Polypropylene resin composition containing filler
By adding acid modified propylene to the propylene polymer composition and designing a multi-dispersed phase structure, the problem of lowering rigidity after adding filler is solved, and the high rigidity and impact resistance of the polypropylene resin composition are achieved, and it is suitable for a variety of purposes. Materials application.
Patent Information
- Application Number
- CN202380036428.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2023-06-12
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the resin composition including acrylic polymer, polyamide resin and modified elastomer has a significantly reduced rigidity after adding filler, making it difficult to achieve a balance between rigidity and impact resistance.
Acid-modified propylene is added to the acrylic polymer composition, and a continuous and dispersed phase is formed by a specific phase structure design, combined with melt-kneading of aliphatic polyamide resin and modified elastomer in the polyolefin composition to form a continuous phase and a dispersed phase multiple dispersed structure.
It has achieved excellent balance between rigidity and impact resistance of the polypropylene resin composition, and is suitable for applications such as automotive interior decoration materials and exterior decoration materials.
Smart Images

Figure BDA0005102000660000311 
Figure BDA0005102000660000381 
Figure BDA0005102000660000391
Abstract
Description
Technical Field
[0001] The present invention relates to a polypropylene resin composition comprising a filler-containing propylene polymer composition and a polyamide resin. Background Art
[0002] Resin compositions comprising propylene polymers and polyamide resins and modified elastomers having acid groups such as acid anhydride groups introduced therein acting as compatibilizers have been studied as resins having improved impact resistance, and it has been found that they form specific phase structures (see, for example, Patent Documents 1 to 4).
[0003] In addition, for the purpose of improving impact resistance and rigidity, a resin composition comprising a propylene polymer, a polyamide resin, and a modified elastomer containing a group reactive with the polyamide resin has been studied, wherein the polyamide resin contains a filler (eg, an inorganic filler, a natural fiber, etc.).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2013 / 094763 Pamphlet
[0007] Patent Document 2: International Publication No. 2013 / 094764 Pamphlet
[0008] Patent Document 3: International Publication No. 2018 / 139378 Pamphlet
[0009] Patent Document 4: International Publication No. 2018 / 135648 Pamphlet Summary of the invention
[0010] Problems to be solved by the invention
[0011] In order to further improve the physical properties (e.g., impact resistance) of the resin composition containing a propylene polymer, a polyamide resin, and a modified elastomer, it is also possible to study a resin composition containing a filler, a polyamide resin, and a modified elastomer, wherein the propylene polymer composition is obtained by adding a filler to the propylene polymer. However, according to the research of the inventors of the present application, it was found that even if only a resin composition containing a filler, a polyamide resin, and a modified elastomer is prepared, the rigidity is greatly reduced, and further improvement is clearly required for practical use.
[0012] An object of the present invention is to provide a polypropylene resin composition having an excellent balance between rigidity and impact resistance, the polypropylene resin composition comprising a propylene polymer composition, a polyamide resin, and a modified elastomer, wherein the propylene polymer composition comprises a filler (e.g., an inorganic filler, a natural fiber, etc.).
[0013] Means for solving problems
[0014] Under such circumstances, the inventors of the present application conducted research and found that the above-mentioned problems can be solved by adding acid-modified propylene to a propylene polymer composition having a specific phase structure in addition to a propylene polymer composition containing a filler and a polyolefin composition containing a polyolefin, an aliphatic polyamide resin, and a modified elastomer, thereby completing the present invention.
[0015] That is, the present invention relates to, for example, the following [1] to
[11] .
[0016] [1] A polypropylene resin composition comprising a propylene polymer composition (a), a polyolefin composition (b), and an acid-modified polypropylene (c).
[0017] The propylene polymer composition (a) comprises a propylene polymer (a1) and a filler (a2).
[0018] The polyolefin composition (b) comprises a polyolefin (b1), an aliphatic polyamide resin (b2), and a modified elastomer (b3), and
[0019] The invention comprises a continuous phase (α) containing a polyolefin (b1) and a dispersed phase (β) containing an aliphatic polyamide resin (b2) and a modified elastomer (b3) dispersed in the continuous phase (α).
[0020] The dispersed phase (β) is formed from a melt-kneaded product of the aliphatic polyamide resin (b2) and the modified elastomer (b3).
[0021] The modified elastomer (b3) is an elastomer obtained by adding a portion of the aliphatic polyamide resin (b2) containing a group reactive therewith to an unmodified elastomer (b3'), wherein the unmodified elastomer (b3') is an olefin-based thermoplastic elastomer containing a structural unit derived from ethylene and a structural unit derived from an α-olefin having 3 to 8 carbon atoms, or a styrene-based thermoplastic elastomer containing a structural unit derived from a styrene-based compound.
[0022] When the total of the continuous phase (α) and the dispersed phase (β) is 100% by mass, the dispersed phase (β) is 80% by mass or less.
[0023] [2] The polypropylene resin composition according to [1], wherein the filler (a2) is an inorganic filler (a2-1).
[0024] [3] The polypropylene resin composition according to [1], wherein the filler (a2) is a natural fiber (a2-2).
[0025] [4] The polypropylene resin composition according to any one of [1] to [3], wherein the propylene-based polymer (a1) is a propylene-ethylene block copolymer having a dispersed phase of ethylene polymer blocks.
[0026] [5] The polypropylene resin composition according to [2] or [4], wherein the inorganic filler (a2-1) is one or more inorganic fillers selected from the group consisting of talc, mica, glass fiber, and calcium carbonate.
[0027] [6] The polypropylene resin composition according to [3] or [4], wherein the natural fiber (a2-2) is one or more natural fibers selected from the group consisting of cellulose fibers, wood powder, and wood powder fibers.
[0028] [7] The polypropylene resin composition according to any one of [1] to [6], wherein the polyolefin (b1) is a propylene homopolymer.
[0029] [8] The polypropylene resin composition according to any one of [1] to [7], wherein the aliphatic polyamide resin (b2) is one or more aliphatic polyamide resins selected from the group consisting of polyamide 6, polyamide 11, polyamide 12, polyamide 612, polyamide 610 and polyamide 1010.
[0030] [9] The polypropylene resin composition as described in any one of [1] to [8], wherein the dispersed phase (β) has a continuous phase (β1) containing the aliphatic polyamide resin (b2) and a finely dispersed phase (β2) containing the modified elastomer (b3) dispersed in the continuous phase (β1).
[0031]
[10] The polypropylene resin composition according to any one of [1] to [9], wherein the content of the propylene polymer composition (a) is 50 to 94.9 parts by mass, the content of the polyolefin composition (b) is 5 to 49.9 parts by mass, and the content of the modified polypropylene (c) is 0.1 to 15 parts by mass (wherein the total content of the propylene polymer composition (a), the polyolefin composition (b), and the modified polypropylene (c) is 100 parts by mass).
[0032]
[11] The polypropylene resin composition as described in any one of [1] to [9], wherein the content of the aforementioned propylene-based polymer composition (a) is 50 to 94.9 parts by mass, the content of the aforementioned polyolefin composition (b) is 5 to 49.9 parts by mass, and the content of the aforementioned modified polypropylene (c) is 0.1 to 5 parts by mass (wherein the total content of the aforementioned propylene-based polymer composition (a), the aforementioned polyolefin composition (b), and the aforementioned modified polypropylene (c) is set to 100 parts by mass).
[0033] Effects of the Invention
[0034] According to the present invention, a polypropylene resin composition having excellent balance between rigidity and impact resistance can be provided, the polypropylene resin composition comprising a propylene-based polymer composition, a polyamide resin, and a modified elastomer, wherein the propylene-based polymer composition contains a filler. DETAILED DESCRIPTION
[0035] Hereinafter, the present invention will be described.
[0036] 《Polypropylene resin composition》
[0037] The polypropylene resin composition of the present invention comprises a propylene polymer composition (a), a polyolefin composition (b), and an acid-modified polypropylene (c).
[0038] <Propylene polymer composition (a)>
[0039] The propylene polymer composition (a) used in the present invention contains a propylene polymer (a1) and a filler (a2).
[0040] [Propylene-based polymer (a1)]
[0041] The propylene-based polymer (a1) is not particularly limited as long as it is a polymer containing a structural unit derived from propylene as a main component (typically, containing a structural unit derived from propylene in an amount of more than 50 mol%), and may be a propylene homopolymer or a copolymer of propylene and an α-olefin other than propylene (hereinafter also referred to as “other α-olefin”) (hereinafter also referred to as “propylene·α-olefin copolymer”). The propylene·α-olefin copolymer may be a propylene·α-olefin block copolymer or a propylene·α-olefin random copolymer.
[0042] Examples of the other α-olefins include ethylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 4-methyl-1-pentene, 2-methyl-1-butene, 3-methyl-1-butene, 3-methyl-1-butene, 3,3-dimethyl-1-butene, 3-methyl-1-pentene, 3-methyl-1-hexene, 3,5,5-trimethyl-1-hexene, and α-olefins having 4 to 20 carbon atoms.
[0043] Among them, as the other α-olefin, ethylene and 1-butene are preferred, and ethylene is more preferred.
[0044] Preferred specific examples of the propylene·α-olefin copolymer include propylene·ethylene copolymer and propylene·1-butene copolymer, and propylene·ethylene copolymer is preferred.
[0045] The propylene-based polymer (a1) is preferably a propylene-ethylene block copolymer having a dispersed phase of an ethylene polymer block, from the viewpoint that the obtained polypropylene resin composition has a better balance between rigidity and impact resistance.
[0046] The monomers used as the raw materials of the propylene-based polymer (a1) may be, for example, monomers derived from fossil fuels, monomers derived from biomass, or both. These monomers may be used alone or in combination of two or more.
[0047] The amount of the decane-soluble portion of the propylene-based polymer (a1) at room temperature (23° C.) is preferably 5% by mass to 30% by mass based on the total mass of the propylene-based polymer (a1).
[0048] The room temperature (23°C) decane soluble portion refers to the components that are soluble in n-decane at 23°C when the propylene polymer (a1) is fractionated using n-decane solvent (hereinafter, also referred to as "decane soluble portion"). In addition, the room temperature (23°C) decane insoluble portion refers to the components that are insoluble in n-decane at 23°C when the propylene polymer (a1) is fractionated using n-decane solvent (hereinafter, also referred to as "decane insoluble portion").
[0049] In addition, the decane-soluble portion amount and the decane-insoluble portion amount can be measured by the following method.
