Multilayer sintered porous body

By adopting a multi-layer sintered inorganic film and using a combined structure of coarse and fine nanoparticles, the stability problem of supercritical fluid filtration under high temperature and high pressure is solved, and effective filtration of nanoscale impurities and improved equipment durability.

CN119095665APending Publication Date: 2024-12-06ENTEGRIS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036817.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-29
Filing Date
2023-04-28
Publication Date
2024-12-06

Smart Images

  • Figure CN119095665A_ABST
    Figure CN119095665A_ABST
Patent Text Reader

Abstract

The present disclosure describes porous sintered inorganic bodies comprising a plurality of layers made of different types of metal particles, which can be used as filter membranes, and methods of making and using the porous sintered inorganic bodies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to porous sintered inorganic bodies comprising multiple layers made of different metal particles, useful as filter membranes, and also to methods of making and using the porous sintered inorganic bodies. Background Art

[0002] Porous sintered bodies are used in a variety of industrial applications, including applications where the porous sintered bodies are used as filter membranes to remove contaminants from fluids used in manufacturing. Many manufacturing processes require extremely pure fluids as raw materials or process fluids. For example, many different stages of semiconductor and microelectronic device manufacturing require the use of high-purity gases or liquids as raw materials, and the use of high-purity process fluids for steps such as cleaning, etching, drying, and other surface or material preparation steps. To provide high-purity fluids during manufacturing, inorganic porous films are often used as filter elements to remove contaminants from the fluid just before the fluid is used.

[0003] Fluid can be in the form of gas, liquid or supercritical fluid. Supercritical carbon dioxide has multiple uses in industry, including for cleaning, drying and for solvent extraction applications. High-purity, supercritical carbon dioxide can be used for electronic devices and semiconductor manufacturing industries that require extremely high cleanliness and material purity. In one such application, supercritical carbon dioxide can be used to remove photoresist materials and wafer drying from the surface of semiconductor wafers. Typically, the supply of supercritical carbon dioxide is filtered to remove particles in the size range of 10 nanometers or 20 nanometers or less before use to remove particulate impurities in low nanometer scales, for example.

[0004] Carbon dioxide (CO 2 ) exists as a supercritical fluid at temperatures and pressures above its critical temperature (31.10°C, 87.98°F, 304.25K) and critical pressure (7.39 MPa, 72.9 atm, 1,071 psi, 73.9 bar). Typical operating conditions for the process of filtering supercritical carbon dioxide include temperatures exceeding 70, 90 or 100 degrees Celsius and pressures exceeding 25, 30, 35 or 40 megapascals (MPa).

[0005] The equipment for handling supercritical carbon dioxide must work under the temperature and pressure required to maintain carbon dioxide in the supercritical state. These conditions are significantly more harsh than the conditions for filtering many other types of industrial raw materials or process fluids. Many filtering steps of other fluids occur at ambient temperature or at a temperature that is only slightly elevated and at a pressure that is approximately atmospheric pressure, slightly higher than atmospheric pressure or far below atmospheric pressure. Developing new, useful and improved methods and equipment for filtering supercritical fluids (such as supercritical carbon dioxide) can be particularly challenging because equipment and components (such as filter membranes) must be stable and durable in an effective operating life at relatively high pressures and temperatures. Summary of the invention

[0006] The following description relates to novel and inventive porous sintered bodies, filter membranes, methods of making porous sintered bodies, and methods of using porous sintered bodies as filter membranes.

[0007] A porous sintered membrane comprises (at least) two layers made of sintered inorganic particles: a first layer, which is mainly or completely derived from a combination of coarse particles and fine particles; and a second layer, which is mainly or completely derived from a combination of fine particles and nanoparticles. The first layer essentially serves as a structural base supporting the multilayer membrane and exhibits high flow properties and sufficient strength and structure to support the second layer. The second layer serves as a filtration layer and a reinforcement layer. The second layer contains fine particles and nanoparticles, which in combination form a second layer that is effective for filtration applications while also contributing to the overall strength of the multilayer membrane.

[0008] The porous sintered body described can be effectively used as a filter membrane for filtering a variety of different fluids in a wide temperature and pressure range. The fluid can be a gas, a liquid or a fluid in a supercritical state. The pressure can be ambient pressure, an increased pressure or a reduced pressure. And the temperature can be ambient temperature, an increased temperature or a reduced temperature. As a specific example, some currently preferred porous sintered bodies can be used as a filter membrane for filtering fluids under relatively high temperature and pressure conditions, as a method for filtering supercritical fluids (such as supercritical carbon dioxide).

[0009] In one aspect, the present disclosure relates to a porous film. The film comprises a first layer, the first layer containing a combination of sintered inorganic particles including coarse particles having a particle size of at least 10 microns and a coarse particle sintering point and first fine particles having a particle size of at least 1 micron and a first fine particle sintering point lower than the coarse particle sintering point. The film also comprises a second layer, the second layer containing a combination of sintered inorganic particles including second fine particles having a particle size of at least 1 micron and a second fine particle sintering point lower than the coarse particle sintering point and nanoparticles having a particle size of less than 1 micron and a nanoparticle sintering point higher than the first fine particle sintering point and higher than the second fine particle sintering point.

[0010] In another aspect, the present disclosure relates to a method for forming a porous film. The method comprises: preparing a precursor comprising a first blend of inorganic particles, the first blend comprising: coarse particles having a particle size of at least 10 microns and a coarse particle sintering point; and first fine particles having a particle size of at least 1 micron and a first fine particle sintering point lower than the coarse particle sintering point; applying a second blend of inorganic particles to the surface of the precursor, the second blend comprising second fine particles having a particle size of at least 1 micron and a second fine particle sintering point lower than the coarse particle sintering point, and nanoparticles having a particle size of less than 1 micron and a nanoparticle sintering point higher than the first fine particle sintering point and higher than the second fine particle sintering point.

[0011] In another aspect, the present disclosure relates to a tubular porous film. The film comprises: coarse particles having a particle size of at least 10 microns; fine particles having a particle size of at least 1 micron; and nanoparticles having a particle size of less than 1 micron. The film has: a bubble point of at least 30 pounds per square inch measured by ASTM E 128-99 (2019) using 60 / 40 isopropyl alcohol (IPA) / water; an air flux value of at least 0.07 slpm / cm2 at 30 psi; and a radial crush test value of at least 35 thousand pounds per square inch measured using ASTM B939-21. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 is a schematic diagram of a cross-sectional view of the described example porous metal body. This schematic diagram is illustrative and not necessarily drawn to scale.

[0013] Figure 2 is a photomicrograph of the example porous metal body described.

[0014] Figure 3 An example of the described filter assembly is shown that includes a filter housing and a multi-layer porous sintered body. DETAILED DESCRIPTION

[0015] Described below are novel porous sintered inorganic bodies (eg, "porous bodies," "porous sintered bodies," or sometimes simply referred to herein as "membranes" or "bodies") that can be used as filter membranes for filtering fluid streams to remove small-scale (eg, nanoscale) impurities from the fluid.

