UV LED curable hot melt pressure sensitive adhesive composition

Through the combination of acrylic-epoxy copolymers, sulfonium salts and thioxanthone photosensitizers, the problem of unstable hot melt adhesives at high temperatures is solved, and efficient curing under UV-LED irradiation is achieved. It is suitable for Industrial coating machines reduce dependence on mercury bulbs and meet energy and environmental requirements.

CN119095896APending Publication Date: 2024-12-06HENKEL KGAA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380036340.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-11-28
Filing Date
2023-04-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, hot melt adhesives are unstable at high temperatures and are not suitable for rapid curing of industrial coating machines, and cannot effectively replace mercury bulbs, resulting in energy consumption and environmental problems.

Method used

Using a composition of acrylic-epoxy copolymers, sulfonium-based photoinitiators and thioxanthone-based photosensitizers, the curing of hot melt pressure-sensitive adhesives is achieved through UV-LED irradiation to ensure high belt speeds and stability at high temperatures.

Benefits of technology

It realizes efficient curing under LED irradiation, reduces dependence on mercury bulbs, meets the high temperature and high belt speed requirements of industrial coating machines, and is energy-saving and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005101519180000031
    Figure BDA0005101519180000031
  • Figure BDA0005101519180000041
    Figure BDA0005101519180000041
  • Figure BDA0005101519180000051
    Figure BDA0005101519180000051
Patent Text Reader

Abstract

The present invention relates to a UV LED curable hot melt pressure sensitive adhesive composition, a method of preparing the same, and an article comprising a first substrate and a second substrate bonded to each other with an adhesive composition according to the present invention.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a UV LED-curable hot melt pressure-sensitive adhesive composition, a method for preparing the same, and an article comprising a first substrate and a second substrate bonded to each other using the adhesive composition according to the present invention.

[0002] Hot melt adhesives offer several advantages over solvent-based adhesives in that volatile organic compounds are reduced or even eliminated, they have a long shelf life and can generally be handled without special precautions. As pressure sensitive adhesives, they are used in pressure sensitive tapes, labels, glue dots, stickers, sticky note pads, vehicle trim and a variety of other products.

[0003] US 9,469,794 discloses a UV cross-linkable acrylic pressure sensitive adhesive comprising an acrylic copolymer comprising pendant reactive functional groups and a cationic photoinitiator.

[0004] US 10,711,166 relates to a UV-curable adhesive composition comprising: a) a UV-curable acrylic polymer comprising at least one covalently bound UV-reactive group, wherein the at least one covalently bound UV-reactive group is a benzophenone; b) a cationic photoinitiator; c) a photosensitizer; and d) an unsaturated oligomer, wherein the UV-curable acrylic polymer is a polymer of the formula CH 2 =CH(R 1 )(COOR 2 ) is constructed from a single acrylic monomer, wherein R 1 is H or CH 3 , and R 2 Is branched or unbranched C 1-20 Alkyl chain.

[0005] US 8,796,350 relates to a UV-curable pressure-sensitive adhesive composition, the UV-curable pressure-sensitive adhesive composition comprising an acrylic polymer and a cationic photoinitiator, wherein the acrylic polymer is prepared from the following substances: (i) an acrylic monomer, the acrylic monomer having a formula of CH 2 =CH(R 1 )(COOR 2 ) of acrylic acid or methacrylic acid derivatives, wherein R 1 is H or CH 3 , and R 2 It is C 1-20(ii) a monomer comprising a pendant reactive functional group selected from a cycloaliphatic epoxide, an oxetane or a mixture thereof and present in an amount of about 0.001 to about 0.015 equivalents per 100 g of the acrylic polymer, wherein the acrylic polymer (a) is substantially free of multi(meth)acrylate, (b) has a Tg value below 0° C., and (c) has a weight average molecular weight of about 50,000 g / mol to about 1,000,000 g / mol; and wherein the UV-curable pressure sensitive adhesive has a viscosity in the range of 1,000 to 500,000 mPas at 80 to 180° C.

