Polymer compositions with improved flame retardant properties and flexibility
By combining a heterogeneous propylene copolymer and a flame retardant in the polymer composition, the problem of difficulty in taking into account both the brittleness and flame retardant properties of polymers in the battery case assembly in the prior art is solved, and excellent flame retardant of the battery case material is achieved Performance and flexibility, suitable for snap fit assembly of electric vehicle battery case.
Patent Information
- Application Number
- CN202380037096.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-21
- Filing Date
- 2023-04-18
- Publication Date
- 2024-12-06
AI Technical Summary
The existing flame retardant polymer compositions are not suitable for assembly of electric vehicle battery housings due to brittleness problems when used in snap fitting mechanisms, and it is difficult to take into account both flame retardant performance and sufficient flexibility.
Using a polymer composition comprising a first heterophase propylene copolymer, a second heterophase propylene copolymer, a flame retardant composition and an aryl phosphate, the polymer detachment is increased by adjusting the melt flow index and the flame retardant ratio. and flame retardant properties.
It achieves excellent flame retardant performance and sufficient flexibility in battery housing materials, and is suitable for snap fit assembly of electric vehicle battery housings, and has optimized density and cost.
Abstract
Description
[0001] The present invention relates to a polymer composition comprising: (A) a first heterophasic propylene copolymer, (B) a second heterophasic propylene copolymer, (C) a flame retardant composition and (D) a phosphate aromatic ester. The present invention also relates to a method for preparing the polymer composition and the use of the polymer composition.
[0002] Polymer compositions having flame retardant properties are well known in the art. For example, EP3255095 discloses a flame retardant polyolefin resin composition comprising polypropylene, melamine pyrophosphate, piperazine pyrophosphate, glass fiber and zinc oxide.
[0003] EP3202841 discloses a flame retardant polypropylene resin composition comprising a polypropylene resin, glass fiber, a phosphorus-containing flame retardant (FP2200 from Adeka), an antioxidant, a neutralizer and a surfactant.
[0004] WO2018 / 019762A1 discloses a flame retardant polypropylene composition comprising:
[0005] (A) a polypropylene-based polymer,
[0006] (B) a first flame retardant in an amount of 15-40 wt% of the total composition, wherein the first flame retardant is in the form of particles comprising ammonium polyphosphate and at least one phosphate ester / salt selected from the following:
[0007] Melamine phosphate,
[0008] Melamine polyphosphate,
[0009] Melamine pyrophosphate,
[0010] Piperazine phosphate,
[0011] Piperazine polyphosphate,
[0012] Piperazine pyrophosphate,
[0013] 2-Methylpiperazine monophosphate,
[0014] Tricresyl phosphate,
[0015] Alkyl phosphates,
[0016] Haloalkyl phosphates,
[0017] Tetraphenyl pyrophosphate,
[0018] Poly(2-hydroxypropylene spirocyclopentaerythritol diphosphate), and
[0019] Poly(2,2-dimethylpropylene spirocyclic pentaerythritol diphosphonate), and
[0020] (C) a second flame retardant in an amount of 0.1 to 15 wt % of the total composition, wherein the second flame retardant comprises aryl phosphate.
[0021] The combination of stiffness and flame retardant properties of such polymer compositions makes them a promising candidate material for electric vehicle (EV) battery housing materials. In order to improve the production efficiency of EV batteries, it is desirable to perform the assembly of EV battery housings by means of a snap-fit mechanism. The snap-fit mechanism typically includes at least one snap-fit joint, wherein the snap-fit joint consists of a protruding edge on one component to be assembled and a snap-fit region on another component to be assembled. In the process of assembling two components with a snap-fit mechanism and when shortening the distance between the two components, the protruding edge is first deformed, such as bent, and then the protruding edge is fitted into the snap-fit region and restored to its original shape, wherein the protruding edge and the snap-fit region form a snap-fit joint. The material used for the snap-fit mechanism should have sufficient flexibility so that the protruding edge will not break during deformation.