[0016] The porous sintered body described is in the form of a porous inorganic body containing two layers, each layer being made to contain sintered inorganic particles. The first layer is mainly or completely derived from a combination of coarse particles and fine particles. The second layer is mainly or completely derived from a combination of fine particles and nanoparticles. Each layer is made of a matrix containing the described inorganic particles that have become interconnected at the surface of the particles by a sintering step.

[0017] The first layer basically serves as a structural base for supporting the multilayer film, and exhibits high flow properties and sufficient strength and structure to support the second layer. The second layer serves as a filter layer and a reinforcement layer. To provide both strength and filtering functions, the second layer contains two types of particles, i.e., fine particles and nanoparticles, that are combined to form a second layer that performs filtering functionality and also increases the strength of the multilayer film. The fine particles in the second layer provide a porous structure in which nanoparticles are contained and supported. The fine particles of the second layer provide structure and strength. Nanoparticles provide a filtering effect by providing a matrix that defines very small holes that can remove small-scale contaminants (such as nanoscale contaminants) from the fluid passing through the second layer.

[0018] A porous sintered body is a porous inorganic structure that comprises (e.g., includes, consists of, or consists essentially of) inorganic (e.g., metal, ceramic) particles that are derived from and are therefore referred to as "comprising" particles that have been connected together (e.g., "interconnected") at their surfaces by a step of sintering the particles. The particles are fused or bonded together at contacting surfaces to form an interconnected matrix by a step of sintering a precursor containing different types of inorganic particles under unsintered, optionally compressed conditions.

[0019] The term "sintering" as used herein has a meaning consistent with the meaning given to this term when used in the art of porous sintered structures, such as porous sintered inorganic thin films of the type that can be used as metal filters. Consistent with this, the term "sintering" can be used to refer to the process of bonding (e.g., "welding" or "fusing") together a collection of one or more small inorganic particles of different types (size, composition, shape, etc.) by applying heat to a non-sintered body (e.g., "precursor") containing the particles so that the particles reach a temperature that causes the particles to become fused together (i.e., welded together) by material bonds between the surfaces of adjacent particles, but does not cause the particles to melt (i.e., the particles do not reach a melting temperature or become a flowable liquid).

[0020] As used herein, the "sintering point" or "sintering temperature" of a collection of inorganic particles is the temperature at which the particles are able to be sintered (i.e., the temperature at which particles within a collection of particles having surfaces in contact with each other are able to fuse together without melting under a particular pressure (e.g., atmospheric pressure). The sintering point of inorganic particles is generally below the melting temperature of the particles, meaning the temperature at which the material of the particles becomes liquid. The sintering point of a collection of particles depends on factors including the chemical composition of the particles and the size and shape of the particles; smaller particles made of an inorganic material may have a lower sintering point than larger particles made of the same inorganic material.

[0021] The porous sintered bodies described may be in the form of porous, sintered inorganic multilayer films. Different layers of the multilayer film contain different types of inorganic particles that operate differently in providing strength and filtering properties to the sintered film. The inner or "first" layer may be used to provide significant strength to the sintered film and to provide strength to the unsintered (green) form used to prepare the sintered porous film; the first layer need not exhibit filtering properties for small-scale particles (via a screening mechanism) and may have pores of a size that allow a relatively high level of fluid flow through the first layer compared to a lower level of fluid flow through the second layer.

[0022] The outer or "second" layer may add an additional amount of strength to the porous sintered membrane and also contain pores formed by the sintered nanoparticles to act as, for example, a mesh-type filter layer.

[0023] Different layers contain at least three different types of inorganic particles, referred to as "coarse" particles, "fine" particles, and "nanoparticles", which may have different sizes, different compositions, different sintering points, or a combination of these. Examples of inorganic particles of any different types of particles that may be used as the first or second layer of the sintered film include inorganic particles that may be metals or ceramics. The metal particles may contain one or more metals (including one or more metals, consisting of or consisting essentially of one or more metals), whether as pure metals or as alloys. Example metals include iron, refractory metals (such as tungsten, molybdenum, tantalum), titanium, and nickel. Examples of metal alloys include stainless steel, another iron or steel alloy, a nickel alloy, a titanium alloy, and the like. Example ceramics include metal oxides, such as zirconium oxide (ZrO 2 ), aluminum oxide (Al 2 O 3 ) etc. According to a specific example film, the fine particles may be made of the same material as the coarse particles, for example, the fine particles of the film are made of a metal or a metal alloy (such as stainless steel, nickel or a nickel alloy), and the coarse particles of the same film are made of the same metal or metal alloy.

[0024] Particles referred to as "coarse" particles may be included in and may constitute a major portion of the first film layer. Coarse particles provide strength to the first layer and the sintered multilayer film, and may produce a first layer with relatively large pores that allow relatively high fluid flow through the first layer, but do not perform a screen-type filtering function with respect to small-scale (e.g., nanoscale) contaminants.

[0025] The coarse particles start out as a raw material in powder form, meaning a collection of small (micrometer-scale) particles that are generally of similar composition and size range. The coarse particles used to make the first layer can have a shape and size that allows the coarse particles to be useful in forming the described first layer based on the described method, which shape and size will be effective for the particles to form the first layer of the porous sintered body after sintering.

[0026] Example coarse particles can have a particle size in the range of tens of microns (e.g., from 10 to 200 microns, from 10 to 150 microns, from 10 to 100 microns, from 25 to 200 microns, from 25 to 150 microns, from 25 to 100 microns, from 25 to 75 microns, from 50 to 200 microns, from 50 to 150 microns, or any range or sub-range therebetween). The particle size of metal and ceramic particles can be measured by ASTM B822-17 (Standard Test Method for Particle Size Distribution of Metal Powders and Related Compounds by Light Scattering).

[0027] The coarse particles may comprise a shape or surface that may be regular (e.g., uniform within a powder) or irregular (e.g., a shape that is round or spherical, spherical, branched, etc.). Examples of useful coarse particles may be generally round, non-high aspect ratio particles in the multi-micrometer size range. The particles are typically round, non-dendritic, and do not exhibit a high aspect ratio, for example, exhibiting an aspect ratio that is less than 10, less than 5, or less than 4 or 3 on average.

[0028] Example coarse particles for forming the first layer may be made substantially or entirely of (may include, consist of or consist substantially of) ceramics, metals or metal alloys, such as refractory metals, stainless steel, nickel, nickel alloys, and may contain, for example, at least 90 wt%, 95 wt%, 98 wt% or 99 wt% of ceramics, metals (pure metals) or metal alloys, such as stainless steel, nickel or nickel alloys. Coarse particles containing a large amount of stainless steel may have a sintering point in the range of from 900 degrees Celsius to 1200 degrees Celsius. Coarse particles containing a large amount of nickel or nickel alloys may have a sintering point in the range of from 1000 degrees Celsius to 1300 degrees Celsius. Coarse particles containing a large amount of ceramics or refractory metals (e.g., at least 90 wt%, 95 wt%, 98 wt% or 99 wt% of ceramics or refractory metals) may have a sintering point greater than 1300 degrees Celsius or 1400 degrees Celsius.

