB、LiBETI、LiBF 4 In some embodiments, the lithium salt is selected from LiPF 6 、Lithium bis(oxalate)borate (LiBOB), lithium bis(perfluoroethanesulfonyl)imide (LIBETI), LiTFSi, LiBF 4 、LiClO 4 、LiAsF 6 , LiFSI or LiI . In some embodiments, the lithium salt is LiPF 6 In some examples, the lithium salt is LiBOB. In some examples, the lithium salt is LiTFSi. In some examples, the lithium salt is LiBF 4 In some examples, the lithium salt is LiClO 4 In some examples, the lithium salt is LiAsF 6In some examples, the lithium salt is LiI. In some examples, the lithium salt is LiBF 4 In some examples, several lithium salts may be present simultaneously at different concentrations. In some examples, the concentration is about 0.5, about 0.6, about 0.7, about 0.8, about 0.9, about 1.0, about 1.1, about 1.2, about 1.3, about 1.4, about 1.5, about 1.6, about 1.7, about 1.8, about 1.9, or about 2.0 M. In some examples, the bonding layer may include a selected LiPF 6 、LiBOB、LiTFSi、LiBF 4 、LiClO 4 、LiAsF 6 In some examples, the bonding layer may include two salts selected from LiPF 6 、LiBOB、LiTFSi、LiBF 4 、LiClO 4 、LiAsF 6 In some examples, the lithium salt is selected from LiPF 6 In some examples, the lithium salt is LiPF at a concentration of 0.5 M to 2 M. 6 In some examples, the concentration is 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or 2.0 M. In some examples, the lithium salt is LiTFSI at a concentration of 0.5 M to 2 M. In some examples, the concentration is 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or 2.0 M.

[0137] In some examples, the lithium salt is present at a concentration of 0.01M to 10M. In some examples, the concentration is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.3, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 2.0, 0.3, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3 .5, 3.6, 3.7, 3.8, 3.9, 4.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3 ,7.4,7.5,7.6,7.7,7.8,7.9,8.0,8.1,8.2,8.8,8.4,8.5,8.6,8.7,8.8,8.9,9.9,9.1,9.2,9.3,9.4,9.5,9.6,9.7,9.8,9.9,9.9,10.0M.

[0138] Other components

[0139] In some examples, including any of the foregoing, the buffer layer comprises a binder in an amount of 0.01% to 10% by weight. In some examples, the binder may include a polyolefin. The binder may include an ethylene α-olefin copolymer, an ethylene-octene copolymer, a polyolefin plastomer, a polyolefin elastomer, a styrene-butadiene rubber, polyvinylidene fluoride, poly(vinylidene fluoride-co-hexafluoropropylene), and the like.

[0140] In some examples, including any of the foregoing, the buffer layer includes 10% or less by volume of the organic polymer.

[0141] In some examples, including any of the foregoing, the polymer is selected from polyacrylonitrile (PAN), polypropylene, polyethylene oxide (PEO), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyethylene oxide poly (allyl glycidyl ether) PEO-AGE, polyethylene oxide 2-methoxyethoxy) ethyl glycidyl ether (PEO-MEEGE), polyethylene oxide 2-methoxyethoxy) ethyl glycidyl poly (allyl glycidyl ether) (PEO -MEEGE-AGE), polysiloxane, polyvinylidene fluoride (PVDF), polyvinylidene fluoride hexafluoropropylene (PVDF-HFP), ethylene propylene (EPR), nitrile rubber (NPR), styrene butadiene rubber (SBR), polybutadiene polymer, polybutadiene rubber (PB), polyisobutadiene rubber (PIB), polyisoprene rubber (PI), polychloroprene rubber (CR), acrylonitrile-butadiene rubber (NBR), polyethyl acrylate (PEA), polyvinylidene fluoride (PVDF) and polyethylene.

[0142] In some examples, including any of the foregoing, the buffer layer or buffer component does not include an organic polymer.

[0143] In some examples, including any of the foregoing, the positive electrode potential is shielded such that the potential of the lithium-filled garnet layer is not affected by the positive electrode potential.

[0144] In some examples, including any of the foregoing, the potential of the active material in the positive electrode is shielded so that the potential of the lithium-filled garnet layer is not affected by the potential of the active material in the positive electrode.

[0145] In some examples, the cathode includes an active material, wherein the active material is selected from LiNi x Mn y Co z O 2 (NMC) and LiNi x Al y Co z O 2 (NCA), where x+y+z=1.

[0146] In some examples, including any of the foregoing, the active material has a coating.

[0147] In some examples, including any of the foregoing, the active material is coated or partially coated with a coating selected from the group consisting of lithium niobium oxide, lithium zirconium oxide, lithium aluminum oxide, lithium phosphate, lithium tantalum oxide, lithium hafnium oxide, niobium oxide, zirconium oxide, aluminum oxide, tantalum oxide, hafnium oxide.

[0148] In some examples, including any of the foregoing, the active material is uncoated.

[0149] In some examples, including any of the foregoing, the positive electrode includes a lithium intercalation material, a lithium conversion material, or both a lithium intercalation material and a lithium conversion material.

[0150] In some instances, the positive electrode has a porosity of less than about 20% v / v, 15% v / v, 12.5% ​​v / v, 10% v / v, 5% v / v, 1% v / v or less. In some instances, the positive electrode has a porosity of about 5% v / v to 20% v / v or about 10% v / v to 15% v / v.

[0151] In some examples, including any of the foregoing, the embedding material is selected from nickel manganese cobalt oxide (NMC), nickel cobalt aluminum oxide (NCA), Li(NiCoAl)O 2 , lithium cobalt oxide (LCO), lithium manganese cobalt oxide (LMCO), lithium nickel manganese cobalt oxide (LMNCO), lithium nickel manganese oxide (LNMO), Li(NiCoMn)O 2 、LiMn 2 O 4 、LiCoO 2 and LiMn 2-a Ni a O 4 , where a is 0 to 2 or LiMPO 4 , wherein M is Fe, Ni, Co or Mn.

[0152] In some examples, including any of the foregoing, the lithium conversion material is selected from FeF 2 、NiF 2 , FeOxF 3-2x , FeF 3 、MnF 3 , CoF 3 ,CuF 2 Materials, their alloys and their combinations.

[0153] In some examples, including any of the foregoing, the sulfide cathode electrolyte and the single-ion conducting solid buffer are made of the same type of material.

[0154] In some examples, including any of the foregoing, the sulfide cathode electrolyte and the solid buffer conducting a single ion or both thereof are selected from LSS, SLOPS, LSTPS, LSTPSC1, SLOBS, LATS and LPS+X, wherein X is selected from Cl, I, Br and combinations thereof. In some examples, X is Cl. In some examples, X is I. In some examples, X is Br.

[0155] In some examples, including any of the foregoing, the sulfide cathode electrolyte or the solid buffer conducting a single ion or both thereof are selected from the group consisting of LSS, SLOPS, LSTPS, LSTPSCl, LSPSCl, SLOBS, LATS, and LPS+X, wherein X is selected from Cl, I, Br, and combinations thereof. In some examples, X is Cl. In some examples, X is I. In some examples, X is Br.

[0156] In some examples, including any of the foregoing, the sulfide cathode electrolyte or the single-ion conducting solid buffer, or both, is selected from LPSI, LXPS, LSTPS, LSPSCl, LPCS1, LSPSBr, and LPSBr.

[0157] In some examples, including any of the foregoing, the sulfide cathode electrolyte or the solid buffer conducting a single ion or both are selected from x·Li 2 S:y·SiS 2 , wherein x and y are each independently a number from 0 to 1, and x+y=1.

[0158] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte or the solid buffer conducting a single ion or both are selected from LSS, LGPS, LSTPS and LSPS 2 S:ySiS 2 , wherein x and y are each independently a number from 0 to 1, and x+y=1.

[0159] In some examples, including any of the foregoing, the borohydride adhesion layer includes lithium borohydride, sodium borohydride, or potassium borohydride.

[0160] In some embodiments, including any of the foregoing, the lithium borohydride, sodium borohydride or potassium borohydride is doped with LiNH 2 .

[0161] In some examples, including any of the foregoing, any one or more of the lithium borohydride, sodium borohydride, or potassium borohydride is doped with LiI.

[0162] In some embodiments, including any of the foregoing, any one or more of lithium borohydride, sodium borohydride, or potassium borohydride is doped with LiNH 2 and LiI.

[0163] In some examples, including any of the foregoing, the borohydride bonding layer comprises A(LiBH 4 )(1-A)(P 2 S 5) borohydride composition, where 0.05 ≤ A ≤ 0.95. In some instances, 0.5 < A < 0.95. In some instances, A is 0.85, 0.9, or 0.95.

[0164] In some instances, including any of the foregoing, the borohydride adhesive layer comprises 0.9(LiBH 4 )0.1(P 2 S 5 ).

[0165] In some instances, including any of the foregoing, the borohydride adhesive layer is amorphous. In some instances, including any of the foregoing, the borohydride adhesive layer is semi-crystalline. In some instances, including any of the foregoing, the borohydride adhesive layer is polycrystalline.

[0166] In some instances, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet selected from Li x La y Zr z O t ·qAl 2 O 3 , where 4 < x < 10, 1 < y < 4, 1 < z < 3, 6 < t < 14, and 0 ≤ q ≤ 1.

[0167] In some instances, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet selected from Li 7 La 3 Zr 2 O 12 ·Al 2 O 2 O 3 and Li 7 La 3 Zr 2 O 12 ·0.35Al 2 O 3 .

[0168] In some instances, including any of the foregoing, the lithium-filled garnet is doped with Nb, Ga, and / or Ta in Li 7 La 3 Zr 2 O 12 ·Al 2 O 3 and Li 7 La 3 Zr 2 O 12 ·0.35Al 2 O 3 .

[0169] In some instances, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet characterized by the formula Li a La b Zr c Al d Me” e O f where 5 < a < 8.5, 2 < b < 4, 0 ≤ c ≤ 2.5, 0 ≤ d < 2, 0 ≤ e < 2, and 10 < f < 13, and Me” is a metal selected from Nb, Ga, Ta, and combinations thereof.

[0170] In some instances, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet oxide characterized by the formula Li u La v Zr x O y ·zAl 2 O 3 where u is a rational number from 4 to 8; v is a rational number between 2 and 4; x is a rational number from 1 to 3; y is a rational number from 10 to 14; z is a rational number from 0.05 to 1; u, v, x, y, and z are selected such that the lithium-filled garnet oxide is charge-neutral.

[0171] In some instances, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet oxide characterized by the formula Li u La v Zr x O y ·zTa 2 O 5 , where u is a rational number from 4 to 10; v is a rational number between 2 and 4; x is a rational number from 1 to 3; y is a rational number from 10 to 14; z is a rational number from 0 to 1; u, v, x, y, and z are selected such that the lithium-filled garnet oxide is charge-neutral.

[0172] In some instances, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet oxide characterized by the formula Li u La v Zr x O y ·zNb 2 O 5 where u is a rational number from 4 to 10; v is a rational number between 2 and 4; x is a rational number from 1 to 3; y is a rational number from 10 to 14; z is a rational number from 0 to 1; u, v, x, y, and z are selected such that the lithium-filled garnet oxide is charge-neutral.

[0173] In some examples, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet layer characterized by the formula Li u La v Zr x O y ·zGa 2 O 3 A lithium-filled garnet oxide, wherein u is a rational number from 4 to 10; v is a rational number from 2 to 4; x is a rational number from 1 to 3; y is a rational number from 10 to 14; z is a rational number from 0 to 1; u, v, x, y and z are selected so that the lithium-filled garnet oxide is charge neutral.

[0174] In some examples, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet layer characterized by the formula Li u La v Zr x O y ·zTa 2 O 5 ·bAl 2 O 3 A lithium-filled garnet oxide, wherein u is a rational number from 4 to 10; v is a rational number from 2 to 4; x is a rational number from 1 to 3; y is a rational number from 10 to 14; z is a rational number from 0 to 1; b is a rational number from 0 to 1; wherein z+b≤1; u, v, x, y and z are selected so that the lithium-filled garnet oxide is charge neutral.

[0175] In some examples, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet layer characterized by the formula Li u La v Zr x O y ·zNb 2 O 5 ·bAl 2 O 3 A lithium-filled garnet oxide, wherein u is a rational number from 4 to 10; v is a rational number from 2 to 4; x is a rational number from 1 to 3; y is a rational number from 10 to 14; z is a rational number from 0 to 1; b is a rational number from 0 to 1; wherein z+b≤1; u, v, x, y and z are selected so that the lithium-filled garnet oxide is charge neutral.

[0176] In some examples, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet layer characterized by the formula Li u La v Zr x O y ·zGa 2 O 3 ·bAl 2 O 3A lithium-filled garnet oxide, wherein u is a rational number from 4 to 10; v is a rational number from 2 to 4; x is a rational number from 1 to 3; y is a rational number from 10 to 14; is a rational number from 0 to 1; b is a rational number from 0 to 1; wherein z+b≤1; u, v, x, y and z are selected so that the lithium-filled garnet oxide is charge neutral.

[0177] In some examples, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet layer characterized by the formula Li 6.4 Ga 0.2 La 3 Zr 2 O 12.3 ·bAl 2 O 3 A lithium-filled garnet, wherein u is a rational number from 4 to 10; v is a rational number from 2 to 4; x is a rational number from 1 to 3; y is a rational number from 10 to 14; is a rational number from 0 to 1; b is a rational number from 0 to 1; wherein z+b≤1; u, v, x, y and z are selected so that the lithium-filled garnet oxide is charge neutral.

[0178] In some examples, including any of the foregoing, the SSEC further comprises a positive electrode current collector layer.

[0179] In some examples, including any of the foregoing, the SSEC further comprises a negative electrode current collector layer. In some examples, the negative electrode current collector layer is a sintered metal. In some examples, the sintered metal is selected from Al, Cu, Ni, Ag, Au, Pt, Pd or Sn. In some examples, the metal is Ni.

[0180] In some examples, including any of the foregoing, the positive electrode layer further comprises a binder, carbon, or both a binder and carbon.

[0181] In some examples, including any of the foregoing, the lithium-filled garnet layer is between and in contact with the negative electrode current collector layer and the borohydride binding layer.

[0182] In some examples, including any of the foregoing, the borohydride adhesion layer is between and in contact with the lithium-filled garnet layer and the buffer layer.

[0183] In some examples, including any of the foregoing, the buffer layer is between and in contact with the borohydride bonding layer and the positive electrode layer.

[0184] In some examples, including any of the foregoing, the positive electrode layer is between and in contact with the buffer layer and the positive electrode current collector layer.

[0185] In some examples, including any of the foregoing, the active material includes a coating or the active material is coated. In some examples, the active material has a coating. In some examples, the active material is coated. In some examples, the active material includes a coating of a material selected from lithium lanthanum zirconium oxide (LLZO).

[0186] The lithium-filled garnet layer may include any lithium-filled garnet described in U.S. Patent No. 9,806,372B2, entitled "Garnet Materials for Li Secondary Batteries and Methods of Making and Using Garnet Materials", issued on October 31, 2017, and U.S. Patent No. 9,970,711, entitled "Lithium Stuffer Garnet Setter Plates for Solid Electric Fabrication", issued on May 15, 2018. The entire contents of each of the patents are incorporated herein by reference for all purposes. The lithium-filled garnet layer is made by forming a layer or film of the lithium-filled garnet layer described in the patent, for example, by using the method in U.S. Patent No. 9,806,372B2. The lithium-filled garnet layer may include any lithium-filled garnet set forth in U.S. Patent No. 9,966,630, published on May 8, 2018, entitled “ANNEALED GARNET ELECTROLYTE SEPARATORS”, the entire contents of which are incorporated herein by reference for all purposes. The lithium-filled garnet layer is made by forming a layer or film of the lithium-filled garnet layer described in this patent, for example, by using the method of U.S. Patent No. 9,966,630B2. The lithium-filled garnet layer may include any lithium-filled garnet set forth in U.S. Patent Application No. 15 / 631,884, entitled “LITHIUM-STUFFED GARNET ELECTROLYTES WITH SECONDARY PHASE INCLUSIONS”, filed on June 23, 2017, and published as US20180375149A1, the entire contents of which are incorporated herein by reference for all purposes. The lithium-filled garnet layer is made by forming a layer or film of the lithium-filled garnet layer described in this patent, for example, by using the method of U.S. Patent Application No. 15 / 631,884. The lithium-filled garnet layer may include any lithium-filled garnet set forth in International PCT Patent Application PCT / US2017 / 039069, entitled "LITHIUM-STUFFED GARNET ELECTROLYTES WITH SECONDARY PHASE INCLUSIONS", filed on June 23, 2017, the entire contents of which are incorporated herein by reference for all purposes. The lithium-filled garnet layer is made by forming a layer or film of the lithium-filled garnet layer described in this patent, for example, by using the method of PCT / US2017 / 039069.

[0187] In some examples, the lithium-filled garnet layer is chemically stable when in contact with lithium metal. In some examples, the lithium-filled garnet layer is kinetically stable when in contact with lithium metal.