[0022] The presence of flame retardants in polymer compositions generally results in brittleness, making the polymer compositions unsuitable for battery housings assembled by snap-fit mechanisms. Therefore, there is a need for a polymer composition having excellent flame retardant properties and sufficient flexibility. Preferably, the density of the polymer composition is less than 0.93 g / cm 3 , to reduce the weight of electric vehicles.
[0023] The objects of the present invention are achieved by a polymer composition comprising:
[0024] (A) a first heterophasic propylene copolymer, wherein the MFI of the first heterophasic propylene copolymer is 3.6 to 14 g / 10 min, measured according to ISO 1133:1-2011 at 230 °C and 2.16 kg, wherein the first heterophasic propylene copolymer comprises a first propylene-based matrix and a first ethylene-propylene copolymer, wherein the amount of the first ethylene-propylene copolymer is 18 to 26 wt%, based on the total amount of the first heterophasic propylene copolymer;
[0025] (B) a second heterophasic propylene copolymer, wherein the second heterophasic propylene copolymer has an MFI of 18 to 51 g / 10 min, measured according to ISO 1133:1-2011 at 230 °C and 2.16 kg, wherein the second heterophasic propylene copolymer comprises a second propylene-based matrix and a second ethylene-propylene copolymer, wherein the amount of the second ethylene-propylene copolymer is 15 to 23 wt%, based on the total amount of the second heterophasic propylene copolymer;
[0026] (C) a flame retardant composition comprising at least one phosphate ester / salt;
[0027] (D) aryl phosphate,
[0028] The amount of the first heterophasic propylene copolymer is 10-38 wt%, the amount of the second heterophasic propylene copolymer is 35-60 wt%, the amount of the fuel composition is 13-33 wt%, and the amount of the aromatic phosphate is 0.3-13 wt%, based on the total amount of the polymer composition.
[0029] The inventors of the present invention have found that the polymer composition according to the present invention has excellent flame retardant properties and sufficient flexibility for use in materials suitable for snap-fit assembly of EV battery housings. In the context of the present invention, "flexibility" is quantified as the elongation at break in a tensile measurement with a 1A specimen according to ISO 527-1:2019.
[0030] (A) a first heterophasic propylene copolymer and (B) a second heterophasic propylene copolymer
[0031] Heterophasic propylene copolymers, also called impact propylene copolymers or propylene block copolymers, are an important class of polymers due to their attractive combination of mechanical properties (e.g. impact strength over a wide temperature range) and their low cost. These copolymers have a wide range of applications, from consumer industry (e.g. packaging and household appliances), automotive industry to electrical applications.
[0032] Heterophasic propylene copolymers are usually prepared in one or more reactors by polymerizing propylene in the presence of a catalyst followed by polymerization of an ethylene-α-olefin mixture. The polymer material formed is heterophasic, but the specific morphology usually depends on the preparation method and the ratio of the monomers used.
[0033] The first heterophasic propylene copolymer and the second heterophasic propylene copolymer may be produced using any conventional technique known to those skilled in the art, such as a multistage process polymerization, such as bulk polymerization, gas phase polymerization, slurry polymerization, solution polymerization or any combination thereof. Any conventional catalyst system may be used, such as Ziegler-Natta or metallocene. Such techniques and catalysts are described in, for example, WO06 / 010414; Polypropylene and other Polyolefins, Ser van der Ven, Studies in Polymer Science 7, Elsevier 1990; WO06 / 010414, US4399054 and US4472524. Preferably, the first heterophasic propylene copolymer and the second heterophasic propylene copolymer are produced in the presence of a Ziegler-Natta catalyst.
[0034] The first heterophasic propylene copolymer and the second heterophasic propylene copolymer may be prepared by a process comprising the following steps:
[0035] - polymerizing propylene and optionally ethylene and / or α-olefins in the presence of a catalyst system to obtain a propylene-based substrate, and
[0036] - Subsequently polymerizing ethylene and α-olefins in the propylene-based matrix in the presence of a catalyst system to obtain a dispersed ethylene-α-olefin copolymer. These steps are preferably carried out in different reactors. The catalyst systems used for the first step and for the second step may be different or identical.