[0050] (Ratio of n-decane soluble (insoluble) components at 23°C)
[0051] About 3 g of propylene polymer, 500 ml of n-decane, and a small amount of heat-resistant stabilizer soluble in n-decane are placed in a glass measuring container. Under a nitrogen atmosphere, the temperature is raised to 150°C within 2 hours while stirring with a stirrer to dissolve the propylene polymer. After maintaining at 150°C for 2 hours, the temperature is slowly cooled to 23°C over 8 hours. The obtained liquid containing the precipitate of the propylene polymer is filtered under reduced pressure using a 25G-4 specification glass filter manufactured by Iwata Glass Co., Ltd. 100 ml of the filtrate is collected and dried under reduced pressure to obtain a portion of the n-decane soluble component. After this operation, the proportion (mass %) of the n-decane soluble component and the proportion (mass %) of the insoluble component at 23°C are determined using the following formula. It should be noted that the mass of the propylene polymer is measured to 10 -4 The unit of g is expressed as b(g) in the following formula. In addition, the mass of a part of the decane-soluble component is measured to 10 -4 The unit is g, and this mass is represented by a(g) in the following formula.
[0052] Ratio of n-decane soluble components at 23°C (mass %) = 100 × (500 × a) / (100 × b)
[0053] Ratio of n-decane insoluble components at 23°C (mass %) = 100 - 100 × (500 × a) / (100 × b)
[0054] Regarding the amount of decane soluble portion, relative to the total mass of the propylene-based polymer (a1), the decane soluble portion is preferably 5 to 30 mass %, more preferably 7 to 25 mass %, further preferably 10 to 20 mass %, and the decane insoluble portion is preferably 70 to 95 mass %, more preferably 75 to 93 mass %, further preferably 80 to 90 mass %.
[0055] When the contents of the decane soluble portion and the decane insoluble portion are within the above ranges, a molded body (eg, an automobile interior material or an automobile exterior material) formed from the composition will have excellent mechanical properties such as rigidity and impact resistance.
[0056] When the propylene-based polymer (a1) is mainly a copolymer, the decane-soluble portion is preferably composed of a propylene-α-olefin copolymer such as a propylene-ethylene random copolymer, and may contain a portion of a propylene homopolymer, for example, byproducts generated during polymerization of low molecular weight products, and the like.
[0057] When the propylene polymer (a1) is a copolymer of the above-mentioned propylene and other α-olefins, the α-olefins of the other α-olefins contained in the decane-soluble part and the propylene·α-olefin copolymer of the decane-soluble part can include ethylene and / or α-olefins having 4 to 12 carbon atoms. As specific examples of such other α-olefins, ethylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, 1-decene and 1-dodecene can be mentioned. Among them, ethylene is preferably used as the other α-olefin.
[0058] The decane-insoluble portion usually contains only structural units derived from propylene, but when the propylene-based polymer (a1) is a copolymer of propylene and other α-olefins, it may contain a small amount, for example, 10 mol% or less, preferably 5 mol% or less, of structural units derived from monomers other than propylene.
[0059] Examples of the monomer other than propylene include α-olefins other than propylene such as ethylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, 1-decene and 1-dodecene.
[0060] Among them, ethylene and α-olefins having 4 to 10 carbon atoms are preferred. These may be copolymerized alone or in combination of two or more.
[0061] The intrinsic viscosity ([η]) of the decane-soluble portion of the propylene-based polymer (a1) measured in decalin at 135°C is preferably 0.1 to 10.0 dl / g, more preferably 1.0 to 9.8 dl / g, further preferably 1.5 to 9.5 dl / g, particularly preferably 2.0 to 9.0 dl / g.
[0062] When the intrinsic viscosity ([η]) of the decane-soluble portion is within the above range, the automotive interior material and automotive exterior material formed from the composition will have a better balance between rigidity and impact resistance.
[0063] When further mechanical properties are required for automobile interior materials and automobile exterior materials formed from the composition, the intrinsic viscosity ([η]) of the decane-soluble portion is preferably 4.0 to 9.0 dl / g, more preferably 4.5 to 8.7 dl / g, and even more preferably 5.0 to 8.4 dl / g.
[0064] The MFR (ASTM D1238, 230°C, 2.16 kg load) of the propylene polymer (a1) is preferably 1 to 200 g / 10 min, more preferably 10 to 100 g / 10 min, further preferably 20 to 70 g / 10 min.
[0065] When the propylene-based polymer (a1) having an MFR within the above range is used, the obtained polypropylene resin composition has a better balance between fluidity and impact resistance.
[0066] [Filler (a2)]
[0067] The filler (a2) is not particularly limited, and various conventionally known inorganic fillers (a2-1), natural fibers (a2-2), and the like can be used without limitation within a range not impairing the effects of the present invention.
[0068] Inorganic fillers (a2-1) are not particularly limited as long as they are fillers formed of inorganic compounds, and for example, known inorganic fillers can be used. Examples of inorganic fillers (a2-1) include carbon black or graphite or carbon black obtained by surface treatment using a silane coupling agent or the like; oxide-based fillers including fine powder silicic acid, silicon dioxide (including fumed silicon dioxide, precipitated silicon dioxide, diatomaceous earth, quartz, etc.), aluminum oxide, iron oxide, ferrite, magnesium oxide, titanium oxide, antimony trioxide, zirconium oxide, barium oxide, and calcium oxide; hydroxide-based fillers including aluminum hydroxide and magnesium hydroxide; silicate-based fillers including aluminum silicate (clay), magnesium silicate (talc), mica, kaolin, calcium silicate, glass fiber, glass flakes, glass beads, etc.; sedimentary rock-based fillers including diatomaceous earth and limestone; and montmorillonite-based fillers including montmorillonite. orillonite), magnesium montmorillonite, iron montmorillonite, iron-magnesium montmorillonite, beidellite, aluminum beidellite, nontronite, aluminum nontronite, saponite (saponite), aluminum saponite, hectorite, sauconite, sphenestone, and bentonite; magnetic fillers including ferrite, iron and cobalt; conductive fillers including silver, gold, copper and their alloys; thermal conductive fillers including aluminum nitride, boron nitride, silicon carbide, etc.; sulfate fillers including aluminum sulfate, magnesium sulfate, barium sulfate, calcium sulfate, etc.; sulfite fillers including calcium sulfite, etc.; carbonate fillers including calcium carbonate, basic magnesium carbonate, dolomite, etc.; titanate fillers including barium titanate, potassium titanate, etc.; and so on.
[0069] From the viewpoint of achieving a better balance between the rigidity and impact resistance of the obtained polypropylene resin composition, the inorganic filler (a2-1) is preferably talc, mica, glass fiber, and calcium carbonate, and more preferably talc.
[0070] These inorganic fillers (a2-1) may be used alone or in combination of two or more.
[0071] From the perspective of making the dispersibility in the propylene polymer composition (a) better, the particle size of the inorganic filler (a2-1) is preferably 0.01 μm to 100 μm, more preferably 0.1 μm to 80 μm, and further preferably 1 μm to 50 μm. The particle size (average particle size) of the inorganic filler is the 50% particle size (d50) obtained from the distribution curve of cumulative % measured by a laser diffraction particle size distribution measuring device.
[0072] As long as the natural fiber (a2-2) can be used as a filler, there is no particular restriction, and for example, known natural fibers can be used. As natural fibers (a2-2), for example, wood powder (wood powder obtained by peeling off the bark of wood and processing it with a pulverizer), wood fiber, bamboo powder, bamboo fiber, cellulose fiber obtained by separation, wool, agricultural product fiber, wood pulp (paper pulp using wood as raw material, which is obtained by mechanical treatment, scientific treatment or composite treatment of the product obtained by directly flaking the bark of the trunk), other natural pulps, rayon, cotton, etc. Examples of the above-mentioned agricultural product fibers include wheat straw, rice straw, hemp, flax, kenaf, kapok, jute, ramie, sisal, Henakun fiber, corn fiber, coconut shell fiber, nut shell, and rice bran, etc. Examples of the above-mentioned wood pulp include NBKP (bleached coniferous wood pulp) and LBKP (bleached kraft pulp of broadleaf trees). Examples of the above-mentioned other natural pulps include Manila hemp, paper mulberry, mit sumata, and wild geese, etc. Among them, wood powder, wood fiber, bamboo, bamboo fiber, cotton, and separated cellulose fibers are preferred, and separated cellulose fibers are more preferred from the viewpoint of suppressing the deviation of the mechanical strength of the molded body and improving the predictability of the strength of the obtained molded body.
[0073] The source of the above-mentioned cellulose fiber is not particularly limited, and can be cellulose fiber obtained from any material such as tree, grass, pulp, and paper. The cellulose fiber obtained from tree can be cellulose fiber obtained from any wood raw material of coniferous trees and broad-leaved trees. The cellulose fiber obtained from grass can be cellulose fiber obtained from non-wood raw materials such as Gramineae, Malvaceae, Leguminosae, and Palmaceae. The cellulose fiber obtained from pulp can be cellulose fiber obtained from any pulp such as cotton linter pulp obtained from the fibers around the seeds of cotton. The cellulose fiber obtained from paper can be cellulose fiber obtained from any paper such as newspaper, corrugated paper, magazine, and high-grade paper. Among them, from the aspect of being easy to obtain and cheap, it is preferably cellulose fiber obtained from tree or grass, and more preferably cellulose fiber obtained from tree.
[0074] From the viewpoint of improving the mechanical strength and impact resistance of the obtained polypropylene resin composition, the average degree of polymerization of the cellulose fibers is preferably 50 to 2000, more preferably 100 to 1500. The average degree of polymerization of the cellulose fibers can be measured by the reduced specific viscosity method using a copper ethylenediamine solution as described in the confirmation test (3) of "Explanation of the Japanese Pharmacopoeia, 15th Revised Edition (published by Hirokawa Shoten)".
[0075] The cellulose fibers may be unmodified or un-amorphized fibers, modified fibers, or amorphized fibers. The modified cellulose fibers may be fibers obtained by reacting ether compounds, alkyl chlorides, alkyl acid anhydrides, alkyl acid chlorides, etc. with hydroxyl groups of cellulose. The amorphized cellulose fibers may be fibers obtained by reducing the crystallinity of cellulose by a known method.
[0076] The cellulose fibers have hydroxyl groups and polar functional groups such as hydroxyl groups, carboxyl groups, amino groups, and quaternary ammonium groups introduced by modification.
[0077] Examples of commercially available products of the cellulose fibers include KC FLOCK GK series ("KC FLOCK" is a registered trademark of the company) which is cellulose fiber manufactured by Nippon Paper Industries, Ltd., and the like.
[0078] These natural fibers (a2-2) may be used alone or in combination of two or more.
[0079] The mass ratio of the propylene polymer (a1) and the filler (a2) contained in the propylene polymer composition (a) (mass of the propylene polymer (a1) / mass of the filler (a2), hereinafter also referred to as "(a1) / (a2)".) is preferably 65 / 35 to 99 / 1. In other words, in the propylene polymer composition (a) of the present invention, when the total amount of the propylene polymer (a1) and the filler (a2) is 100 parts by mass, the content of the propylene polymer (a1) is 65 to 99 parts by mass, and the content of the filler (a2) is 1 to 35 parts by mass.
