Malleable flame retardant polyamide composition and use thereof, in particular for railways

The balance between mechanical strength and fire resistance in the railway field is solved by a combination of semi-crystalline aliphatic polyamides, phosphinate flame retardants, functionalized polyolefins and plasticizers in a specific proportion. It realizes efficient protection of train materials.

CN119095713APending Publication Date: 2024-12-06ARKEMA FRANCE SA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380036630.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing polyamide materials are difficult to meet the requirements of high mechanical strength and good fire resistance in the railway field, especially in the protection of train materials in the case of fire.

Method used

Using a specific proportion of semi-crystalline aliphatic polyamide, phosphinate flame retardant, functionalized polyolefin and plasticizer, the compositions of the viscosity range and proportions are adjusted to form flame retardant with excellent mechanical properties and fire resistance. agent composition.

Benefits of technology

It achieves the dual requirements of railway materials for mechanical properties and fire resistance while providing effective protection in fire situations, ensuring the safety of trains.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005102742920000091
    Figure BDA0005102742920000091
  • Figure BDA0005102742920000092
    Figure BDA0005102742920000092
  • Figure BDA0005102742920000221
    Figure BDA0005102742920000221
Patent Text Reader

Abstract

The present invention relates to a flame retardant composition comprising: (a) 30 to 85% by weight, e.g. 33 to 83% by weight, in particular 50 to 78.9% by weight, of at least one semi-crystalline aliphatic polyamide, when determined according to the standard ISO 307: 2007 but with meta-cresol instead of sulfuric acid, a temperature of 20 DEG C and a concentration of 0.5% by weight; the invention relates to a thermoplastic elastomer having an intrinsic viscosity in the range of 1.2 to 1.6, in particular 1.2 to 1.5, in particular 1.3 to 1.5, in particular strictly less than 1.5, in particular in the range of 1.30 to 1.48; (b) 10% to 30% by weight, for example 10% to 25% by weight, for example 14% to 25% by weight, for example 14% to 22% by weight, for example 17% to 22% by weight, of at least one phosphinate flame retardant, (c) 5% to 20% by weight, in particular 5% to 15% by weight, of at least one functionalized polyolefin, (d) 2 to 8 wt%, in particular 2 to 6 wt%, of at least one plasticizer, (e) 0 to 10 wt%, in particular 0.1 to 5 wt%, of at least one additive.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to ductile flame retardant polyamide compositions and their use, in particular for railway applications and the preparation of pipes, in particular corrugated pipes.

[0002] The railway sector tends to use materials with high mechanical strength and good ageing resistance.

[0003] More recently, materials used in trains have had to meet technical requirements in terms of fire resistance. These requirements depend on the type of object and its use in trains. The EN 45545 standard sets various specifications depending on the material category. Polyamide pipes correspond to the R22 and R23 categories.

[0004] Products are classified according to their limiting oxygen index as well as the density and toxicity of the smoke they produce during combustion. Depending on their fire properties, three classifications HL1, HL2 or HL3 are achieved.

[0005] The higher the classification, the more likely the product can be used in large trains, whereas products classified as HL1 cannot be used, for example, in underground subway trains.

[0006] Currently, the HL2 category covers most of the existing market and is generally targeted, which specifically means a Limiting Oxygen Index (LOI) >28.

[0007] In addition to this fire resistance, the materials used in trains are also subject to a number of mechanical stresses covering the following properties:

[0008] -Flexibility: modulus must be between 500 and 1200 MPa,

[0009] - Flexibility / Bendability: The ability to deform the tube without cracking, related to the behavior at the yield point (low stress and high elongation)

[0010] -Breaking strength: The tensile elongation at break must be greater than 100%

[0011] - Impact strength in a temperature range extending to -30°C,

[0012] -Fatigue strength.

[0013] These properties must be maintained over time. Therefore, the product must be able to withstand accelerated heat aging at 150°C for several days.

[0014] Finally, the polyamide must remain easily processable by extrusion, which limits the viscosity that the formulation can have.

[0015] The prior art has described flame retardant formulations, such as in application US20170037198, which describes formulations for the railway sector with a particular focus on PA12 matrices.

[0016] However, these formulations do not meet all the requirements listed above, especially with regard to mechanical properties.

[0017] Still in the railway field, international application WO 2013 / 092302 relates to glass-fiber reinforced polyamides flame-retarded with melamine derivatives.

[0018] Finally, application US 2007 / 0021535 uses phosphinates, melamine cyanurate and polyols in combination as flame retardants for polyamides.

[0019] However, the same disadvantages associated with the requirements listed above still exist, especially with regard to mechanical properties.

[0020] Therefore, new products must be developed to protect equipment and passengers well in the event of a fire.

[0021] Therefore, there is a need for more complete formulations with an improved compromise, in particular an optimum, between mechanical strength and fire resistance.

[0022] Therefore, the present invention relates to a flame retardant composition comprising, by weight:

[0023] (a) 30% to 85% by weight, for example 33% to 83% by weight, in particular 50% to 78.9% by weight, of at least one semicrystalline aliphatic polyamide having an intrinsic viscosity ranging from 1.2 to 1.6, in particular from 1.2 to 1.5, in particular from 1.3 to 1.5, in particular strictly less than 1.5, in particular in the range of 1.30 to 1.48, when measured according to standard ISO 307:2007 but using m-cresol instead of sulfuric acid, a temperature of 20° C. and a concentration of 0.5% by weight,

[0024] (b) 10 to 30 wt %, for example 10 to 25 wt %, for example 14 to 25 wt %, for example 14 to 22 wt %, for example 17 to 22 wt %, of at least one phosphinate flame retardant,

[0025] (c) 5 to 20%, in particular 5 to 15%, of at least one functionalized polyolefin,

[0026] (d) 2 to 8% by weight, in particular 2 to 6% by weight, of at least one plasticizer,

[0027] (e) 0 to 10% by weight, in particular 0.1 to 5% by weight, of at least one additive.

[0028] The inventors have thus found that a semicrystalline aliphatic polyamide, in specific proportions and with a specific intrinsic viscosity, combined at least with a phosphinate flame retardant, with a functionalized polyolefin and with a plasticizer (all three also in specific proportions), and optionally with additives, makes it possible to form a composition which meets all the requirements listed above.

[0029] In particular, the viscosity of the semicrystalline aliphatic polyamide matrix is ​​essential for fatigue strength. An intrinsic viscosity that is too low, i.e. less than 1.2, will not have sufficient fatigue strength. Therefore, a composition based on a semicrystalline aliphatic polyamide with a viscosity of less than 1.2 will have insufficient mechanical properties for the intended application, in particular for applications as pipes, in particular corrugated pipes, for railway applications. A composition based on a semicrystalline aliphatic polyamide with a viscosity of less than 1.2 will have insufficient fatigue strength in particular. Fatigue strength can be measured in particular by the Ross flex test as described in the examples. The composition according to the invention, i.e. in particular a composition comprising a semicrystalline aliphatic polyamide with a viscosity greater than 1.2, advantageously makes it possible to satisfy this test, that is to say, to prepare a rod that does not break after 400 000 cycles according to the Ross flex test described in the examples.

[0030] A viscosity that is too high, in particular greater than 1.6, will no longer allow the composition to be shaped, in particular in the form of a bellows.

[0031] Compositions based on semicrystalline aliphatic polyamides having a viscosity in particular greater than 1.6 are not extrudable in particular at standard forming temperatures, in particular at temperatures lower than or equal to 350°C, preferably lower than or equal to 320°C, preferably from 170°C to 300°C, for example from 200°C to 280°C.