[0037] The first heterophasic propylene copolymer comprises a first propylene-based matrix and a first ethylene-propylene copolymer, wherein the amount of the first ethylene-propylene copolymer is 18-26 wt%, preferably 20-24 wt%, based on the total amount of the first heterophasic propylene copolymer. The first propylene-based matrix typically forms a continuous phase in the first heterophasic propylene copolymer. The amounts of the first propylene-based matrix and the first ethylene-propylene copolymer can be determined by methods known in the art. 13 Preferably, the amount of the structural part derived from ethylene in the first ethylene-propylene copolymer is 15-65 wt%, preferably 30-57 wt%, more preferably 45-52 wt%, based on the total amount of the first ethylene-propylene copolymer.
[0038] The first propylene-based matrix preferably consists of a first propylene homopolymer and / or a first propylene copolymer consisting of at least 96 wt% of propylene monomer units and at most 4 wt% of comonomer units selected from ethylene monomer units and α-olefin monomer units having 4 to 10 carbon atoms.
[0039] Preferably, the comonomer in the first propylene-α-olefin copolymer is selected from the group consisting of ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene and 1-octene, preferably ethylene.
[0040] It is known that the first propylene-based matrix is different from the first ethylene-propylene copolymer.
[0041] Preferably, the first propylene-based matrix consists of a first propylene homopolymer.The fact that the first propylene-based matrix consists of a first propylene homopolymer is advantageous in that a higher stiffness is obtained compared to in case the first propylene-based matrix is a first propylene copolymer.
[0042] The melt flow index (MFI) of the first heterophasic propylene copolymer is 3.6 to 14 g / 10 min, preferably 5.1 to 12 g / 10 min, preferably 6.7 to 9.8 g / 10 min, measured according to ISO 1133: 1-2011 at 230 °C and 2.16 kg.
[0043] The second heterophasic propylene copolymer comprises a second propylene-based matrix and a second ethylene-propylene copolymer, wherein the amount of the second ethylene-propylene copolymer is 15-23 wt%, preferably 19-22 wt%, based on the total amount of the second heterophasic propylene copolymer. The second propylene-based matrix typically forms a continuous phase in the second heterophasic propylene copolymer. The amount of the second propylene-based matrix and the second ethylene-propylene copolymer can be determined by methods known in the art. 13 Preferably, the amount of the structural part derived from ethylene in the second ethylene-propylene copolymer is 16-63 wt%, preferably 31-51 wt%, more preferably 40-45 wt%, based on the total amount of the second ethylene-propylene copolymer.
[0044] The second propylene-based matrix preferably consists of a second propylene homopolymer and / or a second propylene copolymer consisting of at least 96 wt% of propylene monomer units and at most 4 wt% of comonomer units selected from ethylene monomer units and α-olefin monomer units having 4 to 10 carbon atoms.
[0045] Preferably, the comonomer in the second propylene-α-olefin copolymer is selected from the group consisting of ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene and 1-octene, preferably ethylene.
[0046] It is known that the second propylene-based matrix is different from the second ethylene-propylene copolymer.
[0047] Preferably, the second propylene based matrix consists of a second propylene homopolymer.The fact that the second propylene based matrix consists of a second propylene homopolymer is advantageous in that a higher stiffness is obtained compared to in case the second propylene based matrix is a second propylene copolymer.
[0048] The second heterophasic propylene copolymer has a melt flow index (MFI) of 18 to 51 g / 10 min, preferably 22 to 42 g / 10 min, more preferably 26 to 36 g / 10 min, measured according to ISO 1133: 1-2011 at 230 °C and 2.16 kg.
[0049] In a preferred embodiment the MFI of the first heterophasic propylene copolymer and the MFI of the second heterophasic propylene copolymer are in the preferred ranges, the polymer composition shows an even better balance between flame retardancy and flexibility.
[0050] In a preferred embodiment the first heterophasic propylene copolymer consists of a first propylene based matrix, a first ethylene-propylene copolymer and optional additives, wherein the first propylene based matrix consists of a first propylene homopolymer wherein the total amount of moieties derived from ethylene is 7.0 to 14 wt%, preferably 8.8 to 12 wt%, even more preferably 9.5 to 11 wt%, based on the total amount of the first heterophasic propylene copolymer.