[0188] In some examples, the lithium-filled garnet includes lithium lanthanum zirconium oxide (LLZO) and has good electrochemical stability and mechanical strength, for example, greater than 500 MPa. In some examples, the LLZO is suitable for use with a lithium metal anode.

[0189] In any of the examples described in this patent, the lithium-filled garnet layer or LLZO can be used with a binder as disclosed in the patent application filed on May 15, 2017, published on November 16, 2017, with publication number WO2017197406A1, international PCT patent application number PCT / US2017 / 032749, and entitled "SOLID ELECTROLYTE SEPARATOR BONDING AGENT", which is incorporated herein by reference in its entirety for all purposes. In any of the examples described in this patent, the lithium-filled garnet is prepared according to the method described in the patent application filed on April 15, 2016, international PCT patent application number PCT / US2016 / 027886, and entitled "LITHIUM STUFFED GARNET SETTER PLATES FOR SOLID ELECTROLYTE FABRICATION", which is incorporated herein by reference in its entirety for all purposes. In any example described in this patent, the lithium-filled garnet is prepared according to the method described in the patent application with the application date of April 15, 2016, the international PCT patent application number of PCT / US2016 / 027922, and the title of "SETTERPLATES FOR SOLID ELECTROLYTE FABRICATION AND METHODS OF USING THE SAME TOPREPARE DENSE SOLID ELECTROLYTES", which is incorporated by reference in its entirety for all purposes. In any example described in this patent, the lithium-filled garnet is prepared according to the method described in the patent application with the application date of July 21, 2016, the international PCT patent application number of PCT / US2016 / 043428, and the title of "PROCESSES AND MATERIALS FOR CASTING AND SINTERING GREEN GARNET THIN FILMS", which is incorporated by reference in its entirety for all purposes. In any of the examples described in this patent, the lithium-filled garnet is prepared according to the method described in U.S. Patent No. 9,970,711, issued on May 15, 2018, and entitled "LITHIUM STUFFED GARNET SETTER PLATES FOR SOLID ELECTROLYTE FABRICATION", the entire contents of which are incorporated by reference into this application for all purposes.In any of the examples described in this patent, the lithium-filled garnet is prepared according to the method described in U.S. Patent No. 9,970,711, entitled "LITHIUM STUFFED GARNET SETTER PLATES FOR SOLIDELECTROLYTE FABRICATION", issued on May 15, 2018, and the entire contents of which are incorporated by reference in this application for all purposes. In any of the examples described in this patent, the sulfide in the sulfide cathode electrolyte can be any sulfide described in U.S. Patent No. 9,172,114, entitled "SOLID STATE CATHOLYTES AND ELECTROLYTES FOR ENERGY STORAGE DEVICES", issued on October 27, 2015, and the entire contents of which are incorporated by reference in this application for all purposes. In any of the examples described in this patent, the sulfide in the sulfide cathode electrolyte can be any sulfide proposed in the patent application with an application date of February 1, 2016, an international PCT patent application number of PCT / US2016 / 015982, a publication number of WO 2016 / 126610, a publication date of August 11, 2016, and titled "METAL SULFIDE ANOLYTE FORELECTROCHEMICAL CELLS", the entire contents of which are incorporated by reference in this application for all purposes. In any of the examples described in this patent, the sulfide in the sulfide cathode electrolyte may be any sulfide described in the patent application with an application date of June 24, 2016, a publication date of December 29, 2016, a publication number of WO 2016 / 210371, an international PCT patent application number of PCT / US2016 / 039424, and a title of "COMPOSITE ELECTROLYTES", which is incorporated by reference in its entirety for all purposes. In any of the examples described in this patent, the sulfide in the sulfide cathode electrolyte may be any sulfide described in the U.S. patent application with a publication date of January 5, 2017, a publication number of 2017-0005367A1, and a title of "COMPOSITE ELECTROLYTES", which is incorporated by reference in its entirety for all purposes.In any example described in this patent, the sulfide in the sulfide cathode electrolyte can be any sulfide described in the patent application with an application date of December 1, 2016, a publication date of June 8, 2017, a publication number of WO 2017 / 096088, a PCT patent application number of PCT / US2016 / 064492, and a title of "LITHIUM, PHOSPHORUS, SULFUR, AND IODINE CONTAINING ELECTROLYTE AND CATHOLYTE COMPOSITIONS, ELECTROLYTE MEMBRANES FOR ELECTROCHEMICAL DEVICES, AND ANNEALING METHODS OF MAKING THESE ELECTROLYTES AND CATHOLYTES", the entire contents of which are incorporated by reference in this application for all purposes.

[0190] In some examples, the sulfide in the buffer layer may be any sulfide described in U.S. Patent No. 9,172,114, issued on October 27, 2015, entitled “SOLID STATE CATHOLYTES AND ELECTROLYTES FOR ENERGY STORAGE DEVICES”, the entire contents of which are incorporated herein by reference for all purposes. In some examples, the sulfide in the buffer layer may be any sulfide set forth in PCT Patent Application No. PCT / US2016 / 015982, filed on February 1, 2016, published on August 11, 2016, and published as WO 2016 / 126610, and any sulfide described in the patent application entitled “METAL SULFIDE ANOLYTE FOR ELECTROCHEMICAL CELLS”, the entire contents of which are incorporated herein by reference for all purposes. In some instances, the sulfide in the buffer layer may be any sulfide described in patent application WO2016 / 210371, filed on June 24, 2016, published on December 29, 2016, entitled “COMPOSITE ELECTROLYTES”, and PCT patent application number PCT / US2016 / 039424, the entire contents of which are incorporated by reference into this application for all purposes.

[0191] In some examples, the cathode includes about 85 wt % of LZO-coated NCA, about 13 wt % of LSTPS, and about 2 wt % of a binder.

[0192] In some examples, including any of the foregoing, the negative electrode is a lithium (Li) metal electrode layer. In some examples, including any of the foregoing, at least one current collector includes a material selected from the group consisting of nickel (Ni), nickel (Ni), copper (Cu), aluminum (Al) and stainless steel coated by carbon (C). In some examples, including any of the foregoing, the negative electrode current collector includes a material selected from the group consisting of nickel (Ni), nickel (Ni) and copper (Cu) coated by carbon (C). In some examples, including any of the foregoing, the positive electrode current collector layer includes a material selected from the group consisting of aluminum and aluminum coated by carbon (C). In some examples, including any of the foregoing, the negative electrode current collector layer is carbon-coated nickel. In some examples, including any of the foregoing, the positive electrode current collector layer is carbon-coated aluminum.

[0193] Buffer layer size

[0194] In some examples, including any of the foregoing, the thickness of the buffer layer is about 1 μm to about 50 μm. In some examples, the thickness of the buffer layer is 1 μm. In some examples, the thickness of the buffer layer is 2 μm. In some examples, the thickness of the buffer layer is 3 μm. In some examples, the thickness of the buffer layer is 4 μm. In some examples, the thickness of the buffer layer is 5 μm. In some examples, the thickness of the buffer layer is 6 μm. In some examples, the thickness of the buffer layer is 7 μm. In some examples, the thickness of the buffer layer is 8 μm. In some examples, the thickness of the buffer layer is 9 μm. In some examples, the thickness of the buffer layer is 10 μm.

[0195] In some examples, including any of the foregoing, the solid buffer that conducts a single ion is mixed in the positive electrode layer, and its penetration depth in the positive electrode layer is about 1 μm to about 50 μm. The penetration depth is measured from the boundary edge of the positive electrode layer and the buffer layer or the borohydride bonding layer. In some examples, if the thickness of the positive electrode layer is 200 μm, and the penetration depth in the positive electrode layer is about 1 μm to about 50 μm, it means that the buffer is on the side of the positive electrode closest to the buffer layer (if present) or the borohydride bonding layer (if no buffer layer is present). In some examples, if the thickness of the positive electrode layer is 200 μm, and the penetration depth in the positive electrode layer is about 1 μm to about 50 μm, it means that there is no buffer component on the side of the positive electrode in contact with the positive electrode collector.

[0196] In some examples, including any of the foregoing, the solid buffer that conducts a single ion is mixed in the positive electrode layer, and its penetration depth in the positive electrode layer is about 1 μm to about 50 μm. The penetration depth is measured from the boundary edge of the positive electrode layer and the buffer layer or the borohydride bonding layer. In some examples, if the thickness of the positive electrode layer is 150 μm, and the penetration depth in the positive electrode layer is about 1 μm to about 50 μm, it means that the buffer is on the side of the positive electrode closest to the buffer layer (if present) or the borohydride bonding layer (if no buffer layer is present). In some examples, if the positive electrode layer is 150 μm thick and the penetration depth in the positive electrode layer is about 1 μm to about 50 μm, it means that the positive electrode has no buffer component on the side in contact with the positive electrode collector.

[0197] In some examples, including any of the foregoing, the buffer layer is between the positive electrode layer and the separator layer and in direct contact with them. In some examples, the thickness of the buffer layer is about 1 μm to about 15 μm. In some examples, the thickness of the buffer layer is 1 μm. In some examples, the thickness of the buffer layer is 1 μm. In some examples, the thickness of the buffer layer is 2 μm. In some examples, the thickness of the buffer layer is 3 μm. In some examples, the thickness of the buffer layer is 4 μm. In some examples, the thickness of the buffer layer is 5 μm. In some examples, the thickness of the buffer layer is 6 μm. In some examples, the thickness of the buffer layer is 7 μm. In some examples, the thickness of the buffer layer is 8 μm. In some examples, the thickness of the buffer layer is 9 μm. In some examples, the thickness of the buffer layer is 10 μm. In some examples, the thickness of the buffer layer is 11 μm. In some examples, the thickness of the buffer layer is 12 μm. In some examples, the thickness of the buffer layer is 13 μm. In some examples, the thickness of the buffer layer is 14 μm. In some examples, the thickness of the buffer layer is 15 μm.

[0198] Adhesive layer size

[0199] In some examples, the bonding layer includes lithium borohydride. In some examples, the bonding layer includes lithium borohydride particles having an average diameter of at least about 1 μm. In some examples, the bonding layer includes lithium borohydride particles having an average diameter of about 1 μm to about 50 μm, about 2 μm to about 20 μm, or about 1 μm to about 10 μm.

[0200] In some examples, before assembling the battery, the bonding layer includes particles having an average diameter of at least about 1 μm. In some examples, the bonding layer particles have an average diameter of about 1 μm to about 50 μm, about 2 μm to about 20 μm, or about 1 μm to about 10 μm.

[0201] In some examples, including any of the foregoing, the borohydride bonding layer has a thickness of about 1 μm to about 50 μm. In some examples, including any of the foregoing, the borohydride bonding layer has a thickness of about 1 μm to about 50 μm. In some examples, the borohydride bonding layer has a thickness of 1 μm. In some examples, the borohydride bonding layer has a thickness of 2 μm. In some examples, the borohydride bonding layer has a thickness of 3 μm. In some examples, the borohydride bonding layer has a thickness of 4 μm. In some examples, the borohydride bonding layer has a thickness of 5 μm. In some examples, the borohydride bonding layer has a thickness of 6 μm. In some examples, the borohydride bonding layer has a thickness of 7 μm. In some examples, the borohydride bonding layer has a thickness of 8 μm. In some examples, the borohydride bonding layer has a thickness of 9 μm. In some examples, the borohydride bonding layer has a thickness of 10 μm. In some examples, the thickness of the borohydride bonding layer is 11 μm. In some examples, the thickness of the borohydride bonding layer is 12 μm. In some examples, the thickness of the borohydride bonding layer is 13 μm. In some examples, the thickness of the borohydride bonding layer is 14 μm. In some examples, the thickness of the borohydride bonding layer is 15 μm. In some examples, the thickness of the borohydride bonding layer is 16 μm. In some examples, the thickness of the borohydride bonding layer is 17 μm. In some examples, the thickness of the borohydride bonding layer is 18 μm. In some examples, the thickness of the borohydride bonding layer is 19 μm. In some examples, the thickness of the borohydride bonding layer is 20 μm. In some examples, the thickness of the borohydride bonding layer is 31 μm. In some examples, the thickness of the borohydride bonding layer is 32 μm. In some examples, the thickness of the borohydride bonding layer is 33 μm. In some examples, the thickness of the borohydride bonding layer is 34 μm. In some examples, the thickness of the borohydride bonding layer is 35 μm. In some examples, the thickness of the borohydride bonding layer is 36 μm. In some examples, the thickness of the borohydride bonding layer is 37 μm. In some examples, the thickness of the borohydride bonding layer is 38 μm. In some examples, the thickness of the borohydride bonding layer is 39 μm. In some examples, the thickness of the borohydride bonding layer is 40 μm. In some examples, the thickness of the borohydride bonding layer is 41 μm. In some examples, the thickness of the borohydride bonding layer is 42 μm. In some examples, the thickness of the borohydride bonding layer is 43 μm. In some examples, the thickness of the borohydride bonding layer is 44 μm. In some examples, the thickness of the borohydride bonding layer is 45 μm. In some examples, the thickness of the borohydride bonding layer is 46 μm. In some examples, the thickness of the borohydride bonding layer is 47 μm.In some examples, the thickness of the borohydride bonding layer is 48 μm. In some examples, the thickness of the borohydride bonding layer is 49 μm. In some examples, the thickness of the borohydride bonding layer is 50 μm.

[0202] In some examples, including any of the foregoing, the borohydride adhesion layer penetrates into the buffer layer.

[0203] In some examples, including any of the foregoing, the borohydride adhesion layer infiltrates the lithium-filled garnet layer.

[0204] In some examples, including any of the foregoing, the borohydride adhesion layer penetrates into the buffer layer and the lithium-filled garnet layer.

[0205] In some examples, including any of the foregoing, the density of the borohydride bonding layer is 90% or greater of the raw material density measured by quantitative analysis of cross-sectional SEM images. The density is determined by analyzing porosity as a function of total area using SEM images and analysis software.

[0206] In some examples, including any of the foregoing, the borohydride bonding layer has a density that is 90% or greater of the density of the raw material as measured by quantitative analysis of cross-sectional SEM images.

[0207] In some examples, including any of the foregoing, the borohydride bonding layer has a melting point below 250° C. In some examples, including any of the foregoing, the borohydride bonding layer has a melting point above 250° C.

[0208] In some examples, including any of the foregoing, the SSEC further comprises a negative electrode.

[0209] In some examples, including any of the foregoing, the negative electrode is a lithium (Li) metal negative electrode.

[0210] In some examples, including any of the foregoing, the lithium-filled garnet layer contacts the negative electrode.

[0211] In certain embodiments, the composition may be a film and includes a porosity of the film determined by SEM. For example, in one embodiment, the composition described in this patent may have a porosity of less than 5%. As a further example, in one embodiment, the composition described in this patent may have a porosity of less than 6%. As a further example, in one embodiment, the composition described in this patent may have a porosity of less than 7%. As a further example, in one embodiment, the composition described in this patent may have a porosity of less than 8%. As a further example, in one embodiment, the composition described in this patent may have a porosity of less than 4%. As a further example, in one embodiment, the composition described in this patent may have a porosity of less than 3%. As a further example, in one embodiment, the composition described in this patent may have a porosity of less than 2%. As a further example, in one embodiment, the composition described in this patent may have a porosity of less than 1%. As a further example, in one embodiment, the composition described in this patent may have a porosity of less than 0.5%.

[0212] In some examples, the solid-state electrochemical stack further includes a bonding layer between and in direct contact with the buffer layer and the separator layer.

[0213] In some examples, the present invention discloses an adhesive layer having a thickness of about 1 nm. In some examples, the present invention discloses an adhesive layer having a thickness of about 5 nm to about 100 nm.

[0214] In some examples, the present invention discloses an adhesive layer having a thickness of about 100 nm to about 1000 nm. In some examples, the adhesive layer has a thickness of about 200 nm to about 900 nm, about 300 nm to about 800 nm, or about 500 nm.

[0215] In some examples, the present patent describes an adhesive layer having a thickness of about 1 μm. In some examples, the present patent describes an adhesive layer having a thickness of about 2 μm. In some examples, the present patent describes an adhesive layer having a thickness of about 3 μm. In some examples, the present patent describes an adhesive layer having a thickness of about 4 μm. In some examples, the present patent describes an adhesive layer having a thickness of about 5 μm to about 100 μm. In some examples, the present patent describes an adhesive layer having a thickness of about 10 μm to about 50 μm, about 15 μm to about 40 μm, or 20 μm to about 40 μm. In some examples, the present patent describes an adhesive layer having a thickness of about 1 μm. In some examples, the present patent describes an adhesive layer having a thickness of about 2 μm. In some examples, the present patent describes an adhesive layer having a thickness of about 3 μm. In some examples, the present patent describes an adhesive layer having a thickness of about 4 μm. In some examples, the present invention describes an adhesive layer having a thickness of about 5 μm. In some examples, the present invention describes an adhesive layer having a thickness of about 100 μm. In some examples, the present invention describes an adhesive layer having a thickness of about 1 μm to about 100 μm, about 1 μm to about 50 μm, or about 5 μm to about 50 μm.