[0029] As used herein, a material or combination of materials that is referred to as "consisting essentially of" a material or combination of materials will contain the material or combination of materials and no more than minute amounts of other materials, e.g., no more than 1 weight percent, 0.5 weight percent, or 0.1 weight percent of any other ingredient; for example, a coarse particle consisting essentially of nickel will be made of nickel and no more than 1 weight percent, 0.5 weight percent, or 0.1 weight percent of any other ingredient.

[0030] Particles referred to as "fine" particles may be included in or may constitute a major portion of the first layer and a major portion of the second layer. Fine particles are smaller than coarse particles and larger than nanoparticles, for example, may have a particle size greater than 1 micron but less than 10 microns. Fine particles can be used to provide strength, continuity and integrity to the multilayer sintered film by being present in both the first layer and the second layer, thereby providing a continuous sintered network that creates continuity and strength between the two layers.

[0031] In certain example films, the fine particles may have the same chemical composition as the coarse particles to facilitate sintering of coarse and fine particles of different sizes in the first layer. The sintering point of the fine particles may be at a temperature lower than the sintering point of the coarse particles and lower than the sintering point of the nanoparticles. In certain example films, the fine particles may have a different chemical composition than the chemical composition of the nanoparticles to allow the fine particles to have a sintering point lower than the sintering point of the nanoparticles.

[0032] The fine particles contained in the first layer ("first fine particles") may be the same or different from the fine particles of the second layer ("second fine particles") in terms of particle size and particle composition. In the example film, the first fine particles may have the same chemical composition and the same size and shape (average size, size distribution, shape and morphology (e.g., dendritic)) as the second fine particles.

[0033] The example fine particles (first fine particles and second fine particles) may be in the form of a powder containing a collection of particles made of (may include, consist of, or consist essentially of) ceramics, metals (e.g., refractory metals, nickel) or metal alloys (e.g., stainless steel) or nickel alloys, for example, may contain at least 90%, 95%, 98%, or 99% by weight of ceramics, refractory metals, stainless steel, nickel, or nickel alloys. Fine particles containing a large amount of stainless steel may have a sintering point in the range of 900 to 1200 degrees Celsius, wherein the fine particles contained in any particular sintered film have a sintering point lower than the sintering point of the coarse particles in the film. Fine particles containing a large amount of nickel or nickel alloys may have a sintering point in the range of 600 to 1100 degrees Celsius, wherein the fine particles used in a particular sintered film have a sintering point lower than the sintering point of the coarse particles in the film. Fine particles containing a large amount of ceramic or refractory metal (e.g., at least 90%, 95%, 98%, or 99% by weight ceramic or refractory metal) can have a sintering point greater than 1300 degrees Celsius or 1400 degrees Celsius.

[0034] The fine particles may be formed to have a shape or surface that may be regular (e.g., uniform within a powder) or irregular, such as round or spherical, spherical, branched, elongated, dendritic, etc. In a particular example, the first fine particles and the second fine particles may be of a type sometimes referred to as highly anisotropic dendritic particles, such as described in U.S. Pat. No. 5,814,272 ("the '272 patent"), the entire contents of which are incorporated herein by reference.

[0035] According to the '272 patent, and as used herein, the term "dendritic" refers to a highly anisotropic, irregular particle morphology in which the particle has a structure comprising one or, typically, a plurality of filaments or branches, each filament or branch individually having one dimension (one of the three dimensions) greater than the other two dimensions of the filament. One or more branches or filaments may independently be straight or curved, and may be branched or unbranched. Dendritic particles are characterized by low packing efficiency compared to particles of more regular morphology, and therefore, form powders having lower apparent density than powders formed from particles fabricated to have the same chemical composition but with a more regular (non-dendritic) morphology. Under magnification, dendritic particles may appear as aggregates or agglomerates of non-dendritic starting particles. See FIG6 of the '272 patent.

[0036] Dendritic powders can effectively form self-supporting precursors (eg, in green form, see below) and sintered bodies of relatively lower density and higher porosity than precursors and sintered bodies made from comparable non-dendritic powders.

[0037] Dendritic particles can be formed by fusing together non-dendritic particles or partially dendritic particles that are part of the collection of particles in the powder. In short, a powder of dendritic particles can be formed by the method described in the '272 patent. Thus, a powder of dendritic particles can be formed from a powder of substantially non-dendritic particles by heating the non-dendritic powder under conditions suitable for initial stage sintering to form a lightly sintered material. The lightly sintered material can then be treated to break up some of the sintered and bonded particles to form dendritic particles. These steps can be repeated if necessary.

[0038] The term "lightly sintered material" refers to a material defined by Randall as being produced by fusion of metal powder particles through an initial stage of sintering (Randall, Powder Metallurgy Science, 2nd ed., German edition, Metal Powder Industry Association (1994), the contents of which are incorporated herein by reference). In the initial stage of sintering, or short-distance diffusion sintering, bonds are formed between particles at the contact surfaces of the particles, resulting in the fusion of metal powder particles only with their directly adjacent particles. Therefore, the initial stage of sintering produces a brittle structure with low mechanical strength. For a given material, sintering proceeds slowly beyond this initial stage at temperatures at the lower end of the sintering range of the material. For the purposes of this description, the term "initial stage sintering" refers to sintering a powder under conditions where sintering does not substantially proceed beyond the initial stage.

[0039] The term "substantially non-dendritic particles" refers to particles (e.g., in powder form or as part of a green or sintered film) that contain a majority or all (e.g., at least 80%, 90%, or 95% by weight) of particles having a non-dendritic morphology.

[0040] Particles referred to as "nanoparticles" may be included in and constitute a major portion of the second layer to produce a second layer having pores small enough to remove very small scale (nanoscale) contaminants from the fluid through a sieving filtration mechanism. Nanoparticles are much smaller than coarse particles and smaller than fine particles, for example, nanoparticles may have a submicron particle size (e.g., less than 1.0 or 0.9 microns, such as in the range of from 0.001 to 0.5 microns).

[0041] In certain example films, the nanoparticles may have a chemical composition that is different from the chemical composition of the coarse particles and also different from the chemical composition of the fine particles. The nanoparticles may also have a sintering point that is higher than the sintering point of the fine particles (both the first fine particles and the second fine particles). The sintering point of the nanoparticles may be higher than the sintering point of the coarse particles, lower than the sintering point of the coarse particles, or approximately the same as the sintering point of the coarse particles.

[0042] The use of nanoscale inorganic particles in the second layer of the sintered film can produce a sintered film that can exhibit pore sizes (e.g., indicated by a bubble point) in the nanometer range (e.g., less than 50, 20, or 10 nanometers). For nanoscale pore sizes, the sintered film can effectively remove nanoscale particle contaminants from a fluid through a sieving mechanism, through a filter having pores smaller than the size of the contaminant.