[0080] From the viewpoint of more ideally exerting the effects of the present invention, the content of the propylene polymer (a1) in the propylene polymer composition (a) is preferably 70 parts by mass or more, more preferably 75 parts by mass or more, and even more preferably 80 parts by mass or more, and is preferably 97 parts by mass or less, more preferably 95 parts by mass or less, and even more preferably 93 parts by mass or less. In particular, when the content of the propylene polymer (a1) in the propylene polymer composition (a) is within the above range, the rigidity of the obtained polypropylene resin composition can be easily further improved, and a significant decrease in impact resistance is unlikely to occur.
[0081] The content of the filler (a2) in the propylene polymer composition (a) is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, further preferably 7 parts by mass or more, and is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, further preferably 20 parts by mass or less.
[0082] Here, when two or more propylene-based polymers (a1) are used, the total amount of the propylene-based polymers (a1) is the above-mentioned "content of the propylene-based polymers (a1)". In addition, when two or more fillers (a2) are used, the total amount of the fillers (a2) is the above-mentioned "content of the filler (a2)".
[0083] The propylene polymer composition (a) may contain, in addition to the propylene polymer (a1) and the filler (a2), additives such as heat stabilizers, antistatic agents, weather stabilizers, light stabilizers, anti-aging agents, antioxidants, fatty acid metal salts, softeners, dispersants, fillers, colorants, lubricants, pigments, etc., as needed within a range that does not impair the effects of the present invention.
[0084] The propylene polymer composition (a) can be produced by mixing the above-mentioned components using a conventionally known method. For example, the propylene polymer (a1), the filler (a2) and the additives included as required can be mixed using a Henschel mixer, a V-type mixer, a ribbon mixer or a tumble mixer, and the obtained mixture is melt-kneaded using an extruder to produce a pelletized propylene polymer composition (a).
[0085] <Polyolefin composition (b)>
[0086] The polyolefin composition (b) used in the present invention comprises a polyolefin (b1), an aliphatic polyamide resin (b2), and a modified elastomer (b3).
[0087] [Polyolefin (b1)]
[0088] The polyolefin (b1) is a homopolymer of α-olefins (including ethylene) such as ethylene, propylene, 1-butene, 4-methyl-1-pentene, etc., a copolymer of the aforementioned α-olefin and other α-olefins, and a copolymer of the aforementioned α-olefin and a monomer other than the α-olefin, and is a polymer with α-olefin as the main component. Specifically, the following ethylene-based polymers, propylene-based polymers, and 1-butene-based polymers can be cited as the above-mentioned polyolefin (b1).
[0089] 〈Ethylene polymers〉
[0090] The above-mentioned ethylene-based polymers are homopolymers of ethylene, copolymers of ethylene and α-olefins having 3 to 20 carbon atoms, and examples thereof include polymers generally referred to as high-density polyethylene (HDPE), medium-density polyethylene (MDPE), low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and ethylene·α-olefin copolymers, which are mainly composed of structural units derived from ethylene (typically, containing more than 50 mol % of structural units derived from ethylene). Specific examples of the α-olefin having 3 to 20 carbon atoms to be copolymerized with ethylene include α-olefin having 4 to 20 carbon atoms such as propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 2-methyl-1-butene, 3-methyl-1-butene, 3,3-dimethyl-1-butene, 3-methyl-1-pentene, and 3-methyl-1-hexene. Among them, α-olefin having 3 to 10 carbon atoms is preferred, α-olefin having 3 to 8 carbon atoms is more preferred, and ethylene, 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene are even more preferred. The molar ratio of ethylene to α-olefin (ethylene / α-olefin) is preferably 99 / 1 to 60 / 40, more preferably 95 / 5 to 70 / 30, and further preferably 90 / 10 to 60 / 25.
[0091] Preferred specific examples of the ethylene·α-olefin copolymer include ethylene·propylene copolymer, ethylene·1-butene copolymer, ethylene·1-hexene copolymer, ethylene·4-methyl-1-pentene copolymer, ethylene·1-octene copolymer, and ethylene·propylene·1-butene copolymer.
[0092] 〈Propylene polymer〉
[0093] The propylene-based polymer is a polymer containing a structural unit derived from propylene as a main component (typically, containing more than 50 mol% of a structural unit derived from propylene) such as a homopolymer of propylene (homopolymer PP), a copolymer of propylene and ethylene and / or an α-olefin having 4 to 20 carbon atoms (random copolymer: random PP), and a composition of a homopolymer of propylene and an ethylene·propylene copolymer (block copolymer: block PP). Specific examples of the α-olefin in the propylene·α-olefin copolymer include ethylene and α-olefins having 4 to 20 carbon atoms such as ethylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 2-methyl-1-butene, 3-methyl-1-butene, 3,3-dimethyl-1-butene, 3-methyl-1-pentene, and 3-methyl-1-hexene. Among them, ethylene and α-olefins having 4 to 10 carbon atoms are preferred, ethylene and α-olefins having 4 to 8 carbon atoms are more preferred, and ethylene, 1-butene, 1-hexene, 4-methyl-1-pentene and 1-octene are even more preferred. The molar ratio of propylene to α-olefin (propylene / α-olefin) is preferably 99 / 1 to 60 / 40, more preferably 95 / 5 to 70 / 30, and even more preferably 90 / 10 to 60 / 25.
[0094] Preferred specific examples of the propylene α-olefin copolymer (random PP) include propylene ethylene copolymer, propylene 1-butene copolymer, propylene 1-hexene copolymer, propylene 4-methyl-1-pentene copolymer, propylene 1-octene copolymer, and propylene ethylene 1-butene copolymer. Among them, propylene ethylene copolymer is particularly preferred.
[0095] In the case where the above-mentioned propylene-based polymer is a propylene·ethylene block copolymer (block PP), the room temperature (23°C) decane-soluble portion of the propylene·ethylene block copolymer is preferably 8% by mass or more and 35% by mass or less, and more preferably 8% by mass or more and 28% by mass or less. In addition, the intrinsic viscosity [η] of the room temperature (23°C) decane-soluble portion measured in 135°C decalin is preferably 1.0 dl / g or more and 10.0 dl / g or less. In addition, the ethylene content (content of structural units derived from ethylene) of the room temperature (23°C) decane-soluble portion is preferably 33 mol% or more and 48 mol% or less, and more preferably 37 mol% or more and 43 mol% or less.
[0096] When the propylene-based polymer is a propylene homopolymer, the melting point is preferably 155 to 170°C, more preferably 158 to 165°C.
[0097] When the propylene-based polymer is a propylene·ethylene random copolymer, the ethylene content of the propylene·ethylene random copolymer is preferably 1.9 to 5.4% by mass, more preferably 2.0 to 4.8% by mass. In addition, the crystalline melting point of the propylene·ethylene random copolymer measured by a differential scanning calorimeter (DSC) in accordance with JIS K7121 is usually preferably 130 to 150° C., more preferably 130 to 145° C., and particularly preferably 135 to 145° C.
[0098] The propylene-ethylene block copolymer and the propylene-ethylene random copolymer may be used alone or in combination of two or more copolymers. For example, two or more copolymers may be mixed in order to adjust the MFR.
[0099] 〈1-Butene polymer〉
[0100] The 1-butene-based polymers are polymers containing structural units derived from 1-butene as the main component (typically, containing more than 50 mol % of structural units derived from 1-butene), such as homopolymers of 1-butene (polybutene) and copolymers of 1-butene with ethylene, propylene and α-olefins having 5 to 20 carbon atoms (1-butene·α-olefin copolymers).
[0101] Among these polyolefins (b1), from the viewpoint that the obtained polypropylene resin composition has a better balance between rigidity and impact resistance, a propylene-based polymer is preferred, and a propylene homopolymer is more preferred.
[0102] The polyolefin (b1) may be used alone or as a mixture of two or more copolymers.
[0103] The MFR (ASTM D1238, 230°C, 2.16 kg load) of the polyolefin (b1) is preferably 1 to 200 g / 10 min, more preferably 5 to 100 g / 10 min, further preferably 10 to 70 g / 10 min.
[0104] When a polyolefin (b1) having an MFR within the above range is used, the phase structure of the polyolefin composition (b) described below can be easily formed, and the obtained polypropylene resin composition can have a better balance between rigidity and impact resistance.
[0105] Monomers used as raw materials of the polyolefin (b1) may be, for example, monomers derived from fossil fuels, monomers derived from biomass, or both. These monomers may be used alone or in combination of two or more.
[0106] [Aliphatic polyamide resin (b2)]
[0107] The aliphatic polyamide resin (b2) is not particularly limited, and various aliphatic polyamide resins known in the past can be used without restriction within the scope of not damaging the effect of the present invention. For example, an aliphatic polyamide resin that can be melt-molded by the polycondensation reaction of amino acid lactam or diamine and dicarboxylic acid can be used. As a specific example of the aliphatic polyamide resin (b2), the following resins can be cited.
[0108] (1) Polycondensates of an organic dicarboxylic acid having 4 to 12 carbon atoms and an organic diamine having 2 to 13 carbon atoms, for example, polyhexamethylenediamine adipamide [polyamide 66] which is a polycondensate of hexamethylenediamine and adipic acid, polyhexamethylenediamine azelaic acid [polyamide 69] which is a polycondensate of hexamethylenediamine and sebacic acid, polyhexamethylenediamine sebacamide [polyamide 610] which is a polycondensate of hexamethylenediamine and sebacic acid, polyhexamethylenediamine dodecanediacid [polyamide 612] which is a polycondensate of hexamethylenediamine and dodecanedioic acid, and a polycondensate of a diamine having 10 carbon atoms (1,10-decanediamine (decamethylenediamine) made from castor oil) and a dicarboxylic acid having 10 carbon atoms (sebacic acid) [polyamide 1010].
[0109] Examples of the organic dicarboxylic acids include adipic acid, pimelic acid, suberic acid, sebacic acid, and dodecanedioic acid. Examples of the organic diamines include hexamethylenediamine, octamethylenediamine, nonanediamine, octanediamine, decanediamine, undecanediamine, and dodecanediamine.
[0110] (2) Polycondensates of ω-amino acids, for example, polyundecanoic acid, which is a polycondensate of ω-aminoundecanoic acid (polyamide 11).
[0111] (3) Ring-opening polymers of lactams, for example, polycaprolactam [polyamide 6] which is a ring-opening polymer of ε-aminocaprolactam, and polylaurolactam [polyamide 12] which is a ring-opening polymer of ε-aminolaurolactam.
[0112] Among the aliphatic polyamide resins (b2), polyamide 6, polyamide 11, polyamide 12, polyamide 612, polyamide 610 and polyamide 1010 are preferred from the viewpoint of providing a polypropylene resin composition with a better balance between rigidity and impact resistance.
[0113] The aliphatic polyamide resin (b2) can be used alone or in combination of two or more. The raw material of the aliphatic polyamide resin (b2) can be any raw material from a raw material from fossil fuels or a raw material from biomass. In addition, the raw material from fossil fuels and the raw material from biomass can also be used in combination.