[0051] In a preferred embodiment the second heterophasic propylene copolymer consists of a second propylene based matrix, a second ethylene-propylene copolymer and optional additives, wherein the second propylene based matrix consists of a second propylene homopolymer, wherein the total amount of moieties derived from ethylene is 5.0 to 12 wt%, preferably 6.7 to 11 wt%, even more preferably 8.2 to 10 wt%, based on the total amount of the second heterophasic propylene copolymer.
[0052] (C) Flame retardant composition
[0053] The flame retardant composition comprises at least one phosphate ester / salt, wherein the phosphate ester / salt is preferably selected from:
[0054] Melamine phosphate,
[0055] Melamine polyphosphate,
[0056] Melamine pyrophosphate,
[0057] Piperazine phosphate,
[0058] Piperazine polyphosphate,
[0059] Piperazine pyrophosphate,
[0060] 2-Methylpiperazine monophosphate,
[0061] Tricresyl phosphate,
[0062] Alkyl phosphates,
[0063] Haloalkyl phosphates,
[0064] Tetraphenyl pyrophosphate,
[0065] Poly(2-hydroxypropylene spirocyclopentaerythritol diphosphate),
[0066] Poly(2,2-dimethylpropylene spirocyclic pentaerythritol diphosphonate).
[0067] The flame retardant composition is preferably in the form of particles. Preferably, the flame retardant composition has a normal particle size distribution (D 50 ), which is determined by a Mastersizer 2000 available from Malvern.
[0068] Preferably, the amount of phosphate in the flame retardant composition is 40-75 wt %, which is measured using an ICP-OES spectrometer (iCAP 6300Duo, available from Thermo Fisher) after treatment with nitric acid.
[0069] Preferably, the flame retardant composition comprises piperazine pyrophosphate, melamine phosphate and zinc oxide.
[0070] Preferably, the amount of piperazine pyrophosphate is 40-69 wt%, more preferably 50-67 wt%; the amount of melamine phosphate is 29-49 wt%, and the amount of zinc oxide is 1-10 wt%, based on the total amount of the flame retardant composition.
[0071] (D) Aryl phosphate
[0072] Preferably, the aryl phosphate is selected from:
[0073] Resorcinol bis(diphenyl phosphate);
[0074] Tetraphenylresorcinol bis(diphenyl phosphate);
[0075] Bisphenol A bis(diphenyl phosphate);
[0076] Bisphenol A diphosphate;
[0077] Resorcinol bis(di-2,6-ditolyl phosphate);
[0078] Phosphoric acid, mixed esters with [1,1'-biphenyl]-4,4'-diol and phenol;
[0079] Phosphorus trichloride, polymer with 1,3-benzenediol, phenyl ester;
[0080] 1,3-phenylene-tetrakis(2,6-dimethylphenyl)diphosphate;
[0081] Isopropenylphenyl diphenyl phosphate;
[0082] 4-Phenylphenol formaldehyde phenylphosphonate;
[0083] Tris(2,6-diphenylyl) phosphate;
[0084] Resorcinol bis(di-2,6-ditolyl phosphate);
[0085] Bisphenol S bis(diphenyl phosphate);
[0086] Resorcinol-bisphenol A phenyl phosphate.
[0087] Preferably, the aryl phosphate is added in liquid form.
[0088] Preferably, the aromatic phosphate is bisphenol A bis(diphenyl phosphate).
[0089] Polymer composition
[0090] The amount of the first heterophasic propylene copolymer is 10-38 wt%, preferably 15-30 wt%, more preferably 20-28 wt%, even more preferably 22-26 wt%, the amount of the second heterophasic propylene copolymer is 35-60 wt%, preferably 40-55 wt%, more preferably 42-50 wt%, the amount of the flame retardant composition is 13-33 wt%, preferably 18-27 wt%, more preferably 19-24 wt%, the amount of the aromatic phosphate is 0.3-13 wt%, preferably 1.8-8.0 wt%, more preferably 2.5-4.5 wt%, based on the total amount of the polymer composition.