[0216] In some instances, including any of the foregoing, the median thickness of the bonding layer is greater than 100 nm and less than 10 μm. In some instances, including any of the foregoing, the crosslink density of the polymer measured by ASTM D2765 is greater than 0.1% and less than 30%. In some instances, including any of the foregoing, the bonding layer reduces the interfacial impedance between the electrolyte membrane and the positive electrode compared to the case where the bonding layer is not present. In some instances, the bonding layer reduces the interfacial impedance between the electrolyte membrane and the positive electrode compared to the case where the bonding layer is not present. In some instances, when the bonding layer is located between the oxide electrolyte membrane and the positive electrode and is in direct contact with them, the interfacial impedance between the oxide electrolyte membrane and the positive electrode is less than 50Ω·cm at 50°C 2 In some examples, the interface impedance between the oxide electrolyte membrane and the positive electrode is less than 25 Ω·cm at 50°C. 2 In some examples, the interface impedance between the oxide electrolyte membrane and the positive electrode is less than 10Ω·cm at 50°C. 2 In some examples, the interface impedance between the oxide electrolyte membrane and the positive electrode is less than 5Ω·cm at 50°C. 2 In some examples, the interface impedance between the oxide electrolyte membrane and the positive electrode is less than 5Ω·cm at 30°C. 2 In some examples, the interface impedance between the oxide electrolyte membrane and the positive electrode is less than 5Ω·cm at 20°C. 2In some examples, the interface impedance between the oxide electrolyte membrane and the positive electrode is less than 5Ω·cm at 10°C. 2 In some examples, the interface impedance between the oxide electrolyte membrane and the positive electrode is less than 5Ω·cm at 0°C. 2 In some embodiments, including any of the foregoing, the interface impedance between the electrolyte separator and the positive electrode is less than 50°C.

[0217] Ω·cm 2 In some embodiments, including any of the foregoing, the interface impedance between the electrolyte separator and the positive electrode is less than 25Ω·cm at 50°C. 2 In some embodiments, including any of the foregoing, the interface impedance between the electrolyte separator and the positive electrode is less than 10Ω·cm at 50°C. 2 In some embodiments, including any of the foregoing, the interface impedance between the electrolyte separator and the positive electrode is less than 5Ω·cm at 50°C. 2 In some examples, including any of the foregoing, the positive electrode comprises a lithium insertion material, a lithium conversion material, or a combination thereof.

[0218] In some examples, the adhesive layer penetrates into the positive electrode. In other examples, the thickness of the adhesive layer penetrating into the positive electrode is at least 10% of the thickness of the positive electrode. In other examples, the thickness of the adhesive layer penetrating into the positive electrode is at least 9% of the thickness of the positive electrode. In other examples, the thickness of the adhesive layer penetrating into the positive electrode is at least 8% of the thickness of the positive electrode. In other examples, the thickness of the adhesive layer penetrating into the positive electrode is at least 7% of the thickness of the positive electrode. In other examples, the thickness of the adhesive layer penetrating into the positive electrode is at least 6% of the thickness of the positive electrode. In other examples, the thickness of the adhesive layer penetrating into the positive electrode is at least 5% of the thickness of the positive electrode. In other examples, the thickness of the adhesive layer penetrating into the positive electrode is at least 4% of the thickness of the positive electrode. In other examples, the thickness of the adhesive layer penetrating into the positive electrode is at least 3% of the thickness of the positive electrode. In other examples, the thickness of the adhesive layer penetrating into the positive electrode is at least 2% of the thickness of the positive electrode. In other examples, the thickness of the adhesive layer penetrating into the positive electrode is at least 1% of the thickness of the positive electrode.

[0219] In some examples, the bonding layer contacts the cathode electrolyte in the positive electrode. In some examples, the bonding layer does not creep around the electrolyte separator. In some examples, the bonding layer does not include components that volatilize and diffuse around the electrolyte separator, thereby not contacting the Li metal negative electrode.

[0220] In some examples, including any of the foregoing, the thickness of the adhesive layer penetrating into the positive electrode is at least 10% of the thickness of the positive electrode.

[0221] In some examples, including any of the foregoing, the bonding layer contacts a solid cathode electrolyte in the positive electrode.

[0222] In some examples, including any of the foregoing, the diameter of the electrolyte separator is greater than the diameter of the positive electrode.

[0223] In some examples, including any of the foregoing, the width or diameter of the electrolyte separator is greater than the width or diameter of the positive electrode, respectively.

[0224] In some examples, including any of the foregoing, the electrolyte separator has a raised edge that protects the adhesive layer or its components from creeping around the electrolyte separator.

[0225] In some examples, including any of the foregoing, the coating edge comprises a material selected from polyparaxylene, polypropylene, polyethylene, aluminum oxide, Al 2 O 3 、ZrO 2 、TiO 2 、SiO 2 , binary oxides, La 2 Zr 2 O 7 , lithium carbonate or glass, wherein the glass is selected from SiO 2 -B 2 O 3 or Al 2 O 3 .

[0226] In some examples, the borohydride adhesion layer includes LBHI, LBHIN, [LBH-X], LBHPS, LiI, LPS, L[X]PS, or Li 3 PO 4 In some examples, the borohydride bonding layer includes a functionalized polymer such as PEO-LiTFSI, polypropylene carbonate (PPC)-LiTFSI, polyethylene carbonate (PEC)-LiTFSI, lithium-poly (2-acrylamido-2-methyl-1-propane sulfonic acid) (PAMPS), Li-Nafion, lithium-polyphenylene sulfide (PPS) or a solid organic salt associate such as ethylene carbonate (EC)-LiTFSI, dimethyl sulfide (DMS)-LiPF 6 and succinonitrile (SCN)-LiBF 4 .

[0227] Dimensions of other components

[0228] In some examples, including any of the foregoing, the thickness of the positive electrode layer is about 100 μm to about 1000 μm. In some examples, the thickness of the positive electrode layer is 10 μm. In some examples, the thickness of the positive electrode layer is 20 μm. In some examples, the thickness of the positive electrode layer is 30 μm. In some examples, the thickness of the positive electrode layer is 40 μm. In some examples, the thickness of the positive electrode layer is 50 μm. In some examples, the thickness of the positive electrode layer is 60 μm. In some examples, the thickness of the positive electrode layer is 70 μm. In some examples, the thickness of the positive electrode layer is 80 μm. In some examples, the thickness of the positive electrode layer is 90 μm. In some examples, the thickness of the positive electrode layer is 100 μm. In some examples, the thickness of the positive electrode layer is 110 μm. In some examples, the thickness of the positive electrode layer is 120 μm. In some examples, the thickness of the positive electrode layer is 130 μm. In some examples, the thickness of the positive electrode layer is 140 μm. In some examples, the thickness of the positive electrode layer is 150 μm. In some examples, the thickness of the positive electrode layer is 160 μm. In some examples, the thickness of the positive electrode layer is 170 μm. In some examples, the thickness of the positive electrode layer is 180 μm. In some examples, the thickness of the positive electrode layer is 190 μm. In some examples, the thickness of the positive electrode layer is 200 μm.

[0229] In some examples, including any of the foregoing, the thickness of the lithium-filled garnet layer is about 1 μm to about 200 μm. In some examples, the thickness of the lithium-filled garnet layer is 10 μm. In some examples, the thickness of the lithium-filled garnet layer is 20 μm. In some examples, the thickness of the lithium-filled garnet layer is 30 μm. In some examples, the thickness of the lithium-filled garnet layer is 40 μm. In some examples, the thickness of the lithium-filled garnet layer is 50 μm. In some examples, the thickness of the lithium-filled garnet layer is 60 μm. In some examples, the thickness of the lithium-filled garnet layer is 70 μm. In some examples, the thickness of the lithium-filled garnet layer is 80 μm. In some examples, the thickness of the lithium-filled garnet layer is 90 μm. In some examples, the thickness of the lithium-filled garnet layer is 100 μm. In some examples, the thickness of the lithium-filled garnet layer is 110 μm. In some instances, the thickness of the lithium-filled garnet layer is 120 μm. In some instances, the thickness of the lithium-filled garnet layer is 130 μm. In some instances, the thickness of the lithium-filled garnet layer is 140 μm. In some instances, the thickness of the lithium-filled garnet layer is 150 μm. In some instances, the thickness of the lithium-filled garnet layer is 160 μm. In some instances, the thickness of the lithium-filled garnet layer is 170 μm. In some instances, the thickness of the lithium-filled garnet layer is 180 μm. In some instances, the thickness of the lithium-filled garnet layer is 190 μm. In some instances, the thickness of the lithium-filled garnet layer is 200 μm.

[0230] In some examples, including any of the foregoing, the separator layer in the solid-state electrochemical stack described in this patent is rectangular. In another embodiment, the positive electrode layer in the solid-state electrochemical stack described in this patent is rectangular. In different embodiments, the separator layer in the solid-state electrochemical stack described in this patent is circular. In one embodiment, the positive electrode layer in the solid-state electrochemical stack described in this patent is circular.

[0231] In some examples, including any of the foregoing, the geometric surface area of ​​the positive electrode layer and the geometric surface area of ​​the separator layer are substantially the same.

[0232] In some examples, including any of the foregoing, the length of one edge of the positive electrode layer is from 2 cm to 30 cm. In some examples, the length of one edge of the positive electrode layer is 2 cm, 3 cm, 4 cm, 5 cm, 6 cm, 7 cm, 8 cm, 9 cm, 10 cm, 11 cm, 12 cm, 13 cm, 14 cm, 15 cm, 16 cm, 17 cm, 18 cm, 19 cm, 20 cm, 21 cm, 22 cm, 23 cm, 24 cm, 25 cm, 26 cm, 27 cm, 28 cm, 29 cm, or 30 cm. In some examples, the length of one edge of the separator layer is from 2 cm to 30 cm. In some examples, the length of one edge of the separator layer is 2 cm, 3 cm, 4 cm, 5 cm, 6 cm, 7 cm, 8 cm, 9 cm, 10 cm, 11 cm, 12 cm, 13 cm, 14 cm, 15 cm, 16 cm, 17 cm, 18 cm, 19 cm, 20 cm, 21 cm, 22 cm, 23 cm, 24 cm, 25 cm, 26 cm, 27 cm, 28 cm, 29 cm, or 30 cm.

[0233] In certain embodiments, the present patent provides a composite material containing lithium-filled garnet and LBHI, wherein the LBHI fills at least 90% of the through-holes and / or surface holes of the lithium-filled garnet, and wherein LBHI can be a composition having A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), where 3 ≤ A ≤ 6, 2 ≤ B ≤ 5, and 0 ≤ C ≤ 9, and X is a halide.

[0234] In some examples, including any of the foregoing, the electrolyte separator is characterized by the empirical formula Li x La A Zr B O h +yAl 2 O 3 , where 3 ≤ x ≤ 8, 2 < A < 4, 1 < B < 3, 0 ≤ y ≤ 1, 6 ≤ h ≤ 15; and the subscripts x and h and the coefficient y are selected such that the electrolyte separator is charge-neutral.

[0235] In some examples, including any of the foregoing, the electrolyte separator is doped with Ga, Nb, or Ta.

[0236] In some examples, including any of the foregoing, the electrolyte membrane has a surface roughness of about 0.01 μm to 10 μm on at least one surface. In some examples, including any of the foregoing, the electrolyte membrane has a surface roughness of about 0.01 μm to 5 μm on at least one surface. In some examples, including any of the foregoing, the electrolyte membrane has a surface roughness of about 0.01 μm to 2 μm on at least one surface. In some examples, including any of the foregoing, the density of the electrolyte membrane is greater than 95% of its theoretical density. In some examples, including any of the foregoing, the density of the electrolyte membrane is greater than 95% of the theoretical density determined by a scanning electron microscope (SEM). In some examples, including any of the foregoing, the density of the electrolyte membrane is greater than 95% of the theoretical density measured by the Archimedes method. In some examples, including any of the foregoing, the surface flatness of the electrolyte membrane is 0.1 μm to about 50 μm.

[0237] In some examples, including any of the foregoing, the lithium intercalation material is selected from the group consisting of nickel manganese cobalt oxide (NMC), nickel cobalt aluminum oxide (NCA), Li(NiCoAl)O 2 , lithium cobalt oxide (LCO), lithium manganese cobalt oxide (LMCO), lithium nickel manganese cobalt oxide (LMNCO), lithium nickel manganese oxide (LNMO), Li(NiCoMn)O 2 、LiMn 2 O 4 、LiCoO 2 、LiMn 2- a Ni a O 4 , where a is 0 to 2, or LiMPO 4 , wherein M is Fe, Ni, Co and Mn.

[0238] In some examples, including any of the foregoing, the lithium conversion material is selected from the group consisting of: FeF 2 、NiF 2 ,FeO x F 3-2x , FeF 3 、MnF 3 , CoF 3 ,CuF 2 Materials and their alloys and combinations.

[0239] In some examples, including any of the foregoing, the bonding layer permeates into the positive electrode.

[0240] In some examples, this patent discloses an electrochemical stack, wherein the thickness of the electrolyte separator is between about 10 nm and 50 μm; the thickness of the bonding layer is between about 1 μm and 20 μm; and the thickness of the positive electrode excluding the current collector is between about 5 μm and 150 μm.

[0241] In some examples, the electrolyte separator has a surface roughness Ra or Rt of about 0.1 μm to 10 μm on at least one surface. In other examples, the electrolyte separator has a surface roughness of about 0.1 μm to 5 μm on at least one surface. In other examples, the electrolyte separator has a surface roughness of about 0.1 μm to 2 μm on at least one surface. In some examples, the electrolyte has a surface roughness of about 0.1 μm to 10 μm at the surface interfacing with the electrolyte separator and the Li metal negative electrode.

[0242] In some examples, the density of the electrolyte separator is greater than 95% of its theoretical density. In other examples, the density of the electrolyte separator is greater than 95% of its theoretical density determined by scanning electron microscopy (SEM). In certain examples, the density of the electrolyte separator is greater than 95% of its theoretical density measured by the Archimedean method. In some examples, the surface flatness of the electrolyte separator is 0.1 μm to about 50 μm. In some examples, the lithium salt in the bonding layer is selected from LiPF 6 、LiBOB、LiTFSi、LiBF 4 、LiClO 4 、LiAsF 6 , LiFSI, LiI or LiBF 4 In some embodiments, the lithium salt in the adhesive layer is selected from LiPF 6 In some embodiments, the lithium salt in the bonding layer is LiPF with a concentration of 0.5M to 2M. 6 In some examples, the lithium salt in the bonding layer is LiTFSI with a concentration of 0.5M to 2M. In some examples, the lithium salt concentration in the bonding layer is 0.01M to 10M.

[0243] In some examples, the positive electrode includes a lithium insertion material, a lithium conversion material, or both. In some examples, the lithium insertion material is selected from lithium nickel cobalt manganese oxide Li(NiCoMn)O 2 、(NMC), Nickel Cobalt Aluminum Oxide (NCA), Li(NiCoAl)O 2 、Lithium cobalt oxide (LCO), lithium manganese cobalt oxide (LMCO), lithium nickel manganese cobalt oxide (LMNCO), lithium nickel manganese oxide (LNMO), LiMn 2 O 4、LiCoO 2 、LiMn 2-a Ni a O 4 (where a is 0 to 2) or LiMPO 4 , wherein M is Fe, Ni, Co or Mn. In other cases, the lithium conversion material is selected from FeF 2 、NiF 2 ,FeO x F 3-2x , FeF 3 、MnF 3 , CoF 3 ,CuF 2 In other embodiments, the conversion material is doped with other transition metal fluorides or oxides.

[0244] In some examples, the positive electrode includes an electronically conductive source of carbon.

[0245] In some examples, the positive electrode comprises a solid cathode electrolyte and a lithium insertion material or a lithium conversion material; wherein the cathode electrolyte and the lithium insertion material or the lithium conversion material each independently have a d 50 In some examples, the positive electrode includes a solid cathode electrolyte and a lithium insertion material or a lithium conversion material. The cathode electrolyte and the lithium insertion material or the lithium conversion material each independently have a particle size of about 0.1 μm to 15 μm. 50 In some examples, the bonding layer is characterized by having a thickness of about 1 nm to about 5 μm. In some examples, the lithium negative electrode is characterized by having a thickness of about 10 nm to about 50 μm. In some examples, the oxide separator is characterized by having a thickness of about 0.1 μm to about 150 μm. In some examples, the oxide separator is characterized by having a thickness of about 10 μm to about 50 μm.

[0246] In some embodiments, the coating edge comprises a material selected from the group consisting of polyparaxylene, epoxy resin, polypropylene, polyethylene, aluminum oxide, Al 2 O 3 、ZrO 2 , TiO, SiO 2 , binary oxides, lithium carbonate, La 2 Zr 2 O 7 , or a coating of glass, wherein the glass is selected from SiO 2 -B 2 O 3 or Al 2 O 3In some examples, the thickness of the edge of the electrolyte separator is gradually reduced to protect the adhesive layer from creeping around the electrolyte separator. In some examples, the edge of the separator electrolyte has been selectively treated with high temperature (e.g., laser beam) or chemicals (e.g., plasma, water, acid, etc.).