[0032] Such compositions would have to be extruded at significantly higher temperatures and / or at higher shear rates, which would have the effect of influencing the fire resistance, in particular of the resulting pipes, the flame retardant being at least partially or even completely degraded under such processing conditions. These compositions would therefore have a fire resistance that is insufficient for the intended application, in particular for use as pipes, in particular corrugated pipes, for railway applications. Compositions based on semicrystalline aliphatic polyamides of too high a viscosity, in particular greater than 1.6, would in particular have a limiting oxygen index (LOI) that is lower than the desired value in order to satisfy the standard EN45545 for categories R22 and R23. The composition according to the invention, i.e. in particular a composition comprising a semicrystalline aliphatic polyamide having a viscosity of less than 1.6, preferably less than 1.5, preferably strictly less than 1.5, advantageously makes it possible to satisfy this test, as shown in the examples.

[0033] The plasticizer range is such as to provide a composition having a sufficiently low modulus without compromising cold impact strength.

[0034] Thus, a composition comprising less than 2% by weight of plasticizer relative to the total weight of the composition may have mechanical properties that are insufficient for the intended application, in particular for application as a pipe, in particular a corrugated pipe, for railway applications. A composition comprising less than 2% by weight of plasticizer relative to the total weight of the composition may have in particular a too high tensile modulus, in particular a tensile modulus greater than 1200 MPa, this parameter being measured as described in the examples. The composition according to the invention, i.e. in particular comprising at least 2% by weight of plasticizer relative to the total weight of the composition, advantageously makes it possible to obtain satisfactory mechanical properties, in particular a tensile modulus less than 1200 MPa, this parameter being measured as described in the examples.

[0035] A composition comprising more than 8% by weight of plasticizer relative to the total weight of the composition may itself have mechanical properties that are insufficient for the intended application, in particular for use as a pipe, in particular a corrugated pipe, in particular for railway applications. A composition comprising more than 8% by weight of plasticizer relative to the total weight of the composition may in particular have a cold notched impact strength of less than 5 kJ / m2, this parameter being measured as described in the examples. The composition according to the invention, that is to say in particular comprising up to 8% by weight of plasticizer relative to the total weight of the composition, advantageously makes it possible to obtain satisfactory mechanical properties, in particular a cold notched impact strength greater than or equal to 5 kJ / m2, this parameter being measured as described in the examples.

[0036] The functionalized polyolefin range is such that good fatigue strength and / or good cold impact strength can be obtained without excessively increasing the fire sensitivity of the composition.

[0037] Thus, a composition comprising less than 5% by weight of functionalized polyolefin relative to the total weight of the composition will have mechanical properties that are insufficient for the intended application, in particular for application as pipes, in particular corrugated pipes, for railway applications. A composition comprising less than 5% by weight of functionalized polyolefin relative to the total weight of the composition will have a cold notched impact strength in particular less than 5 kJ / m2, this parameter measured as described in the examples. The composition according to the invention, that is to say comprising in particular at least 5% by weight of functionalized polyolefin relative to the total weight of the composition, advantageously makes it possible to obtain satisfactory mechanical properties, in particular a cold notched impact strength greater than or equal to 5 kJ / m2, this parameter measured as described in the examples.

[0038] A composition comprising more than 20% by weight of functionalized polyolefin relative to the total weight of the composition will also have a fire resistance that is insufficient for the intended application, in particular for application as a pipe, in particular a corrugated pipe, for railway applications. A composition comprising more than 20% by weight of functionalized polyolefin relative to the total weight of the composition will in particular have a limiting oxygen index (LOI) below the desired value in order to meet the standard EN 45545 for categories R22 and R23. The composition according to the invention, i.e. comprising in particular a content of less than 20% by weight of functionalized polyolefin relative to the total weight of the composition, advantageously makes it possible to meet this test, as shown in the examples. The flame retardant range defined according to the invention itself makes it possible to obtain a sufficient fire resistance and in particular makes it possible to obtain a limiting oxygen index (LOI) that is in particular greater than the desired value in order to meet the standard EN 45545 for categories R22 and R23, while maintaining satisfactory mechanical properties, in particular without excessively weakening the product. Compositions comprising less than 10% by weight of flame retardant relative to the total weight of the composition generally do not make it possible to achieve the desired values ​​in order to satisfy standard EN 45545 for categories R22 and R23, as defined in the examples. Compositions comprising more than 30% by weight of flame retardant relative to the total weight of the composition may themselves have insufficient mechanical properties, in particular a cold notched impact strength of less than 5 kJ / m2, this parameter measured as described in the examples. The composition according to the invention, i.e. in particular comprising up to 30% by weight, preferably up to 25% by weight, in particular up to 22% by weight of flame retardant relative to the total weight of the composition, advantageously makes it possible to achieve satisfactory mechanical properties, in particular a cold notched impact strength greater than or equal to 5 kJ / m2, this parameter measured as described in the examples.

[0039] This is therefore a compromise, in particular an optimization, which can only be achieved by specifically selecting the ranges of the various components of the composition.

[0040] Advantageously, the composition is intended for use in railway applications.

[0041] The invention also encompasses the use of a composition as defined according to the invention for the manufacture of flame retardant articles, in particular pipes, intended for railway applications and in particular for applications in trains.

[0042] About semi-crystalline aliphatic polyamide (a)

[0043] The composition of the invention comprises at least one semicrystalline aliphatic polyamide having an intrinsic viscosity ranging from 1.2 to 1.6, in particular from 1.2 to 1.5, especially from 1.3 to 1.5, when measured according to standard ISO 307:2007 but using m-cresol instead of sulfuric acid, a temperature of 20° C. and a concentration of 0.5% by weight.

[0044] According to one embodiment, the composition of the invention comprises at least one semicrystalline aliphatic polyamide having an intrinsic viscosity strictly less than 1.5, in particular ranging from 1.30 to 1.48, when measured according to standard ISO 307:2007 but using m-cresol instead of sulfuric acid, a temperature of 20° C. and a concentration of 0.5% by weight.

[0045] The at least one semicrystalline aliphatic polyamide (a) is present in a content ranging from 30% to 85% by weight, particularly from 33% to 83% by weight, in particular from 50% to 78.9% by weight relative to the total weight of the composition.

[0046] Semicrystalline polyamides are understood to mean materials which are generally solid at room temperature and which soften during temperature increase, in particular after exceeding their glass transition temperature (Tg), and which can melt sharply above their so-called melting temperature (Tm) and which become solid again when the temperature drops below their crystallization temperature.

[0047] Tg, Tc and Tm were determined by differential scanning calorimetry (DSC) according to standards 11357-2:2013 and 11357-3:2013, respectively.

[0048] The number average molecular weight Mn of the semicrystalline polyamide is preferably in the range from 10 000 to 85 000, in particular from 10 000 to 60 000, preferably from 10 000 to 50 000 and even more preferably from 12 000 to 50 000.

[0049] The nomenclature used to define polyamides is described in standard ISO 1874-1:2011, “Plastics—Polyamide (PA) moulding and extrusion materials—Part 1: Designation”, in particular page 3 (Tables 1 and 2), and is familiar to the person skilled in the art.

[0050] The term polyamide covers both homopolyamides and copolyamides.

[0051] The at least one semicrystalline aliphatic polyamide is obtained from the polycondensation of at least one lactam, or from the polycondensation of at least one amino acid, or from the polycondensation of at least one diamine X with at least one dicarboxylic acid Y or a mixture thereof.

[0052] When the at least one semicrystalline aliphatic polyamide is obtained by polycondensation of at least one lactam, the at least one lactam may be selected from C6 to C18, preferably C9 to C18, more preferably C10 to C18, more preferably C10 to C11 lactams. The C8 to C18 lactams are in particular caprolactam or undecanoic acid lactam.