[0006] US2019 / 0085221 describes a UV-curable pressure-sensitive acrylic adhesive which can be obtained by reacting, in a first step, a mixture comprising: (i) at least one compound of the formula CH 2 =CH(R 1 )(COOR 2 R 3 CH 3 ) n acrylic monomer or a mixture thereof, wherein R 1 is H or CH 3 , and where R 2 and R 3 Both are H or both are CH 3 , and n is an integer from 0 to 22; and (ii) at least one monomer comprising a pendant reactive functional group selected from alicyclic epoxides, oxetanes, monosubstituted oxiranes or mixtures thereof; and, in a second step, reacting the mixture obtained from the first step with (iii) at least one cationic photoinitiator and (iv) optionally other additives.

[0007] UV-curable pressure-sensitive adhesives are usually cured using standard mercury bulbs as the radiation source. However, those bulbs consume a lot of energy and are expected to be banned in the next few years due to their poor environmental characteristics regarding energy consumption, poor service life and the health hazards of mercury. Therefore, efforts are being made to develop pressure-sensitive hot melt adhesives that can be cured by other radiation sources, preferably LEDs.

[0008] In the publication “Specific cationic photoinitiators for near UV and visible LEDs: Iodonium versus ferrocenium structures” by H. Mokbel et al., Journal of Applied Polymer Science, 2015, 42759, the polymerization of two iodonium salts based on coumarin chromophores under irradiation with light-emitting diodes (LEDs) was studied.

[0009] M. Rodrigues et al. studied the cationic photopolymerization of tetrahydrofuran, which was initiated by irradiating a solution containing a sulfonium salt and thioxanthone in dichloromethane at 366 nm. The results were published in "Mechanistic Study of Tetrahydrofuran Polymerization Photoinitiated by a Sulfonium Salt / Thioxanthone System", Macromol. Chem. Phys. 2001, 202, 2776-2782.

[0010] In “Photopolymerization of hybrid monomer Part I: Comparison of the performance of selected photoinitiators in cationic and free-radical polymerization of hybrid monomer” published in Polymer Testing 64 (2017) 313-320, D. Nowak et al. reported the photopolymerization of hybrid monomers 3,4-epoxycyclohexylmethyl methacrylate and 2-(2-vinyloxyethoxy)ethyl acrylate using fluorescent probe technology.

[0011] When adapting the current system to be curable by other radiation sources than mercury bulbs, certain aspects have to be taken into account, including the fact that the hot melt adhesive must be efficiently curable at high belt speeds on industrial coaters and requires temperature stability up to 130°C.

[0012] Current efforts are limited by the poor absorption of commercially available cationic photoinitiators in the UVA region. While attempts have been made to address this poor absorption pattern by using modified iodonium salts or by using standard iodonium salts in combination with sensitizers, both approaches have been found to be unsuitable for hot melt adhesives as they result in products that are unstable at higher temperatures. Furthermore, these systems have been found to be unsuitable for rapid curing on industrial coaters where it is important not to rely on dark curing.

[0013] Therefore, there is still a need for hot melt pressure sensitive adhesives that are UV-LED curable on industrial coating machines at high belt speeds.It is therefore an object of the present invention to meet said need and to provide a UV-LED curable hot melt pressure sensitive adhesive for industrial applications.

[0014] In the course of the present invention it was surprisingly found that this object is solved by a composition comprising an acrylic-epoxy copolymer in combination with a specific photoinitiator / photosensitizer system.

[0015] Therefore, a first object of the present invention is a UV-LED curable hot melt pressure-sensitive adhesive composition, the UV-LED curable hot melt pressure-sensitive adhesive composition comprising:

[0016] a. acrylic-epoxy copolymer;

[0017] b. at least one sulfonium salt-based photoinitiator; and

[0018] c. At least one thioxanthone-based photosensitizer.

[0019] The adhesive compositions of the present invention were found to be curable under LED irradiation, even at high belt speeds, thereby eliminating the need for mercury bulbs.

[0020] In a preferred embodiment of the present invention, the acrylic-epoxy copolymer is prepared by copolymerizing a monomeric acrylic mixture with an alicyclic epoxide. Preferably, the acrylic mixture comprises at least one aliphatic acrylic monomer of the general structure (I):

[0021]

[0022] in

[0023] R 1 It is C 1 -C 18 Alkyl or H,

[0024] R 2 is H or CH 3 ,

[0025] R 3 is H or CH 3 , n is an integer from 0 to 18.