[0043] Example nanoparticles of sintered films or precursors may be substantially or completely made of stainless steel, titanium or titanium alloys, refractory metals, ceramics such as zirconium oxide (ZrO 2 ) or aluminum oxide (Al 2 O3 )) (may include stainless steel, titanium or titanium alloy, refractory metal, ceramic, consisting of or consisting essentially of stainless steel, titanium or titanium alloy, refractory metal, ceramic), for example, may contain at least 90 weight %, 95 weight %, 98 weight % or 99 weight % of stainless steel, titanium, titanium alloy or ceramic. Nanoparticles containing a large amount of stainless steel may have a sintering point in the range of from 800 degrees Celsius to 1100 degrees Celsius, wherein the nanoparticles used in any particular sintered film have a sintering point greater than the sintering point of the first fine particles and the second fine particles of the sintered film. Nanoparticles containing a large amount of titanium, titanium alloy or ceramic may have a sintering point in the range of from 1000 degrees Celsius to 1400 degrees Celsius, wherein the nanoparticles used in a particular sintered film have a sintering point higher than the sintering point of the first fine particles and the second fine particles in the sintered film. Nanoparticles containing a substantial amount of ceramic or refractory metal (eg, at least 90%, 95%, 98%, or 99% by weight ceramic or refractory metal) can have a sintering point greater than 1300 or 1400 degrees Celsius.

[0044] The shape of the nanoparticles may include shapes or surfaces that may be regular (eg, uniform within a powder) or irregular, such as round or spherical, globular, branched, etc. and may be non-dendritic.

[0045] The sintered film contains three different types of particles (coarse particles, fine particles, nanoparticles), comprising two visually distinct but physically interconnected layers, which when present together in a multilayer film, provide a film with very fine pore size for filtering very fine particles, while also having high strength. The different sizes, chemical compositions and sintering points of the coarse particles, fine particles and nanoparticles are selected to produce the desired combination of filtering effect, strength properties and handling (sintering) properties.

[0046] The first film layer comprises fine particles (first fine particles) and coarse particles, wherein the chemical composition of the fine particles and the coarse particles is preferably similar or identical. Selecting fine particles and coarse particles with similar or identical chemical composition can improve the ability of particles to become bonded by sintering. The fine particles (first fine particles) of the first layer can also have a chemical composition similar or identical to the fine particles of the second layer to provide strength and physical continuity between the first layer and the second layer. In the example film, the first layer does not need nanoparticles and preferably does not contain nanoparticles, for example, contains less than 1 weight %, 0.5 weight % or 0.1 weight % of nanoparticles.

[0047] The second layer comprises second fine particles combined with smaller "nanoparticles" without any coarse particles. The second fine particles may have a chemical composition similar to or identical to the first fine particles to provide strength and continuity between the first and second layers. Nanoparticles may have different chemical compositions (chemical ingredients) compared to the first fine particles, compared to the second fine particles, and compared to the coarse particles.

[0048] The fine particles and nanoparticles of the second layer provide a combination of useful functions for the second layer. When sintered, the nanoparticles define a desired small pore size for filtering nanoscale particles through a sieving filter mechanism. The fine particles, especially if these are the same (size, chemical composition) as the fine particles of the first layer, provide the desired handling, strength and stability properties because the fine particles of both the first and second layers will undergo similar levels of sintering, which can result in a physical connection between the first and second film layers.

[0049] Nanoparticles also have a higher sintering point than the first fine particles and the second fine particles, and may optionally have a sintering point higher than the sintering point of the coarse particles. During processing (sintering), the nanoscale particles may only undergo an initial stage of sintering, while other particles will sinter more fully. It is desirable that the nanoparticles do not undergo any melting during sintering. Melting or over-sintering may cause cracking or distortion of the second film layer, poor flow through the sintered film, and a reduced bubble point.

[0050] Selecting nanoparticles having a higher sintering point than the first and second fine particles, and optionally a higher sintering point than the coarse particles, can result in a desired relatively lower sintering degree of the nanoparticles compared to the higher sintering degrees of the fine and coarse particles. The lower sintering degree of the nanoparticles allows for increased control over the filtration and flow properties of the sintered membrane, such as increased control over fluid flow as measured by pressure drop and pore size as measured by bubble point. Adjusting the relative amounts of nanoparticles in the second layer of the membrane and the entire multilayer membrane can be used to achieve desired flow properties, pore size (for filtration), bubble point, etc.

[0051] Different layers may contain a range of useful amounts of different types of particles. The first layer may contain effective relative amounts of coarse particles and fine particles. In certain examples, the first layer may include, consist of, or consist essentially of 50% to 70% by weight coarse particles and 30% to 50% by weight fine metal particles.

[0052] The second layer may include any effective relative amounts of fine particles and nanoparticles. In certain examples, the second layer may include (including, consisting of, or substantially consisting of) 40 wt % to 75 wt % fine particles and 25 wt % to 60 wt % nanoparticles.

[0053] The sintered film may contain any useful relative amounts of the first layer and the second layer. In certain examples, the sintered film may comprise (comprising, consisting of, or consisting essentially of) 50 wt % to 75 wt % of the first layer and 25 wt % to 50 wt % of the second layer, based on the total weight of the sintered film.

[0054] The total film thickness and the relative thickness of the first and second layers of the film can be selected as desired. The first layer can have a thickness that will provide support for the second layer without unduly restricting fluid flow through the body. The second layer can have a thickness that provides the desired filtration efficiency and can also contribute to the overall strength of the film, especially a tubular film.

[0055] The overall thickness of the porous sintered body used as a filter membrane can be relatively thin, for example having a relatively small thickness in magnitude. A relatively thinner filter membrane can result in certain desirable properties of the filter membrane, including reduced mass and reduced pressure drop across the filter during use. Examples of useful or preferred porous sintered membranes suitable for use as filter membranes (e.g., in tubular form and useful for filtering supercritical fluids) can have a thickness of less than 1.5 or 2 mm (e.g., less than 1, 0.9 or 0.8 mm, for example, in the range of from 0.4 to 1 mm).

[0056] In an example porous sintered film, the first (coarse) layer may be thicker or thinner than the second layer. According to certain examples, the described film may have a first (coarse) layer thickness of at least 50% of the total thickness of the body, such as at least 55%, 60%, 70%, or 80% of the total thickness of the body. The second layer may have a thickness of up to (i.e., not more than) 50% of the total thickness of the body, such as up to 20%, 30%, 40%, 45%, or 50% of the total thickness of the body.

[0057] The porous sintered film contains a first layer, a second layer, and may also contain but not require other layers or materials. According to some examples, the porous sintered body can be made to consist of only or substantially only the first and second layers. The porous sintered body "substantially consisting of" the first and second layers contains these two layers and no more than a minute amount of any other layer or material, such as no more than 1 weight %, 0.5 weight % or 0.1 weight % of any other layer or material.

[0058] The described porous sintered membrane and its precursors include two (or more) identifiable parts or "layers" made of different types of particles. Without limiting the functions of the different layers, the "first" layer is sometimes referred to as a "coarse layer" or "support layer" in this article, and the "second" layer is sometimes referred to as a "fine layer" or "filtration layer". The first layer is made of and includes a combination or "blend" of coarse particles and first fine particles, without nanoparticles or substantially free of nanoparticles. The second layer is made of and includes a combination or "blend" of second fine particles and nanoparticles, without coarse particles or substantially free of coarse particles.

[0059] The two different layers can be visually inspected using magnification. In the form of a sintered film, the first layer comprising coarse particles and fine particles will be seen as containing a combination of coarse particles bonded together at the particle surface by the sintering step, with the fine particles bonded to the coarse particles and other fine particles. The first layer will have a relatively high porosity compared to the second layer and will not contain a large amount of nanoparticles.