[0114] The melt volume rate (MVR) of the aliphatic polyamide resin (b2) measured at 275°C and a load of 2.16 kg is preferably 50 to 300 cm 3 / 10min, more preferably 100-250cm 3 / 10min, particularly preferably 125 to 200cm 3 By using such an aliphatic polyamide resin, the impact resistance inherent in the polyamide resin tends to be fully exhibited, and even if it is mixed with the modified elastomer (b3) and used, the impact resistance is not greatly impaired.
[0115] [Modified elastomer (b3)]
[0116] The modified elastomer (b3) is an elastomer obtained by adding a portion containing a group reactive with the aliphatic polyamide resin (b2) to an unmodified elastomer (b3′).
[0117] The unmodified elastomer (b3') serving as a raw material for the modified elastomer (b3) is an olefin-based thermoplastic elastomer (b3'-1) comprising a structural unit derived from ethylene and a structural unit derived from an α-olefin having 3 to 8 carbon atoms, or a styrene-based thermoplastic elastomer (b3'-2) comprising a structural unit derived from a styrene-based compound.
[0118] The olefin-based thermoplastic elastomer (b3'-1) is an elastomer comprising structural units derived from ethylene and structural units derived from an α-olefin having 3 to 8 carbon atoms, and is an elastomer comprising structural units derived from ethylene in an amount of preferably 75 to 95 mol%, more preferably 75 to 90 mol%, and structural units derived from an α-olefin having 3 to 8 carbon atoms in an amount of preferably 5 to 25 mol%, more preferably 10 to 25 mol%.
[0119] Examples of the α-olefins having 3 to 8 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, and 1-octene. Among these α-olefins having 3 to 8 carbon atoms, 1-butene, 1-hexene, and 1-octene are preferred.
[0120] The α-olefins having 3 to 8 carbon atoms may be used alone or in combination of two or more.
[0121] Ethylene and α-olefin having 3 to 8 carbon atoms as monomers constituting the olefin-based thermoplastic elastomer (b3′-1) may be, for example, monomers derived from fossil fuels and / or monomers derived from biomass, and these monomers may be used alone or in combination of two or more.
[0122] The content of the structural unit derived from the α-olefin having 3 to 8 carbon atoms in the olefin-based thermoplastic elastomer (b3'-1) is preferably 5 to 25 mol%, more preferably 10 to 25 mol%, further preferably 11 to 22 mol%, and particularly preferably 12 to 20 mol%. If the content of the structural unit derived from the α-olefin having 3 to 8 carbon atoms is within the above range, a modified elastomer having good flexibility and easy handling can be obtained. In addition, a polypropylene resin composition having excellent impact resistance can be obtained.
[0123] The melt flow rate (MFR) of the olefin-based thermoplastic elastomer (b3'-1) measured at 230°C and a load of 2.16 kg is preferably 0.1 to 30 g / 10 minutes, more preferably 0.3 to 20 g / 10 minutes, and further preferably 0.5 to 10 (g / 10 minutes). If the melt flow rate is within the above range, the miscibility of the modified elastomer (b3) obtained by adding a reactive group to the olefin-based thermoplastic elastomer (b3'-1) and the aliphatic polyamide resin (b2) becomes good, and a polypropylene resin composition excellent in impact resistance can be obtained.
[0124] The olefin-based thermoplastic elastomer (b3'-1) can be prepared, for example, by randomly copolymerizing ethylene and an α-olefin having 3 to 8 carbon atoms in the presence of a vanadium-based catalyst formed by a soluble vanadium compound and an alkylaluminum halide compound, or a zirconium-based catalyst formed by a zirconium metallocene compound and an organic aluminum oxide compound.
[0125] Examples of the styrene-based thermoplastic elastomer (b3′-2) include block copolymers of a styrene-based compound and a conjugated diene compound, and hydrogenated products thereof.
[0126] Examples of the styrene-based compound include styrene, alkyl styrenes such as α-methylstyrene, p-methylstyrene and p-tert-butylstyrene, p-methoxystyrene and vinylnaphthalene.
[0127] These styrene compounds may be used alone or in combination of two or more.
[0128] Examples of the conjugated diene compound include butadiene, isoprene, piperylene, methylpentadiene, phenylbutadiene, 3,4-dimethyl-1,3-hexadiene, and 4,5-diethyl-1,3-octadiene.
[0129] These conjugated diene compounds may be used alone or in combination of two or more.
[0130] Specific examples of the styrene-based thermoplastic elastomer (b3'-2) include styrene-butadiene-styrene copolymers (SBS), styrene-isoprene-styrene copolymers (SIS), styrene-ethylene / butylene-styrene copolymers (SEBS), and styrene-ethylene / propylene-styrene copolymers (SEPS). Among these styrene-based thermoplastic elastomers (b3'-2), SEBS is preferred.
[0131] These styrene-based thermoplastic elastomers (b3′-2) may be used alone or in combination of two or more.
[0132] As the group reactive with the aliphatic polyamide resin (b2) (the group reactive with the aliphatic polyamide resin (b2) contained in the modified elastomer (b3), hereinafter also referred to as the "reactive group"), there can be mentioned an acid anhydride group (-CO-O-OC-), a carboxyl group (-COOH) and an epoxy group {-COC- (a three-membered ring structure formed by 2 carbon atoms and 1 oxygen atom)}, an oxazoline group (-C3H4NO) and an isocyanate group (-NCO) and the like.
[0133] The modified elastomer (b3) may contain only one kind of these reactive groups or two or more kinds thereof.
[0134] The amount of graft modification in the modified elastomer (b3) (the content of the portion derived from the monomer containing a reactive group) is not particularly limited as long as the effect of the present invention is achieved, but is preferably 0.1 to 5% by mass, more preferably 0.5 to 2% by mass, and still more preferably 0.8 to 1.4% by mass, relative to the mass of the modified elastomer (b3).
[0135] There is no particular limitation on the method for adding a portion containing a reactive group to the unmodified elastomer (b3'). Examples include a method of adding a reactive group by subjecting a specific group contained in the unmodified elastomer (b3') to a chemical reaction (for example, when a carbon-carbon double bond exists in the unmodified elastomer (b3'), an epoxy group is introduced by oxidizing the carbon-carbon double bond), a method of adding a monomer containing a reactive group to the unmodified elastomer (b3') by graft modification, and the like.
[0136] Examples of the reactive group-containing monomer used for graft modification include a monomer having a polymerizable unsaturated bond and an acid anhydride group, a monomer having a polymerizable unsaturated bond and a carboxyl group, and a monomer having a polymerizable unsaturated bond and an epoxy group.
[0137] Specific examples include acid anhydrides such as maleic anhydride, itaconic anhydride, succinic anhydride, glutaric anhydride, adipic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, butenylsuccinic anhydride; and carboxylic acids such as maleic acid, itaconic acid, fumaric acid, acrylic acid, and methacrylic acid.
[0138] Among these reactive group-containing monomers, acid anhydrides are preferred, maleic anhydride and itaconic anhydride are more preferred, and maleic anhydride is further preferred.
[0139] These reactive group-containing monomers may be used alone or in combination of two or more.
[0140] The reactive group-containing monomer used in the graft modification (eg, maleic acid or its anhydride) may be a fossil fuel-derived monomer (monomer), a biomass-derived monomer, or a combination of a fossil fuel-derived monomer and a biomass-derived monomer.
[0141] When the modified elastomer (b3) is prepared by graft-modifying the unmodified elastomer (b3') and adding a monomer containing a reactive group, the graft modification amount of the modified elastomer (b3) is preferably 0.1 to 5% by mass, more preferably 0.5 to 2% by mass, and further preferably 0.8 to 1.4% by mass. If the modification amount is too small, the impact resistance of the obtained polypropylene resin composition may be reduced. If the modification amount is too large, foreign matter such as gel may be mixed into the modified elastomer (b3).
[0142] When the modified elastomer (b3) is produced by graft modification, it can be produced, for example, by graft-modifying the unmodified elastomer (b3') with the above-mentioned carboxylic acid (eg maleic acid) or anhydride (eg maleic anhydride) in the presence of a radical initiator.
[0143] The amount of the carboxylic acid or the acid anhydride added is usually 0.010 to 15 parts by mass, preferably 0.010 to 5.0 parts by mass, based on 100 parts by mass of the unmodified elastomer (b3').
[0144] The amount of the radical initiator used is usually 0.0010 to 1.0 part by mass, preferably 0.0010 to 0.30 part by mass, based on 100 parts by mass of the unmodified elastomer (b3').
[0145] As the free radical initiator, for example, an organic peroxide, an azo compound or a metal hydride can be used. The free radical initiator can also be directly mixed with a carboxylic acid or anhydride, and an unmodified elastomer (b3') and the like, or can be used after being dissolved in a small amount of an organic solvent. As the organic solvent, an organic solvent that can dissolve the free radical initiator can be used.
[0146] The graft modification based on carboxylic acid or anhydride can be carried out by a conventionally known method. For example, the unmodified elastomer (b3') can be dissolved in an organic solvent, and then the carboxylic acid or anhydride and a free radical initiator are added to the solution, and the reaction is carried out at a temperature of 70 to 200°C, preferably 80 to 190°C, for 0.5 to 15 hours, preferably 1 to 10 hours, thereby preparing the modified elastomer (b3) through graft modification.
[0147] Alternatively, the modified elastomer (b3) can be produced by reacting a carboxylic acid or anhydride with an unmodified elastomer (b3') in the presence of a free radical initiator under solvent-free conditions using an extruder, etc. The reaction is preferably carried out for 0.5 to 10 minutes at a temperature above the temperature at which the unmodified elastomer (b3') becomes molten.
[0148] The modified elastomer (b3) has a melt flow rate (MFR) of 0.1 to 50 g / 10 min, preferably 0.5 to 10 g / 10 min, as measured at 230°C and under a load of 2.16 kg. When the MFR is within this range, the obtained polypropylene resin composition has excellent impact resistance.
[0149] [Phase structure of polyolefin composition (b)]
[0150] The polyolefin composition (b) comprises a continuous phase (α) containing a polyolefin (b1), and a dispersed phase (β) containing an aliphatic polyamide resin (b2) and a modified elastomer (b3) dispersed in the continuous phase (α), wherein the dispersed phase (β) is formed by a melt-kneaded product of the aliphatic polyamide resin (b2) and the modified elastomer (b3).
[0151] Since the polyolefin composition (b) having such a phase structure is included in the polypropylene resin composition, a polypropylene resin composition having a better balance between rigidity and impact resistance can be obtained.
[0152] The dispersed phase (β) preferably has a continuous phase (β1) containing the aliphatic polyamide resin (b2) and a finely dispersed phase (β2) containing the modified elastomer (b3) dispersed in the continuous phase (β1). By making the dispersed phase (β) have such a phase structure, a polypropylene resin composition with better impact resistance can be obtained.