[0026] Preferably, the acrylic monomer mixture comprises at least one hard acrylic monomer and at least one soft acrylic monomer. Thus, in a preferred embodiment, the monomer acrylic mixture comprises at least one first acrylic ester selected from methyl acrylate, ethyl acrylate and isobutyl acrylate and at least one second acrylic monomer selected from 2-ethylhexyl acrylate, n-butyl acrylate, 2-propylheptyl acrylate and isodecyl acrylate.

[0027] The acrylic-epoxy copolymer contained in the adhesive composition of the present invention is obtained from a reaction mixture comprising an acrylic monomer mixture and at least one epoxy acrylic monomer of the general structure (II):

[0028]

[0029] in

[0030] R 1 It is C 1 -C 18 Alkyl or H,

[0031] R 2 It is C 1 -C 18 Alkyl or C 1 -C 18 Alkoxy,

[0032] R 3 It is an alicyclic epoxy or epoxide group.

[0033] Preferably, the at least one epoxy acrylic monomer is selected from 3,4-epoxycyclohexylmethyl methacrylate or glycidyl methacrylate.

[0034] The acrylic-epoxy copolymer is preferably obtained via solution polymerization.Preferred solvents are those selected from ethyl acetate, methyl ethyl ketone, heptane, hexane, pentanone, acetone, toluene, propyl acetate, benzene, and mixtures thereof.

[0035] The molecular weight of the acrylic-epoxy copolymer can be adjusted as desired, but is preferably maintained within a weight average molecular weight Mw of 50,000 to 400,000 Da, preferably 50,000 to 250,000 Da, as determined by GPC using polystyrene as a standard.

[0036] The adhesive composition of the present invention comprises at least one sulfonium salt-based photoinitiator. In a preferred embodiment, the sulfonium salt-based photoinitiator is represented by the general formula (III):

[0037]

[0038] in

[0039] R 1 is selected from H, aryl, thioaryl, C 1 -C 18 Alkyl, C 1 -C 18 Alkoxy, SH or NR 2 , R 2 is selected from P, Sb, B, As or Bi, and

[0040] R 3 Yes F 6 - or F 3 (C 2 F 5 ) 3 - .

[0041] In a particularly preferred embodiment, the at least one sulfonium salt-based photoinitiator is selected from ([1,1′-biphenyl]-4-yl)(diphenyl)sulfonium trifluoro[tris(pentafluoroethyl)]-phosphate or triarylsulfonium hexafluoroantimonate.

[0042] In addition to at least one sulfonium salt-based photoinitiator, the adhesive composition also includes at least one thioxanthone-based photosensitizer. It was unexpectedly found that the combination of a sulfonium salt-based photoinitiator and a thioxanthone-based photosensitizer with an acrylic-epoxy copolymer provides a hot melt pressure-sensitive adhesive that can be easily cured under UV-LED irradiation. In a preferred embodiment, at least one thioxanthone-based photosensitizer is represented by the general formula (IV):

[0043]

[0044] in

[0045] R 1 NH, CH 2 , S or O, and

[0046] R 2 To R 9 Independently H, C 1 -C 18 Alkyl or isoalkyl, C 1 -C 18 Alkoxy, aryl, COOH, OH, NR 2, COOR, urea, carbamate, S or SH.

[0047] R 2 To R 9 At least one of may be composed of a polymerizable group in an ABC structure, wherein

[0048] A is O, NR 2 , S, C 1 -C 18 Alkyl or isoalkyl, COOH, C 1 -C 18 Alkoxy, S or aryl,

[0049] B is C 1 -C 18 alkyl or isoalkyl, carboxyl, vinyl or aryl,

[0050] C is acrylic or methacrylic, epoxy or alicyclic epoxy, vinyl or aryl.

[0051] In a particularly preferred embodiment of the present invention, the thioxanthone-based photosensitizer is selected from isopropylthioxanthone, 2,4-diethyl-9H-thioxanthen-9-one, or a derivative thereof.