[0053] When the at least one semicrystalline aliphatic polyamide is obtained from the polycondensation of at least one lactam, it may therefore comprise a single lactam or a plurality of lactams.

[0054] When the at least one semicrystalline aliphatic polyamide is obtained from the polycondensation of at least one amino acid, the at least one amino acid may be chosen from C6 to C18, preferably C9 to C18, more preferably C10 to C18, more preferably C10 to C11 amino acids.

[0055] The C6 to C18 amino acids are especially 9-aminononanoic acid, 10-aminodecanoic acid and 11-aminoundecanoic acid, and derivatives thereof, especially N-heptyl-11-aminoundecanoic acid.

[0056] When the at least one semicrystalline aliphatic polyamide is obtained from the polycondensation of at least one amino acid, it may therefore comprise a single amino acid or a plurality of amino acids.

[0057] Advantageously, the semicrystalline aliphatic polyamide is obtained by polycondensation of a single amino acid, and the amino acid is chosen from 10-aminodecanoic acid and 11-aminoundecanoic acid, advantageously 11-aminoundecanoic acid.

[0058] When the at least one aliphatic semi-crystalline polyamide is obtained by the polycondensation of at least one C4-C36, preferably C6-C18, preferably C6-C12, more preferably C10-C12 diamine X and at least one C4-C36, preferably C6-C18, preferably C6-C12, more preferably C10-C12 diacid Y, then the at least one diamine X is an aliphatic diamine and the at least one diacid Y is an aliphatic diacid.

[0059] The diamine may be linear or branched. Advantageously, it is linear.

[0060] The at least one C4-C36 diamine X may be chosen in particular from 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undemethylenediamine, 1,12-dodecamethylenediamine, 1,13-tridecamethylenediamine, 1,14-tetradecamethylenediamine, 1,16-hexadecamethylenediamine, and 1,18-octadecamethylenediamine, octadecenediamine, eicosanediamine, docosanediamine, and diamines obtained from fatty acids.

[0061] Advantageously, the at least one diamine X is C6-C18 and is chosen from 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undemethylenediamine, 1,12-dodecamethylenediamine, 1,13-tridecamethylenediamine, 1,14-tetradecamethylenediamine, 1,16-hexamethylenediamine and 1,18-octadecamethylenediamine.

[0062] Advantageously, the at least one C6 to C12 diamine X is in particular chosen from 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undemethylenediamine and 1,12-dodecamethylenediamine.

[0063] Advantageously, the diamine X used is a C10-C12 diamine, in particular chosen from 1,10-decamethylenediamine, 1,11-undemethylenediamine and 1,12-dodecamethylenediamine.

[0064] The at least one C4 to C36 dicarboxylic acid Y may be selected from succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, octadecanedioic acid, and diacids obtained from fatty acids.

[0065] The diacid may be linear or branched. Advantageously, it is linear.

[0066] Advantageously, the at least one dicarboxylic acid Y is a C6-C18 dicarboxylic acid and is chosen from adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid and octadecanedioic acid.

[0067] Advantageously, the at least one dicarboxylic acid Y is a C6-C12 dicarboxylic acid and is chosen from adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid and dodecanedioic acid.

[0068] Advantageously, said at least one dicarboxylic acid Y is a C10-C12 dicarboxylic acid and is chosen from sebacic acid, undecanedioic acid and dodecanedioic acid.

[0069] When the semicrystalline aliphatic polyamide is obtained from the polycondensation of at least one diamine X and at least one dicarboxylic acid Y, it may therefore comprise a single diamine or a plurality of diamines and a single dicarboxylic acid or a plurality of dicarboxylic acids.

[0070] Advantageously, the semicrystalline aliphatic polyamide is obtained by the polycondensation of a single diamine X with a single dicarboxylic acid Y.

[0071] In one embodiment, the at least one polyamide is a long-chain polyamide having a number of carbons greater than or equal to 8, in particular greater than or equal to 9, in particular greater than or equal to 10, per nitrogen atom.

[0072] In another embodiment, the at least one semi-crystalline aliphatic polyamide is chosen from polyamides PA610, PA612, PA1010, PA 012 and PA11.

[0073] Advantageously, said at least one semicrystalline aliphatic polyamide is chosen from polyamides PA1010, PA1012 and PA11, in particular PA11.

[0074] According to one embodiment, the semicrystalline aliphatic polyamide of the present invention may be a polyether block amide (PEBA).

[0075] The polyether block amide (PEBA) is a copolymer containing amide units (Ba1) corresponding to aliphatic repeating units chosen from units obtained from at least one amino acid, or from at least one lactam, or from the polycondensation of:

[0076] - at least one diamine chosen from linear or branched aliphatic diamines, and

[0077] - at least one dicarboxylic acid, said diacid being an aliphatic diacid,

[0078] The polyether units (Ba2) are obtained in particular from at least one polyalkylene ether polyol, in particular polyalkylene ether glycol.

[0079] According to one embodiment, the semicrystalline aliphatic polyamide according to the invention is not a polyether block amide (PEBA).

[0080] According to one embodiment, the semicrystalline aliphatic polyamide according to the invention is not PA12.

[0081] About phosphinate flame retardants (b)

[0082] The composition according to the invention must contain a quantity of phosphinate flame retardant (b) sufficient to give said composition the desired fire resistance and in particular a classification according to HL2 or even HL3 hazard class of standard EN 45545, and preferably a classification according to HL2 hazard class of standard EN 45545.

[0083] The at least one phosphinate flame retardant (b) may be present in an amount of at least 10 wt%, such as at least 14 wt%, such as at least 15 wt%, such as at least 17 wt%, relative to the total weight of the composition.

[0084] Excessively small amounts of phosphinate flame retardant (b) do not enable sufficient fire resistance to be achieved and in particular do not enable classification to hazard class HL2 or even HL3 according to standard EN 45545 and in particular classification to hazard class HL2 according to standard EN 45545.

[0085] Phosphinate flame retardant (b) should also not be present in excessive proportions, at the risk of negatively affecting the mechanical properties. Phosphinate flame retardant (b) is therefore generally present in a content of up to 40% by weight, typically up to 30% by weight, relative to the total weight of the composition.

[0086] Too high amounts of phosphinate flame retardants (b) can have a negative effect on the mechanical properties and in particular can reduce the tensile strength and / or the impact strength and / or the fatigue strength.

[0087] According to one embodiment, the phosphinate flame retardant (b) is present in an amount ranging from 10% to 30% by weight, such as from 10% to 25% by weight, such as from 14% to 25% by weight, such as from 14% to 22% by weight, such as from 17% to 22% by weight, relative to the total weight of the composition. For example, the at least one phosphinate flame retardant (b) may be present in an amount ranging from 14% to 20% by weight relative to the total weight of the composition.

[0088] The flame retardant is in particular a metal salt selected from the group consisting of metal salts of phosphinic acid, metal salts of diphosphinic acid, polymers containing at least one metal salt of phosphinic acid, or polymers containing at least one metal salt of diphosphinic acid. The flame retardant may also be a mixture of the above flame retardants.

[0089] The flame retardant may also be selected from metal salts of phosphinic acid of the following formula (I) and metal salts of diphosphinic acid of the following formula (II):

[0090] [Chem 1]

[0091]

[0092] [Chem 1]

[0093]

[0094] in

[0095] R1 and R2 independently represent a linear or branched C1-C6 alkyl group or an aryl group;

[0096] R3 represents a linear or branched C1-C10 alkylene, C6-C10 arylene, C6-C10 alkylarylene, or C6-C10 arylalkylene group,

[0097] M is Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, or K ion, and / or a protonated amine base,

[0098] m represents an integer from 1 to 4,

[0099] n represents an integer from 1 to 4,

[0100] x represents an integer from 1 to 4,

[0101] n and m are chosen so that the salt is neutral, ie so that it has no charge.