[0153] In addition, in the polyolefin composition (b), when a propylene-ethylene block copolymer having a dispersed phase of an ethylene block is used as the propylene-based polymer (a1) contained in the propylene-based polymer composition (a), at least a portion of the ethylene block can be agglomerated at the interface between the continuous phase (α) and the dispersed phase (β). By having such a phase structure, there is a tendency that the impact resistance of the obtained polypropylene resin composition is more excellent.
[0154] The size of the dispersed phase (β) in the continuous phase (α) of the polyolefin composition (b) is not particularly limited as long as the effect of the present invention is achieved, and its average diameter (average particle diameter) is preferably 10000 nm or less, more preferably 50 nm or more and 8000 nm or less, and further preferably 100 nm or more and 4000 nm or less. The average diameter of the dispersed phase (β) is the average value (nm) of the maximum lengths of 50 randomly selected dispersed phases (β) in an image obtained by electron microscope observation.
[0155] When the dispersed phase (β) of the polyolefin composition (b) comprises the continuous phase (β1) and the finely dispersed phase (β2) dispersed in the continuous phase (β1), the size of the finely dispersed phase (β2) is not particularly limited as long as the effect of the present invention is achieved, and the average diameter (average particle diameter) is preferably 5 nm to 1000 nm, more preferably 5 nm to 600 nm, further preferably 10 nm to 400 nm, and particularly preferably 15 nm to 350 nm. The average diameter of the finely dispersed phase (β2) is the average value (nm) of the maximum lengths of 100 finely dispersed phases (β2) randomly selected from an image obtained using an electron microscope.
[0156] In the polyolefin composition (b), when the total of the continuous phase (α) and the dispersed phase (β) is 100 mass %, the dispersed phase (β) is preferably 80 mass % or less. b1 The total amount of the aliphatic polyamide resin (b2) and the modified elastomer (b3) is W b2+b3 In the case of W b1 With W b2+b3 When the total of W is set to 100 mass %, b2+b3 The ratio of is preferably 80% by mass or less (usually 0.5% by mass or more). By setting it to the above-mentioned range of the amount ratio, the impact resistance, rigidity and moldability of the obtained polypropylene resin composition can be made more excellent. From this viewpoint, the above-mentioned ratio is preferably 5% by mass or more and 78% by mass or less, more preferably 10% by mass or more and 77% by mass or less, further preferably 23% by mass or more and 76% by mass or less, further preferably 30% by mass or more and 75% by mass or less, particularly preferably 33% by mass or more and 72% by mass or less, more particularly preferably 35% by mass or more and 67% by mass or less, and particularly preferably 37% by mass or more and 63% by mass or less.
[0157] When the total of aliphatic polyamide resin (b2) and modified elastomer (b3) is set to 100% by mass, the content ratio of aliphatic polyamide resin (b2) is preferably 10% by mass or more and 80% by mass or less. By making the content ratio of aliphatic polyamide resin (b2) be this range, it is easy to form a phase structure in which polyolefin (b1) is a continuous phase (α) and the phase containing aliphatic polyamide resin (b2) is a dispersed phase (β). Thus, it is easy to obtain a polypropylene resin composition with excellent impact resistance and excellent rigidity. From this viewpoint, the content ratio of aliphatic polyamide resin (b2) is preferably 12% by mass or more and 78% by mass or less, more preferably 14% by mass or more and 75% by mass or less, further preferably 25% by mass or more and 73% by mass or less, further preferably 30% by mass or more and 71% by mass or less, particularly preferably 34% by mass or more and 68% by mass or less, and more particularly preferably 40% by mass or more and 64% by mass or less. By making the content ratio of the aliphatic polyamide resin (b2) within the above range, the dispersed phase (β) obtained from the aliphatic polyamide resin (b2) and the modified elastomer (b3) can be dispersed more finely. In addition, the amount of the aliphatic polyamide resin (b2) with a large specific gravity can be reduced, and the specific gravity of the polypropylene resin composition can be reduced. Thus, a lightweight polypropylene resin composition having excellent impact resistance and rigidity can be obtained.
[0158] The polyolefin composition (b) used in the present invention can be produced, for example, as follows. First, the aliphatic polyamide resin (b2) and the modified elastomer (b3) are melt-kneaded in a manner such as the above-mentioned content ratio to produce their melt-kneaded product. The obtained melt-kneaded product of the aliphatic polyamide resin (b2) and the modified elastomer (b3) is melt-kneaded with a polyolefin (b1) in a manner such as the above-mentioned content ratio to produce a polyolefin composition (b).
[0159] The melt-kneading method is not particularly limited, and for example, a method of melt-kneading the components using a mixing device such as an extruder (single-screw extruder, twin-screw extruder, etc.), a kneader, and a mixer (high-speed flow mixer, paddle mixer, ribbon mixer, etc.) can be cited. These devices can be used alone or in combination of two or more. In addition, when the polyolefin composition (b) is produced by melt-kneading, the melt-kneaded product can be produced by melt-kneading the aliphatic polyamide resin (b2) and the modified elastomer (b3), and then the melt-kneaded product and the polyolefin (b1) are continuously kneaded to produce the polyolefin composition (b); or, the melt-kneaded product can be produced by melt-kneading the aliphatic polyamide resin (b2) and the modified elastomer (b3), for example, after temporarily producing pellets of the melt-kneaded product, the pellets of the melt-kneaded product are melt-kneaded with the polyolefin (b1), thereby producing the polyolefin composition (b). In the melt-kneading, the components may be added all at once and melt-kneaded, or may be added in multiple portions and melt-kneaded.
[0160] The melt kneading temperature can be appropriately set depending on the type of resin used, etc., but is preferably kneaded in a molten state, and is usually 190 to 350°C, preferably 200 to 330°C, and more preferably 205 to 310°C.
[0161] <Acid-modified polypropylene (c)>
[0162] Acid-modified polypropylene (c) is an acid-modified product of unmodified polypropylene. Acid-modified polypropylene (c) can be obtained by acid-modifying unmodified polypropylene using a compound selected from unsaturated carboxylic acids and their derivatives, and preferably can be obtained by modifying unmodified polypropylene using maleic acid or its anhydride. Acid-modified polypropylene (c) can be prepared by using one unmodified polypropylene alone, or by using two or more unmodified polypropylenes in combination. Regarding the monomers used as the raw materials of the acid-modified polypropylene (c), for example, monomers from fossil fuels can be used, monomers from biomass can be used, or monomers from fossil fuels and monomers from biomass can be used. These monomers can be used alone or in combination.
[0163] The acid-modified polypropylene (c) can be produced, for example, by graft-modifying unmodified polypropylene with a compound selected from unsaturated carboxylic acids and derivatives thereof. When the acid-modified polypropylene (c) is produced by graft modification, it can be produced, for example, by graft-modifying unmodified polypropylene with an unsaturated carboxylic acid (e.g., maleic acid) or an unsaturated carboxylic acid derivative (e.g., anhydride such as maleic anhydride) in the presence of a free radical initiator. The conditions for graft modification are the same as those for producing the modified elastomer (b3) by graft modification.
[0164] Examples of the free radical initiator that can be used when producing the acid-modified polypropylene (c) by graft modification include 1,1-di(tert-butylperoxy)cyclohexane, 2,2-di(4,4-di(tert-butylperoxy)cyclohexyl)propane, tert-hexyl peroxyisopropyl monocarbonate, tert-butyl peroxymaleate, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxylaurate, tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy-2-ethylhexyl monocarbonate, tert-hexyl peroxybenzoate, 2,5 -dimethyl-2,5-di(benzoylperoxy)hexane, tert-butyl peroxyacetate, 2,2-di(tert-butylperoxy)butane, tert-butyl peroxybenzoate, n-butyl 4,4-di(tert-butylperoxy)valerate, di(2-tert-butylperoxyisopropyl)benzene, diisopropylbenzene peroxide, di-tert-hexyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, tert-butylcumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane. Among them, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane is preferred.
[0165] The acid-modified polypropylene (c) preferably satisfies at least one of the following requirements (ci) and (c-ii), and more preferably satisfies both of the following requirements (ci) and (c-ii).
[0166] Requirements (ci)
[0167] The melt flow rate (MFR) of the acid-modified polypropylene (c) at 230°C and a load of 2.16 kg is in the range of 100 to 300 g / 10 minutes. The melt flow rate of the acid-modified polypropylene (c) can be measured under the conditions of 230°C and a load of 2.16 kg in accordance with ASTM D1238. The melt flow rate of the acid-modified polypropylene (c) is preferably in the range of 120 to 280 g / 10 minutes, more preferably in the range of 140 to 260 g / 10 minutes, and further preferably in the range of 160 to 240 g / 10 minutes. When the melt flow rate of the acid-modified polypropylene (c) is in the above range, there is a tendency that the strength of the obtained polypropylene resin composition is more excellent.
[0168] Requirement (c-ii)
[0169] Density: 895~920kg / m 3 The density of the acid-modified polypropylene (c) can be measured according to ASTM D1505.
[0170] The density of the acid-modified polyolefin (c) is preferably 896 to 915 kg / m 3 The range is more preferably 897 to 910 kg / m 3 range.
[0171] When the density of the acid-modified polyolefin (c) is within the above range, the pellets of the acid-modified polyolefin (c) are excellent in handleability and there is a tendency that a decrease in the rigidity of the obtained polypropylene resin composition can be further suppressed.
[0172] The polypropylene resin composition of the present invention may further contain the following ethylene-based copolymer (d).
[0173] <Ethylene copolymer (d)>
[0174] The ethylene-based copolymer (d) is a copolymer consisting only of ethylene and an α-olefin having 3 to 20 carbon atoms, and is preferably a copolymer of ethylene and an α-olefin having 3 to 10 carbon atoms. That is, the ethylene-based copolymer (d) according to the present invention is a copolymer consisting of a structural unit derived from ethylene and a structural unit derived from an α-olefin having 3 to 20 carbon atoms.
[0175] As for the α-olefin having 3 to 20 carbon atoms as a copolymer component, for example, propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, etc. can be mentioned. The α-olefin having 3 to 20 carbon atoms is preferably an α-olefin having 3 to 10 carbon atoms. The α-olefin having 3 to 20 carbon atoms as a copolymer component can be used alone or in combination of two or more.
[0176] Ethylene and α-olefin having 3 to 20 carbon atoms as monomers constituting the ethylene-based copolymer (d) may be, for example, monomers derived from fossil fuels and / or monomers derived from biomass, and these monomers may be used alone or in combination of two or more.
[0177] Among them, the ethylene-1-butene copolymer is particularly preferred as the ethylene-based copolymer (d).
[0178] The type of α-olefin constituting the ethylene copolymer (d) is determined by the type of comonomer used in the production of the ethylene copolymer (d). For example, the type of α-olefin in the ethylene copolymer can be determined by uniformly dissolving about 200 mg of the ethylene copolymer in 1 ml of hexachlorobutadiene in a 10 mmφ test tube to obtain a sample, and measuring the α-olefin of the sample under the measurement conditions of a temperature of 120°C, a frequency of 25.05 MHz, a spectrum width of 1500 Hz, a pulse repetition time of 4.2 seconds, and a 45° pulse width of 6 μsec. 13 C-NMR spectroscopy and identification.