[0052] The adhesive composition of the present invention may contain other additives (such as plasticizers, tackifiers, antioxidants and fillers). It was unexpectedly found that conventionally used additives can be used without affecting the UV-LED curing performance of the adhesive composition of the present invention.

[0053] The adhesive optionally contains one or more suitable tackifiers conventionally used for preparing PSAs (in an amount of about 10-50% by weight of the adhesive). Reference may be made expressly to the description of the prior art in the "Handbook of Pressure Sensitive Adhesive Technology" by Donatas Satas (van Nostrand, 1989) or in any literature related to PSAs. In general, any natural resin compatible with the corresponding acrylic polymer may be used; all natural resins may be specifically mentioned. Non-limiting examples include pinene resins, indene resins, rosins, terpene resins, terpene-phenolic resins, gum rosins, wood rosins, tall oil rosins, distilled rosins, hydrogenated rosins, dimerized rosins, polymerized rosins; and disproportionated and esterified derivatives and salts thereof.

[0054] Other suitable tackifiers include aliphatic and aromatic hydrocarbon resins, hydrogenated hydrocarbon resins, and functional hydrocarbon resins. Non-limiting examples include aliphatic and aromatic hydrocarbon resins, C5 resins, C9 resins, and other hydrocarbon resins. Any desired combination of these resins may be used to adjust the properties of the resulting PSA according to the desired final properties.

[0055] Specific examples of these tackifiers include TECKROS R86, SYLVALITE RE 85GB, FORAL 85-E, WINGTACK 95, CLEARTACK W85. A preferred embodiment of the tackifier is a liquid tackifier, which can further reduce the viscosity of the adhesive. Examples include polymerized C5 petroleum feed streams and polyterpenes (such as WINGTACK 10 and ESCOREZ 2520), liquid rosin ester tackifier SYLVALITE 2038.

[0056] Hot melt adhesives are characterized in that they are solid at room temperature. They are applied in a molten state at elevated temperatures. In order to protect valuable energy sources, hot melt adhesives that can be applied at relatively low temperatures are preferred. Although conventional hot melt adhesives generally require a temperature of about 160-175°C, it is unexpectedly found that the hot melt adhesive composition according to the present invention can be applied at a much lower temperature. Therefore, in a preferred embodiment, the adhesive composition according to the present invention is characterized in that the application temperature is 60-150°C, preferably 100-130°C, more preferably 110-120°C.

[0057] The adhesive composition according to the present invention is intended for industrial-scale applications, in particular applications by industrial coating machines. In order to be compatible with existing systems, the curing temperature of the hot melt adhesive composition should be within the temperature range usually associated with mercury bulb curing. It was unexpectedly found that the adhesive composition according to the present invention meets this requirement despite the curing being initiated by UV-LED. Therefore, in a preferred embodiment, the curing temperature of the hot melt pressure-sensitive adhesive composition of the present invention is 25-150°C, preferably 25-110°C.

[0058] The hot melt adhesive composition according to the present invention is designed to be used in combination with the high belt speed of the industrial coating machine. In order to be easy to apply, the viscosity of the adhesive composition of the present invention is preferably 10000 to 130000 mPa*s at 120°C, more preferably 20000 to 100000 mPa*s at 120°C, which is measured with Brookfield DV-II, No. 27 rotor (SP.27).

[0059] Furthermore, the hot melt pressure-sensitive adhesive composition of the invention is UV-curable, in particular UV-curable by UV radiation generated by an LED. Therefore, in a preferred embodiment, the adhesive composition is UV-curable at 100 to 10000 mJ / cm 2 as determined according to the UV radiation Puk measurement (here: EIT Power Puk II). 2 , preferably 300-3000mJ / cm 2Curable at a limited UVA dose. By being curable at a limited UVA dose, the need for mercury bulbs can be eliminated and more energy-efficient LEDs can be employed.

[0060] In a preferred embodiment, the adhesive composition according to the invention is characterized in that the cured adhesive has a shear adhesion failure temperature (SAFT) of 50-200° C., preferably 120-200° C., measured according to GTF 6001 (Afera 5013).