[0102] Preferably, M represents a calcium, magnesium, aluminum or zinc ion.

[0103] Preferably, R1 and R2 independently of one another represent a methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-pentyl, and / or phenyl group.

[0104] Preferably, R3 represents a methylene group, an ethylene group, an n-propylene group, an isopropylene group, an n-butylene group, a tert-butylene group, an n-pentylene group, an n-octylene group, an n-dodecylene group; a phenylene group, a naphthylene group; a methylphenylene group, an ethylphenylene group, a tert-butylphenylene group, a methylnaphthylene group, an ethylnaphthylene group, a tert-butylnaphthylene group; a phenylmethylene group, a phenylethylene group, a phenylpropylene group, or a phenylbutylene group.

[0105] According to one embodiment, the flame retardant may be aluminum diethylphosphinate. As an example of such a compound, mention may in particular be made of the product Exolit OP1311 sold by Clariant.

[0106] About functionalized polyolefins (c)

[0107] The composition according to the invention must contain a functionalized polyolefin in an amount sufficient to give said composition the desired mechanical properties for the intended application, in particular good fatigue strength.

[0108] The at least one functionalized polyolefin (c) is present in an amount ranging from 5% to 20% by weight, in particular from 5% to 15% by weight, relative to the total weight of the composition.

[0109] The functionalized polyolefin may be a polymer of an alpha olefin with a reactive unit (functionality); such a reactive unit is an acid, anhydride or epoxy function. As an example, non-functionalized polyolefins grafted with or copolymerized or trimerized with unsaturated epoxides, such as glycidyl (meth)acrylate, or carboxylic acids or corresponding salts or esters, such as (meth)acrylic acid (the latter may be completely or partially neutralized with a metal such as Zn, etc.), or carboxylic anhydrides, such as maleic anhydride, may be mentioned.

[0110] The non-functionalized polyolefins are conventionally homopolymers or copolymers of α-olefins or dienes such as ethylene, propylene, 1-butene, 1-octene or butadiene. Examples that may be mentioned include:

[0111] - polyethylene homopolymers and copolymers, in particular LDPE, HDPE, LLDPE (linear low-density polyethylene), VLDPE (very low-density polyethylene) and metallocene polyethylene;

[0112] - propylene homopolymer or copolymer,

[0113] - ethylene / α-olefins such as ethylene / propylene, EPR (abbreviation for ethylene-propylene-rubber) and ethylene-propylene-diene (EPDM) copolymers;

[0114] - styrene / ethylene-butylene / styrene (SEBS), styrene / butadiene / styrene (SBS), styrene / isoprene / styrene (SIS) and styrene / ethylene-propylene / styrene (SEPS) block copolymers;

[0115] - copolymers of ethylene with at least one product selected from the group consisting of salts or esters of unsaturated carboxylic acids, such as alkyl (meth)acrylates (eg methyl acrylate), or vinyl esters of saturated carboxylic acids, such as vinyl acetate (EVA), the proportion of comonomer being up to 40% by weight.

[0116] Functionalized polyolefins are, for example, PE / EPR blends, the weight ratio of which can vary within a wide range, for example 40 / 60 to 90 / 10, which are co-grafted with anhydrides, in particular maleic anhydride, wherein the degree of grafting is, for example, 0.01 to 5% by weight.

[0117] The functionalized polyolefin can be selected from the following (co)polymers grafted with maleic anhydride or glycidyl methacrylate, wherein the degree of grafting is, for example, from 0.01% to 5% by weight:

[0118] PE, PP, copolymers of ethylene with propylene, butene, hexene or octene containing, for example, 35 to 80% by weight of ethylene,

[0119] - ethylene / α-olefins such as ethylene / propylene, EPR (abbreviation for ethylene-propylene-rubber) and ethylene-propylene-diene (EPDM) copolymers;

[0120] - styrene / ethylene-butylene / styrene (SEBS), styrene / butadiene / styrene (SBS), styrene / isoprene / styrene (SIS) and styrene / ethylene-propylene / styrene (SEPS) block copolymers;

[0121] - copolymers of ethylene and vinyl acetate (EVA) containing up to 40% by weight of vinyl acetate;

[0122] - copolymers of ethylene and alkyl (meth)acrylates containing up to 40% by weight of alkyl (meth)acrylates;

[0123] - Copolymers of ethylene and vinyl acetate (EVA) and alkyl (meth)acrylates containing up to 40% by weight of comonomers.

[0124] The functionalized polyolefin may also be chosen from ethylene / propylene copolymers, mostly propylene, grafted with maleic anhydride and then condensed with a monoaminated polyamide (or polyamide oligomer) (products described in EP-A-0342066).

[0125] The functionalized polyolefin may also be a copolymer or terpolymer of at least the following units: (1) ethylene, (2) an alkyl (meth)acrylate or a saturated vinyl carboxylate, and (3) an anhydride, such as maleic anhydride or (meth)acrylic anhydride, or an epoxide, such as glycidyl (meth)acrylate.

[0126] As examples of functionalized polyolefins of the latter type, mention may be made of the following copolymers, in which ethylene preferably represents at least 60% by weight and in which the termonomer (functional group) represents, for example, from 0.1% to 10% by weight of the copolymer:

[0127] - ethylene / alkyl (meth)acrylate / (meth)acrylic acid or maleic anhydride or glycidyl methacrylate copolymers;

[0128] - ethylene / vinyl acetate / maleic anhydride or glycidyl methacrylate copolymers;

[0129] - Ethylene / vinyl acetate or alkyl (meth)acrylate / (meth)acrylic acid or maleic anhydride or glycidyl methacrylate copolymers.

[0130] In the aforementioned copolymer, the (meth)acrylic acid may form a salt with Zn or Li.

[0131] The term "alkyl (meth)acrylate" refers to C1 to C8 alkyl methacrylate and C1 to C8 alkyl acrylate, and may be selected from methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, methyl methacrylate and ethyl methacrylate.

[0132] In addition, the above functionalized polyolefins can also be crosslinked by any suitable process or reagent (diepoxy, diacid, peroxide, etc.); the term functionalized polyolefin also includes mixtures of the above polyolefins with difunctional reagents capable of reacting with them, such as diacids, dianhydrides, diepoxy, etc., or mixtures of at least two functionalized polyolefins capable of reacting with each other.

[0133] The above copolymers may be copolymerized randomly or sequentially, and may have a linear or branched structure.

[0134] As will be appreciated by those skilled in the art, the molecular weight, MFI index and density of these polyolefins may also vary over a wide range. MFI is an abbreviation for melt flow index. It is measured according to standard ASTM 1238.

[0135] In one embodiment, the polyolefin is cross-linked.

[0136] According to one embodiment, the functionalized polyolefin may be chosen from polyethylene homopolymers and copolymers, in particular LDPE, HDPE, LLDPE (linear low density polyethylene), VLDPE (very low density polyethylene) and metallocene polyethylene, and in particular from VLDPE (very low density polyethylene).

[0137] As example of such a compound, mention may in particular be made of the product Orevac IM800 sold by SK Functional Polymer.

[0138] According to one embodiment, the functionalized polyolefin may be selected from ethylene / alkyl (meth)acrylate / (meth)acrylic acid or maleic anhydride or glycidyl methacrylate copolymers; ethylene / vinyl acetate / maleic anhydride or glycidyl methacrylate copolymers; ethylene / vinyl acetate or alkyl (meth)acrylate / (meth)acrylic acid or maleic anhydride or glycidyl methacrylate copolymers.