[0247] In some examples, the present patent proposes an electrochemical stack having the following structure: an electrolyte membrane with a thickness of about 10 to 20 μm; an adhesive layer with a thickness of about 1 μm to 5 μm; a positive electrode, excluding the current collector, the thickness of the positive electrode is between about 5 μm and 150 um. In some embodiments, the present patent proposes an electrochemical stack having the following structure: an electrolyte membrane with a thickness of about 10 to 50 μm; an adhesive layer with a thickness of about 1 μm to 5 μm; a positive electrode, excluding the current collector, the thickness of the positive electrode is between about 5 μm and 200 um. In some examples, the present patent proposes an electrochemical stack having the following structure: an electrolyte membrane with a thickness of about 10 to 100 μm; an adhesive layer with a thickness of about 1 μm to 5 μm; a positive electrode, excluding the current collector, the thickness of the positive electrode is between about 5 μm and 200 um.

[0248] method

[0249] In some examples, the present patent proposes a method for manufacturing an electrochemical cell, the method comprising: providing a first slurry comprising an active material, a cathode electrolyte and a solvent; depositing the first slurry onto a current collector; drying the first slurry; providing a second slurry comprising a solid buffer that conducts a single ion; depositing the second slurry onto a substrate; drying the second slurry; transferring the dried second slurry to the first slurry after drying to form a stack; applying pressure and heat to the stack; providing a solid separator; depositing a borohydride layer onto the solid separator; combining the stack with the solid separator having the borohydride layer thereon to form an electrochemical cell stack; and applying pressure and heat to the cell stack.

[0250] In some examples, including any of the foregoing, the solid loading is at least 60 wt %.

[0251] In some examples, including any of the foregoing, the buffer is LSTPS.

[0252] In some examples, the buffer layer is made by a calendaring process, wherein the pressure is at least about 100 psi, 500 psi, 1000 psi, 2000 psi or greater. In some examples, the buffer layer is made under elevated temperature conditions, such as above about 40° C., 50° C., 75° C., 100° C., 120° C., 140° C. or greater. In some examples, the buffer layer is heated to greater than about 100° C.

[0253] In some examples, including any of the foregoing, the pressure is applied uniaxially.

[0254] In certain embodiments, the present invention discloses a method for preparing a LiBH 4 )·B·(LiX)·C·(LiNH 2 ) composition, the method comprising a) preparing A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ) composite material, b) providing a molten mixture, the mixture comprising A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein X is fluorine, bromine, chlorine, iodine or a combination thereof, and 3≤A≤6, 2≤B≤5 and 0≤C≤9; c) dip coating a substrate in the molten mixture; d) removing the substrate; e) cooling the substrate to room temperature. In some examples, the substrate is a current collector. In some examples, the substrate is a solid electrolyte. In some examples, the substrate is a lithium-filled garnet.

[0255] In certain embodiments, the present invention provides a method for coating a conductive lithium ion separator electrolyte, the method comprising: a) providing a separator electrolyte; b) pressing A·(LiBH) on at least one surface of the separator at a temperature of 100-280° C. and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X can be fluorine, bromine, chlorine, iodine or a combination thereof, and 3≤A≤6, 2≤B≤5, 0≤C≤9. For example, in one embodiment, the method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X is fluorine, and 3≤A≤6, 2≤B≤5 and 0≤C≤9. As a further example, in one embodiment, a method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2O2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2) composition, wherein X is bromine, and 3≤A≤6, 2≤B≤5, 0≤C≤9 As a further example, in one embodiment, the method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2) on at least one surface of the separator at a temperature of 100-280° C. and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X is chlorine, and 3≤A≤6, 2≤B≤5 and 0≤C≤9. As a further example, in one embodiment, the method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2O2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X is iodine, and wherein 3≤A≤6, 2≤B≤5 and 0≤C≤9. As a further example, in one embodiment, a method for coating a lithium ion conductive separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2O2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X is fluorine, bromine and chlorine, and 3≤A≤6, 2≤B≤5, 0≤C≤9. As a further example, in one embodiment, the method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2O2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X is fluorine, bromine and iodine, wherein 3≤A≤6, 2≤B≤5, 0≤C≤9. As a further example, in one embodiment, a method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2) composition, wherein X is fluorine, chlorine and iodine, wherein 3≤A≤6, 2≤B≤5, 0≤C≤9. As a further example, in one embodiment, the method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X is bromine, chlorine and iodine, wherein 3≤A≤6, 2≤B≤5, 0≤C≤9.

[0256] In certain embodiments, the present invention provides a method for coating a conductive lithium ion separator electrolyte, the method comprising: a) providing a separator electrolyte; b) pressing A·(LiBH) on at least one surface of the separator at a temperature of 100-280° C. and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X can be fluorine, bromine, chlorine, iodine or a combination thereof, and 3≤A≤6, 2≤B≤5, 0≤C≤9. For example, in one embodiment, the method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X is fluorine, and 3≤A≤6, 2≤B≤5 and 0≤C≤9. As a further example, in one embodiment, a method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2O2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X is bromine, and 3≤A≤6, 2≤B≤5, 0≤C≤9 As a further example, in one embodiment, the method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2) on at least one surface of the separator at a temperature of 100-280° C. and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2) composition, wherein X is chlorine, and 3≤A≤6, 2≤B≤5 and 0≤C≤9. As a further example, in one embodiment, the method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2O2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X is iodine, and wherein 3≤A≤6, 2≤B≤5 and 0≤C≤9. As a further example, in one embodiment, a method for coating a lithium ion conductive separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2O2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X is fluorine, bromine and chlorine, and 3≤A≤6, 2≤B≤5, 0≤C≤9. As a further example, in one embodiment, the method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2O2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X is fluorine, bromine or iodine, wherein 3≤A≤6, 2≤B≤5, 0≤C≤9. As a further example, in one embodiment, a method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2O2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X is fluorine, chlorine or iodine, wherein 3≤A≤6, 2≤B≤5, 0≤C≤9. As a further example, in one embodiment, a method for coating a conductive lithium ion separator electrolyte comprises: a) providing a separator electrolyte; b) pressing A·(LiBH2O2) on at least one surface of the separator at a temperature of 100-280°C and a pressure of 10-2000 PSI. 4 )·B·(LiX)·C·(LiNH 2 ) composition, wherein X is bromine, chlorine or iodine, wherein 3≤A≤6, 2≤B≤5, 0≤C≤9.

[0257] In certain embodiments, the temperature in the method is below the melting point (T m ), and is about 0.8T m, where T m It is expressed in Kelvin (K). In certain embodiments, the method further comprises c) maintaining the pressure between the composition and the membrane for 1 to 300 minutes.

[0258] In some embodiments, the method further comprises d) cooling the coated conductive lithium ion separator electrolyte under pressure for 10-1000 minutes. In some embodiments, the method further comprises d) cooling the coated conductive lithium ion separator electrolyte under pressure for 10-1000 minutes to room temperature. In some embodiments, a method for coating a conductive lithium ion separator electrolyte is provided, the method comprising: a) providing a separator electrolyte that is stable to lithium; b) providing a solvent and A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ) precursor mixture; c) depositing the mixture on the separator by spraying, spin coating, dip coating, slot coating, gravure coating or micro gravure coating. For example, in one embodiment, a method for coating a lithium ion conductive separator electrolyte is provided, the method comprising: a) providing a separator electrolyte that is stable to lithium; b) providing a solvent and A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ) precursor mixture; c) depositing the mixture on the separator by spraying. As a further example, in one embodiment, a method for coating a lithium ion conductive separator electrolyte is provided, the method comprising: a) providing a separator electrolyte that is stable to lithium; b) providing a solvent and A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ) precursor mixture; c) depositing the mixture on the separator by spin coating. As a further example, in one embodiment, a method for coating a lithium ion conductive separator electrolyte is provided, the method comprising: a) providing a separator electrolyte that is stable to lithium; b) providing a solvent and A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ) precursor mixture; c) depositing the mixture on the separator by dip coating. As a further example, in one embodiment, a method for coating a lithium ion conductive separator electrolyte is provided, the method comprising: a) providing a separator electrolyte that is stable to lithium; b) providing a solvent and A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ) precursor mixture; c) depositing the mixture on the separator by slot coating. As a further example, in one embodiment, a method for coating a lithium ion conductive separator electrolyte is provided, the method comprising: a) providing a separator electrolyte that is stable to lithium; b) providing a solvent and A·(LiBH4 )·B·(LiX)·C·(LiNH 2 ) precursor mixture; c) depositing the mixture on the separator by gravure coating. As a further example, in one embodiment, a method for coating a conductive lithium ion separator electrolyte is provided, the method comprising: a) providing a separator electrolyte that is stable to lithium; b) providing a solvent and A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ) a mixture of precursors; c) depositing the mixture on a diaphragm by micro-gravure coating.

[0259] In certain embodiments, the solvent in the method is selected from tetrahydrofuran, ether, methanol and ethanol. For example, in one embodiment, the solvent in the method is tetrahydrofuran. As another example, in one embodiment, the solvent in the method is ether. As another example, in one embodiment, the solvent in the method is ethanol. As another example, in one embodiment, the solvent in the method is methanol.

[0260] In certain embodiments, the lithium-stable separator of the method has defects on the surface.

[0261] In certain embodiments, a method comprising: providing a 4 )·B·(LiX)·C·(LiNH 2 ), wherein X is fluorine, bromine, chlorine, iodine or a combination thereof, 3≤A≤6, 2≤B≤5, 0≤C≤9, and its XRD pattern has characteristic peaks at about 14.5°, 15.5°, 16.4°, 19.3° and 29.6° of 2θ. For example, in one embodiment, there is provided a composition containing A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein X is fluorine, and 3≤A≤6, 2≤B≤5, 0≤C≤9, and its XRD pattern has characteristic peaks at about 14.5°, 15.5°, 16.4°, 19.3° and 29.6° of 2θ. As a further example, in one embodiment, there is provided a composition containing A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein X is bromine, and 3≤A≤6, 2≤B≤5, 0≤C≤9, and its XRD pattern has characteristic peaks at 2θ of about 14.5°, 15.5°, 16.4°, 19.3° and 29.6°. As a further example, in one embodiment, there is provided a composition comprising A·(LiBH 4 )·B·(LiX)·C·(LiNH 2), wherein X is chlorine, and 3≤A≤6, 2≤B≤5, 0≤C≤9, and its XRD pattern has characteristic peaks at 2θ of about 14.5°, 15.5°, 16.4°, 19.3° and 29.6°. As a further example, in one embodiment, there is provided a composition containing A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein X is iodine, and 3≤A≤6, 2≤B≤5, 0≤C≤9, and its XRD pattern has characteristic peaks at 2θ of about 14.5°, 15.5°, 16.4°, 19.3° and 29.6°. As a further example, in one embodiment, there is provided a composition containing A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein X is fluorine, bromine and chlorine, and 3≤A≤6, 2≤B≤5, 0≤C≤9, and its XRD pattern has characteristic peaks at 2θ of about 14.5°, 15.5°, 16.4°, 19.3° and 29.6°. As a further example, in one embodiment, there is provided a composition containing A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein X is fluorine, bromine and iodine, and 3≤A≤6, 2≤B≤5, 0≤C≤9, and its XRD pattern has characteristic peaks at 2θ of about 14.5°, 15.5°, 16.4°, 19.3° and 29.6°. As a further example, in one embodiment, there is provided a composition containing A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein X is fluorine, chlorine and iodine, and 3≤A≤6, 2≤B≤5, 0≤C≤9, and its XRD pattern has characteristic peaks at 2θ of about 14.5°, 15.5°, 16.4°, 19.3° and 29.6°. As a further example, in one embodiment, there is provided a composition containing A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ) wherein X is bromine, chlorine and iodine, and 3≤A≤6, 2≤B≤5, 0≤C≤9, and its XRD pattern has characteristic peaks at 2θ of about 14.5°, 15.5°, 16.4°, 19.3° and 29.6°.

[0262] In some examples, including any of the foregoing, the polymer adhesive layer should be as thin as possible, for example, less than 5 μm, less than 2 μm or less than 1 μm. The adhesive layer can be a film, which is deposited from a solution using spraying, gravure coating, slot coating, dip coating, spin coating and similar techniques, and the solution is a solution of DMF, NMP, THF, toluene, acetonitrile or similar solvents. The adhesive layer can also be deposited from a melt above 50°C. The self-supporting film can also be pressed onto the cathode and the diaphragm at low temperatures (less than 120°C) and low pressures (less than 1000 psi).

[0263] In certain embodiments, the melted LBHXN is applied by spin coating. This embodiment uses a spin coater with heating capability. The powder is first applied to the substrate to be coated. The spin coater is heated to a temperature equal to or above the melting point of the LBHXN. After melting, the substrate is rotated at a speed of 100-5000 rpm while heating. It should be understood that the rotation speed is closely related to the thickness of the coating. After the rotation is stopped, a second layer can be laminated under a pressure of 10-2000 pounds per square inch (PSI), and the second layer is a solid cathode film or another conductive lithium ion separator (the same or different Li ion conductor as the first substrate). Whether to heat is optional. After the laminate is cooled to room temperature, the substrate, LBHXN and top layer will be firmly bonded together and will not fall apart or break if not damaged.

[0264] In some examples, the substrate can be spin coated at a speed of at least about 100 rpm, 500 rpm, 1000 rpm, 2000 rpm, 3000 rpm, or more.

[0265] In some examples, the present patent provides a method for manufacturing an electrochemical device, comprising the following steps: providing a positive electrode comprising an electrochemically active material and a solid cathode electrolyte; providing a solid cathode electrolyte comprising a sulfide single ion conductor; providing an electrolyte separator comprising a lithium-filled garnet; providing an adhesive layer comprising a polymer and a lithium salt; providing a stack, wherein the electrolyte separator is between and in contact with the lithium metal negative electrode and the adhesive layer; the adhesive layer is between and in contact with the electrolyte separator and the positive electrode; pressing the stack at low temperature and low pressure to bond, adhere or laminate the adhesive layer to the positive electrode and the electrolyte separator.

[0266] In some examples, the pressure used during the formation of the bonding layer, the buffer layer, the positive electrode layer, or any combination thereof is at least 5000 Pascals, 10 kilopascals (kPa), 100 kPa, 500 kPa, 1000 kPa, 10,000 kPa, 100,000 kPa, 1 MPa, 10 MPa, or 100 MPa. In some examples, the pressure used during the formation of the bonding layer, the buffer layer, the positive electrode layer, or any combination thereof is at least 1000 kPa, 10,000 kPa, 100,000 kPa, 1 MPa, 10 MPa, or 100 MPa.

[0267] In some examples, the pressure used during cycling of the electrochemical cells described herein is greater than atmospheric pressure and is at least 100 Pascals, 1000 Pascals, 5000 Pascals, 10 kilopascals (kPa), 100 kPa, 500 kPa, 1000 kPa, 10,000 kPa, 100,000 kPa, 1 MPa, 10 MPa, or 100 MPa.

[0268] In some examples, including any of the foregoing, the pressure is less than 1000 PSI. In some examples, including any of the foregoing, the pressure is less than 300 PSI. In some examples, including any of the foregoing, the temperature is less than 180°C. In some examples, including any of the foregoing, the temperature is less than 120°C. In some examples, including any of the foregoing, the process is performed in a clean room. In some examples, including any of the foregoing, the dew point of the clean room is less than -20°C or less than -40°C. In some examples, including any of the foregoing, the clean room is a Class 10,000 clean room.

[0269] In some examples, the patent describes a method for manufacturing an electrochemical device, comprising: providing a positive electrode containing an electrochemically active material and a solid cathode electrolyte; providing a solid cathode electrolyte containing a sulfide single ion conductor; providing an electrolyte separator containing a lithium-filled garnet; providing a bonding layer containing a polymer and a lithium salt; providing a stack, wherein the electrolyte separator is in contact with the bonding layer; the bonding layer is located between the electrolyte separator and the positive electrode and in contact with them. Pressing the stack at low temperature and low pressure to bond, adhere or laminate the bonding layer to the positive electrode and the electrolyte separator.

[0270] In some examples, including any of the foregoing, the pressure is less than 1000 PSI. In some examples, including any of the foregoing, the pressure is less than 300 PSI.

[0271] In some examples, including any of the foregoing, the temperature is less than 180° C. In some examples, including any of the foregoing, the temperature is less than 120° C.

[0272] In some examples, including any of the foregoing, the process is performed in a clean room. In some examples, including any of the foregoing, the dew point of the clean room is less than -20°C or less than -40°C. In some examples, including any of the foregoing, the clean room is rated at Class 10,000 or higher.

[0273] In some examples, during processing, the borohydride bonding layer is heated to a temperature at which it melts or partially melts to form an intimate contact with the lithium-filled garnet layer and the buffer layer in contact with the positive electrode.