[0060] The second layer of the sintered film comprising the second fine particles and nanoparticles will be considered to contain a combination of fine particles and nanoparticles bonded together at the particle surfaces by the sintering step. Compared to the first layer, the second layer will have a relatively low porosity and will not contain a large amount of coarse particles.

[0061] Figure 1 A side cross-sectional view of a portion of the described porous sintered film is schematically shown. The film 10 includes a first layer 20 made primarily or entirely of coarse particles 22 and first fine particles 24. The film 10 also includes a second layer 30 made primarily or entirely of second fine particles 26 and nanoparticles 28. The particles, when formed into the porous sintered film 10, are interconnected at the surface of the sintered particles.

[0062] Figure 2 is Figure 1 A photomicrograph image of a porous sintered film is schematically shown. The figure depicts a bulk film 10, a first layer 20 made primarily or entirely of coarse particles 22 and first fine particles 24, and a second layer 30 made primarily or entirely of second fine particles 26 and nanoparticles 28. The particles, when forming the porous sintered film 10, are interconnected at the surface of the sintered particles.

[0063] Exemplary porous sintered bodies can be assembled and formed into sintered films of any useful size and configuration, such as as flat plates, or alternatively as three-dimensional shapes, such as in the form of a circular cup, a cone, an open tube (open at two opposite ends), or a closed end tube (also referred to as a "closed cylinder", meaning a tube or cylinder having one closed end and one open end). A specific example of a filter body that can be used to filter supercritical carbon dioxide can be an open cylindrical filter membrane (i.e., tube) having a length in the range of from 10 to 100 mm and a diameter in the range of from 0.5 to 2 inches (e.g., in the range of from 0.75 to 1.5 inches).

[0064] The porous sintered membrane and each of its layers may have properties that allow the membrane to be used as a filter membrane. Properties include porosity, bubble point (which indicates pore size), airflow, and strength (for tubular filters, strength can be measured using a radial crush test).

[0065] The first and second layers of the described membranes may have porosity values ​​that will allow the layers to be combined together to be effective for the intended use (e.g., as a filter membrane). According to a useful example, the first layer of the described porous sintered body may have a porosity of at least 40% (e.g., a porosity in the range of from 35% to 60%). The second layer of the porous sintered membrane may have a porosity in the range of from about 15% to about 30%.

[0066] As used herein, and in the art of porous sintered bodies, the "porosity" (sometimes also referred to as void fraction) of a porous sintered body is a measure of the void (i.e., "empty") space in the body as a percentage of the total volume of the body, and is calculated as the fraction of the void volume of the body to the total volume of the body. A body with 0% porosity is completely solid.

[0067] The sintered membranes of the present description may have a bubble point useful for allowing the body to effectively filter fluids (e.g., supercritical fluids, such as supercritical carbon dioxide). Examples of useful or preferred bubble points for the membranes may be at least 25, 30, 40, or 45 pounds per square inch (psi) measured by the bubble point test method ASTM E128-99 (2019) using a 60 / 40 mixture of isopropyl alcohol (IPA) and water (by volume).

[0068] The sintered films of the present description having a tubular shape may have a strength to withstand a pressure of at least 20, 25, 30, 35, 40, or 45 kilopounds per square inch (ksi) as measured by the radial crush test (ASTM B939-21).

[0069] A sintered membrane of the present description having a tubular shape may have an "air flux" of at least 0.03, 0.04, 0.05, 0.06, 0.07, or 0.08 standard liters per minute (slpm) per square centimeter measured at 30 psig.

[0070] The porous bodies described, prepared and used as filter membranes (e.g., for filtering supercritical carbon dioxide) will exhibit filtration properties and flow properties comparable to or improved relative to previous porous sintered filter membranes. The described filter membranes, especially tubular filter membranes, can exhibit useful combinations of airflow, bubble point, and strength, or can exhibit improved combinations of two or more of these, compared to porous sintered filter membranes that do not include the two specific layers made of the specific three types of inorganic particles described herein.

[0071] Without being bound by theory, the different types of particles of the first and second layers effectively provide useful or even advantageous combinations of strength, airflow, and filtration properties (e.g., small pore size, desired bubble point, and strength). The coarse particles of the first film layer effectively provide high strength in the sintered film; the nanoparticles in the second layer effectively provide effective filtration (small pore size, relatively high bubble point); and the fine particles present in both the first and second layers provide increased strength and integrity by providing a sintered particle network connecting the first and second layers.

[0072] The porous sintered body described can be used as a filter membrane to remove particle contaminants having a particle size of nanometer scale from a fluid stream guided through the filter membrane. The fluid can be any type of fluid, including a gas, a liquid, or a supercritical fluid. The fluid can be any fluid that needs to be filtered to remove nanometer scale particle contaminants from any source, including supercritical carbon dioxide containing low levels of particulate impurities as a specific example.

[0073] Supercritical carbon dioxide can be used to process or manufacture semiconductors and microelectronic devices. The porous sintered membrane can effectively remove particulate contaminants from a fluid stream through a sieving or non-sieving filtration mechanism or both. Advantageously, a filter membrane containing the described sintered nanoparticles (e.g., as part of a second layer) can contain pores formed between the sintered nanoparticles that are small enough to allow the membrane to remove nanoscale particles through a sieving mechanism, such as removing contaminant particles having a particle size of less than 50, 20, 10 nanometers by physically preventing the particles from passing through the pores of the membrane that are smaller than the size of the contaminant particles.

[0074] The pressure of the fluid handled by the filtration system including the described sintered membrane can be relatively low pressure or relatively high pressure. For methods and apparatus for filtering certain types of fluids (including supercritical carbon dioxide), the pressure of the fluid within the filtration system (e.g., when the fluid passes through the filter membrane) is relatively high, such as at least 10, 20, or up to or exceeding 30 megapascals (MPa).

[0075] During use of the filter membrane, the pressure differential (or "pressure drop") across the thickness of the described filter membrane (between the upstream side of the filter and the downstream side of the filter) can be any pressure differential that allows for the desired effectiveness (e.g., particle retention) during the filtration step (e.g., for a given fluid flow rate of the fluid) and is also commercially feasible. For use of the described sintered membranes to filter supercritical carbon dioxide at elevated pressures, the pressure differential across the filter membrane can be at least 1, 2, or 3 megapascals (MPa).

[0076] The amount of fluid flowing through the filter membrane during the filtration step (volume passing through the filter in time) can be an amount that allows for the desired effectiveness (eg, particle retention) in the filtration step and that is also commercially feasible.

[0077] The temperature of the fluid stream passing through the described filter membranes may be any temperature that allows for commercially effective filtration. For filtering supercritical carbon dioxide, the temperature may be relatively high, such as a temperature of at least 100 degrees Celsius, 150 degrees Celsius, or 200 degrees Celsius.

[0078] The described sintered films can be prepared by a multi-step process of forming a precursor containing a first layer of the described combination of particles and a second layer of the described combination of particles, followed by sintering the precursor to bond the particles of the layers together to form a porous sintered film.