[0061] In addition to being UV-LED curable, the adhesive composition of the present invention also exhibits excellent adhesive properties when cured. In a preferred embodiment, the cured adhesive exhibits a 180° peel performance on a steel substrate at 300 mm / min of 2 to 45 N / 25 mm, preferably 5 to 35 N / 25 mm, measured according to DIN ES ISO 11339 / 2010-06. 2 The irradiated cured polymer film has a thickness of 15-150 gsm.

[0062] Another object of the present invention is a method for preparing a hot melt pressure-sensitive adhesive composition according to the present invention. According to the method of the present invention, an acrylic monomer mixture is copolymerized with an alicyclic epoxide, and the obtained acrylic-epoxy copolymer is formulated with at least one sulfonium salt-based photoinitiator and at least one thioxanthone-based photosensitizer to produce an adhesive composition. The copolymerization in solution polymerization allows crosslinking of the polymer by cationic polymerization.

[0063] The solvent used is preferably selected from ethyl acetate, butanone, heptane, hexane, pentanone, acetone, toluene, propyl acetate, benzene, and mixtures thereof.

[0064] The acrylic monomer mixture and the alicyclic epoxide are preferably copolymerized in the presence of a polymerization initiator. The polymerization initiator is preferably selected from azo initiators, such as AIBN, AMBN or ACCN. Preferably, the amount of the polymerization initiator is 0.01-5% based on the total weight of the acrylic monomer mixture and the alicyclic epoxide.

[0065] In a preferred embodiment, the method of the present invention comprises the steps of: copolymerizing an acrylic monomer mixture and an alicyclic epoxide in a solvent polymerization, preferably copolymerizing an acrylic monomer mixture and an alicyclic epoxide in a solvent polymerization in the presence of a polymerization initiator; then, formulating the obtained copolymer with a sulfonium salt-based photoinitiator and a thioxanthone-based photosensitizer to obtain the adhesive composition of the present invention after removing the solvent.

[0066] The amount of the sulfonium salt-based photoinitiator used is preferably 0.001 to 5% by weight, preferably 0.001 to 3.5% by weight, based on the total weight of the adhesive composition.

[0067] The amount of the thioxanthone-based photosensitizer used is preferably 0.001-5 wt%, preferably 0.001-3.5 wt%, based on the total weight of the adhesive composition.

[0068] Another object of the present invention is the article obtained using the hot melt pressure-sensitive adhesive composition of the present invention.Article comprises the first substrate and the second substrate bonded to each other with the adhesive composition according to the present invention.In a preferred embodiment, the article is selected from polymer foil substrate, polymer substrate, metal substrate, glass substrate or wood substrate or paper substrate.

[0069] The present invention will be explained in more detail with reference to the following examples, which, however, should by no means be construed as limiting the scope and spirit of the present invention.

[0070] Example 1: Preparation of UV-curable polymer

[0071] First, an acrylic copolymer is prepared by free radical copolymerization of about 45% by weight of methyl acrylate and 54% by weight of 2-EHA. In addition, about 1% by weight of epoxy acrylate M100 is copolymerized. The polymerization is carried out in ethyl acetate and initiated with an azo initiator (such as AIBN) (0.11%). After the polymerization, the polymer product is formulated with 0.5g of Irganox 1726, 0.5g of cationic photoinitiator CPI200K (50% propylene carbonate solution) and 0.25g of isopropylthioxanthone (ITX) as a sensitizer. Then, ethyl acetate is removed under reduced pressure at 120°C, and the acrylic copolymer is obtained. The weight average molecular weight of the acrylic polymer is 120000Da (GPC), and the hot melt viscosity (Brookfield, S27) of the polymer at 120°C is 50000mPa*s.

[0072] Example 2: Preparation of UV-curable polymer

[0073] First, an acrylic copolymer is prepared by free radical copolymerization of about 45% by weight of methyl acrylate and 54% by weight of 2-EHA. In addition, about 2% by weight of epoxy acrylate M100 is copolymerized. The polymerization is carried out in ethyl acetate and initiated with an azo initiator (such as AIBN) (0.11%). After the polymerization, the polymer product is formulated with 0.5g of Irganox 1726, 0.5g of cationic photoinitiator Omnicat320 (50% propylene carbonate solution) and 0.25g of isopropylthioxanthone (ITX) as a sensitizer. Then, ethyl acetate is removed under reduced pressure at 120°C, and the acrylic copolymer is obtained. The weight average molecular weight of the acrylic polymer is 110,000 Da (GPC), and the hot melt viscosity (Brookfield, S27) of the polymer at 110°C is 75,000 mPa*s.