[0274] In some examples, during processing, the borohydride bonding layer melts or partially melts to come into intimate contact with the lithium-filled garnet layer and the positive electrode mixed with the buffer.

[0275] In some examples, the present invention proposes a multilayer adhesive layer. In some examples, the present invention proposes a "oxide-sulfide interface layer" multilayer structure, i.e., a multilayer adhesive layer. In some examples, the adhesive layer is kinetically stable to the oxide or sulfide. In some examples, the adhesive layer promotes or maintains the interface contact of the oxide-sulfide. In some examples, the adhesive layer fills the gap between the oxide and the sulfide, improving the ionic conductivity therebetween.

[0276] In some examples, the borohydride bonding layer is spin coated onto a lithium filled garnet layer, i.e., shielding the positive electrode of the high voltage. In some examples, the borohydride bonding layer is melt cast onto a lithium filled garnet layer. In some examples, the borohydride bonding layer is melt cast onto a lithium filled garnet layer.

[0277] In some examples, the present patent proposes a method for producing a solid-state electrochemical stack, the method comprising: (a) pouring a first slurry containing sulfide solid electrolyte powder onto a first substrate to form a first layer; (b) pouring a second slurry containing sulfide solid electrolyte powder and positive electrode active powder onto a second substrate to form a second layer; (c) calendering the first layer and the second layer, wherein the first layer and the second layer are in contact with each other.

[0278] In one set of embodiments, before step (a), the method includes providing a first substrate. In this case, before step (a), the method includes providing a first slurry containing a sulfide solid electrolyte powder. In this case, before step (b), the method includes providing a second substrate. In this case, before step (b), the method includes providing a second slurry containing a sulfide solid electrolyte powder and a positive electrode active powder. In some cases, the method includes step (f) of contacting the second layer with the first layer.

[0279] Additional Embodiments

[0280] In one embodiment, the present patent provides a solid-state electrochemical stack comprising: (a) a positive electrode layer comprising a positive electrode active material and a sulfide cathode electrolyte, wherein the volume porosity of the positive electrode layer is less than 15%; (b) a buffer layer comprising a sulfide electrolyte in contact with the positive electrode layer, the volume porosity of the buffer layer is less than 15%; (c) a separator layer, the separator layer containing lithium-filled garnet and LPSX, the volume porosity of the separator layer is less than 10%; the buffer layer is between the positive electrode layer and the separator layer.

[0281] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte and sulfide electrolyte are solid.

[0282] In some embodiments, including any of the foregoing, the buffer layer substantially covers the positive electrode layer.

[0283] In some embodiments, including any of the foregoing, the buffer layer covers the positive electrode layer.

[0284] In some embodiments, including any of the foregoing, the buffer layer is uniform and dense.

[0285] In some embodiments, including any of the foregoing, the buffer layer has a uniform thickness.

[0286] In some embodiments, including any of the foregoing, the buffer layer is in direct contact with the positive electrode layer and the separator layer.

[0287] In some embodiments, including any of the foregoing, the adhesive layer is between and in direct contact with the buffer layer and the separator layer.

[0288] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte is a sulfide single ion conductor.

[0289] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte is an electrolyte comprising lithium (Li), phosphorus (P), and sulfur (S).

[0290] In some embodiments, including any of the foregoing, the cathode electrolyte comprises iodine (I).

[0291] In some embodiments, including any of the foregoing, the cathode electrolyte comprises chlorine (Cl), bromine (Br), iodine (I), or a combination thereof.

[0292] In some embodiments, including any of the foregoing, the cathode electrolyte comprises a material selected from tin (Sn), germanium (Ge), arsenic (As), silicon (Si), and combinations thereof.

[0293] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte is selected from LPSI, LSTPS, LSPSC1, LBHI, and LPS.

[0294] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte is LSTPS.

[0295] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte is LPSI.

[0296] In some embodiments, including any of the foregoing, the sulfide electrolyte is a sulfide single ion conductor.

[0297] In some embodiments, including any of the foregoing, the positive electrode layer includes a positive electrode active material having a mass loading of about 75%-90%.

[0298] In some embodiments, including any of the foregoing, the positive electrode active material comprises a lithium insertion material, a lithium conversion material, or both.

[0299] In some embodiments, including any of the foregoing, the positive electrode active material comprises a lithium insertion material; wherein the insertion material is selected from nickel manganese cobalt oxide (NMC), nickel cobalt aluminum oxide (NCA), Li(NiCoAl)O 2 , lithium cobalt oxide (LCO), lithium manganese cobalt oxide (LMCO), lithium nickel manganese cobalt oxide (LMNCO), lithium nickel manganese oxide (LNMO), Li(NiCoMn)O 2 、LiMn 2 O 4 、LiCoO 2 and LiMn 2-a Ni a O 4 , where a is 0 to 2 or LiMPO 4 , wherein M is Fe, Ni, Co or Mn.

[0300] In some embodiments, including any of the foregoing, the positive electrode active material comprises a lithium conversion material; the lithium conversion material is selected from FeF 2 、NiF 2 ,FeO x F 3-2x , FeF 3 、MnF 3 , CoF 3 ,CuF 2 materials and their alloys or combinations.

[0301] In some embodiments, including any of the foregoing, the embedding material is NCA.

[0302] In some embodiments, including any of the foregoing, the embedding material is NMC.

[0303] In some embodiments, including any of the foregoing, the solid-state electrochemical stack further comprises a bonding layer.

[0304] In some embodiments, including any of the foregoing, the bonding layer comprises a borohydride composition.

[0305] In some embodiments, including any of the foregoing, the buffer layer is between and in direct contact with the positive electrode layer and the borohydride layer, and the borohydride layer is between and in direct contact with the buffer layer and the separator layer.

[0306] In some embodiments, including any of the foregoing, the borohydride composition is represented by the formula:

[0307] A.(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein X is selected from fluorine (F), bromine (Br), chloride (Cl), iodine (I) and combinations thereof, wherein 3≤A≤6, 2≤B≤5 and 0≤C≤9.

[0308] In some embodiments, including any of the foregoing, the borohydride composition is represented by the formula A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein X is selected from fluorine (F), bromine (Br), chlorine (Cl), iodine (I) and combinations thereof, wherein 3≤A≤6, 2≤B≤5 and 3≤C≤9.

[0309] In some embodiments, including any of the foregoing, the borohydride composition is represented by the following formula: A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein X is selected from fluorine (F), bromine (Br), chlorine (Cl), iodine (I) and combinations thereof, wherein 3≤A≤6, 2≤B≤5 and 3≤C≤6.

[0310] In some embodiments, including any of the foregoing, the borohydride composition is selected from one of the following formulas: 3LiBH 4 2LiI 3LiNH 2 or 3LiBH 4 ·4LiI·9LiNH 2 .

[0311] In some embodiments, including any of the foregoing, the adhesive layer further comprises LiI, LPS, LXPS, Li 3 PO4 or a combination thereof.

[0312] In some embodiments, including any of the foregoing, the solid-state electrochemical stack includes (d) a negative electrode current collector in direct contact with the separator layer.

[0313] In some embodiments, including any of the foregoing, the solid-state electrochemical stack includes (e) a positive electrode current collector in direct contact with the positive electrode layer.

[0314] In some embodiments, including any of the foregoing, the solid-state electrochemical stack includes (d) a negative electrode current collector and (e) a negative electrode, wherein the (e) negative electrode is between the separator layer and the negative electrode current collector and is in direct contact with them.

[0315] In some embodiments, including any of the foregoing, the negative electrode is a lithium (Li) metal electrode layer.

[0316] In some embodiments, including any of the foregoing, at least one current collector comprises an alloy selected from carbon (C) coated nickel (Ni), nickel (Ni), copper (Cu), aluminum (Al), stainless steel, and combinations thereof.

[0317] In some embodiments, including any of the foregoing, the negative electrode current collector includes a material selected from the group consisting of carbon (C)-coated nickel (Ni), nickel (Ni), copper (Cu), and alloys thereof, or combinations thereof.

[0318] In some embodiments, including any of the foregoing, the positive electrode current collector layer includes a material selected from the group consisting of carbon (C)-coated aluminum and aluminum.

[0319] In some embodiments, including any of the foregoing, the negative electrode current collector layer is carbon-coated Ni.

[0320] In some embodiments, including any of the foregoing, the diaphragm layer is rectangular.

[0321] In some embodiments, including any of the foregoing, the positive electrode layer is rectangular.

[0322] In some embodiments, including any of the foregoing, the diaphragm layer is circular.

[0323] In some embodiments, including any of the foregoing, the geometric surface area of ​​the positive electrode layer and the geometric surface area of ​​the separator layer are substantially the same.

[0324] In some embodiments, including any of the foregoing, a length of one edge of the positive electrode layer is 2 cm-30 cm.

[0325] In some embodiments, including any of the foregoing, a length of one edge of the diaphragm layer is 2 cm-30 cm.

[0326] In some embodiments, including any of the foregoing, the diameter of the positive electrode layer is 10 cm.

[0327] In some embodiments, including any of the foregoing, the diameter of the diaphragm layer is 10 cm.

[0328] In some embodiments, including any of the foregoing, the positive electrode layer comprises a percolating web of ion conductor.

[0329] In some embodiments, including any of the foregoing, the separator layer comprises a percolating network of ion conductors.

[0330] In some embodiments, including any of the foregoing, the membrane layer comprises a polymer.

[0331] In some embodiments, including any of the foregoing, the cathode layer comprises carbon at a mass loading of about 0 to about 1%.

[0332] In some embodiments, including any of the foregoing, the carbon having a mass loading of about 0 to about 1% is C65 or vapor grown carbon fiber (VGCF).

[0333] In some embodiments, including any of the foregoing, the positive electrode layer comprises a binder having a mass loading of about 0 to about 2.5%.

[0334] In some embodiments, including any of the foregoing, the binder loaded at a mass content of about 0 to about 2.5% comprises a binder selected from the group consisting of polyacrylonitrile (PAN), polypropylene, polyethylene oxide (PEO), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyethylene oxide poly (allyl glycidyl ether) PEO-AGE, polyethylene oxide 2-methoxyethoxy) ethyl glycidyl ether (PEO-MEEGE), polyethylene oxide 2-methoxyethoxy) ethyl glycidyl poly (allyl glycidyl ether) (PEO-MEEGE-AGE), polysiloxane , polyvinylidene fluoride (PVDF), polyvinylidene fluoride hexafluoropropylene (PVDF-HFP), ethylene propylene (EPR), nitrile rubber (NPR), styrene butadiene rubber (SBR), polybutadiene polymer, polybutadiene rubber (PB), polyisobutadiene rubber (PIB), polyolefin, α-polyolefin, α-olefin, ethylene α-polyolefin, polyisoprene rubber (PI), polychloroprene rubber (CR), acrylonitrile-butadiene rubber (NBR), polyethyl acrylate (PEA), polyvinylidene fluoride (PVDF), polyethylene, POB3, polyolefin, rubber or adhesives thereof.

[0335] In some embodiments, including any of the foregoing, the thickness of the positive electrode layer is from about 10 μm to about 500 μm.

[0336] In some embodiments, including any of the foregoing, the positive electrode layer has a thickness of 100 μm to about 500 μm.

[0337] In some embodiments, including any of the foregoing, the isolation layer has a thickness of about 1 μm to about 200 μm.

[0338] In some embodiments, including any of the foregoing, the thickness of the positive electrode current collector layer is from about 3 μm to about 100 μm.

[0339] In some embodiments, including any of the foregoing, the thickness of the positive electrode current collector layer is about 15 μm.

[0340] In some embodiments, including any of the foregoing, the thickness of the negative electrode current collector layer is from about 3 μm to about 100 μm.

[0341] In some embodiments, including any of the foregoing, the thickness of the positive electrode current collector layer is about 15 μm.

[0342] In some embodiments, including any of the foregoing, the thickness of the tab on the positive current collector or the negative current collector is about 5 μm to about 100 μm.

[0343] In some embodiments, including any of the foregoing, the positive electrode layer has a porosity of less than 1% v / v.

[0344] In some embodiments, including any of the foregoing, the buffer layer has a porosity of less than 1% v / v.

[0345] In some embodiments, including any of the foregoing, the positive electrode layer has a porosity of at least 0.01% v / v.

[0346] In some embodiments, including any of the foregoing, the buffer layer has a porosity of at least 0.01% v / v.

[0347] In some embodiments, including any of the foregoing, the separator layer contains an empirical formula Li 7 La 3 Zr 2 O 12 -xAl 2 O 3 A lithium-filled garnet, where x is a rational number and 0≤x≤1.

[0348] In some embodiments, including any of the foregoing, the separator layer comprises a Li u La v Zr x Oy ·zAl 2 O 3 A lithium-filled garnet oxide where u is a rational number from 4 to 8; v is a rational number between 2 and 4; x is a rational number from 1 to 3; y is a rational number between 10 and 14; z is a rational number from 0.05 to 1; u, v, x, y, and z are selected such that the lithium-filled garnet oxide is charge-neutral.

[0349] In some embodiments, including any of the foregoing, the separator layer comprises Li x La y Zr z O t ·qAl 2 O 3 , where 4 < x < 10, 1 < y < 4, 1 < z < 3, 6 < t < 14, and 0 ≤ q ≤ 1.

[0350] In some embodiments, including any of the foregoing, the separator layer comprises Li 7 La 3 Zr 2 O 12 ·Al 2 O 3 or Li 7 La 3 Zr 2 O 12 ·0.35Al 2 O 3 。

[0351] In some embodiments, including any of the foregoing, the lithium-filled garnet is doped with Nb, Ga, and / or Ta.

[0352] In another embodiment, the present patent presents a solid-state electrochemical single cell (SSEC), comprising: (a) a positive electrode layer containing an active material and a sulfide cathode electrolyte; (b) a solid-state buffer that conducts a single ion; (c) a borohydride adhesive layer; (d) a lithium-filled garnet layer. Wherein the buffer is mixed within the positive electrode layer, or is a layer in contact with the positive electrode layer, or both; the borohydride adhesive layer is between the lithium-filled garnet layer and (i) the positive electrode layer in which the buffer is mixed or (ii) the buffer layer in contact with the positive electrode and is in contact with them.

[0353] In some embodiments, including any of the foregoing, the solid-state buffer that conducts a single ion is mixed within the positive electrode layer.

[0354] In some embodiments, including any of the foregoing, the solid-state buffer that conducts a single ion is a layer in contact with the positive electrode layer.

[0355] In some embodiments, including any of the foregoing, the single-ion conductive solid buffer is mixed in the positive electrode layer and serves as a layer in contact with the positive electrode layer.

[0356] In some embodiments, including any of the foregoing, the single-ion conducting solid buffer layer can avoid direct contact between the borohydride bonding layer and the positive electrode layer.

[0357] In some embodiments, including any of the foregoing, the positive electrode layer has a thickness of about 100 μm to about 1000 μm.

[0358] In some embodiments, including any of the foregoing, the buffer layer has a thickness of about 0.5 μm to about 50 μm.

[0359] In some embodiments, including any of the foregoing, a solid buffer mixture that conducts a single ion is infiltrated into the positive electrode layer, and the penetration depth is about 1 μm to about 50 μm from the edge within the positive electrode layer, wherein the edge is the edge where the positive electrode layer intersects with the buffer layer or the borohydride bonding layer.

[0360] In some embodiments, including any of the foregoing, the lithium-filled garnet layer has a thickness of about 1 μm to about 200 μm.

[0361] In some embodiments, including any of the foregoing, the borohydride adhesion layer has a thickness of about 0.5 μm to about 50 μm.

[0362] In some embodiments, including any of the foregoing, the borohydride adhesion layer penetrates into the buffer layer.

[0363] In some embodiments, including any of the foregoing, the borohydride adhesion layer infiltrates into the lithium-filled garnet layer.

[0364] In some embodiments, including any of the foregoing, the density of the borohydride bonding layer is 90% or more of the density of the feedstock.

[0365] In some embodiments, including any of the foregoing, the borohydride bonding layer has a volumetric porosity of less than 10%.

[0366] In some embodiments, including any of the foregoing, the borohydride adhesion layer has a melting point below 250°C.

[0367] In some embodiments, including any of the foregoing, the borohydride adhesion layer has a melting point above 250°C.

[0368] In some embodiments, including any of the foregoing, the solid-state electrochemical stack includes a negative electrode.

[0369] In some embodiments, including any of the foregoing, the negative electrode is a lithium (Li) metal negative electrode.

[0370] In some embodiments, including any of the foregoing, the lithium-filled garnet layer is in contact with a negative electrode.

[0371] In some embodiments, including any of the foregoing, the buffer layer includes 0.01% to 10% by weight of the binder.

[0372] Embodiment 120: The SSEC of embodiment 120, wherein the binder is a polymer and does not conduct electrons or Li ions.

[0373] In some embodiments, including any of the foregoing, the buffer layer comprises 10% by volume or less of an organic polymer.