[0139] As example of such a compound, mention may in particular be made of the product Lodater AX8900 sold by SK Functional Polymer.

[0140] About Plasticizer (d)

[0141] The at least one plasticizer (e) may be present in an amount ranging from 2% to 8% by weight, in particular from 2% to 6% by weight, relative to the total weight of the composition.

[0142] The plasticizer may be a plasticizer conventionally used in polyamide-based compositions.

[0143] Advantageously, plasticizers are used which exhibit good thermal stability so that no fumes are formed during the stages of blending the various polymers and converting the composition obtained.

[0144] In particular, the plasticizer may be chosen from:

[0145] benzenesulfonamide derivatives, such as the ortho- and para-isomers of n-butylbenzenesulfonamide (BBSA), N-(2-hydroxypropyl)benzenesulfonamide (HP-BSA), N-cyclohexyltoluenesulfonamide and ethyltoluenesulfonamide (ETSA),

[0146] Esters of hydroxybenzoic acid, such as 2-ethylhexyl p-hydroxybenzoate (EHPB) and 2-hexyldecyl p-hydroxybenzoate (HDPB),

[0147] Esters or ethers of tetrahydrofurfuryl alcohol, such as oligoethyleneoxy-tetrahydrofurfuryl alcohol, and

[0148] Esters of citric acid or hydroxymalonic acid, for example oligoethyleneoxymalonates.

[0149] A preferred plasticizer is n-butylbenzenesulfonamide (BBSA).

[0150] Another particularly preferred plasticizer is N-(2-hydroxypropyl)benzenesulfonamide (HP-BSA). This is because the latter exhibits the advantage of preventing the formation of deposits ("die drool") on the extrusion screw and / or the die during the conversion phase through extrusion.

[0151] Obviously, mixtures of plasticizers may be used.

[0152] About Additives (e)

[0153] The at least one additive (f) may be present in an amount ranging from 0% to 10% by weight, in particular from 0.1% to 5% by weight, relative to the total weight of the composition.

[0154] The at least one additive may be selected from stabilizers, dyes, auxiliaries to assist conversion (processing aids), surfactants, nucleating agents, pigments, brighteners, antioxidants, lubricants, waxes, flame retardant synergists, or mixtures thereof.

[0155] Advantageously, the at least one additive is chosen from antioxidants, colored pigments and flame retardant synergists, in particular melamine-based nitrogen synergists.

[0156] As an example, the stabilizer may be a UV stabilizer, an organic stabilizer or more generally a combination of organic stabilizers, such as a phenolic type antioxidant (e.g. TUNA® from BASF). 245, 1098 or 1010), phosphite type antioxidants (e.g. 126 or 168), and even optionally other stabilizers, such as HALS, which stands for hindered amine light stabilizers (e.g. 770), UV absorbers (e.g. 312) or phosphorus-based stabilizers. Amine-type antioxidants such as those from Crompton may also be used. 445, or a multifunctional stabilizer such as Clariant S-EED.

[0157] The stabilizer may also be an inorganic stabilizer, such as a copper-based stabilizer. Examples of such inorganic stabilizers include copper halides and copper acetate. Second, other metals such as silver may be considered, but these metals are known to be less effective. These copper-based compounds are typically combined with alkali metal halides, particularly potassium halides.

[0158] The flame retardant synergist is in particular as described in WO2005121234.

[0159] They may be selected from nitrogen synergists and phosphorus / nitrogen synergists.

[0160] The nitrogen synergist preferably comprises benzoguanamine, tris(hydroxyethyl)isocyanurate, allantoin, glycoluril, melamine, melamine cyanurate, dicyandiamide, guanidine and carbodiimide.

[0161] The nitrogen synergist preferably comprises a melamine condensation product, which is exemplified by melem, melam or melonamine, or compounds of this type with a higher degree of condensation, or mixtures thereof, and which can be prepared, for example, by the process described in US Pat. No. 5,985,960.

[0162] The phosphorus / nitrogen synergist may comprise a reaction product of melamine with phosphoric acid or with condensed phosphoric acid, or may comprise a reaction product of a melamine condensation product with phosphoric acid or with condensed phosphoric acid, or may comprise a mixture of specific products.

[0163] In one embodiment, the additive is selected from antioxidants, colored pigments and flame retardant synergists, in particular nitrogen synergists, especially melamine-based synergists.

[0164] About composition

[0165] According to one embodiment, the flame retardant composition comprises by weight:

[0166] (a) 30% to 85% by weight, for example 33% to 83% by weight, in particular 50% to 78.9% by weight, of at least one semicrystalline aliphatic polyamide having an intrinsic viscosity ranging from 1.2 to 1.6, in particular from 1.2 to 1.5, in particular from 1.3 to 1.5, in particular strictly less than 1.5, in particular in the range of 1.30 to 1.48, when measured according to standard ISO 307:2007 but using m-cresol instead of sulfuric acid, a temperature of 20° C. and a concentration of 0.5% by weight,

[0167] (b) 10 to 30 wt %, for example 10 to 25 wt %, for example 14 to 25 wt %, for example 14 to 22 wt %, for example 17 to 22 wt %, for example 14 to 20 wt % of at least one phosphinate flame retardant,

[0168] (c) 5 to 20%, in particular 5 to 15%, of at least one functionalized polyolefin,

[0169] (d) 2 to 8% by weight, in particular 2 to 6% by weight, of at least one plasticizer,

[0170] (e) 0 to 10% by weight, in particular 0.1 to 5% by weight, of at least one additive,

[0171] The sum of components (a) to (e) equals 100% by weight.

[0172] According to one embodiment, the composition comprises by weight:

[0173] (a) 30% to 85% by weight, for example 33% to 83% by weight, in particular 50% to 78.9% by weight, of at least one semicrystalline aliphatic polyamide having an intrinsic viscosity ranging from 1.2 to 1.6, in particular from 1.2 to 1.5, in particular from 1.3 to 1.5, in particular strictly less than 1.5, in particular in the range of 1.30 to 1.48, when measured according to standard ISO 307:2007 but using m-cresol instead of sulfuric acid, a temperature of 20° C. and a concentration of 0.5% by weight,

[0174] (b) 10 to 30 wt %, for example 10 to 25 wt %, for example 14 to 25 wt %, for example 14 to 22 wt %, for example 17 to 22 wt %, for example 14 to 20 wt % of at least one phosphinate flame retardant,

[0175] (c) 5 to 20%, in particular 5 to 15%, of at least one functionalized polyolefin,

[0176] (d) 2 to 8% by weight, in particular 2 to 6% by weight, of at least one plasticizer,

[0177] (e) 0 to 10% by weight, in particular 0.1 to 5% by weight, of at least one additive,

[0178] The composition does not include PA12.

[0179] According to one embodiment, the composition comprises by weight:

[0180] (a) 30% to 85% by weight, for example 33% to 83% by weight, in particular 50% to 78.9% by weight, of at least one semicrystalline aliphatic polyamide having an intrinsic viscosity of 1.2 to 1.6, in particular 1.2 to 1.5, in particular 1.3 to 1.5, in particular strictly less than 1.5, in particular in the range of 1.30 to 1.48, when measured according to standard ISO 307:2007 but using m-cresol instead of sulfuric acid, a temperature of 20° C. and a concentration of 0.5% by weight,

[0181] (b) 10 to 30 wt %, for example 10 to 25 wt %, for example 14 to 25 wt %, for example 14 to 22 wt %, for example 17 to 22 wt %, for example 14 to 20 wt % of at least one phosphinate flame retardant,

[0182] (c) 5 to 20%, in particular 5 to 15%, of at least one functionalized polyolefin,

[0183] (d) 2 to 8% by weight, in particular 2 to 6% by weight, of at least one plasticizer,

[0184] (e) 0 to 10% by weight, in particular 0.1 to 5% by weight, of at least one additive,

[0185] The composition does not include PA12 and the sum of components (a) to (e) is equal to 100% by weight.