[0079] In certain example methods, the precursor can be formed by a dry method using a dry powder of metal particles without the presence of any polymer or other liquid component in the powder. The first layer of the precursor can be formed by molding the first layer from a first dry powder comprising a blend of coarse particles and fine particles (including, consisting of, or consisting essentially of a blend of coarse particles and fine particles) to form a first layer of green body (e.g., using an isostatic molding technique). After the first layer of green body is formed, a dry powder containing a blend of the described fine particles and nanoparticles of the second layer (including, consisting of, or consisting essentially of a blend of the described fine particles and nanoparticles of the second layer) is uniformly applied to the surface of the first layer of green body, again by an isostatic molding technique, and compressed against the surface. Then, the resulting green body having the first (coarse) layer and the second (fine) layer is sintered to produce a sintered porous body having the first and second layers described herein. The green body and each of its two separate layers consists of or consists essentially of the layers generated from the powder, and does not require and may not include any other materials such as polymers (binders), surfactants, solvents, or the like.

[0080] According to one example step, a collection of particles in the form of a dry powder, which mainly or entirely comprises a blend of coarse particles and fine particles (first fine particles) (consists of or is substantially composed of a blend of coarse particles and fine particles (first fine particles)) is molded under pressure to compress the particles to form a film, for example in the form of a small tube. By one technique, the molding step can be of a type known as isobaric molding or isobaric wet compression molding. (For example, see U.S. Pat. No. 7,534,287, the entire contents of which are incorporated herein by reference.) The resulting film, which mainly or entirely contains a blend of coarse particles and fine particles compressed together by the molding step, will become the first layer of the porous sintered body. The film is held together by the contact between the particles produced by the compression of the particles. The film, which is specifically the "first layer precursor" here (referred to as the "precursor" or "green body"), is self-supporting but fragile.

[0081] The second blend of particles contains mainly or entirely (consists of or consists essentially of) a blend of fine particles ("second" fine particles) and nanoparticles. This blend of particles is applied to one surface of the first layer precursor (e.g., to the outer surface of the first layer precursor in the form of a tube). The second blend is applied in a manner that places a uniform (even) amount of the blend over the surface of the first layer precursor. Effective methods for applying mixed particles to the surface of the first layer precursor are known and include methods referred to as "air laying" techniques, such as by placing a screen or mesh over the surface of the first layer and then passing the blend of particles through the screen, optionally using a brush to evenly distribute the particles.

[0082] After the second blend of particles is uniformly placed over the surface of the first layer, the formed body is molded again under pressure to compress the particles of the second blend to form a second layer compressed on the surface of the first layer. The second blend of particles can be molded and compressed on the surface of the first layer by an isostatic molding technique (e.g., an isostatic wet compression molding technique). The resulting precursor ("green body") contains a compressed and unsintered first layer made of a blend of coarse particles and first fine particles, and a compressed and sintered second layer made of a second blend containing fine particles and nanoparticles.

[0083] In a subsequent step, the precursor is sintered at a sintering temperature, which will effectively bond the particles of the two layers into a single porous sintered body. During sintering, the fine particles begin to sinter first before the coarse particles begin to sinter and before the nanoparticles begin to sinter. The first fine particles of the first layer and the second fine particles of the second layer will preferably experience similar levels of sintering during the sintering step, which can lead to stability of the sintered film and can prevent cracking and deformation of the film.

[0084] The nanoparticles and the coarse particles will begin sintering at a temperature (sintering point) that is higher than the sintering point of the first fine particles and the sintering point of the second fine particles (these sintering points may be the same). The nanoparticles may optionally begin sintering before (at a lower temperature) or after (at a higher temperature) the coarse particles begin sintering. During sintering, the nanoscale particles may preferably only undergo an initial stage of sintering while the other particles will sinter more fully. It is desirable that the nanoparticles do not undergo any melting during sintering.

[0085] The porous sintered membrane may be included in a filtration system or apparatus including a filter housing that houses and supports a filter membrane at a location of fluid flow to allow fluid to flow through the membrane as the fluid passes through the filter housing. The filter housing may have an inlet, an outlet, and an interior volume that houses the filter membrane.

[0086] Figure 3 An example of a filter housing is shown (in cross-section). The example filter housing 100 includes an outer housing 110, a fluid inlet 112, a fluid outlet 114, and an interior 120. A tubular multi-layer porous sintered body 130 is housed at the interior 120, such as by being welded to a housing base 124 at weld 130. In use, a fluid (not shown) flows into the inlet 112, through the filter membrane 130, through the interior 120, and exits the filter housing through the outlet 114 as indicated by the arrows.

[0087] The described example tubular filter membranes are capable of withstanding the pressure differentials used in supercritical carbon dioxide filtration processes without breaking, distorting, or otherwise physically compromising useful product life. One method of determining the strength of a porous sintered tubular filter membrane is the so-called radial crush test performed in accordance with ASTM B939-21. By this test, a multilayer sintered film in the form of a tubular film having two layers made from the sintered particles described herein is capable of withstanding at least 25, 30, 35, 40, or 45 kilopounds per square inch (ksi) when tested using the radial crush test.

[0088] Examples

[0089] Example 1 - Method for preparing sintered thin films

[0090] The multilayer porous sintered membrane is prepared by multiple steps, which include the following. The first step is to prepare a first (inner) non-sintered membrane layer (first layer green form), followed by a second step of preparing a second (outer) non-sintered layer on the outer surface of the first non-sintered layer. The two layers of precursors are then sintered to form a sintered, monolithic, inorganic (e.g., metal), bilayer, composite, asymmetric nanoporous tubular sieving membrane.

[0091] The first layer is a blend of 1 to 5 micron ("fine"), dendritic particles, and 50 to 75 micron ("coarse") particles of the same chemical composition in a ratio of approximately 50% by mass of each type of particle. A rubber tube isostatic mold with a central steel mandrel is filled with the blend of both particles and pressed at a pressure sufficient to form a cohesive green form.

[0092] The second layer is made of a blend comprising 1 to 5 micron ("fine"), non-dendritic particles and 30 to 150 nanometer ("nanoparticles") particles, wherein the nanoparticles have a different chemical composition than the fine particles. The two different particles are combined to form a blend containing approximately 50% by weight of each of the two different types of particles. The blend is dispensed into a rubber isopipe mold, where the green form from the previous step serves as the central mandrel and is pressed under pressure to form a cohesive green form and further define the compactness (pore size) of the constructed porous matrix.

[0093] The resulting bi-layer green form precursor is sintered in an appropriate atmosphere (one that is compatible with the materials used) with heat input that sinters all materials to adjacent materials and to themselves, but is insufficient to over-sinter or melt the nanoparticles defining the pores.

[0094] Example 2 - Sintered Film Performance

[0095]

[0096]

[0097] *use:

[0098] As the first layer, a 50 / 50 mass mix of fine and coarse particles

[0099] compounds; and

[0100] As the second layer, a 50 / 50 mass blend of nanoparticles and fine particles

[0101] Example membranes prepared according to the present disclosure can exhibit relatively high bubble points (pore size reduction) compared to existing commercial products, while maintaining or exceeding strength as measured by radial crush tests, or flux (flow / area) for tubular designs.