[0374] In some embodiments, including any of the foregoing, the polymer is selected from polyacrylonitrile (PAN), polypropylene, polyethylene oxide (PEO), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyethylene oxide poly (allyl glycidyl ether) PEO-AGE, polyethylene oxide 2-methoxyethoxy) ethyl glycidyl ether (PEO-MEEGE), polyethylene oxide 2-methoxyethoxy) ethyl glycidyl poly (allyl glycidyl ether) (PEO-MEEGE -AGE), polysiloxane, polyvinylidene fluoride (PVDF), ethylene α-olefin copolymer, polyvinylidene fluoride hexafluoropropylene (PVDF-HFP), ethylene propylene (EPR), nitrile rubber (NPR), styrene butadiene rubber (SBR), polybutadiene polymer, polybutadiene rubber (PB), polyisobutadiene rubber (PIB), polyisoprene rubber (PI), polychloroprene rubber (CR), acrylonitrile-butadiene rubber (NBR), polyethyl acrylate (PEA), polyvinylidene fluoride (PVDF) and polyethylene.

[0375] In some embodiments, including any of the foregoing, the buffer layer or buffer component does not include an organic polymer.

[0376] In some embodiments, including any of the foregoing, the positive electrode potential is shielded from the potential of the lithium-filled garnet layer.

[0377] In some embodiments, including any of the foregoing, the potential of the active material in the positive electrode is shielded from the potential of the lithium-filled garnet layer.

[0378] In some embodiments, including any of the foregoing, the active material is coated.

[0379] In some embodiments, including any of the foregoing, the coated active material has a coating selected from the group consisting of lithium niobium oxide, lithium zirconium oxide, lithium aluminum oxide, lithium tantalum oxide, lithium hafnium oxide, niobium oxide, zirconium oxide, aluminum oxide, tantalum oxide, and hafnium oxide.

[0380] In some embodiments, including any of the foregoing, the active material is uncoated.

[0381] In some embodiments, including any of the foregoing, the positive electrode comprises a lithium insertion material, a lithium conversion material, or both.

[0382] In some embodiments, including any of the foregoing, the embedded material is selected from nickel manganese cobalt oxide (NMC), nickel cobalt aluminum oxide (NCA), Li(NiCoAl)O 2 , lithium cobalt oxide (LCO), lithium manganese cobalt oxide (LMCO), lithium nickel manganese cobalt oxide (LMNCO), lithium nickel manganese oxide (LNMO), Li(NiCoMn)O 2 、LiMn 2 O 4 、LiCoO 2 and LiMn 2-a Ni a O 4 , where a is 0 to 2 or LiMPO 4 , wherein M is Fe, Ni, Co or Mn.

[0383] In some embodiments, including any of the foregoing, the lithium conversion material is selected from FeF 2 、NiF 2 ,FeO x F 3-2x , FeF 3 、MnF 3 , CoF 3 ,CuF 2 alloys or combinations thereof.

[0384] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte and the single-ion conducting solid buffer comprise the same type of material.

[0385] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte or the solid buffer conducting a single ion, or both, are selected from LSS, SLOPS, LSTPS, LSTPSC1, SLOBS, LATS, and LPS+X, wherein X is selected from Cl, I, Br, and combinations thereof.

[0386] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte or the single-ion conducting solid-state buffer or both are selected from LPSI, LXPS, LSTPS, LSPSCl, LPCS1, LSPSBr, and LPSBr.

[0387] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte or the single-ion conducting solid-state buffer or both are selected from x·Li 2 S:y·SiS 2 , where x and y are each independently from 0 to 1, where x + y = 1.

[0388] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte or the single-ion conducting solid-state buffer or both are selected from LSS, LGPS, LSTPS, and LSPS.

[0389] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte or the single-ion conducting solid-state buffer or both are characterized by one of the following formulas: Li a Si b Sn c P d S e , where 2 ≤ a ≤ 8, 0 ≤ b ≤ 1, 0 ≤ c ≤ 1, 0.5 ≤ d ≤ 2.5, and 2 ≤ e ≤ 12; Li a Si b P c S d X e , where 8 < a < 12, 1 < b < 3, 1 < c < 3, 8 < d < 14, and 0 < e < 1, where X is F, Cl, Br, or I; Li g As h Sn j S k O l , where 2 ≤ g ≤ 6, 0 ≤ h ≤ 1, 0 ≤ j ≤ 1, 2 ≤ k ≤ 6, and 0 ≤ l ≤ 10; or Li m P n S p I q , where 2 ≤ m ≤ 6, 0 ≤ n ≤ 1, 0 ≤ p ≤ 1, 2 ≤ q ≤ 6; or a mixture of (Li 2 S):(P 2 S 5 ) and LiI with a molar ratio of about 10:1 to about 6:4, where the ratio of [(Li 2 S):(P 2 S 5 ):LiI is from 95:5 to 50:50; LPS + X, where X is selected from Cl, I, or Br; vLi 2 S + wP2 S 5 +yLiX;vLi 2 S+W 2 +yLiX or vLi 2 S+B 2 S 3 +yLiX.

[0390] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte comprises LSTPS.

[0391] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte is characterized by the formula: Li a Si b Sn c P d S e , where 2≤a≤8, 0≤b≤1, 0≤c≤1, 0.5≤d≤2.5, 2≤e≤12.

[0392] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte is characterized by the formula: Li a Si b Sn c P d S e , where 2≤a≤5, 0≤b≤0.5, 0≤c≤0.5, 0.5≤d≤2, 2≤e≤12.

[0393] In some embodiments, including any of the foregoing, the single-ion conducting solid buffer comprises LSTPS.

[0394] In some embodiments, including any of the foregoing, the borohydride adhesion layer comprises lithium borohydride, sodium borohydride, or potassium borohydride.

[0395] In some embodiments, including any of the foregoing, the lithium borohydride, sodium borohydride or potassium borohydride is doped with LiNH 2 .

[0396] In some embodiments, including any of the foregoing, any one or more of the lithium borohydride, sodium borohydride, or potassium borohydride is doped with LiI.

[0397] In some embodiments, including any of the foregoing, any one or more of the lithium borohydride, sodium borohydride or potassium borohydride is doped with LiNH 2 and LiI.

[0398] In some embodiments, including any of the foregoing, the borohydride adhesion layer comprises A(LiBH 4 )(1-A)(P 2 S5 ) of a borohydride composition wherein 0.05≤A≤0.95.

[0399] In some embodiments, including any of the foregoing, 0.5 <A<0.95。

[0400] In some embodiments, including any of the foregoing, A is 0.85, 0.9 or 9.95.

[0401] In some embodiments, including any of the foregoing, the borohydride bonding layer comprises 0.9 (LiBH 4 )0.1(P 2 S 5 ).

[0402] In some embodiments, including any of the foregoing, the borohydride bonding layer comprises a borohydride composition comprising A·(LiBH 4 )·B·(LiX)·C·(LiNH 2 ), wherein X is fluorine, bromine, chlorine, iodine or a combination thereof, wherein 3≤A≤6, 2≤B≤5 and 0≤C≤9.

[0403] In some embodiments, including any of the foregoing, 3≤A≤6, 2≤B≤5, and 3≤C≤9.

[0404] In some embodiments, including any of the foregoing, X is bromine, chlorine, iodine, or a combination thereof.

[0405] In some embodiments, including any of the foregoing, X is chloro.

[0406] In some embodiments, including any of the foregoing, X is bromine.

[0407] In some embodiments, including any of the foregoing, X is iodine.

[0408] In some embodiments, including any of the foregoing, 3≤A≤6, 3≤B≤5, and 3≤C≤9

[0409] In some embodiments, including any of the foregoing, 4≤A≤6, 4≤B≤5, and 4≤C≤6

[0410] In some embodiments, including any of the foregoing, the borohydride bonding layer comprises a borohydride composition, wherein the composition is 3LiBH 4 2LiCl 3LiNH 2 or 3LiBH 4 ·4LiCl·9LiNH 2 .

[0411] In some embodiments, including any of the foregoing, the borohydride adhesive layer comprises a borohydride composition, the composition being 3LiBH 4 ·2LiBr·3LiNH 2 or 3LiBH 4 ·4LiBr·9LiNH 2 .

[0412] In some embodiments, including any of the foregoing, the borohydride adhesive layer comprises a borohydride composition, the composition being 3LiBH 4 ·2LiI·3LiNH 2 or 3LiBH 4 ·4LiI·9LiNH 2 .

[0413] In some embodiments, including any of the foregoing, the borohydride adhesive layer comprises a borohydride composition selected from LBHIN and LBHN.

[0414] In some embodiments, including any of the foregoing, the borohydride adhesive layer comprises KBH 4 +LiNH 2 .

[0415] In some embodiments, including any of the foregoing, the borohydride adhesive layer is amorphous.

[0416] In some embodiments, including any of the foregoing, the borohydride adhesive layer is semi-crystalline.

[0417] In some embodiments, including any of the foregoing, the borohydride adhesive layer is polycrystalline.

[0418] In some embodiments, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet selected from Li x La y Zr z O t ·qAl 2 O 3 where 4 < x < 10, 1 < y < 4, 1 < z < 3, 6 < t < 14, and 0 ≤ q ≤ 1.

[0419] In some embodiments, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet selected from Li 7 La 3 Zr 2 O 12 ·Al 2 O 3 and Li 7 La 3 Zr 2 O12 · 0.35Al 2 O 3 lithium-filled garnet.

[0420] In some embodiments, including any of the foregoing, the lithium-filled garnet is doped with Nb, Ga, and / or Ta.

[0421] In some embodiments, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet characterized by the formula Li a La b Zr c Al d Me” e O f where 5 < a < 8.5, 2 < b < 4, 0 ≤ c ≤ 2.5, 0 ≤ d < 2, 0 ≤ e < 2, 0 < f < 13, and Me” is a metal selected from Nb, Ga, Ta, and combinations thereof.

[0422] In some embodiments, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet oxide characterized by the formula Li u La v Zr x O y · zAl 2 O 3 where u is a rational number from 4 to 8; v is a rational number between 2 and 4; x is a rational number from 1 to 3; y is a rational number between 10 and 14; z is a rational number from 0.05 to 1; u, v, x, y, and z are selected such that the lithium-filled garnet oxide is charge-neutral. In some embodiments, including any of the foregoing, the lithium-filled garnet layer contains a lithium-filled garnet oxide characterized by the formula Li u La v Zr x O y · zTa 2 O 5 where u is a rational number from 4 to 10; v is a rational number between 2 and 4; x is a rational number from 1 to 3; y is a rational number between 10 and 14; z is a rational number from 0 to 1; u, v, x, y, and z are selected such that the lithium-filled garnet oxide is charge-neutral.

[0423] In some embodiments, including any of the foregoing, the lithium-filled garnet layer contains a lithium-filled garnet oxide characterized by the formula Li u La v Zr x O y · zNb 2 O 5A lithium-filled garnet oxide, wherein u is a rational number from 4 to 10; v is a rational number from 2 to 4; x is a rational number from 1 to 3; y is a rational number from 10 to 14; z is a rational number from 0 to 1; u, v, x, y and z are selected so that the lithium-filled garnet oxide is charge neutral.

[0424] In some embodiments, including any of the foregoing, the lithium-filled garnet layer comprises a garnet layer having a formula Li u La v Zr x O y ·zGa 2 O 3 A lithium-filled garnet oxide, wherein u is a rational number from 4 to 10; v is a rational number from 2 to 4; x is a rational number from 1 to 3; y is a rational number from 10 to 14; z is a rational number from 0 to 1; u, v, x, y and z are selected so that the lithium-filled garnet oxide is charge neutral.

[0425] In some embodiments, including any of the foregoing, the lithium-filled garnet layer comprises a garnet layer characterized by the formula Li u La v Zr x O y ·zTa 2 O 5 ·bAl 2 O 3 A lithium-filled garnet oxide, wherein u is a rational number from 4 to 10; v is a rational number between 2 and 4; x is a rational number from 1 to 3; y is a rational number between 10 and 14; z is a rational number from 0 to 1; b is a rational number from 0 to 1; wherein z+b≤1; u, v, x, y and z are selected so that the lithium-filled garnet oxide is charge neutral.

[0426] In some embodiments, including any of the foregoing, the lithium-filled garnet layer comprises a lithium-filled garnet layer characterized by the formula Li u La v Zr x O y ·zNb 2 O 5 ·bAl 2 O 3 A lithium-filled garnet oxide, wherein u is a rational number from 4 to 10; v is a rational number between 2 and 4; x is a rational number from 1 to 3; y is a rational number between 10 and 14; z is a rational number from 0 to 1; b is a rational number from 0 to 1; wherein z+b≤1; u, v, x, y and z are selected so that the lithium-filled garnet oxide is charge neutral.

[0427] In some embodiments, including any of the foregoing, the lithium-filled garnet layer comprises a garnet layer characterized by the formula Li u La v Zr x O y ·zGa 2 O 3 ·bAl 2 O 3 A lithium-filled garnet oxide, wherein u is a rational number from 4 to 10; v is a rational number between 2 and 4; x is a rational number from 1 to 3; y is a rational number between 10 and 14; z is a rational number from 0 to 1; b is a rational number from 0 to 1; wherein z+b≤1; u, v, x, y and z are selected so that the lithium-filled garnet oxide is charge neutral.

[0428] In some embodiments, including any of the foregoing, the lithium-filled garnet layer comprises a garnet layer characterized by the formula Li 6.4 Ga 0.2 La 3 Zr 2 O 12 of lithium-filled garnets.

[0429] In some embodiments, including any of the foregoing, the SSEC includes a positive current collector layer.

[0430] In some embodiments, including any of the foregoing, the SSEC includes a negative current collector layer.

[0431] In some embodiments, including any of the foregoing, the negative electrode current collector layer is a sintered metal.

[0432] In some embodiments, including any of the foregoing, the sintered metal is selected from Al, Cu, Ni, Ag, Au, Pt, Pd, or Sn.

[0433] In some embodiments, including any of the foregoing, the metal is Ni.

[0434] In some embodiments, including any of the foregoing, the positive electrode layer further comprises a binder, carbon, or both.

[0435] In some embodiments, including any of the foregoing, the lithium-filled garnet layer is between and in contact with the negative electrode current collector layer and the borohydride bonding layer.

[0436] In some embodiments, including any of the foregoing, the borohydride adhesion layer is between and in contact with the lithium-filled garnet layer and the buffer layer.

[0437] In some embodiments, including any of the foregoing, the buffer layer is between and in contact with the borohydride adhesion layer and the positive electrode layer.

[0438] In some embodiments, including any of the foregoing, the positive electrode layer is between the buffer layer and the positive electrode current collector layer and in contact with them.

[0439] In some embodiments, including any of the foregoing, the negative electrode layer is between and in contact with the lithium-filled garnet layer and the negative electrode current collector layer.

[0440] In one embodiment, the present patent provides a battery comprising the SSEC described in any one of the embodiments.

[0441] In one embodiment, this patent proposes an electric vehicle comprising the battery described in any embodiment.

[0442] In one embodiment, the present patent discloses a method for manufacturing an electrochemical cell: providing a first slurry comprising an active material, a cathode electrolyte and a solvent; depositing the first slurry onto a current collector; drying the first slurry; providing a second slurry comprising a solid buffer that conducts a single ion; depositing the second slurry onto a substrate; drying the second slurry; transferring the dried second slurry onto the first slurry to form a stack; pressurizing and heating the stack; providing a solid separator; depositing a borohydride layer onto the solid separator; combining the stack with the solid separator having the borohydride layer thereon to form an electrochemical cell stack; pressurizing and heating the cell stack.

[0443] In some embodiments, including any of the foregoing, the solid loading is at least 60 wt %.

[0444] In some embodiments, including any of the foregoing, the buffer is LSTPS.

[0445] In some embodiments, including any of the foregoing, pressurization is unidirectional.

[0446] In one embodiment, the present patent proposes a double-layer stack comprising: (a) a positive electrode layer comprising an active material and a sulfide cathode electrolyte; (b) a solid buffer that conducts a single ion, wherein the buffer is mixed within the positive electrode layer, or is a layer in contact with the positive electrode layer, or both.

[0447] In some embodiments, including any of the foregoing, the single-ion conducting solid buffer is mixed in the positive electrode layer.

[0448] In some embodiments, including any of the foregoing, the single-ion conducting solid buffer is a layer in contact with the positive electrode layer.

[0449] In some embodiments, including any of the foregoing, the single-ion conducting solid buffer is mixed within the positive electrode layer and serves as a layer in contact with the positive electrode layer.

[0450] In some embodiments, including any of the foregoing, the buffer mixture is infiltrated in the positive electrode layer, and the penetration depth is about 1 μm to about 50 μm from the edge in the positive electrode layer, wherein the edge is the edge where the positive electrode layer intersects with the buffer layer or the borohydride bonding layer.

[0451] In some embodiments, including any of the foregoing, the lithium-filled garnet layer has a thickness of about 1 μm to about 200 μm.

[0452] In some embodiments, including any of the foregoing, the buffer layer comprises 10% by volume or less of an organic polymer.