[0091] Preferably, the polymer composition is according to any one of the preceding claims, wherein the polymer composition has a UL94 rating of V0 at 0.8 mm, wherein after forming and before UL94 measurement, the specimens are conditioned at 23°C and 50% RH for 48 hours.
[0092] Preferably, the polymer composition has a tensile elongation at break of at least 42%, measured according to ISO 527-1:2019 using a 1A specimen.
[0093] Preferably, the density of the polymer composition is 0.956-1.200 g / cm 3 , preferably 0.989-1.158g / cm 3 , more preferably 1.002-1.098 g / cm 3 , which is measured according to ISO 1183-1:2004.
[0094] The present invention further relates to a process for preparing a polymer composition according to the invention comprising the following sequential steps:
[0095] - providing a first heterophasic propylene copolymer, a second heterophasic propylene copolymer, a flame retardant composition and an aromatic phosphate ester;
[0096] - The first heterophasic propylene copolymer, the second heterophasic propylene copolymer, the flame retardant composition and the aryl phosphate ester are mixed in an extruder.
[0097] The present invention further relates to the use of the polymer composition according to the invention for improving the flame retardancy and flexibility of an article, wherein the article is preferably a battery housing.
[0098] The present invention further relates to an article comprising the polymer composition according to the invention, wherein the amount of the polymer composition is at least 95 wt%, preferably at least 98 wt%, based on the total amount of the article, wherein the article is preferably a battery housing.
[0099] experiment
[0100] Material
[0101] SABIC® 595A is a propylene homopolymer commercially available from SABIC having an MFI of 47 g / 10 min measured according to ISO 1133: 1-2011 at 230°C and 2.16 kg.
[0102] 591A is a propylene homopolymer commercially available from SABIC having an MFI of 6 g / 10 min measured according to ISO 1133: 1-2011 at 230°C and 2.16 kg.
[0103] 87MK40T is a heterophasic propylene copolymer commercially available from SABIC having an MFI of 8 g / 10 min measured at 230°C and 2.16 kg according to ISO 1133:1-2011. 87MK40T contains 22 wt% of ethylene-propylene copolymer and the total amount of moieties derived from ethylene in 87MK40T is 10.5 wt%, which is determined by NMR.
[0104] 511MK40T is a heterophasic propylene copolymer commercially available from SABIC having an MFI of 30 g / 10 min measured according to ISO 1133:1-2011 at 230°C and 2.16 kg. 511MK40T contains 21 wt% of ethylene-propylene copolymer and the total amount of moieties derived from ethylene in 511MK40T is 9 wt%, determined by NMR.
[0105] FP2500S is a flame retardant composition commercially available from Adeka ADK STAB FP-2500S. FP-2500S is a flame retardant composition according to the most preferred embodiment of the present invention.
[0106] CR741 is bisphenol A bis(diphenyl phosphate) commercially available from Daihachi.
[0107] Additive package: The additive package includes 30 wt% stabilizer, 15 wt% anti-soaking agent (TSANF449 from SABIC), 8 wt% nucleating agent, 7 wt% slip agent, 40 wt% color masterbatch. The weight percentage is based on the total amount of the additive package.
[0108] Sample preparation
[0109] All IE and CE were prepared in a twin-screw extruder. The formulations of IE and CE are shown in Table 1.
[0110] Table 1 Formulations of IE and CE
[0111] CE1 CE2 CE3 IE1 IE2 IE3 CE4 CE5 595A (wt%) 45.8 591A (wt%) 33 87MK40T (wt%) 76.7 26 24 26 25 73.2 6 511MK40T (wt%) 48.7 47.2 49.2 48.2 67.2 FP2500S (wt%) 20 22 24 24 20 22 22 22 CR741 (wt%) 3.5 3.5 3.5 3.5 3.5 Additive Package (wt%) 1.2 1.3 1.3 1.3 1.3 1.3 1.3 1.3
[0112] IE and CE obtained from the extruder were in the form of pellets. The pellets were further injection molded into specimens for measurement.