[0179] The content of the structural units derived from ethylene in the above-mentioned ethylene-based copolymer (d) (ethylene content) is not particularly limited, and is generally in the range of 50 to 99 mol%, preferably 60 to 98 mol%, and more preferably 75 to 97 mol% of the total structural units of the ethylene-based copolymer (d). In addition, the content of the structural units derived from α-olefins having 3 to 20 carbon atoms (α-olefin content) in the ethylene-based copolymer (d) is generally in the range of 1 to 50 mol%, preferably 2 to 40 mol%, and more preferably 3 to 25 mol% of the total structural units of the ethylene-based copolymer (d).
[0180] The ethylene-based copolymer (d) preferably satisfies at least one of the following requirements (di) and (d-ii), and more preferably satisfies both of the following requirements (di) and (d-ii).
[0181] (di) Melt flow rate
[0182] The melt flow rate (MFR) of the ethylene copolymer (d) measured at 190°C and 2.16 kg load is 0.1 to 50 g / 10 minutes. The melt flow rate (MFR) of the ethylene copolymer (d) can be measured at 190°C and 2.16 kg load according to ASTM D1238. The melt flow rate of the ethylene copolymer (d) is preferably in the range of 0.2 to 25 g / 10 minutes, more preferably in the range of 0.3 to 10 g / 10 minutes. If the melt flow rate of the ethylene copolymer (d) is within the above range, the strength of the obtained polypropylene resin composition is easily increased, there is a tendency for good dispersibility in the polypropylene resin composition, and the impact resistance of the obtained polypropylene resin composition is more excellent.
[0183] (d-ii) Density
[0184] The density of the ethylene copolymer (d) is 850 to 890 kg / m 3 The density of the ethylene copolymer (d) can be measured according to ASTM D1505. The density of the ethylene copolymer (d) is preferably 853 to 880 kg / m3 , more preferably 855 to 870 kg / m 3 When the density of the ethylene copolymer (d) is within the above range, the pellets of the ethylene copolymer (d) are more easily handled and the impact resistance of the polypropylene resin composition at room temperature and low temperature is also more excellent.
[0185] When the polypropylene resin composition of the present invention contains the ethylene copolymer (d), when the total content of the propylene polymer composition (a), the polyolefin composition (b), the modified polypropylene (c), and the ethylene copolymer (d) is set to 100 parts by mass, it is preferred that the content of the propylene polymer composition (a) is 50 to 89.9 parts by mass, the content of the polyolefin composition (b) is 5 to 44.9 parts by mass, the content of the modified polypropylene (c) is 0.1 to 15 parts by mass, and the content of the ethylene copolymer (d) is 5 to 30 parts by mass; more preferably, Preferably, the content of the propylene polymer composition (a) is 55 to 85.5 parts by mass, the content of the polyolefin composition (b) is 8 to 30 parts by mass, the content of the modified polypropylene (c) is 1 to 12 parts by mass, and the content of the ethylene copolymer (d) is 5 to 25 parts by mass; more preferably, the content of the propylene polymer composition (a) is 60 to 80 parts by mass, the content of the polyolefin composition (b) is 10 to 25 parts by mass, the content of the modified polypropylene (c) is 2.5 to 11 parts by mass, and the content of the ethylene copolymer (d) is 8 to 20 parts by mass. By including each component in such a mixing ratio, there is a tendency that the obtained polypropylene resin composition has a better balance between rigidity and heat resistance.
[0186] When the polypropylene resin composition of the present invention contains an ethylene copolymer (d), when the total content of the propylene polymer composition (a), the polyolefin composition (b), the modified polypropylene (c), and the ethylene copolymer (d) is 100 parts by mass, it is preferred that the content of the propylene polymer composition (a) is 50 to 89.9 parts by mass, the content of the polyolefin composition (b) is 5 to 44.9 parts by mass, the content of the modified polypropylene (c) is 0.1 to 5 parts by mass, and the content of the ethylene copolymer (d) is 5 to 30 parts by mass. Parts; more preferably, the content of the propylene polymer composition (a) is 55 to 85 parts by mass, the content of the polyolefin composition (b) is 8 to 30 parts by mass, the content of the modified polypropylene (c) is 0.5 to 4 parts by mass, and the content of the ethylene copolymer (d) is 5 to 25 parts by mass; further preferably, the content of the propylene polymer composition (a) is 60 to 80 parts by mass, the content of the polyolefin composition (b) is 10 to 25 parts by mass, the content of the modified polypropylene (c) is 1 to 3 parts by mass, and the content of the ethylene copolymer (d) is 8 to 20 parts by mass. By including each component in such a mixing ratio, there is a tendency that the obtained polypropylene resin composition has a better balance between rigidity and impact resistance.
[0187] In the polypropylene resin composition of the present invention, in addition to the propylene polymer composition (a), the polyolefin composition (b), and the acid-modified polypropylene (c), other polymers such as the above-mentioned ethylene copolymer (d) may be included within the scope that does not impair the effect of the present invention. Other polymers may be used alone or in combination of two or more.
[0188] In addition, the polypropylene resin composition of the present invention may contain additives within a range that does not impair the effects of the present invention. Examples of the additives include flame retardants, flame retardant aids, fillers, colorants, antibacterial agents, antistatic agents, etc. The additives may be used alone or in combination of two or more.
[0189] In the polypropylene resin composition of the present invention, the propylene polymer (a1) contained in the propylene polymer composition (a), the polyolefin (b1) contained in the polyolefin composition (b), and the acid-modified polypropylene (c) are integrated to form a continuous phase (α').
[0190] In addition, usually, the filler (a2) and the dispersed phase (β) composed of the polyolefin composition (b) are dispersed in the continuous phase (α').
[0191] In addition, in the polyolefin composition (b), when the dispersed phase (β) has a continuous phase (β1) containing an aliphatic polyamide resin (b2) and a finely dispersed phase (β2) containing a modified elastomer (b3) dispersed in the continuous phase (β1), the dispersed phase (β) is usually dispersed in the continuous phase (α') in a state where the continuous phase (β1) and the finely dispersed phase (β2) dispersed in the continuous phase (β1) are formed in the dispersed phase (β). By having such a multiple dispersed phase structure, a polypropylene resin composition having better impact resistance can be obtained.
[0192] In addition, when a propylene-ethylene block copolymer having a dispersed phase of an ethylene polymer block is used as the propylene-based polymer (a1), at least a portion of the ethylene polymer block contained in the block copolymer can be agglomerated at the interface between the continuous phase (α') and the dispersed phase (β). By having such a phase structure, a polypropylene resin composition having more excellent impact resistance can be obtained.
[0193] The size of the dispersed phase (β) contained in the continuous phase (α') of the polypropylene resin composition is not particularly limited as long as the effects of the present invention are achieved, and is generally the same as the preferred embodiment of the size of the dispersed phase (β) of the polyolefin composition (b).
[0194] When a finely dispersed phase (β2) is formed in the dispersed phase (β) of the polypropylene resin composition of the present invention, its size is not particularly limited as long as the effects of the present invention are achieved, and is generally the same as the preferred embodiment of the size of the finely dispersed phase (β2) of the above-mentioned polyolefin composition (b).
[0195] In the polypropylene resin composition of the present invention, it is considered that the acid-modified polypropylene (c) is locally present around the filler (a2). On the other hand, in the polypropylene resin composition not containing the acid-modified polypropylene (c), there is a tendency that the dispersed phase (β) in the polyolefin composition (b) is locally present around the filler (a2). Due to such a difference in phase structure, the polypropylene resin composition of the present invention can obtain a polypropylene resin composition having more excellent rigidity than the polypropylene resin composition not containing the acid-modified polypropylene (c).
[0196] In the case of including ethylene copolymer (d) in the polypropylene resin composition of the present invention, it is preferred that the ethylene copolymer (d) forms a dispersed phase (γ) in the continuous phase (α'). The dispersed phase (γ) can be formed. By forming this phase structure, there is a tendency that the rigidity and impact resistance of the obtained polypropylene resin composition are more excellent in balance. In the case of forming a dispersed phase (γ) of an ethylene copolymer (d) in the polypropylene resin composition of the present invention, the size of the dispersed phase (γ) is not particularly limited as long as the effect of the present invention is achieved, and its average diameter (average particle size) is preferably 100nm or more and 1000nm or less, more preferably 100nm or more and 500nm or less, and further preferably 100nm or more and 300nm or less. The average diameter of the dispersed phase (γ) is the average value (nm) of the maximum length of 100 micro-dispersed phases (γ) randomly selected in the image obtained using an electron microscope.
[0197] In the polypropylene resin composition of the present invention, when the total amount of the continuous phase (α') and the dispersed phase (β) is 100 mass %, the dispersed phase (β) is 80 mass % or less. Therefore, usually, when the total amount of the propylene polymer (a1) and the polyolefin (b1) is W a1+b1 The total amount of the aliphatic polyamide resin (b2) and the modified elastomer (b3) is W b2+b3 In the case of W a1+b1 With W b2+b3 For a total of 100 mass %, W b2+b3 The ratio of is 80% by mass or less (usually 0.5% by mass or more). By setting it to the above-mentioned range of the amount ratio, the impact resistance, rigidity and moldability of the obtained polypropylene resin composition can be made more excellent. From this viewpoint, the above-mentioned ratio is preferably 1% by mass or more and 78% by mass or less, more preferably 3% by mass or more and 77% by mass or less, further preferably 5% by mass or more and 76% by mass or less, further preferably 8% by mass or more and 75% by mass or less, particularly preferably 10% by mass or more and 72% by mass or less, more particularly preferably 15% by mass or more and 67% by mass or less, and particularly preferably 25% by mass or more and 63% by mass or less.
[0198] In the polypropylene resin composition of the present invention, the content ratios of the propylene-based polymer (a1) and the polyolefin (b1) are not particularly limited as long as the effects of the present invention are achieved. The content ratio of the polyolefin (b1) is usually 80% by mass or less, preferably 1% by mass or more and 60% by mass or less, more preferably 3% by mass or more and 40% by mass or less, further preferably 5% by mass or more and 30% by mass or less, and still more preferably 10% by mass or more and 25% by mass or less, relative to 100% by mass of the total of the propylene-based polymer (a1) and the polyolefin (b1).
[0199] The specific gravity of the polypropylene resin composition of the present invention is not particularly limited, but is usually 1.05 or less, preferably 0.89 or more and 1.05 or less, and more preferably 0.92 or more and 0.98 or less. Although the polypropylene resin composition of the present invention has such a specific gravity, it has better impact resistance and rigidity than a polyethylene resin alone or a polypropylene resin alone.