[0186] In one embodiment, the composition comprises, by weight:

[0187] (a) 50% to 78.9% by weight of at least one semicrystalline aliphatic polyamide having an intrinsic viscosity of 1.2 to 1.6, in particular 1.2 to 1.5, in particular 1.3 to 1.5, in particular strictly less than 1.5, in particular in the range of 1.30 to 1.48, when measured according to standard ISO 307:2007 but using m-cresol instead of sulfuric acid, a temperature of 20° C. and a concentration of 0.5% by weight,

[0188] (b) 10 to 30 wt %, for example 10 to 25 wt %, for example 14 to 25 wt %, for example 14 to 22 wt %, for example 17 to 22 wt %, for example 14 to 20 wt % of at least one phosphinate flame retardant,

[0189] (c) 5 to 20%, in particular 5 to 15%, of at least one functionalized polyolefin,

[0190] (d) 2 to 8% by weight, in particular 2 to 6% by weight, of at least one plasticizer,

[0191] (e) 0 to 10% by weight, in particular 0.1 to 5% by weight, of at least one additive,

[0192] The composition does not include PA12 and the sum of components (a) to (e) is equal to 100% by weight.

[0193] In another embodiment, the composition comprises, by weight:

[0194] (a) 50% to 78.9% by weight of at least one semicrystalline aliphatic polyamide having an intrinsic viscosity of 1.2 to 1.6, in particular 1.2 to 1.5, in particular 1.3 to 1.5, in particular strictly less than 1.5, in particular in the range of 1.30 to 1.48, when measured according to standard ISO 307:2007 but using m-cresol instead of sulfuric acid, a temperature of 20° C. and a concentration of 0.5% by weight,

[0195] (b) 10 to 30 wt %, for example 10 to 25 wt %, for example 14 to 25 wt %, for example 14 to 22 wt %, for example 17 to 22 wt %, for example 14 to 20 wt % of at least one phosphinate flame retardant,

[0196] (c) 5 to 15% by weight of at least one functionalized polyolefin,

[0197] (d) 2 to 8% by weight, in particular 2 to 6% by weight, of at least one plasticizer,

[0198] (e) 0 to 10% by weight, in particular 0.1 to 5% by weight, of at least one additive,

[0199] The composition does not include PA12, for example, and the sum of components (a) to (e) is equal to 100% by weight.

[0200] In yet another embodiment, the composition comprises, by weight:

[0201] (a) 50% to 78.9% by weight of at least one semicrystalline aliphatic polyamide having an intrinsic viscosity of 1.2 to 1.6, in particular 1.2 to 1.5, in particular 1.3 to 1.5, in particular strictly less than 1.5, in particular in the range of 1.30 to 1.48, when measured according to standard ISO 307:2007 but using m-cresol instead of sulfuric acid, a temperature of 20° C. and a concentration of 0.5% by weight,

[0202] (b) 10 to 30 wt %, for example 10 to 25 wt %, for example 14 to 25 wt %, for example 14 to 22 wt %, for example 17 to 22 wt %, for example 14 to 20 wt % of at least one phosphinate flame retardant,

[0203] (c) 5 to 15% by weight of at least one functionalized polyolefin,

[0204] (d) 2 to 8% by weight, in particular 2 to 6% by weight, of at least one plasticizer,

[0205] (e) 0 to 10% by weight, in particular 0.1 to 5% by weight, of at least one additive,

[0206] The composition does not include PA12, for example, and the sum of components (a) to (e) is equal to 100% by weight.

[0207] In yet another embodiment, the composition comprises, by weight:

[0208] (a) 50% to 78.9% by weight of at least one semicrystalline aliphatic polyamide having an intrinsic viscosity of 1.2 to 1.6, in particular 1.2 to 1.5, in particular 1.3 to 1.5, in particular strictly less than 1.5, in particular in the range of 1.30 to 1.48, when measured according to standard ISO 307:2007 but using m-cresol instead of sulfuric acid, a temperature of 20° C. and a concentration of 0.5% by weight,

[0209] (b) 10 to 30 wt %, for example 10 to 25 wt %, for example 14 to 25 wt %, for example 14 to 22 wt %, for example 17 to 22 wt %, of at least one phosphinate flame retardant,

[0210] (c) 5 to 15% by weight of at least one functionalized polyolefin,

[0211] (d) 2 to 8% by weight, in particular 2 to 6% by weight, of at least one plasticizer,

[0212] (e) 0.1% to 5% by weight of at least one additive,

[0213] The composition does not include PA12, for example, and the sum of components (a) to (e) is equal to 100% by weight.

[0214] In all these embodiments, the present invention also encompasses such compositions wherein the term "comprising" is replaced by the term "consisting of.

[0215] For the purposes of the present invention, the expression "said composition not comprising PA12" means that the composition comprises less than 5% by weight, in particular less than 2% by weight, in particular less than 1% by weight, in particular less than 0.5% by weight, in particular 0% by weight of PA12 relative to its total weight.

[0216] In particular, in all embodiments, the present invention also encompasses compositions wherein the sum of components (a) to (e) equals 100% by weight.

[0217] In a first variant of all these embodiments, the composition is free of melamine. It may in particular contain less than 5% by weight of melamine, in particular less than 2% by weight of melamine, or even 0% by weight of melamine relative to the total weight of the composition.

[0218] Melamine is understood to mean both melamine and melamine cyanurate, or nitrogen compounds based on melamine.

[0219] Obviously, in this case the flame retardant cannot be melamine or melamine cyanurate or a melamine-based nitrogen compound.

[0220] The presence or absence of melamine depends on the processing temperature of the product, and in the case of high temperatures, melamine will be too temperature sensitive.

[0221] During the processing of the polymers that are the subject of the invention, i.e. semi-crystalline aliphatic polymers having an intrinsic viscosity of 1.2 to 1.6, in particular 1.2 to 1.5, in particular 1.3 to 1.5, in particular strictly less than 1.5, when measured according to standard ISO 307:2007 but using at the same time meta-cresol instead of sulfuric acid, a temperature of 20° C. and a concentration of 0.5% by weight, it is not possible to use melamine as flame retardant.

[0222] The processing conditions of such semicrystalline aliphatic polymers, in particular with regard to temperature and / or shear, lead in particular to degradation of such flame retardants and thus to inadequate fire resistance.

[0223] Therefore, by using melamine as flame retardant, it is not possible to obtain a composition having both fire resistance and mechanical properties as desired according to the present invention.

[0224] On the contrary, the inventors have found that only compositions comprising phosphinate flame retardants (b) make it possible to obtain an improved compromise, in particular an optimum, between mechanical strength and fire resistance.

[0225] According to one embodiment, the composition of the invention may comprise less than 50% by weight, in particular less than 30% by weight, in particular less than 20% by weight, in particular less than 10% by weight, in particular less than 5% by weight of PEBA as defined above.

[0226] In particular, according to one embodiment, the composition of the invention may comprise in particular less than 1% by weight of PEBA, in particular less than 0.5% by weight of PEBA, or even 0% by weight of melamine relative to the total weight of the composition.

[0227] In a second variant of these embodiments, the composition is free of PEBA.

[0228] According to one embodiment, the composition of the invention may comprise less than 40 wt. %, in particular less than 30 wt. %, in particular less than 20 wt. %, in particular less than 10 wt. %, in particular less than 5 wt. % of reinforcing fibers as defined above.