[0074] Example 3: Preparation of UV-curable polymer

[0075] First, an acrylic copolymer is prepared by free radical copolymerization of about 45% by weight of ethyl acrylate and 54% by weight of 2-propylheptyl acrylate. In addition, about 1-2% by weight of epoxy acrylate M100 is copolymerized. The polymerization is carried out in ethyl acetate and initiated with an azo initiator (such as AIBN) (0.11% by weight). After the polymerization, the polymer product is formulated with 0.5g Irganox 1726, 0.5g of cationic photoinitiator Omnicat320 (50% propylene carbonate solution) and 0.25g of isopropylthioxanthone (ITX) as a sensitizer. Then, the solvent is removed under reduced pressure at 120°C, and the acrylic copolymer is obtained. The weight average molecular weight of the acrylic polymer is 120,000 Da (GPC), and the hot melt viscosity (Brookfield, S27) of the polymer at 120°C is 50,000 mPa*s.

[0076] Example 4: Preparation of UV-curable polymer

[0077] First, an acrylic copolymer is prepared by free radical copolymerization of 45 wt % of methyl acrylate and 54 wt % of isodecyl acrylate. In addition, about 1-2 wt % of epoxy acrylate M100 is copolymerized. The polymerization is carried out in ethyl acetate or butanone and initiated with an azo initiator (such as AIBN) (0.11 wt %). After the polymerization, the polymer product is formulated with 0.5 g of Irganox 1726, 1 g of cationic photoinitiator Omnicat 320 (50% propylene carbonate solution) and 0.5 g of isopropylthioxanthone (ITX) as a sensitizer. Then, the solvent is removed under reduced pressure at 120° C., and the acrylic copolymer is obtained. The weight average molecular weight of the acrylic polymer is 120,000 Da (GPC), and the hot melt viscosity (Brookfield, S27) of the polymer at 120° C. is 50,000 mPa*s.

[0078] Example 5: Preparation of UV-curable polymer

[0079] First, an acrylic copolymer is prepared by free radical copolymerization of 45 wt % methyl acrylate and 54 wt % 2-EHA. In addition, about 1-2 wt % epoxy acrylate M100 is copolymerized. The polymerization is carried out in ethyl acetate or butanone and initiated with an azo initiator (such as AIBN) (0.11 wt %). After the polymerization, the polymer product is formulated with 0.5 g Irganox1726, 0.5-1 g cationic photoinitiator CPI200K (50% propylene carbonate solution). Then, the solvent is removed under reduced pressure at 120° C., and the acrylic copolymer is obtained. The weight average molecular weight of the acrylic polymer is 175,000 Da (GPC), and the hot melt viscosity (Brookfield, S27) of the polymer at 120° C. is about 75,000 mPa*s.

[0080] Example 6: Coating and curing of acrylic copolymer

[0081] The acrylic copolymer was coated via a laboratory coater in which both rollers could be heated to 120-130°C. Prior to this, the polymer was preheated to 120°C in an oven. The adhesive was coated on a 50 μm thick silicone release liner to achieve a thickness of 80 μm. After coating had been completed, a 365 nm LED was used at 1500 mJ / cm 2 The adhesive was irradiated with a UVA dose of 100 Å. The adhesive film was laminated with an etched polyethylene terephthalate (PET) foil (50 μm) and conditioned at 23° C. and 50% relative humidity for 24 hours.

[0082] Example 7: Peel measurement of adhesive films

[0083] After conditioning, the cured adhesive film is cut into three test strips of 25mm×150mm in size. Clean the stainless steel plate (Rocholl) with ethyl acetate and acetone, and dry for 30 minutes at 23°C and 50% relative humidity. Remove the backing paper of the adhesive test strip, and place the strip along the stainless steel plate. All samples are rolled twice in each direction with a 2kg FINAT roller at a speed of 10mm / s. Afterwards, the test strip is conditioned for 20 minutes at 23°C and 50% relative humidity. The ZWICK tensile tester is set to a speed of 300mm / min, and the free end of the tape is placed in the upper clamping device. The steel plate is fixed in the lower clamping device, and the strip is peeled off from the steel substrate at an angle of 180° according to AFERA ​​4001 / DIN EN ISO11339:2010-06.