[0200] In the polypropylene resin composition of the present invention, when the total content of the propylene polymer composition (a), the polyolefin composition (b), and the modified polypropylene (c) is 100 parts by mass, it is preferred that the content of the propylene polymer composition (a) is 50 to 94.9 parts by mass, the content of the polyolefin composition (b) is 5 to 49.9 parts by mass, and the content of the modified polypropylene (c) is 0.1 to 15 parts by mass; more preferably, the content of the propylene polymer composition (a) is 55 to 90.5 parts by mass, the content of the polyolefin composition (b) is 8 to 40 parts by mass, and the content of the modified polypropylene (c) is 1 to 12 parts by mass; further preferably, the content of the propylene polymer composition (a) is 60 to 80 parts by mass, the content of the polyolefin composition (b) is 10 to 29 parts by mass, and the content of the modified polypropylene (c) is 2.5 to 11 parts by mass. By including each component in such a mixing ratio, there is a tendency that the obtained polypropylene resin composition has a better balance between rigidity and impact resistance.
[0201] In the polypropylene resin composition of the present invention, when the total content of the propylene polymer composition (a), the polyolefin composition (b), and the modified polypropylene (c) is 100 parts by mass, it is preferred that the content of the propylene polymer composition (a) is 50 to 94.9 parts by mass, the content of the polyolefin composition (b) is 4 to 49.9 parts by mass, and the content of the modified polypropylene (c) is 0.1 to 5 parts by mass; more preferably, the content of the propylene polymer composition (a) is 50 to 94.9 parts by mass, the content of the polyolefin composition (b) is 4 to 49.9 parts by mass, and the content of the modified polypropylene (c) is 0.1 to 5 parts by mass. ) is 5 to 49.9 parts by mass, and the content of modified polypropylene (c) is 0.1 to 5 parts by mass; more preferably, the content of propylene polymer composition (a) is 60 to 90 parts by mass, the content of polyolefin composition (b) is 6 to 35 parts by mass, and the content of modified polypropylene (c) is 0.5 to 4 parts by mass; further preferably, the content of propylene polymer composition (a) is 65 to 88 parts by mass, the content of polyolefin composition (b) is 8 to 30 parts by mass, and the content of modified polypropylene (c) is 1 to 3.5 parts by mass. By including each component in such a mixing ratio, there is a tendency that the obtained polypropylene resin composition has a better balance between rigidity and impact resistance.
[0202] The polypropylene resin composition of the present invention can be produced, for example, as follows.
[0203] For example, the propylene polymer composition (a) and the polyolefin composition (b) are prepared by the above-mentioned method. Then, the propylene polymer composition (a), the polyolefin composition (b) and the acid-modified polypropylene (c), and other polymers and additives such as the ethylene copolymer (d) added as required are melt-kneaded to produce. In addition, the propylene polymer composition (a1) and the filler (a2) can be added to replace the propylene polymer composition (a), that is, the propylene polymer (a1), the filler (a2), the polyolefin composition (b) and the acid-modified polypropylene (c), and other polymers and additives such as the ethylene copolymer (d) added as required are melt-kneaded to produce.
[0204] The melt kneading method is not particularly limited, and for example, a method in which each component is melt-kneaded using a kneading device such as an extruder (single-screw extruder, twin-screw extruder, etc.), a kneader, and a mixer (high-speed flow mixer, paddle mixer, ribbon mixer, etc.) can be cited. These devices can be used alone or in combination of two or more.
[0205] In the melt-kneading, the components may be added all at once and melt-kneaded, or may be added in multiple portions and melt-kneaded.
[0206] The melt kneading temperature can be appropriately set depending on the type of resin used, etc., but is preferably kneaded in a molten state, and is usually 190 to 350°C, preferably 200 to 330°C, and more preferably 205 to 310°C.
[0207] The polypropylene resin composition of the present invention can be made into a molded body by various thermoforming. The molded body thus obtained usually has the phase structure formed in the polypropylene resin composition as described above. Therefore, the obtained molded body has excellent balance between rigidity and impact resistance. As the above-mentioned thermoforming method, for example, injection molding, extrusion molding, blow molding, injection blow molding, inflation molding, hollow molding, vacuum molding, compression molding, press molding, stamping die molding, transfer molding, etc. can be cited.
[0208] The molded body may be produced by only one molding method or by combining two or more molding methods.
[0209] The polypropylene resin composition of the present invention can be used for various purposes. For example, the polypropylene resin composition of the present invention can be used as various products used in transportation tools such as automobiles, railway vehicles (vehicles as a whole), aircraft bodies (aircraft bodies as a whole), ships and hulls (hulls as a whole), and bicycles (vehicle bodies as a whole). Examples of automobile products include exterior parts, interior parts, engine parts, and electrical parts.
[0210] Example
[0211] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to these Examples.
[0212] [Manufacturing example]
[0213] <Production Example 1> Preparation of maleic anhydride graft-modified ethylene-1-butene copolymer (modified elastomer (b3-1))
[0214] Using the ethylene·1-butene copolymers shown in Table 1 below, maleic anhydride graft-modified ethylene·1-butene copolymers (modified elastomers (b3-1)) were produced.
[0215] [Table 1]
[0216]
[0217] 10 kg of the ethylene-1-butene copolymer and a solution prepared by dissolving 110 g of maleic anhydride and 6 g of 2,5-dimethyl-2,5-bis(tert-butylperoxy)-3-hexene in 80 g of acetone were mixed in a Henschel mixer.
[0218] The obtained blend was put into a twin-screw melt kneading extruder (manufactured by Nippon Steel Co., Ltd., screw diameter: 30 mm, L / D=42), and extruded in a strand shape under the conditions of a resin temperature of 260°C and an extrusion rate of 7 kg / hour. Then, after water cooling, pelletization was performed to obtain a maleic anhydride graft-modified ethylene-1-butene copolymer (hereinafter also referred to as "modified elastomer").
[0219] The obtained modified elastomer had an MFR (190°C, 2.16 kg load) of 0.6 g / 10 min, an MFR (230°C, 2.16 kg load) of 1.2 g / 10 min, and a density of 866 kg / m 3 The amount of maleic anhydride grafted was measured after extracting the unreacted maleic anhydride with acetone and was 0.99 mass %.
[0220] <Production Example 2> Preparation of polyolefin composition (b-1)
[0221] PA6 (nylon 6 resin, manufactured by Toray Industries, Ltd., product name "AMIRAN CM1007", melting point 225°C) was used as the aliphatic polyamide resin (b2), and the modified elastomer (b3-1) obtained in Production Example 1 was used as the modified elastomer (b3). The pellets were dry-blended in a ratio of PA6 / modified elastomer (b3-1) = 44.4 / 55.6 mass %, and then fed into a twin-screw melt-kneading extruder (manufactured by Nippon Steel & Steel Co., Ltd., screw diameter 30 mm, L / D = 42). Then, the mixture was mixed under the conditions of a kneading temperature of 245°C, an extrusion speed of 15 kg / hour, and a screw rotation speed of 200 rpm, and the extruded mixed resin was cut using a pelletizer to prepare mixed resin pellets.
[0222] Next, a polypropylene resin (homopolypropylene, manufactured by Prime Polymer Co., Ltd., product name "PRIMEPOLYPRO J106G", melting point 163°C) (hereinafter also referred to as "hPP") was used as the polyolefin (b1), and after dry blending with the previously obtained mixed resin pellets in a ratio of hPP / mixed resin pellets = 55 / 45 mass %, the mixture was fed into a twin-screw melt kneading extruder (manufactured by Nippon Steel & Iron Works Co., Ltd., screw diameter 30 mm, L / D = 42). Next, the mixture was mixed under the conditions of a kneading temperature of 245°C, an extrusion speed of 15 kg / hour, and a screw rotation speed of 200 rpm, and the extruded polyolefin composition was cut using a pelletizer to prepare pellets of the polyolefin composition (b-1).
[0223] <Production Example 3> Preparation of Propylene Polymer Composition (a-1)
[0224] As the propylene-based polymer (a1), a propylene-ethylene block copolymer having an ethylene block dispersed phase (manufactured by Prime Polymer Co., Ltd., product name “PRIME POLYPRO J739E", n-decane insoluble component at 23°C: 89% by mass, n-decane soluble component at 23°C: 11% by mass, [η] of n-decane soluble component at 23°C: 6.2 dl / g, MFR: 54 g / 10 min (230°C, 2.16 kg load)) (hereinafter also referred to as "bPP"), and a talc-containing polypropylene resin (manufactured by Asada Flour Milling Co., Ltd., product name "HG-170", talc content of 70 wt%) (hereinafter also referred to as "talc MB") as an inorganic filler (a2-1), were dry-blended in a manner of bPP / talc MB=80 / 20 by mass, and then charged into a twin-screw melt-kneading extruder (manufactured by Nippon Steel Co., Ltd., screw diameter: 30 mm, L / D=42). Next, mixing was performed under the conditions of a kneading temperature of 200°C, an extrusion rate of 15 kg / hour, and a screw speed of 200 rpm, and the extruded mixed resin was cut using a pelletizer to prepare pellets of the propylene polymer composition (a-1).
[0225] <Production Example 4> Preparation of Propylene Polymer Compositions (a-2-1) and (a-2-2)
[0226] Pellets of the propylene polymer compositions (a-2-1) and (a-2-2) were prepared in the same manner as in Production Example 3, except that cellulose fibers (manufactured by Nippon Paper Industries, Ltd., product name "KC FLOCKW-50GK") were used as natural fibers (a-2-2) instead of talc, and dry-blended in a manner such that bPP / cellulose fibers = 90 / 10 mass % (propylene polymer composition (a-2-1)) or 80 / 20 mass % (propylene polymer composition (a-2-2)).
[0227] [Examples 1 to 3]
[0228] (1) Preparation of polypropylene resin composition
[0229] The propylene polymer composition (a-1) obtained in Production Example 3 as the propylene polymer composition (a), the polyolefin composition (b-1) obtained in Production Example 2 as the polyolefin composition (b), and the maleic anhydride-modified polypropylene (c-1) (manufactured by Mitsui Chemicals, Inc., product name "ADMER AT2606", MFR: 220 g / 10 min (230°C, 2.16 kg load), density 900 kg / m 3), dry-blended in a manner as shown in Table 2, and then fed into a twin-screw melt-kneading extruder (manufactured by Nippon Steel Co., Ltd., with a screw diameter of 30 mm and L / D=42). Next, mixing was performed under the conditions of a kneading temperature of 200° C., an extrusion speed of 15 kg / hour, and a screw speed of 200 rpm, and the extruded polypropylene resin composition was cut using a pelletizer to prepare pellets of the polypropylene resin composition.
[0230] (2) Preparation of test pieces for physical property measurement
[0231] The pellets of the polypropylene resin composition obtained in (1) were charged into the feed hopper of a 50-ton injection molding machine (manufactured by Meiki Seisakusho Co., Ltd.), and injection-molded into test pieces for bending test, tensile test, Charpy impact test, and load deflection temperature measurement under injection conditions of a set temperature of 200° C. and a mold temperature of 40° C. Similarly, a 70-ton injection molding machine (manufactured by Meiki Seisakusho Co., Ltd.) was used to injection-mold square plates for puncture impact test and Rockwell hardness measurement under injection conditions of a set temperature of 200° C. and a mold temperature of 40° C.