[0113] Measurement
[0114] Melt flow index (MFI) was measured according to ISO 1133: 1-2011 at 230°C and 2.16 kg.
[0115] Tensile properties were measured according to ISO 527-1:2019 using 1A specimens.
[0116] Density was measured according to ISO 1183-1:2004.
[0117] Flame retardancy measurements were performed according to UL94. Samples of different thicknesses were used and the samples were conditioned under the following two conditions before measurement:
[0118] Condition 1: After injection molding and before flame retardancy measurement, the specimen was conditioned in an environment of 23° C. and 50% RH for 48 hours.
[0119] Condition 2: After injection molding and before flame retardancy measurement, the specimen was conditioned in a first environment of 70° C. and 50% RH for 168 hours, and then conditioned in a second environment of 23° C. and 20% RH for 4 hours.
[0120] result
[0121] The performance of IE and CE is shown in Table 2.
[0122] Table 2 Performance of IE and CE
[0123] CE1 CE2 CE3 IE1 IE2 IE3 CE4 CE5 MFI(g / 10min) 11 5.29 9.92 12.01 12.31 12.43 6.62 17.3 <![CDATA[Density (g / cm 3 )]]> 1.009 1.020 1.028 1.038 1.015 1.022 1.024 1.023 Tensile modulus (MPa) 2104 1937 1985 1688 1600 1684 1676 1652 Tensile elongation at break (%) 23 52.4 26.8 47.4 61.1 61.6 72.4 40.6 UL94 (0.8mm, condition 1) V1 V2 V1 V0 V0 V0 HB V0 UL94 (0.8mm, condition 2) V0 HB V0 V0 V0 V0 V0 V0 UL94(1.0mm, condition 1) V1 V1 V0 V0 V0 V0 V0 V0 UL94 (1.0mm, condition 2) V1 V1 V1 V0 V0 V0 V0 V0 UL94 (1.2mm, condition 1) V0 V1 V0 V0 V0 V0 V0 V0 UL94 (1.2mm, condition 2) V0 V0 V0 V0 V0 V0 V0 V0 UL94 (1.5mm, condition 1) V0 V0 V0 V0 V0 V0 V0 V0 UL94 (1.5mm, condition 2) V0 V0 V0 V0 V0 V0 V0 V0
[0124] According to Table 2, only IE exhibits excellent FR properties, MFI and tensile elongation at break.
Claims
1. A polymer composition comprising: (A) a first heterophasic propylene copolymer, wherein the MFI of the first heterophasic propylene copolymer is 3.6 to 14 g / 10 min, measured according to ISO 1133:1-2011 at 230 °C and 2.16 kg, wherein the first heterophasic propylene copolymer comprises a first propylene-based matrix and a first ethylene-propylene copolymer, wherein the amount of the first ethylene-propylene copolymer is 18 to 26 wt%, based on the total amount of the first heterophasic propylene copolymer; (B) a second heterophasic propylene copolymer, wherein the second heterophasic propylene copolymer has an MFI of 18 to 51 g / 10 min, measured according to ISO 1133:1-2011 at 230 °C and 2.16 kg, wherein the second heterophasic propylene copolymer comprises a second propylene-based matrix and a second ethylene-propylene copolymer, wherein the amount of the second ethylene-propylene copolymer is 15 to 23 wt%, based on the total amount of the second heterophasic propylene copolymer; (C) a flame retardant composition comprising at least one phosphate ester / salt; (D) aryl phosphate, The amount of the first heterophasic propylene copolymer is 10-38 wt%, the amount of the second heterophasic propylene copolymer is 35-60 wt%, the amount of the flame retardant composition is 13-33 wt%, and the amount of the phosphate aromatic ester is 0.3-13 wt%, based on the total amount of the polymer composition.