[0453] In some embodiments, including any of the foregoing, the polymer is selected from polyacrylonitrile (PAN), polypropylene, polyethylene oxide (PEO), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyethylene oxide poly (allyl glycidyl ether) PEO-AGE, polyethylene oxide 2-methoxyethoxy) ethyl glycidyl ether (PEO-MEEGE), polyethylene oxide 2-methoxyethoxy) ethyl glycidyl poly (allyl glycidyl ether) (PEO-AGE-AGE), polyethylene oxide 2-methoxyethoxy) ethyl glycidyl ether (PEO-MEEGE-AGE), polyethylene oxide 2-methoxyethoxy) ethyl glycidyl poly (allyl glycidyl ether) (PEO-AGE ... E), polysiloxane, polyvinylidene fluoride (PVDF), ethylene α-olefin copolymer, polyvinylidene fluoride hexafluoropropylene (PVDF-HFP), ethylene propylene (EPR), nitrile rubber (NPR), styrene butadiene rubber (SBR), polybutadiene polymer, polybutadiene rubber (PB), polyisobutadiene rubber (PIB), polyisoprene rubber (PI), polychloroprene rubber (CR), acrylonitrile-butadiene rubber (NBR), polyethyl acrylate (PEA), polyvinylidene fluoride (PVDF) and polyethylene.

[0454] In some embodiments, including any of the foregoing, the active material is coated.

[0455] In some embodiments, including any of the foregoing, the active material is coated with a coating selected from the group consisting of lithium niobium oxide, lithium zirconium oxide, lithium aluminum oxide, lithium tantalum oxide, lithium hafnium oxide, niobium oxide, zirconium oxide, aluminum oxide, tantalum oxide, hafnium oxide.

[0456] In some embodiments, including any of the foregoing, the active material is uncoated.

[0457] In some embodiments, including any of the foregoing, the positive electrode comprises a lithium insertion material, a lithium conversion material, or both.

[0458] In some embodiments, including any of the foregoing, the embedded material is selected from nickel manganese cobalt oxide (NMC), nickel cobalt aluminum oxide (NCA), Li(NiCoAl)O2 , lithium cobalt oxide (LCO), lithium manganese cobalt oxide (LMCO), lithium nickel manganese cobalt oxide (LMNCO), lithium nickel manganese oxide (LNMO), Li(NiCoMn)O 2 、LiMn 2 O 4 、LiCoO 2 and LiMn 2-a NiO 4 , wherein a is 0 to 2, or LiMPO 4 , wherein M is Fe, Ni, Co or Mn.

[0459] In some embodiments, including any of the foregoing, the lithium conversion material is selected from FeF 2 、NiF 2 , FeOxF 3-2x , FeF 3 、MnF 3 , CoF 3 alloys or combinations thereof.

[0460] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte or the solid buffer conducting a single ion or both thereof are selected from LSS, SLOPS, LSTPS, LSTPSC1, SLOBS, LATS and LPS+X, wherein X is selected from Cl, I, Br and combinations thereof.

[0461] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte or the single-ion conducting solid buffer or both are selected from LPSI, LXPS, LSTPS, LSPSCl, LPSC1, LSPSBr and LPSBr.

[0462] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte or the solid buffer conducting a single ion or both thereof are selected from x·Li 2 S:y·SiS 2 , wherein x and y are each independently a value from 0 to 1, and x+y=1.

[0463] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte or the single-ion conducting solid buffer, or both, are selected from LSS, LGPS, LSTPS, and LSPS.

[0464] In some embodiments including any of the foregoing, the sulfide cathode electrolyte or the single ion conducting solid buffer or both are characterized by one of the following formulas: Li a Si b Sn c P d S e, where 2 ≤ a ≤ 8, 0 ≤ b ≤ 1, 0 ≤ c ≤ 1, 0.5 ≤ d ≤ 2.5, and 2 ≤ e ≤ 12; Li a Si b P c S d X e , where 8 < a < 12, 1 < b < 3, 1 < c < 3, 8 < d < 14, and 0 < e < 1, where X is F, Cl, Br, or I; Li g As h Sn j S k O l , where 2 ≤ g ≤ 6, 0 ≤ h ≤ 1, 0 ≤ j ≤ 1, 2 ≤ k ≤ 6, and 0 ≤ l ≤ 10; or Li m P n S p I q , where 2 ≤ m ≤ 6, 0 ≤ n ≤ 1, 0 ≤ p ≤ 1, 2 ≤ q ≤ 6; or a mixture of (Li 2 S):(P 2 S 5 ) and LiI in a molar ratio of about 10:1 to about 6:4, where [(Li 2 S):(P 2 S 5 ):LiI ratio is 95:5 to 50:50; LPS + X, where X is selected from Cl, I, or Br; vLi 2 S + wP 2 S 5 + yLiX; vLi 2 S + wSiS 2 + yLiX or vLi 2 S + wB 2 S 3 + yLiX. In these embodiments, the values of x, w, and y in each instance range from 0 to 1, inclusive of 0 and 1.

[0465] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte comprises LSTPS.

[0466] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte is characterized by the formula: Li a Si b Sn c P d S e , where 2 ≤ a ≤ 8, 0 ≤ b ≤ 1, 0 ≤ c ≤ 1, 0.5 ≤ d ≤ 2.5, 2 ≤ e ≤ 12.

[0467] In some embodiments, including any of the foregoing, the sulfide cathode electrolyte is characterized by the formula: Li aSi b Sn c P d S e , where 2≤a≤5, 0≤b≤0.5, 0≤c≤0.5, 0.5≤d≤2, 2≤e≤12.

[0468] In some embodiments, including any of the foregoing, the lithium-filled garnet layer comprises a selected from Li x La y Zr z O t ·qAl 2 O 3 of lithium-filled garnets, of which 4 <x<10、1<y<4、1<z<3、6<t<14、0≤q≤1。

[0469] Although specific advantages are listed above, various embodiments may include all, some, or none of the listed advantages. Other technical advantages will be apparent to those skilled in the art based on the following drawings and descriptions. Example

[0470] Unless otherwise stated, reagents, chemicals, and materials were purchased from commercial sources. Chemical reagents and solvents were purchased from commercial sources and used without purification unless otherwise stated. The soft-pack battery container was purchased from Showa Denko. The electrochemical potentiostat used was an Arbin potentiostat. Electrical impedance spectroscopy (EIS) was measured using a Biologic VMP3, VSP, VSP-300, SP-150, or SP-200. The rheometer was used for 100 s -1 Viscosity was measured at a shear rate of 1.5 %. Grinding was performed using a Retsch PM 400 planetary ball mill. Mixing was performed using a Fischer Scientific vortex mixer, a Flktek speed mixer, or a Primix filmix homogenizer. Casting was performed on a TQC casting table. Calendering was performed on an IMC calender. Light scattering was performed on a laser scattering particle size distribution analyzer model Horiba Partica LA-950V2.

[0471] Electron microscopy was performed in a FEI Quanta SEM, Helios 600i or Helios 660 FIB-SEM, which may also be replaced by equivalent tools. XRD was performed at room temperature in a Bruker D8 Advance ECO or Rigaku MiniFlex 2 with CuK-α radiation and a slit width of 6 mm with a scan time of 76 ms / step or 0.4 s / step. Optical imaging was performed with an optical camera. DC cycling was performed using an Arbin BT-2043 or BT-G, which may also be replaced by equivalent tools.

[0472] Example 1

[0473] Step (1): Prepare a solid positive electrode layer. Prepare a slurry with a solid loading of 30-80 wt% using 20-70% toluene. The solid loading comprises 70-95 wt% of lithiated lithium zirconium oxide (LZO) coated with a lithiated nickel cobalt aluminum oxide active material (NCA), 13 wt% of LSTPS and 2 wt% of a binder. The LSTPS composition is characterized by Li a Si b Sn c P d S e , wherein 2≤a≤8, 0≤b≤1, 0≤c≤1, 0.5≤d≤2.5 and 4≤e≤12, and it also contains greater than 0 to 15at% of oxygen element, and is prepared according to the preparation method described in U.S. Patent No. 9,172,114, entitled "SOLID STATE CATHOLYTES AND ELECTROLYTES FORENERGY STORAGE DEVICES", issued on October 27, 2015, the entire contents of which are incorporated by reference in this application for all purposes.

[0474] The slurry is cast on a carbon-coated aluminum foil using a doctor blade. The resulting cast slurry is dried at room temperature to 120° C. for 1-24 hours to form a positive electrode layer film on the carbon-coated aluminum foil. When the electrochemical cell is assembled in step (7), the carbon-coated aluminum foil acts as a current collector. After drying, the positive electrode layer is adhered to the current collector.

[0475] Step (2): Prepare a buffer layer in contact with the solid positive electrode layer. Prepare a slurry with 10-70wt% LSTPS in toluene. Use a doctor blade to cast the slurry on a nickel foil. Dry the resulting cast slurry at room temperature to 120°C for 1-24 hours to form a buffer layer film. In this example, the buffer layer includes LSTPS with the same chemical composition as used in the positive electrode layer. Without being bound by theory, this patent believes that this layer does not contain an electronic conductor. Therefore, the buffer layer prevents electrons from entering the borohydride bonding layer. In this way, the buffer layer shields the positive electrode layer potential from the bonding layer potential. The buffer layer can then protect the negative electrode (anode) potential from being affected by the positive electrode layer.

[0476] Step (3): After drying in step (2), the buffer layer film is peeled off from the nickel foil, i.e., the buffer layer film is removed. The buffer layer is then transferred and placed on top of the positive electrode layer prepared according to step (1) to form a stack (buffer layer-positive electrode layer-current collector).

[0477] Step (4): Apply a uniaxial pressure of about 300 MPa to the laminate formed in step (3) at low temperature (room temperature). Apply pressure to the laminate at high temperature (150-180°C).

[0478] Step (5): The lithium-filled garnet layer is made according to the method for forming a lithium-filled garnet layer or membrane in U.S. Patent No. 9,806,372B2, entitled “GARNET MATERIALS FOR LI SECONDARY BATTERIES AND METHODS OF MAKING AND USING GARNET MATERIALS” and U.S. Patent No. 9,970,711, entitled “LITHIUM STUFFED GARNET SETTER PLATES FOR SOLID ELECTROLYTE FABRICATION”, issued on May 15, 2018, the entire contents of which are incorporated by reference into this application for all purposes.

[0479] Step (6): Prepare a borohydride bonding layer. The borohydride composition for forming a borohydride bonding layer can be found in a patent application filed on October 20, 2017, with an international PCT patent application number of PCT / US2017 / 057735, entitled "ELECTROLYTE SEPARATORS INCLUDING LITHIUM BOROHYDRIDE AND COMPOSITEELECTROLYTE SEPARATORS OF LITHIUM-STUFFED GARNET AND LITHIUM BOROHYDRIDE", and a patent application filed on October 20, 2017, with an international PCT patent application number of PCT / US2017 / 057739, entitled "BOROHYDRIDE-SULFIDE INTERFACIAL LAYER IN ALL SOLID-STATE BATTERY", the entire contents of which are incorporated herein by reference for all purposes. The composition 3LiBH 4 2LiCl 3LiNH 2 Melt and spin-coat onto the lithium-filled garnet film prepared in step (5). The borohydride adhesion layer forms an intimate contact with both the lithium-filled garnet and the buffer layer in contact with the positive electrode layer.

[0480] Step (7): The lithium-filled garnet film with the LBHIN spin-coated layer is placed on top of the stack formed in step (4), wherein the LBHIN borohydride adhesion layer is in direct contact with the buffer layer. The stack is then compacted by applying a pressure of about 10,000 pounds per square inch (PSI) at a temperature that melts the LBHIN (250°C). The stack is then cooled to room temperature.

[0481] Step (8): A current collector is attached to the side of the lithium-filled garnet film without the LBHIN spin coating on the stack formed in step (7) to form an electrochemical cell. Prior to attaching the current collector, lithium metal is evaporated onto the lithium-filled garnet to form a lithium metal negative electrode. The electrochemical cell contains 30 μm of evaporated lithium.

[0482] Step (9): The stack obtained in step (8) is cycled to form a lithium metal anode between the adhered current collector and the lithium filled garnet film.

[0483] Example 2

[0484] An electrochemical cell was manufactured according to steps (1) to (8) of Example 1. The cell was subjected to an initial forming cycle at 45°C at a C / 10 rate and an electrochemical cycle at a C / 3 rate between 3.0 V and 4.2 V. The electrochemical cell was pressurized to 300 pounds per square inch (psi).

[0485] The results are as follows Figure 3-5 shown.

[0486] Figure 3 The results show that the electrochemical cell completed 50 cycles at 45 °C at a rate of C / 3 without significant capacity loss. Figure 3 The 1st and 50th cycles are shown.

[0487] Figure 4 The electrochemical cell was shown to complete 200 cycles and retain more than 80% of its energy in the 200th cycle. Coulombic efficiencies close to unity were observed (greater than 0.999 in most cycles). The first cycle efficiency was greater than 90%. It is necessary to compare these unexpected results with those in the paper by Kato et al. DOI: 10.1038 / NENERGY.2016.30, which reported on LiNbO 3 Coated LiCoO 2 Cathode active materials and sulfide solid electrolytes (Li 9.6 P 3 S 12 ,Li 10 G 2 S 12 ,Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 ) electrochemical cell. Figure 4 reported 90%, 61%, and 39% coulombic efficiencies, respectively. However, Kato et al. only tested low voltage (2.5V) electrochemical cells. It is foreseeable that these low voltage (2.5V) cells have high coulombic efficiencies. However, the 2.5V cell only showed 93% coulombic efficiency at the 1st cycle, and only 99% coulombic efficiency at the 10th and 100th cycles. Unlike Kato et al., Figure 4 As shown, after 10 cycles, the coulombic efficiency of the electrochemical cell prepared in the embodiment of the present patent application is about 100% (greater than 99.9%). If tested under the same conditions, it has a higher coulombic efficiency than the prior art, which indicates that the electrochemical stability at the sulfide-cathode interface is improved.

[0488] Figure 5Demonstrated electrochemical cell with approximately 54Ω-cm at 45°C 2 Both LSTPS and lithium-filled garnets may have high area specific resistance (ASR) (e.g., 1000 Ω-cm) at room temperature. 2 or higher). Therefore, unexpectedly, a single cell including LSTPS and lithium-filled garnet has a low ASR by simply pressing LSTPS and lithium-filled garnet together to form a heterointerface therebetween as in Example 1.

[0489] Figure 6 and Figure 7 Schematic diagram of the electrochemical cell under test. The electrochemical cell was prepared according to Example 1 and tested according to Example 2. Figure 6 The electrochemical cell shown includes: layer 701 representing an evaporated lithium metal anode; layer 702 representing a lithium filled garnet layer; layer 704 representing a buffer layer; and layer 705 representing a positive electrode layer.

[0490] like Figure 7 The electrochemical cell shown includes: layer 801 representing an evaporated lithium metal anode; layer 802 representing a lithium filled garnet layer; layer 803 representing a bonding layer; and layer 805 representing a positive electrode layer.

[0491] Example 3 - Fabrication of an electrochemical cell with a buffer layer

[0492] Step (1): Preparation of solid positive electrode layer (cathode layer, SSC). Prepare a slurry with a solid loading of 30-80 wt% in 20-70% toluene. The solid loading includes 70-95 wt% of lithium zirconium oxide (LZO) coated lithiated nickel cobalt aluminum oxide active material (NCA), 13 wt% of LSTPS and 2 wt% of binder. The LSTPS composition is characterized by Li a Si b Sn c P d S e , wherein a is 4, b is 0.5, c is 0.5, d is 1, and e is 8, and further comprises an oxygen element in an amount of greater than 0 to 15 at%, prepared according to the method described in U.S. Patent No. 9,172,114, entitled “SOLID STATE CATHOLYTES AND ELECTROLYTES FOR ENERGY STORAGE DEVICES”, issued on October 27, 2015, the entire contents of which are incorporated herein by reference for all purposes.

[0493] The slurry was cast on the carbon-coated aluminum foil using a doctor blade. The resulting cast slurry was dried at room temperature to 120° C. for 1 to 24 hours to form a positive electrode layer film on the carbon-coated aluminum foil.

[0494] Step (2): Prepare a sulfide layer that will be in contact with the solid positive electrode layer. Prepare a slurry with 10-70wt% LSTPS in toluene. Cast the slurry on a nickel foil using a doctor blade casting method. Dry the resulting cast slurry at room temperature to 120°C for 1-24 hours to form a buffer layer film. In this example, the buffer layer includes the same chemical composition LSTPS as in the positive electrode layer. Without being bound by theory, this patent believes that this layer does not conduct electrons (electronic conductivity is less than 1E-6S / cm). Therefore, the buffer layer can prevent the negative electrode (anode) potential from being affected by the positive electrode layer.

[0495] Step (3): The two layers of step (1) and step (2) are placed on top of each other so that the sulfide layer and the cathode layer are in direct contact with each other to produce a stack (nickel film-buffer layer-positive electrode layer-aluminum film).