[0232] (3) Charpy impact strength
[0233] Under the following test conditions, a hammer is struck from the back of the notch of the fixed test piece, and the impact strength is calculated from the upward angle of the hammer after the test piece is broken and the upward angle of the hammer before the test.
[0234] (Test conditions)
[0235] Test temperature: 23℃ / -30℃, hammer capacity: 4J, lifting angle: 149.9, test piece: with notch, remaining width 8mm, width 4mm
[0236] (4) Load deflection temperature
[0237] Under the following test conditions, a predetermined test load (0.45 MPa) was applied to the test piece, the temperature was increased in a heat transfer medium, and the temperature at which the deflection amount reached 0.34 mm was determined.
[0238] (Test conditions)
[0239] Test starting temperature: 35.0℃, heating rate: 120℃ / h, test piece: length 80mm×width 10mm×thickness 4mm, test piece direction: flat, test load: 0.45MPa
[0240] (5) Rockwell hardness
[0241] Under the following test conditions, a test load was applied to the test piece for 15 seconds, and then the test load was removed. The hardness was determined based on the indentation depth 15 seconds after the test load was removed.
[0242] (Test conditions)
[0243] Test temperature: 23℃, test load: 60kg, scale: HRR, test piece: 2 overlapping injection square plates with a thickness of 3mm
[0244] (6) Evaluation of rigidity (measurement of flexural modulus)
[0245] The test piece obtained in (2) was used to measure the bending modulus in accordance with JIS K7171. The results are shown in Table 2. It should be noted that the bending modulus was measured by supporting the test piece with two fulcrums (with a curvature radius of 5 mm) having a distance (L) between the fulcrums of 64 mm and applying a load at a speed of 2 mm / min from a point of action (with a curvature radius of 5 mm) disposed at the center between the fulcrums.
[0246] (7) Tensile test
[0247] The measurement was carried out under the following test conditions to determine the tensile elongation at break (between chucks) and the tensile modulus.
[0248] (Test conditions)
[0249] Test temperature: 23°C, Test speed: 50 mm / min, Test piece: ISO527 1A, Distance between chucks: 115 mm
[0250] Calculation formula for tensile elastic modulus: Et = (σ2-σ1) / (ε2-ε1)
[0251] Et: tensile elastic modulus (MPa)
[0252] σ1: stress at strain ε1 = 0.0005 (0.05%) (MPa)
[0253] σ2: Stress at strain ε2 = 0.0025 (0.25%) (MPa)
[0254] (The strain uses the strain between chucks)
[0255] (8) Puncture impact test
[0256] The measurement was carried out under the following test conditions to obtain the maximum impact force point displacement / energy and the puncture point displacement / energy.
[0257] (Test conditions)
[0258] Test temperature: 23℃ / -30℃, test speed 5m / sec, striker diameter 0.5 inches, support table diameter 3 inches, test piece: injection square plate with a thickness of about 1mm
[0259] The displacement at the point with the maximum stress of the stress-displacement curve obtained in the test is taken as the maximum impact point displacement, and the integral value of the curve from the test start point to this point is taken as the maximum impact point energy. In addition, the point where the displacement is greater than the maximum impact point and the stress is 1 / 2 of the maximum impact point is taken as the puncture point, its displacement is taken as the puncture point displacement, and the integral value of the curve from the test start point to this point is taken as the puncture point energy.
[0260] [Examples 4 to 7]
[0261] In addition to the propylene polymer composition (a-1), polyolefin composition (b-1), and maleic anhydride-modified polypropylene used in Examples 1 to 3, an ethylene-1-butene copolymer (manufactured by Mitsui Chemicals, Inc., product name "TAFMERDF610", density = 862 kg / m 3 ) as the ethylene copolymer (d) was dry-blended in the manner of Table 2. The same operation as in Examples 1 to 3 was performed to prepare pellets of the polypropylene resin composition, which were injection-molded into test pieces for property measurement and evaluated. The results are shown in Table 2.
[0262] [Examples 8 to 10]
[0263] The propylene polymer composition (a-1) as the propylene polymer composition (a) was changed to the propylene polymer composition (a-2-1) or (a-2-2) prepared in Production Example 4 so that each component had the mixing ratio shown in Table 3. In the same manner as in Examples 1 to 3, pellets of the polypropylene resin composition were prepared, injection molded into test pieces for measuring physical properties, and evaluated. The results are shown in Table 3.
[0264] [Examples 11-12]
[0265] The propylene polymer composition (a-1) as the propylene polymer composition (a) was changed to the propylene polymer composition (a-2-2) prepared in Production Example 4 so that each component had the mixing ratio shown in Table 4. In the same manner as in Examples 1 to 3, pellets of the polypropylene resin composition were prepared, injection molded into test pieces for measuring physical properties, and evaluated. The results are shown in Table 4.
[0266] [Examples 13-14]
[0267] The propylene polymer composition (a-1) as the propylene polymer composition (a) was changed to the propylene polymer composition (a-2-2) prepared in Production Example 4, and the acid-modified polypropylene (c) was changed to a maleic anhydride-modified polypropylene (c-2) (manufactured by Mitsui Chemicals, Inc., product name "ADMER AT3190", MFR: 235 g / 10 min (190° C., 2.16 kg load), density 900 kg / m 3 ) so that the components were in the proportions shown in Table 4. The same procedures as in Examples 1 to 3 were followed to prepare pellets of the polypropylene resin composition, which were injection molded into test pieces for measuring physical properties and evaluated. The results are shown in Table 4.
[0268] [Comparative Example 1]
[0269] The test pieces for measuring physical properties were injection molded and evaluated in the same manner as in Examples 1 to 3 except that only the propylene polymer composition (a-1) obtained in Production Example 3 was used.
[0270] [Comparative Examples 2 to 4]
[0271] The propylene polymer composition (a-1) obtained in Production Example 3 as the propylene polymer composition (a) and the polyolefin composition (b-1) obtained in Production Example 2 as the polyolefin composition (b) were dry-blended in a manner as shown in Table 2. In the same manner as in Examples 1 to 3, pellets of the polypropylene resin composition were prepared, injection-molded into test pieces for measuring physical properties, and evaluated. The results are shown in Table 2.
[0272] [Comparative Examples 5 to 8]
[0273] The propylene polymer composition (a-1) obtained in Production Example 3 as the propylene polymer composition (a), the polyolefin composition (b-1) obtained in Production Example 2 as the polyolefin composition (b), and the ethylene elastomer were dry-blended in a manner as shown in Table 2. In the same manner as in Examples 1 to 3, pellets of the polypropylene resin composition were prepared, injection-molded into test pieces for measuring physical properties, and evaluated. The results are shown in Table 2.
[0274] [Comparative Examples 9 to 11]
[0275] The propylene polymer composition (a-1) as the propylene polymer composition (a) was changed to the propylene polymer composition (a-2-1) or (a-2-2) prepared in Production Example 4, and the components were dry-blended in the proportions shown in Table 3. The same procedures as in Comparative Examples 5 to 8 were followed to prepare pellets of the polypropylene resin composition, injection-molded into test pieces for measuring physical properties, and evaluated. The results are shown in Table 3.
[0276] [Table 2]
[0277]
[0278] [Table 3]
[0279]
[0280] [Table 4]
[0281]
Claims
1. A polypropylene resin composition, characterized in that The polypropylene resin composition comprises a propylene polymer composition (a), a polyolefin composition (b), and an acid-modified polypropylene (c). The propylene polymer composition (a) comprises a propylene polymer (a1) and a filler (a2). The polyolefin composition (b) comprises a polyolefin (b1), an aliphatic polyamide resin (b2), and a modified elastomer (b3), and The invention comprises a continuous phase (α) containing a polyolefin (b1) and a dispersed phase (β) containing an aliphatic polyamide resin (b2) and a modified elastomer (b3) dispersed in the continuous phase (α). The dispersed phase (β) is formed by a melt-kneaded product of the aliphatic polyamide resin (b2) and the modified elastomer (b3), The modified elastomer (b3) is an elastomer obtained by partially adding a group reactive with the aliphatic polyamide resin (b2) to an unmodified elastomer (b3'), and the unmodified elastomer (b3') is an olefin-based thermoplastic elastomer containing a structural unit derived from ethylene and a structural unit derived from an α-olefin having 3 to 8 carbon atoms, or a styrene-based thermoplastic elastomer containing a structural unit derived from a styrene-based compound. When the total of the continuous phase (α) and the dispersed phase (β) is 100% by mass, the dispersed phase (β) is 80% by mass or less.
2. The polypropylene resin composition according to claim 1, wherein The filler (a2) is an inorganic filler (a2-1).
3. The polypropylene resin composition according to claim 1, wherein The filler (a2) is natural fiber (a2-2).
4. The polypropylene resin composition according to claim 1, wherein The propylene-based polymer (a1) is a propylene-ethylene block copolymer having a dispersed phase of ethylene polymer blocks.
5. The polypropylene resin composition according to claim 2, wherein The inorganic filler (a2-1) is one or more inorganic fillers selected from the group consisting of talc, mica, glass fiber, and calcium carbonate.
6. The polypropylene resin composition according to claim 3, wherein The natural fiber (a2-2) is one or more natural fibers selected from the group consisting of cellulose fibers, wood powder, and wood powder fibers.
7. The polypropylene resin composition according to claim 1, wherein The polyolefin (b1) is a propylene homopolymer.
8. The polypropylene resin composition according to claim 1, wherein The aliphatic polyamide resin (b2) is at least one aliphatic polyamide resin selected from the group consisting of polyamide 6, polyamide 11, polyamide 12, polyamide 612, polyamide 610, and polyamide 1010.
9. The polypropylene resin composition according to claim 1, wherein The dispersed phase (β) includes a continuous phase (β1) containing the aliphatic polyamide resin (b2) and a finely dispersed phase (β2) containing a modified elastomer (b3) dispersed in the continuous phase (β1).
10. The polypropylene resin composition according to any one of claims 1 to 9, wherein The content of the propylene polymer composition (a) is 50 to 94.9 parts by mass, the content of the polyolefin composition (b) is 5 to 49.9 parts by mass, and the content of the modified polypropylene (c) is 0.1 to 15 parts by mass (wherein the total content of the propylene polymer composition (a), the polyolefin composition (b), and the modified polypropylene (c) is 100 parts by mass).
11. The polypropylene resin composition according to any one of claims 1 to 9, wherein The content of the propylene polymer composition (a) is 50 to 94.9 parts by mass, the content of the polyolefin composition (b) is 5 to 49.9 parts by mass, and the content of the modified polypropylene (c) is 0.1 to 5 parts by mass (wherein the total content of the propylene polymer composition (a), the polyolefin composition (b), and the modified polypropylene (c) is 100 parts by mass).