[0084] Example 8: Shear Adhesion Failure Test (SAFT)

[0085] For this test, three strips of 25mm×70mm in size were cut from the cured and conditioned adhesive. SAFT steel plate samples were cleaned with ethyl acetate and acetone, and conditioned for 30 minutes at 23°C, 50% relative humidity. The backing paper of the test strip was removed, and the strip was placed on a steel substrate to form a square test area of ​​25mm×25mm. All strips were rolled twice in each direction with a 2kg FINAT roller at a speed of 10mm / s. After rolling, the test hook was fixed to the test strip, and all samples were conditioned for another 30 minutes at 23°C, 50% relative humidity. Then, the sample was placed in a test oven, a 1kg weight was attached to the hook, and the oven was heated to 200°C with a ramp rate of 0.5°C / min. Test method according to GTF 6001 (Afera 5013).

[0086] Example 9: Preparation of acrylic adhesive

[0087] The four-neck 1L round-bottomed polymerization flask is equipped with a thermometer, a condenser, an overhead mechanical stirrer, two feed funnels and a nitrogen inlet / outlet connected to a temperature control device. The equipment is purged with nitrogen for 15min. Prepare a mixture of the following monomers: butyl acrylate (148.8g) and 1-acryloylmethyl-3,4-cyclohexene epoxide (1.2g). 112g of monomer mixture is loaded into one of the funnels. Initiator 2,2'-azobis-(2-methylpropionitrile) (AIBN, 0.1g), isopropanol (15g) and ethyl acetate (45mL) are loaded into another funnel. The remaining monomer mixture (38g), initiator AIBN (0.2g), isopropanol (6mL), ethyl acetate (34mL) are loaded into the polymerization flask. The mixture is heated to vigorous reflux and kept for 15 minutes. Then, the monomer mixture in the funnel is continuously added at a constant rate for 2 hours. At the same time, the initiator solution in the funnel is continuously added at a constant rate within 3 hours. After complete addition of the initiator solution, the mixture was stirred at reflux for another 2 hours. A short half-life initiator (0.75 g) and ethyl acetate (25 mL) were charged into the initiator funnel and then added to the polymerization flask within 1 hour to reduce residual monomers. After removing the ethyl acetate by vacuum at 55-60° C., an acrylic adhesive having a weight average molecular weight Mw of 58,000 g / mol and a PDI of 2.6 according to GPC and a viscosity of 130,000 cps at 60° C. according to Brookfield was obtained, as disclosed herein.

[0088] Example 10: Coating and curing of acrylic copolymer

[0089] The acrylic polymer from Example 9 (65 g) was mixed with ITX (0.5 g), OMNICAT 320 (0.5 g), reactive diluent epoxidized soybean oil NATUREFLEXX ESO (25 g) and tackifier TECKROS R86 (10 g). The mixture was cured by LED 365 nm lamp. The adhesive film was 1 mil thick and was directly coated on 2 mil PET and cured by LED 365 nm at 600 mJ / cm 2 Although the viscosity of the acrylic polymer obtained from Example 9 at 60°C was about 130,000 cps, the adhesive coating temperature could be lowered to below 60°C.

Claims

1. A UV-LED-curable hot melt pressure-sensitive adhesive composition, the UV-LED-curable hot melt pressure-sensitive adhesive composition comprising: a. acrylic-epoxy copolymer; b. at least one sulfonium salt-based photoinitiator; and c. At least one thioxanthone-based photosensitizer.

2. The adhesive composition according to claim 1, It is characterized in that The acrylic-epoxy copolymer is prepared by copolymerizing a monomeric acrylic mixture with an alicyclic epoxide.