2. The polymer composition according to claim 1, wherein the aryl phosphate is selected from: Resorcinol bis(diphenyl phosphate); Tetraphenylresorcinol bis(diphenyl phosphate); Bisphenol A bis(diphenyl phosphate); Bisphenol A diphosphate; Resorcinol bis(di-2,6-ditolyl phosphate); Phosphoric acid, mixed esters with [1,1'-biphenyl]-4,4'-diol and phenol; Phosphorus trichloride, polymer with 1,3-benzenediol, phenyl ester; 1,3-phenylene-tetrakis(2,6-dimethylphenyl)diphosphate; Isopropenylphenyl diphenyl phosphate; 4-Phenylphenol formaldehyde phenylphosphonate; Tris(2,6-diphenylyl) phosphate; Resorcinol bis(di-2,6-ditolyl phosphate); Bisphenol S bis(diphenyl phosphate); Resorcinol-bisphenol A phenyl phosphate, Preferably the aromatic phosphate is bisphenol A bis(diphenyl phosphate).
3. Polymer composition according to claim 1 or 2, wherein the first heterophasic propylene copolymer has an MFI of 5.1 to 12 g / 10 min, preferably 6.7 to 9.8 g / 10 min, measured according to ISO 1133: 1-2011 at 230 °C and 2.16 kg.
4. Polymer composition according to any of the preceding claims, wherein the second heterophasic propylene copolymer has an MFI of 22 to 42 g / 10 min, preferably 26 to 36 g / 10 min, measured according to ISO 1133: 1-2011 at 230 °C and 2.16 kg.
5. The polymer composition according to any one of the preceding claims, wherein the density of the polymer composition is 0.956-1.200 g / cm 3 , preferably 0.989-1.158g / cm 3 , more preferably 1.002-1.098 g / cm 3 , which is measured according to ISO 1183-1:2004.
6. The polymer composition according to any one of the preceding claims, wherein the flame retardant composition comprises piperazine pyrophosphate, melamine phosphate and zinc oxide.
7. The polymer composition according to claim 6, wherein the amount of the piperazine pyrophosphate is 40-69 wt%, preferably 50-67 wt%; the amount of the melamine phosphate is 29-49 wt%, and the amount of the zinc oxide is 1-10 wt%, based on the total amount of the flame retardant composition.
8. The polymer composition according to anyone of the preceding claims, wherein the amount of the first heterophasic propylene copolymer is 15 to 30 wt%, more preferably 20 to 28 wt%, even more preferably 22 to 26 wt%, based on the total polymer composition.
9. The polymer composition according to anyone of the preceding claims, wherein the amount of the second heterophasic propylene copolymer is 40 to 55 wt%, more preferably 42 to 50 wt%, based on the total polymer composition.
10. The polymer composition according to any one of the preceding claims, wherein the amount of the flame retardant composition is 18-27 wt%, preferably 19-24 wt%, based on the total amount of the polymer composition.
11. The polymer composition according to any one of the preceding claims, wherein the amount of the aromatic phosphate is 1.8-8.0 wt%, more preferably 2.5-4.5 wt%, based on the total amount of the polymer composition.
12. The polymer composition according to any one of the preceding claims, wherein the polymer composition has a UL94 rating of V0 at 0.8 mm, wherein the specimens are conditioned in an environment of 23°C, 50% RH for 48 hours after forming and prior to UL94 measurement.
13. The polymer composition according to any one of the preceding claims, wherein the polymer composition has a tensile elongation at break of at least 42%, measured according to ISO 527-1:2019 using 1A specimens.
14. A method for preparing a polymer composition according to any one of claims 1 to 13, comprising the following sequential steps: - providing a first heterophasic propylene copolymer, a second heterophasic propylene copolymer, the flame retardant composition and the aryl phosphate ester; - Mixing the first heterophasic propylene copolymer, the second heterophasic propylene copolymer, the flame retardant composition and the aryl phosphate ester in an extruder.
15. Use of the polymer composition according to any one of claims 1 to 13 for improving the flame retardant properties and flexibility of articles.
Citation Information
Patent Citations
Catalyst components and catalysts for the polymerization of alpha-olefins
US4399054A
Components and catalysts for the polymerization of olefins
US4472524A
Propylene copolymer compositions with high transparency
WO2006010414A1
Flame retardant propylene composition
WO2018019762A1