[0496] Step (4): The stack from step (3) is placed on an aluminum guide foil. The film is passed through a calender at 140°C at a speed of 1.0 m / min and a hydraulic pressure of about 100-110 kg (10-11 MPa) (1100-1200 N / mm). The calender used is a Saueressig GK 300L or Ono Roll Type 12. After calendering, the sulfide layer is transferred to the cathode layer and the two layers are compacted together in one step. The result is as follows Figure 2 The carbon-coated aluminum foil is also bonded to the aluminum guide foil during the calendering process and forms the first current collector on the side of the SSC.

[0497] The stack of step (4) was incorporated into an electrochemical cell including a lithium-filled garnet separator for testing.

[0498] The lithium-filled garnet layer is made according to the method of forming a lithium-filled garnet layer or membrane in U.S. Patent No. 9,806,372B2, entitled “GARNET MATERIALS FOR LI SECONDARY BATTERIES AND METHODS OF MAKING and USING GARNET MATERIALS”, issued on October 31, 2017, and U.S. Patent No. 9,970,711, entitled “LITHIUM STUFFED GARNET SETTER PLATES FOR SOLID ELECTROLYTE FABRICATION”, issued on May 15, 2018, the entire contents of which are incorporated by reference into this application for all purposes.

[0499] Step (6): Place the lithium-filled garnet film on top of the stack prepared in step (4) so ​​that the lithium-filled garnet film is in direct contact with the buffer layer. Then apply a pressure of about 500 pounds per square inch (PSI) at a temperature of about 140° C. to compact the stack. Then cool the stack to room temperature.

[0500] Step (7): Evaporating lithium metal onto the lithium-filled garnet (evaporated lithium is 30 μm) to form a lithium metal negative electrode in the stack obtained in step (6), and adhering the battery stack to the negative electrode collector to form an electrochemical cell. In some cells, the negative electrode collector is directly attached to the lithium-filled garnet film, and the lithium of the positive electrode is plated between the lithium-filled garnet film and the negative electrode collector.

[0501] Example 4 - Fabrication of an electrochemical cell having a buffer layer and a borohydride layer

[0502] Step (1): Preparation of a solid positive electrode layer (cathode layer, SSC). A slurry with a solid loading of 30-80 wt% in 20-70% toluene was prepared. The solid loading included 70-95 wt% of a lithium zirconium oxide (LZO) coated lithiated nickel cobalt aluminum oxide active material (NCA), 13 wt% of LSTPS and 2 wt% of a binder. The LSTPS composition was characterized as Li a Si b Sn c P d S e, wherein a is 5, b is 0.75, c is 0.25, d is 1, and e is 6, and further comprises an oxygen element in an amount greater than 0 to 15 at%, prepared according to U.S. Patent No. 9,172,114, entitled “SOLID STATE CATHOLYTES AND ELECTROLYTES FOR ENERGY STORAGE DEVICES” and issued on October 27, 2015, the entire contents of which are incorporated herein by reference in their entirety for all purposes.

[0503] The slurry was cast on the carbon-coated aluminum foil using a doctor blade, and the resulting cast slurry was dried at room temperature to 120° C. for 1 to 24 hours to form a positive electrode layer thin film on the carbon-coated aluminum foil.

[0504] Step (2): Prepare a sulfide layer that is subsequently in contact with a solid positive electrode layer. Prepare a slurry with 10-70wt% LSTPS in toluene. Cast the slurry on a nickel foil using a doctor blade casting method. Dry the resulting cast slurry at room temperature to 120°C for 1-24 hours to form a buffer layer film. In this example, the buffer layer includes the same chemical composition component LSTPS as in the positive electrode layer. Without being bound by theory, this patent believes that this layer does not conduct electrons (electronic conductivity is less than 1E-6S / cm). As a result, the buffer layer shields the negative electrode (anode) potential, leaving the positive electrode layer unaffected.

[0505] Step (3): The two layers of step (1) and step (2) are placed on top of each other so that the sulfide layer and the cathode layer are in direct contact with each other to produce a stack (nickel film-buffer layer-positive electrode layer-aluminum film).

[0506] Step (4): The stack of step (3) is placed on an aluminum guide foil. The film is passed through a calender at 140°C at a speed of 1.0 m / min and a hydraulic pressure of about 100-110 kg (10-11 MPa) (1100-1200 N / mm). The calender used is a Saueressig GK 300L or Ono Roll Type 12. After calendering, the sulfide layer is transferred to the cathode layer and the two layers are compacted together in one step. The carbon-coated aluminum foil is also bonded to the aluminum guide foil during the calendering process and forms the first current collector on the side of the SSC.

[0507] The stack of step (4) was incorporated into an electrochemical cell including a lithium-filled garnet separator for testing.

[0508] Step (5): The lithium-filled garnet layer is made according to the method for forming a lithium-filled garnet layer or membrane in U.S. Patent No. 9,806,372B2, entitled “GARNET MATERIALS FOR LISECONDARY BATTERIES AND METHODS OF MAKING and USING GARNET MATERIALS”, issued on October 31, 2017, and U.S. Patent No. 9,970,711, entitled “LITHIUM STUFFED GARNET SETTERPLATES FOR SOLID ELECTROLYTE FABRICATION”, issued on May 15, 2018, the entire contents of which are incorporated by reference in this application for all purposes.

[0509] Step (6): Prepare a borohydride bonding layer. The borohydride composition used to form the borohydride bonding layer is prepared according to the patent application with an application date of October 20, 2017, an international PCT patent application number of PCT / US2017 / 057735, and a title of "ELECTROLYTE SEPARATORS INCLUDING LITHIUM BOROHYDRIDE AND COMPOSITEELECTROLYTE SEPARATORS OF LITHIUM-STUFFED GARNET AND LITHIUM BOROHYDRIDE"; and the patent application with an application date of October 20, 2017, an international PCT patent application number of PCT / US2017 / 057739, and a title of "BOROHYDRIDE-SULFIDE INTERFACIAL LAYER IN ALL SOLID-STATE BATTERY", all of which are incorporated herein by reference for various purposes. The composition 3LiBH 4 2LiCl 3LiNH 2 Melt and spin-coat onto the lithium-filled garnet film prepared in step (5).

[0510] Step (7): The lithium-filled garnet film having the LBHIN spin-coated layer thereon is placed on top of the stack produced in step (4) so ​​that the LBHIN borohydride adhesion layer is in direct contact with the buffer layer. The stack is then compacted by applying a pressure of about 1000 pounds per square inch (PSI) at a temperature of 140° C. The stack is then cooled to room temperature. Figure 3 A SEM FIB image of the resulting stack is shown.

[0511] Step (8): Evaporating lithium metal onto the lithium-filled garnet (evaporated lithium is 30 μm) to form a lithium metal negative electrode in the battery stack obtained in step (7), and adhering the battery stack to the negative electrode collector to form an electrochemical cell. In some cells, the negative electrode collector is directly attached to the lithium-filled garnet film, and the lithium of the positive electrode is plated between the lithium-filled garnet film and the negative electrode collector.

[0512] Example 5

[0513] 3 mol of LiBH 4 LBHI powder was prepared by mixing with 1 mol of LiI. The mixture was ground twice in a zirconia container at 300 rpm for 8 hours, then annealed in a sealed container at 300°C and cooled to room temperature to form annealed mixed LBHI powder.

[0514] Garnet film (roughly characterized by Li 7-x La 3 Zr 2 O 12 Al 2 O 3 The preparation of lithium-filled garnet is as follows. The garnet precursor is mixed with LiOH, ZrO in a molar ratio of 6-7:1.5:2:0.1-1.5. 2 ,La 2 O 3 , boehmite. The mixed precursor is ground in a ball mill and calcined at 700-1000°C for 1-10 hours to form a cubic garnet phase with a second phase. The powder is ground in a wet mill together with a solvent, a surfactant and a dispersant. A binder solution is prepared by dissolving a binder in the same solvent. The binder solution and the powder slurry are mixed and cast on a polyester film substrate with a doctor blade having a gap height of 10-300um to form a tape-shaped film to form a cast green tape. The green tape is peeled off from the substrate, cut into the desired size, sintered at a temperature of 800-1200°C for 1-10 hours, and cooled to form a sintered garnet film.

[0515] Under argon atmosphere, the mixed and annealed LBHI powder (1-4 g) was heated to 300-350°C in a boron nitride or alumina crucible, and the crucible was placed in a stainless steel heating kettle equipped with a belt heater and heated for about 2 hours until the LBHI powder melted. Under argon conditions at 300-350°C, the garnet film was immersed in the molten LBHI once for 600 seconds. The garnet film was then heated at 0.05-300 mm min -1 The LBHI-coated garnet is removed from the molten LBHI at a rate of 1000 rpm and cooled under argon for 5 seconds to 5 minutes to form LBHI-coated garnet.

[0516] Example 6

[0517] As shown in Example 5, LBHI was prepared and heated to 300-350°C. Then, a thin current collector copper foil was immersed in the molten LBHI at 300-350°C under argon conditions for 600 seconds. Then, the copper was heated at 0.05-300 mm min -1 The LBHI is taken out from the molten LBHI at a speed of 1000 rpm and cooled under argon for 5 seconds to 5 minutes to provide a LBHI-dip-coated copper foil.

[0518] Example 7

[0519] The ASR and service life of the LBHI-coated garnet prepared in Example 5 were tested as follows. The uncoated garnet and the LBHI-coated garnet were contacted with Li electrodes (contact area of ​​8 mm) on both sides and charged at 0.5 mA / cm2 at 80°C and 300 PSI. 2 The current density was applied twice a day (forward and reverse) for 30 seconds.

[0520] Example 8

[0521] The separator (the uncoated garnet membrane or the LBHI-coated garnet membrane prepared according to Example 6) was placed in a symmetrical electrochemical cell with Li-metal electrodes on both sides of the electrochemical cell sample. A hydrostatic pressure of 5000 PSI was applied unidirectionally to both sides of the cell under controlled temperature and argon gas at 80°C and 2 mA / cm 2 Under the conditions of 20 micrometers of lithium (about 4 mAh / cm 2 ) were cycled 5 times within the 8 mm electrode contact area. For samples that continued to cycle (non-short-circuited samples), the current was increased to 3 mAh / cm at 80 °C. 2 For samples that continued to cycle, the current was increased to 4 mAh / cm at 80 °C. 2 , and then at 80 ° C, the samples that can continue to cycle are increased to 5 mAh / cm 2 .

[0522] Example 9

[0523] By mixing 3 mol of LiBH 4 , 3 mol of LiNH 2 LBHClN was prepared by mixing with 1 mol of LiCl. The mixture was then ground twice in a zirconia container at 300 rpm for 8 h, and then annealed in a sealed container at 180° C. for 2 h and cooled to form LBHClN powder.

[0524] A lithium-filled garnet film was prepared according to the method of Example 5 and coated with lithium metal on one side. Then LBHClN powder was dropped on the other side of the lithium-filled garnet film. The lithium-filled garnet with LBHClN powder on it was then heated to 80-140° C. to melt the LBHClN powder.

[0525] Sulfide containing solid cathode membrane (SSC) is prepared. The SSC includes a sulfide cathode electrolyte, LSTPS and a cathode active material (NCA) with LSTPS, and the volume ratio of LSTPS:NCA is about 1 / 3 and 2 / 3. A small amount of carbon and binder of about 0-5wt% is added to LSTPS and NCA. The resulting mixture of LSTPS / NCA / carbon / binder is suspended in toluene at a mass loading of 20% powder in toluene. The suspension is then mixed with Flacktek and Filmix for 15 minutes and 6 minutes respectively. The mixture is then cast onto a carbon-coated aluminum foil and dried in an argon atmosphere until toluene evaporates. The membrane is punched to the desired size. The SSC membrane is compacted at 180°C and a pressure of 300,000PSI.

[0526] The SSC film was placed on top of the melted LBHClN powder. The SSC film was then pressed at a pressure of 10-2000 pounds per square inch (PSI) while cooling to room temperature. The single cell was cycled at 45°C at a rate of C / 10.

[0527] Example 10

[0528] LBHXN powder is prepared as described above, wherein X is Cl, Br or I or a mixture thereof. An adhesive layer of LBHXN film is deposited onto a lithium-filled garnet by spin casting. In this process, a small amount of LBHXN powder is added to the center of a lithium-filled garnet, which is placed on the chuck of a spin coater and heated to the LBHXN melting temperature (about 100-280°C). After reaching the melting temperature, the LBHXN melts. Using a flat spatula, the molten LBHXN is poured onto the substrate and covers the area. While the chuck is still at the temperature required to melt the LBHXN, the spin coater is turned on to a speed of 100 rpm to 5000 rpm. The spin coater is turned off after 1-10 minutes. After cooling to room temperature, a uniform coating of LBHXN is obtained on the substrate.

[0529] Embodiment 11

[0530] An organic non-aqueous, aprotic solvent is added to the mixture of LSTPS powder to form a slurry having a solid loading of at least about 35%. The slurry is then poured and coated onto a metal foil using a coater. The buffer layer is then placed in contact with the cathode material layer. The layers are compacted using at least about 1000 psi or more.

[0531] Example 12

[0532] The composition LiNH was prepared by dripping 2 :LiBH 4 :LiI (3:3:2) was coated on the solid cathode film. Specifically, LBHIN powder was prepared and cast on the compacted solid cathode. An uncoated lithium filled film (prepared according to Example 5) was pressed on the LBHIN layer at 20-2000 PSI and 20-350°C.

[0533] Embodiment 13

[0534] Solid state cathode layer (cathode layer, SSC) was prepared. A slurry with a solid loading of 30-80 wt% in 20-70% toluene was prepared. The solid loading included 70-95 wt% of lithium zirconium oxide (LZO) coated lithiated nickel cobalt aluminum oxide active material (NCA), 13 wt% of LSTPS and 2 wt% of binder. The LSTPS composition was characterized as Li a Si b Sn c P d S e , wherein a is 5, b is 0.75, c is 0.25, d is 1, and e is 6, and further comprises an oxygen element in an amount of greater than 0 to 15 at%, prepared according to the method described in U.S. Patent No. 9,172,114, entitled “SOLID STATE CATHOLYTES AND ELECTROLYTES FOR ENERGY STORAGE DEVICES”, issued on October 27, 2015, the entire contents of which are incorporated herein by reference for all purposes.

[0535] Lithium metal was added to one side of the lithium-filled garnet film prepared in Example 5.

[0536] LPSI is cast onto the lithium-filled garnet film on the side opposite to the side with lithium metal.

[0537] The thickness of the lithium-filled garnet film is about 100 μm. The thickness of the cathode is about 150 μm. The thickness of the LPSI is about 10 μm.

[0538] The obtained electrochemical cell was cycled at a rate of C / 10 at 45°C and 30 psi. Fig. 9 shown.

[0539] The above embodiments and examples are illustrative and non-restrictive only. Those skilled in the art will recognize or determine many equivalent specific compounds, materials and procedures using only routine experiments. All these equivalent forms are considered to be within the scope of the appended claims.

Claims

1. A solid-state electrochemical cell (SSEC), include: (a) a positive electrode layer comprising an active material and a sulfide cathode electrolyte; (b) solid buffers that conduct a single ion; (c) a borohydride bonding layer; and (d) Lithium-filled garnet layer; in, The buffer is mixed in the positive electrode layer, the buffer is a layer in contact with the positive electrode layer, or the buffer is mixed in the positive electrode layer, the buffer is a layer in contact with the positive electrode layer; The borohydride bonding layer is between and in contact with the lithium-filled garnet layer and (i) the positive electrode layer in which a buffer is mixed or (ii) a buffer layer in contact with the positive electrode.

2. The SSEC according to claim 1, in, The single ion conducting solid buffer is mixed in the positive electrode layer.

3. The SSEC according to claim 1 or 2, in, The single ion conducting solid buffer is a layer in contact with the positive electrode layer.

4. The SSEC according to any one of claims 1 to 3, in, The buffer is mixed in the positive electrode layer, and the buffer is a layer in contact with the positive electrode layer.

5. The SSEC according to any one of claims 1 to 4, in, The single ion conducting solid buffer layer prevents the borohydride bonding layer from directly contacting the positive electrode layer.

6. The SSEC according to any one of claims 1 to 5, further comprising a negative electrode. The SSEC according to claim 6 , wherein the anode is a lithium (Li) metal anode.

8. The SSEC according to any one of claims 6-7, wherein the lithium filled garnet layer contacts the negative electrode.

9. The SSEC according to any one of claims 1 to 8, wherein the buffer layer comprises an organic polymer in an amount of 10% by volume or less.

10. The SSEC according to any one of claims 1 to 9, wherein the active material is coated.

Citation Information

Patent Citations

  • Garnet materials for li secondary batteries and methods of making and using garnet materials

    US20150099190A1

  • Garnet materials for li secondary batteries and methods of making and using garnet materials

    US20150200420A1

  • Implantable pulse generator that generates spinal cord stimulation signals for a human body

    US20160015982A1

  • Array substrate, method for fabricating the same and display device

    US20160027886A1

  • Semiconductor Device, Power Circuit, And Manufacturing Method Of Semiconductor Device

    US20160027922A1

Cited By

  • Metal tungsten interface modification layer, preparation method and solid-state battery

    CN122455953A