[0102] Examples A and B are tubular inorganic porous films prepared based on the description of U.S. Pat. No. 7,534,287. Examples A and B are prepared from nickel particles comprising fine dendritic particles and nanoparticles but no coarse particles (as the term is used herein). The Example A or Example B film comprises an inner layer made of fine dendritic nickel particles only and an outer layer made of a blend of fine dendritic nickel particles and nickel nanoparticles.

[0103] Although the Example 1 (present disclosure) film has a lower strength than the Example B film, Example 1 exceeds both flux and bubble point. Likewise, the flux of the Example 1 film is lower than that of Example A, but the Example 1 film exceeds in strength and bubble point. As can be seen in the above table, the porous films disclosed herein can achieve a combination of a bubble point of at least 30 psi, an air flux of at least 0.07 slpm / cm2 at 30 psi, and a radial crush test value of at least 35 kpsi.

[0104] In a first aspect, a porous film comprises: a first layer, which comprises a combination of sintered inorganic particles including: coarse particles having a particle size of at least 10 microns and a coarse particle sintering point; and first fine particles having a particle size of at least 1 micron and a first fine particle sintering point lower than the coarse particle sintering point; a second layer, which comprises a combination of sintered inorganic particles including: second fine particles having a particle size of at least 1 micron and a second fine particle sintering point lower than the coarse particle sintering point; and nanoparticles having a particle size lower than 1 micron and a nanoparticle sintering point higher than the first fine particle sintering point and higher than the second fine particle sintering point.

[0105] In a second aspect according to the first aspect, the coarse particles have a particle size ranging from 10 to 200 micrometers.

[0106] In a third aspect according to the previous aspect, the first fine particles have a particle size ranging from 1 to 10 micrometers, and the second fine particles have a particle size ranging from 1 to 10 micrometers.

[0107] In a fourth aspect according to the previous aspect, the nanoparticles have a size in the range from 0.001 to 0.5 microns.

[0108] In a fifth aspect according to the previous aspect, the first fine particles include nickel or a nickel alloy, the second fine particles include nickel or a nickel alloy, the coarse particles include nickel or a nickel alloy, and the nanoparticles include stainless steel.

[0109] In a sixth aspect according to the fifth aspect, the sintering point of the first fine particles is in the range of 600 degrees Celsius to 1100 degrees Celsius, the sintering point of the second fine particles is in the range of 600 degrees Celsius to 1100 degrees Celsius, the sintering point of the coarse particles is in the range from 900 degrees Celsius to 1200 degrees Celsius, and the sintering point of the nanoparticles is in the range of 800 degrees Celsius to 1100 degrees Celsius.

[0110] In a seventh aspect according to any one of the first to fourth aspects, the first fine particles include stainless steel, the second fine particles include stainless steel, the coarse particles include stainless steel, and the nanoparticles include titanium, titanium alloy, aluminum oxide, or zirconium oxide (ZrO 2).

[0111] In the eighth aspect according to the seventh aspect, the sintering point of the first fine particles is in the range of 900 degrees Celsius to 1200 degrees Celsius, the sintering point of the second fine particles is in the range of 900 degrees Celsius to 1200 degrees Celsius, the sintering point of the coarse particles is in the range of 1000 degrees Celsius to 1300 degrees Celsius, and the sintering point of the nanoparticles is in the range of 1000 degrees Celsius to 1400 degrees Celsius.

[0112] In a ninth aspect according to the previous aspect, the first layer comprises: from 50 wt % to 70 wt % of coarse particles and from 30 wt % to 50 wt % of first fine particles.

[0113] In a tenth aspect according to the previous aspect, the second layer comprises: from 40 wt % to 75 wt % of the second fine particles and from 25 wt % to 60 wt % of the nanoparticles.

[0114] In an eleventh aspect according to the previous aspect, there is from 50 wt % to 75 wt % of the first layer and from 25 wt % to 50 wt % of the second layer.

[0115] In a twelfth aspect according to the previous aspect, the first fine particles are dendritic, and the second fine particles are dendritic.

[0116] In a thirteenth aspect according to the previous aspect, the film comprises a tube.

[0117] In a fourteenth aspect according to the thirteenth aspect, the tube has a diameter in the range from 0.5 to 2 inches.

[0118] In a fifteenth aspect according to the thirteenth or fourteenth aspect, the film has a radial crush test value of at least 30 kpsi tested according to ASTM B939-21.

[0119] In a sixteenth aspect according to the previous aspect, the film has a bubble point of at least 25 pounds per square inch as measured by ASTM E 128-99 (2019) using 60 / 40 isopropyl alcohol (IPA) / water.

[0120] In a seventeenth aspect, a filter assembly comprises a filter housing housing the filter membrane of any of the previous aspects.

[0121] In an eighteenth method of processing supercritical carbon dioxide, the method comprises passing the supercritical carbon dioxide through the membrane of any of the previous aspects.

[0122] In a nineteenth method for forming a porous film, the method includes preparing a precursor comprising a first admixture of inorganic particles, the first admixture comprising: coarse particles having a particle size of at least 10 microns and a coarse particle sintering point; and first fine particles having a particle size of at least 1 micron and a first fine particle sintering point lower than the coarse particle sintering point; applying a second admixture of inorganic particles to the surface of the precursor, the second admixture comprising: second fine particles having a particle size of at least 1 micron and a second fine particle sintering point lower than the coarse particle sintering point, and nanoparticles having a particle size of less than 1 micron and a nanoparticle sintering point higher than the first fine particle sintering point and higher than the second fine particle sintering point.

[0123] In a twentieth aspect according to the nineteenth aspect, further comprising compressing the first blend of metal particles to form a first green body, applying the second blend of metal particles to the first green body, compressing the first green body and the second blend of metal particles to form a second green body, and sintering the second green body.

[0124] In a twenty-first aspect according to the twentieth aspect, sintering includes increasing the temperature of the second green body so that: the first fine particles and the second fine metal particles begin to sinter before the coarse metal particles begin to sinter, and the fine particles begin to sinter before the nanoparticles begin to sinter.

[0125] In a twenty-second aspect according to the twenty-first aspect, the coarse particles begin to sinter before the nanoparticles.

[0126] In a twenty-third aspect according to any one of the nineteenth to twenty-second aspects, the film comprises a tube.

[0127] In a twenty-fourth aspect according to the twenty-third aspect, the tube has a diameter in the range from 0.5 to 2 inches.

[0128] In a twenty-fifth aspect according to the twenty-third or twenty-fourth aspect, the film has a radial crush test value of at least 30 kpsi tested according to ASTM B939-21.

[0129] In a twenty-sixth aspect according to the twenty-third, twenty-fourth or twenty-fifth aspect, the film has a bubble point of at least 25 pounds per square inch as measured by ASTM E128-99 (2019) using 60 / 40 isopropyl alcohol (IPA) / water.

[0130] In the twenty-seventh aspect, a tubular porous film comprises: coarse particles having a particle size of at least 10 microns; fine particles having a particle size of at least 1 micron; and nanoparticles having a particle size less than 1 micron, wherein the porous film has: a bubble point of at least 30 pounds per square inch measured by ASTM E 128-99 (2019) using 60 / 40 isopropyl alcohol (IPA) / water, an air flux value of at least 0.07 slpm / cm2 at 30 psi, and a radial crush test value of at least 35 thousand pounds per square inch measured using ASTM B939-21.