[0229] In particular, according to one embodiment, the composition of the invention may comprise in particular less than 1% by weight of reinforcing fibers, in particular less than 0.5% by weight of reinforcing fibers, or even 0% by weight of reinforcing fibers relative to the total weight of the composition.

[0230] In a third variant of all these embodiments, the composition is free of reinforcing fibers.

[0231] In a fourth variant of all these embodiments, the composition is free of melamine and PEBA.

[0232] In a fifth variant of all these embodiments, the composition is free of melamine and reinforcing fibers.

[0233] In a sixth variant of all these embodiments, the composition is free of PEBA and of reinforcing fibers.

[0234] In a seventh variant of all these embodiments, the composition is free of melamine, PEBA and reinforcing fibers.

[0235] According to one embodiment, the composition of the invention may comprise less than 50% by weight, in particular less than 30% by weight, in particular less than 20% by weight, in particular less than 10% by weight, in particular less than 7.5% by weight, in particular less than 5% by weight of PA12 as defined above.

[0236] In particular, according to one embodiment, the composition of the invention may comprise in particular less than 1% by weight of PA12, in particular less than 0.5% by weight of PA12, or even 0% by weight of PA12 relative to the total weight of the composition.

[0237] In one embodiment, the composition is intended for use in railway applications.

[0238] Regarding PEBAs that may not be included

[0239] The polyether block amide (PEBA) is a copolymer containing amide units (Ba1) corresponding to aliphatic repeating units chosen from units obtained from at least one amino acid, or from at least one lactam, or from the polycondensation of:

[0240] - at least one diamine selected from linear or branched aliphatic diamines or aromatic diamines or mixtures thereof, and

[0241] - at least one carboxylic diacid selected from aliphatic diacids or aromatic diacids,

[0242] The polyether units (Ba2) are obtained in particular from at least one polyalkylene ether polyol, in particular polyalkylene ether glycol.

[0243] About reinforcing fibers that may not be included

[0244] The reinforcing fibers may in particular be chosen from reinforcing fibers of inorganic, organic or vegetable origin.

[0245] Among the fibers of inorganic origin, mention may be made, for example, of carbon fibers, glass fibers, basalt fibers or fibers based on basalt, silica fibers, or silicon carbide fibers. Among the fibers of organic origin, mention may be made, for example, of fibers based on thermoplastic or thermosetting polymers, such as semiaromatic polyamide fibers, aramid fibers or polyolefin fibers. Among the fibers of plant origin, mention may be made of natural fibers based on flax, hemp, lignin, bamboo, silk (especially spider silk), sisal, and other cellulosic fibers, especially viscose fibers.

[0246] In one embodiment, the composition has a limiting oxygen index (LOI) >28 after processing.

[0247] According to another aspect, the invention relates to a tube, in particular a partially corrugated tube, comprising at least one layer consisting of the composition as defined above.

[0248] The tube may be a single-layer or multi-layer tube.

[0249] It may be partially smooth or completely smooth.

[0250] Smooth pipes are used in particular for the circulation of pressurized gases.

[0251] It may also be partially corrugated.

[0252] Corrugated tubes are used in particular as cable ducts.

[0253] The expression "partially corrugated" means that the tube has a bellows-like shape over a portion of its length. The corrugated portion may form a single portion of the structure or multiple portions, in which case two corrugated portions are separated by a smooth portion.

[0254] The corrugated portion makes it possible to increase the deformation and extension capabilities of the tubular structure, especially in areas where small angles are required.

[0255] Advantageously, the tubular structure is corrugated over at least 10% of its length.

[0256] Advantageously, the tubular structure is corrugated over a proportion of between 10% and more than 90% of its length.

[0257] Advantageously, the tubular structure is corrugated over a proportion of 20% to 90% of its length.

[0258] Advantageously, the tubular structure is corrugated over a proportion of 30% to more than 90% of its length.

[0259] Advantageously, the tubular structure is corrugated over a proportion of 40% to more than 90% of its length.

[0260] Advantageously, the tubular structure is corrugated over a proportion of 50% to more than 90% of its length.

[0261] Advantageously, the tubular structure is corrugated over a proportion of 60% to more than 90% of its length.

[0262] Advantageously, the tubular structure is corrugated over a proportion of 70% to more than 90% of its length.

[0263] Advantageously, the tubular structure is corrugated over a proportion of 80% to more than 90% of its length.

[0264] Advantageously, the tubular structure is corrugated over more than 90% of its length.

[0265] According to yet another aspect, the present invention relates to the use of a composition as defined above for the manufacture of a flame retardant article for the railway industry, in particular for trains.

[0266] Advantageously, the article is intended for use in the interior or exterior of a train.

[0267] In one embodiment, the article is obtained by extrusion.

[0268] Advantageously, the article obtained by extrusion is a corrugated tube used as a cable duct or a smooth tube allowing the circulation of a pressurized fluid, in particular a pressurized gas, in particular compressed air.

[0269] According to another aspect, the invention relates to the use of a composition as defined above for protecting a part consisting entirely or partly of metal.

[0270] Preferably, the invention relates to such a use for imparting electrical insulation and anti-corrosion properties to the metal-based material to which it is applied.

[0271] For the purposes of the present invention, the term "metal-based material" is intended to mean a metal element which is completely or partially made of metal or a plastic or elastomeric material containing metal fibers.

[0272] The use according to the invention is therefore intended to impart electrical insulation and anti-corrosion properties to a component comprising a part comprising a metal, wherein said part is coated with said copolymer.

[0273] These elements can have very different shapes: cables, ropes, tubes, containers, membranes or plates, preferably tubes.

[0274] According to yet another aspect, the present invention relates to a process for preparing an article for the railway industry comprising the step of extruding a composition as defined above. Example

[0275] The compositions in Table 1 were prepared by melt blending polymer pellets with flame retardants, polyolefins, plasticizers and additives. The blending was carried out by compounding on a co-rotating twin-screw extruder with a diameter of 40 mm and a flat temperature profile (T°) at 250° C. The screw speed was 300 rpm and the throughput was 70 kg / h.

[0276] Polyamide, polyolefin and additives are introduced into the main hopper during the compounding process. Flame retardant is added to the molten polymer via a side feeder in the middle of the screw. Plasticizer is also introduced into the molten polymer via a pump.

[0277] The composition was then injection molded at a temperature of 250° C. to obtain a sample to be tested.

[0278] The compositions of the invention (samples) and comparative compositions were tested, wherein the limiting oxygen index measurement was carried out according to standard ISO 4589-2:2017 on test specimens measuring 80 x 10 x 4 mm.

[0279] The smoke density during burning is carried out according to standard ISO 5659-2:2017 on a plate measuring 75 x 75 x 1 mm. The maximum opacity during the burning period of 10 min is recorded.

[0280] The smoke toxicity was measured according to standard NF X70-100-1:2006 on a 30 g sample at a temperature of 600°C.

[0281] The intrinsic viscosity (IV) is determined according to standard ISO 307:2007, but using m-cresol instead of sulfuric acid, a temperature of 20° C., and a concentration of 0.5% by weight.

[0282] The impact strength is determined according to ISO 179: 1eA:2010 (Charpy impact) on a notched bar with dimensions 80 mm×10 mm×4 mm, at a temperature of 23° C.±2° C. at a relative humidity of 50%±10% or at −30° C.±2° C. at a relative humidity of 50%±10% on dry samples.

[0283] The tensile modulus, stress at 50% strain, stress at break and elongation at break are measured on dry samples at 23° C. according to standard ISO 527-1:2012. For the applications targeted by the present invention, the target properties are: modulus <1200 MPa, elongation at break >100%, stress at 50% strain <40 MPa, stress at break <50 MPa.