3. The adhesive composition according to claim 2, It is characterized in that The acrylic mixture comprises at least one aliphatic acrylic monomer of the general structure (I): in R 1 It is C 1 -C 18 Alkyl or H R 2 is H or CH 3 R 3 is H or CH 3 n is an integer of 0-18.

4. The adhesive composition according to claim 3, It is characterized in that The monomer acrylic mixture comprises at least one acrylic ester selected from methyl acrylate, ethyl acrylate and isobutyl acrylate, and at least one acrylic monomer selected from 2-ethylhexyl acrylate, n-butyl acrylate, 2-propylheptyl acrylate and isodecyl acrylate.

5. The adhesive composition according to any one of claims 2 to 4, It is characterized in that The epoxy acrylic monomer of the general structure (II) is copolymerized: in R 1 It is C 1 -C 18 Alkyl or H R 2 It is C 1 -C 18 Alkyl or C 1 -C 18 Alkoxy R 3 It is an alicyclic epoxy or epoxide group.

6. The adhesive composition according to any one of claims 2 to 5, It is characterized in that The acrylic-epoxy copolymer is obtained via solution polymerization, preferably the acrylic-epoxy copolymer is obtained via solution polymerization in a solvent selected from ethyl acetate, methyl ethyl ketone, heptane, hexane, pentanone, acetone, toluene, propyl acetate, benzene, and mixtures thereof.

7. The adhesive composition according to any one of the preceding claims, It is characterized in that The at least one sulfonium salt-based photoinitiator is represented by the general formula (III): in R 1 is selected from H, aryl, thioaryl, C 1 -C 18 Alkyl, C 1 -C 18 Alkoxy, SH or NR 2 , R 2 is selected from P, Sb, B, As or Bi, and R 3 Yes F 6 - or F 3 (C 2 F 5 ) 3 - .

8. The adhesive composition according to any one of the preceding claims, It is characterized in that The at least one thioxanthone-based photosensitizer is represented by the general formula (IV): in R 1 NH, CH 2 , S or O, and R 2 To R 9 Independently H, C 1 -C 18 Alkyl or isoalkyl, C 1 -C 18 Alkoxy, aryl, COOH, OH, NR 2 , COOR, urea, carbamate, S or SH.

9. The adhesive composition according to any one of the preceding claims, It is characterized in that The application temperature of the adhesive composition is 60-150°C, preferably 100-130°C, more preferably 110-120°C.

10. The adhesive composition according to any one of the preceding claims, It is characterized in that The adhesive composition is 100-10000 mJ / cm2 as determined according to UV radiation Puk measurement (here: EIT Power Puk II). 2 , preferably 300-3000mJ / cm 2 Curable under UVA doses.

11. The adhesive composition according to any one of the preceding claims, It is characterized in that The cured adhesive has a shear adhesion failure temperature (SAFT) of 50-200° C., preferably 120-200° C., measured according to GTF 6001 (Afera 5013).

12. The adhesive composition according to any one of the preceding claims, It is characterized in that The cured adhesive exhibits a 180° peel performance on a steel substrate at 300 mm / min of 2 to 45 N / 25 mm, preferably 5 to 35 N / 25 mm, determined according to DIN ES ISO 11339 / 2010-06.

13. A method for preparing an adhesive composition according to any one of the preceding claims, wherein an acrylic monomer mixture is copolymerized with an alicyclic epoxide, and the obtained acrylic-epoxy copolymer is formulated together with at least one sulfonium salt-based photoinitiator and at least one thioxanthone-based photosensitizer to produce the adhesive composition.

14. The method according to claim 13, It is characterized in that The copolymerization is carried out in a solvent selected from the group consisting of ethyl acetate, methyl ethyl ketone, heptane, hexane, pentanone, acetone, toluene, propyl acetate, benzene, and mixtures thereof.

15. An article comprising a first substrate and a second substrate bonded to each other using the adhesive composition according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • UV curable adhesives based on acrylic polymers

    US10711166B2

  • Cationic pressure sensitive adhesive UV cured by medium mercury bulbs

    US20190085221A1

  • Cationic UV-crosslinkable acrylic polymers for pressure sensitive adhesives

    US8796350B2

  • Cationic UV-crosslinkable acrylic polymers for pressure sensitive adhesives

    US9469794B2