[0131] In aspect 28 according to aspect 27, the film further includes: a first layer comprising a combination of sintered inorganic particles comprising: coarse particles having a particle size of at least 10 microns; and first fine particles having a particle size of at least 1 micron; and a second layer comprising a combination of sintered inorganic particles comprising: second fine particles having a particle size of at least 1 micron; and nanoparticles having a particle size of less than 1 micron.

[0132] In a twenty-ninth aspect according to the twenty-seventh or twenty-eighth aspect, the membrane comprises a tube having a diameter in the range from 0.5 to 2 inches.

Claims

1. A porous film comprising: The first layer comprises a combination of sintered inorganic particles comprising: Coarse particles having a particle size of at least 10 microns and a coarse particle sintering point; and first fine particles having a particle size of at least 1 micrometer and a first fine particle sintering point lower than the coarse particle sintering point, and The second layer comprises a combination of sintered inorganic particles comprising: second fine particles having a particle size of at least 1 micrometer and a second fine particle sintering point lower than the coarse particle sintering point, and The nanoparticles have a particle size of less than 1 micron and a nanoparticle sintering point higher than the first fine particle sintering point and higher than the second fine particle sintering point. 2 . The film according to claim 1 , wherein the coarse particles have a particle size in the range of from 10 to 200 microns.

3. The film according to claim 1 or 2, wherein: The first fine particles have a particle size ranging from 1 to 10 micrometers, and The second fine particles have a particle size ranging from 1 to 10 micrometers.

4. The film of any one of claims 1 to 3, wherein the nanoparticles have a size in the range from 0.001 to 0.5 microns.

5. The film according to any one of claims 1 to 4, wherein: The first fine particles include nickel or a nickel alloy, The second fine particles include nickel or a nickel alloy, The coarse particles include nickel or a nickel alloy, and The nanoparticles include stainless steel.

6. The film according to claim 5, wherein: The first fine particle sintering point is in the range of 600 degrees Celsius to 1100 degrees Celsius, The second fine particles have a sintering point in the range of 600°C to 1100°C, The coarse particle sintering point is in the range of 900 degrees Celsius to 1200 degrees Celsius, and The nanoparticle sintering point is in the range from 800 degrees Celsius to 1100 degrees Celsius.

7. The film according to any one of claims 1 to 4, wherein: The first fine particles include stainless steel, The second fine particles include stainless steel, The coarse particles include stainless steel, and The nanoparticles include titanium, titanium alloy, aluminum oxide or zirconium oxide (ZrO2).

8. The film according to claim 7, wherein: The first fine particle sintering point is in the range of 900 degrees Celsius to 1200 degrees Celsius, The second fine particles have a sintering point in the range of 900 degrees Celsius to 1200 degrees Celsius, The coarse particle sintering point is in the range of 1000 degrees Celsius to 1300 degrees Celsius, and The nanoparticle sintering point is in the range from 1000 degrees Celsius to 1400 degrees Celsius.

9. The film of any one of claims 1 to 8, wherein the first layer comprises: from 50 to 70 wt. % coarse particles, and From 30 wt % to 50 wt % of the first fine particles.

10. The film of any one of claims 1 to 9, wherein the second layer comprises: from 40 wt % to 75 wt % of second fine particles, and From 25 to 60 wt% nanoparticles.

11. The film according to any one of claims 1 to 10, comprising: from 50 wt. % to 75 wt. % of the first layer, and From 25 wt. % to 50 wt. % of the second layer.

12. The film according to any one of claims 1 to 11, wherein The first fine particles are dendritic, and The second fine particles are dendritic.

13. The film of any one of claims 1 to 12, wherein the film comprises a tube.

14. The film of claim 13, wherein the tube has a diameter in the range of from 0.5 to 2 inches.

15. The film of claim 13 or 14, wherein the film has a Radial Crush Test value of at least 30 kpsi when tested according to ASTM B939-21.

16. The film of any one of claims 1 to 15, wherein the film has a bubble point of at least 25 pounds per square inch as measured by ASTM E 128-99 (2019) using 60 / 40 isopropyl alcohol (IPA) / water.

17. A filter assembly comprising a filter housing housing a filter membrane according to any one of claims 1 to 16.

18. A method of processing supercritical carbon dioxide, the method comprising passing supercritical carbon dioxide through a membrane according to any one of claims 1 to 17.

19. A method for forming a porous film, the method comprising: A precursor is prepared that includes a first admixture of inorganic particles, the first admixture comprising: coarse particles having a particle size of at least 10 microns and a coarse particle sintering point, and first fine particles having a particle size of at least 1 micrometer and a first fine particle sintering point lower than the coarse particle sintering point; and applying a second blend of inorganic particles to the surface of the precursor, the second blend comprising: second fine particles having a particle size of at least 1 micrometer and a second fine particle sintering point lower than the coarse particle sintering point, and The nanoparticles have a particle size of less than 1 micron and a nanoparticle sintering point higher than the first fine particle sintering point and higher than the second fine particle sintering point.

20. The method of claim 19, further comprising: compressing the first blend of inorganic particles to form a first green body, applying the second blend of inorganic particles to the first green body, compressing the first green body and the second blend of inorganic particles to form a second green body, and The second green compact is sintered.

21. The method of claim 20, wherein sintering comprises increasing the temperature of the second green body such that: The first fine particles and the second fine inorganic particles begin to sinter before the coarse particles begin to sinter, and The first fine particles and the second fine particles begin to sinter before the nanoparticles begin to sinter.

22. The method of claim 21, wherein the coarse particles begin sintering before the nanoparticles.

23. The method of any one of claims 20 to 22, wherein the film comprises a tube.

24. The method of claim 23, wherein the tube has a diameter in the range of from 0.5 to 2 inches.

25. The method of claim 23 or 24, wherein the film has a radial crush test value of at least 30 kpsi when tested according to ASTM B939-21.

26. The method of any one of claims 23 to 25, wherein the film has a bubble point of at least 25 psi as measured by ASTM E 128-99 (2019) using 60 / 40 isopropyl alcohol (IPA) / water.

27. A tubular porous film comprising: Coarse particles having a particle size of at least 10 microns, fine particles having a particle size of at least 1 micron, and Nanoparticles, which have a particle size below 1 micron, The porous film has: A bubble point of at least 30 psi as measured by ASTM E 128-99 (2019) using 60 / 40 isopropyl alcohol (IPA) / water, An air throughput value of at least 0.07 slpm / cm2 at 30 psi, and A radial crush test value of at least 35 kpsi as measured using ASTM B939-21.

28. The film of claim 27, further comprising: The first layer comprises a combination of sintered inorganic particles comprising: coarse particles having a particle size of at least 10 microns; and first fine particles having a particle size of at least 1 micrometer; and The second layer comprises a combination of sintered inorganic particles comprising: second fine particles having a particle size of at least 1 micrometer; and Nanoparticles have a particle size less than 1 micron.

29. The membrane of claim 27 or 28, wherein the membrane comprises a tube having a diameter in the range from 0.5 to 2 inches.