[0284] The machine used was an INSTRON model 5966. For the measurement of modulus, the crosshead speed was 1 mm / min, and for the stress at 50% strain and the stress at break and the elongation at break, the crosshead speed was 50 mm / min. The test conditions were 23°C ± 2°C, on dry samples.

[0285] The fatigue strength is measured by the Ross flexure test on 10 unnotched bars measuring 150×20×2 mm. The measurement is carried out as follows:

[0286] Number of cycles: 400 000

[0287] Temperature: -10℃

[0288] Bending frequency: 100 cycles / minute

[0289] Bending angle: 60°

[0290] Conditioning of test specimens: 7 days at 70°C

[0291] After 400 000 cycles, the rods obtained from the inventive formulations E1 to E6 did not break, whereas the rods obtained from the comparative compositions CE1, CE3 and CE4 did break.

[0292] [Table 1]

[0293]

[0294] [Table 2]

[0295]

[0296]

[0297] IM 800: Maleic anhydride grafted VLDPE (very low density polyethylene) (SK functionalpolymer).

[0298] AX 8900: Copolymer of ethylene, methyl acrylate and glycidyl methacrylate (Et / MA / GMA - 68 / 24 / 8 by weight) (SK functional polymer).

[0299] Black AF 34132010-ZA: Black masterbatch sold by Clariant.

[0300] TL 91: Antioxidant marketed by SI Group.

[0301] OP 1311 is a Clariant product (flame retardant based on aluminum diethylphosphinate).

[0302] Melapur MC25 is a BASF product (melamine cyanurate-based flame retardant)

[0303] BBSA (Benzylbutylsulfonamide)

[0304] Fire resistance: The EN 45545 standard sets various specifications depending on the material category. Polyamide pipes correspond to categories R22 and R23 and have the following fire protection requirements (Table 3):

[0305] [Table 3]

[0306]

[0307]

[0308] Therefore, products are classified according to their limiting oxygen index and the density and toxicity of the smoke produced during combustion. Depending on their fire properties, three hazard level classifications HL1, HL2 or HL3 are achieved.

[0309] The higher the classification, the more likely the polyamide grade is to be used in large trains, whereas products classified as HL1 cannot be used, for example, in underground subway trains.

[0310] CIT: Conventional toxicity index.

[0311] The examples show in particular the influence of the intrinsic viscosity and the range of plasticizers and other components on the mechanical criteria and in particular on fatigue strength and cold shock.

[0312] Corrugated pipes with an outer diameter of 32 mm were extruded at 230° C. with the formulations according to examples E1 to E6 of the invention. These confirm the mechanical properties and the fire resistance of these products.

Claims

1. A flame retardant composition comprising, by weight: (a) 30% to 85% by weight, for example 33% to 83% by weight, in particular 50% to 78.9% by weight, of at least one semicrystalline aliphatic polyamide having an intrinsic viscosity ranging from 1.2 to 1.6, in particular from 1.2 to 1.5, in particular from 1.3 to 1.5, in particular strictly less than 1.5, in particular in the range of 1.30 to 1.48, when measured according to standard ISO 307:2007 but using m-cresol instead of sulfuric acid, a temperature of 20° C. and a concentration of 0.5% by weight, (b) 10 to 30 wt %, for example 10 to 25 wt %, for example 14 to 25 wt %, for example 14 to 22 wt %, for example 17 to 22 wt %, of at least one phosphinate flame retardant, (c) 5 to 20%, in particular 5 to 15%, of at least one functionalized polyolefin, (d) 2 to 8%, in particular 2 to 6%, of at least one plasticizer, (e) 0 to 10%, in particular 0.1 to 5%, of at least one additive.

2. The composition as claimed in claim 1, characterized in that The semi-crystalline aliphatic polyamide (a) is obtained by polycondensation as follows: At least one C6 to C 18 Amino acid, preferably a C9 to C 18 , more preferably C 10 To C 18 , especially C 10 To C 11 Amino acids, or At least one C6 to C 18 lactam, preferably a C9 to C 18 , more preferably C 10 To C 18 , especially C 10 To C 11 Amino acids, or At least one C4-C 36 , preferably C6-C 18 , preferably C6-C 12 , more preferably C 10 -C 12 diamine X, with at least one C4-C 36 , preferably C6-C 18 , preferably C6-C 12 , more preferably C 10 -C 12 Dicarboxylic acid Y.

3. The composition according to claim 1 or 2, characterized in that The polyamide is a long-chain polyamide having a carbon number greater than or equal to 8, in particular greater than or equal to 9, in particular greater than or equal to 10, per nitrogen atom.

4. The composition as claimed in claim 3, characterized in that The long-chain polyamide is selected from PA610, PA612, PA1010, PA1012 and PA11.

5. The composition as claimed in claim 4, characterized in that The at least one semi-crystalline aliphatic polyamide is chosen from PA1010, PA1012 and PA11, in particular PA11.

6. The composition according to any one of claims 1 to 5, characterized in that The flame retardant is a metal salt selected from the group consisting of a metal salt of phosphinic acid, a metal salt of diphosphinic acid, a polymer containing at least one metal salt of phosphinic acid, and a polymer containing at least one metal salt of diphosphinic acid.

7. The composition according to any one of claims 1 to 6, characterized in that The additives are selected from antioxidants, colored pigments and flame retardant synergists, in particular nitrogen synergists, especially melamine-based synergists.

8. The composition according to any one of claims 1 to 7, characterized in that It does not contain polyether block amide (PEBA).

9. The composition as claimed in any one of claims 1 to 8, characterized in that It contains no reinforcing fibers.

10. A composition as claimed in any one of the preceding claims, comprising by weight: (a) 33% to 83%, in particular 50% to 78.9%, of at least one semicrystalline aliphatic polyamide having an intrinsic viscosity of between 1.2 and 1.6, in particular between 1.2 and 1.5, in particular between 1.3 and 1.5, when measured according to standard ISO 307:2007 but using m-cresol instead of sulfuric acid, a temperature of 20° C. and a concentration of 0.5% by weight, (b) 10 to 25% by weight, in particular 14 to 20% by weight, of at least one phosphinate flame retardant, (c) 5 to 20%, in particular 5 to 15%, of at least one functionalized polyolefin, (d) 2 to 8%, in particular 2 to 6%, of at least one plasticizer, (e) 0 to 10%, in particular 0.1 to 5%, of at least one additive, The composition does not include PA12 and the sum of components (a) to (e) is equal to 100% by weight.

11. A tube, in particular a partially corrugated tube, comprising at least one layer consisting of a composition as defined in one of claims 1 to 10.

12. Use of a composition as defined in claims 1 to 10 for the manufacture of flame retardant articles for the railway industry, in particular for trains.

13. The use as claimed in claim 11, characterized in that The article is intended for use in the interior or exterior of a train.

14. The use according to claim 12 or 13, characterized in that The article is obtained by extrusion.

15. The use as claimed in claim 14, characterized in that The articles obtained by extrusion are either corrugated tubes used as cable ducts or smooth tubes allowing the circulation of pressurized gases.

16. Use of a composition as defined in claims 1 to 10 for protecting parts consisting entirely or partly of metal.

17. Process for preparing an article for the railway industry comprising a step of extruding a composition as defined in any one of claims 1 to 10.

Citation Information

Patent Citations

  • Graft copolymer on the basis of alpha-mono-olefin, its process of fabrication, its application for the fabrication of thermoplastic blends, thermoplastic blends obtained

    EP0342066A1

  • Flame-retardant polyamide molding composition

    US20070021535A1

  • Flame-retardant polyamide 12 moulding composition for railway applications

    US20170037198A1

  • Polymer composition containing condensation product of melamine

    US5985960A

  • Flame retarded polymer composition with improved thermal stability

    WO2005121234A2