Polymer composition with high thermal shock resistance
By using a combination of high-performance thermoplastic polymer matrix, impact modifier and fiber filler in electric vehicle components, the problems of existing materials' aging sensitivity and insufficient performance at high temperatures are solved, and high thermal shock resistance and machinery are achieved The combination of performance meets the heat resistance and safety needs of electric vehicles.
Patent Information
- Application Number
- CN202380032133.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-07
- Filing Date
- 2023-01-27
- Publication Date
- 2024-12-06
AI Technical Summary
It is difficult for existing polymer materials to achieve high thermal shock resistance, good insulation and flow properties in electric vehicle components at the same time, and it is sensitive to aging at high temperatures, which cannot meet the demands of electric vehicles for heat resistance and mechanical properties.
A polymer composition containing a high-performance thermoplastic polymer matrix is developed to improve its thermal impact resistance and mechanical properties by dispersing impact modifiers and fiber fillers in the polymer and maintain its performance at high temperatures.
The polymer composition is realized in combination with high thermal shock resistance, good insulation performance and flow performance in electric vehicle components, and maintains mechanical properties at high temperatures to meet the heat resistance and safety requirements of electric vehicles.
Smart Images

Figure CN119095912A_ABST
Abstract
Description
[0001] Related Applications
[0002] This application is based on and claims the benefit of priority of U.S. Provisional Patent Application Serial No. 63 / 361,948, filed on February 1, 2022; U.S. Provisional Patent Application Serial No. 63 / 309,695, filed on February 14, 2022; U.S. Provisional Patent Application Serial No. 63 / 330,807, filed on April 14, 2022; and U.S. Provisional Patent Application Serial No. 63 / 358,904, filed on July 7, 2022, the entire contents of which are incorporated herein by reference. Background Art
[0003] Electric vehicles, such as battery electric vehicles, plug-in hybrid electric vehicles, mild hybrid electric vehicles or full hybrid electric vehicles, typically have an electric powertrain including an electric propulsion source (e.g., a battery) and a transmission. High-performance polymer materials are typically used for various components of electric vehicles, such as high-voltage connectors, power converter housings, battery assembly housings, fluid pumps, inverters, busbars, twisted cables, single-inductance wires, cable crimping, grommet moldings, quick connectors, tees, interconnectors, rails, seals (e.g., brushless DC seals, battery cell seals, etc.), etc. Many of these components are "insert molded" because they are formed by embedding components (e.g., metals) into polymer compositions during the molding process of the polymer composition. Although this process is capable of forming complex parts, the differences in thermal expansion coefficients of different materials are significant, which may cause parts to crack when exposed to temperature changes. Therefore, various attempts have been made to develop performance polymer compositions with high thermal shock resistance. Unfortunately, all attempts have failed to achieve sufficiently high thermal shock resistance to enable them to be used in many EV product applications. Furthermore, to the extent that higher thermal shock resistance can be achieved, there will generally be a corresponding decrease in the insulating, mechanical and / or flow properties of the resulting composition.
[0004] Therefore, there currently exists a need for polymer compositions that can exhibit a combination of high thermal shock resistance and other beneficial properties for use in electric vehicle components. Summary of the invention
[0005] According to one embodiment of the present invention, a polymer composition comprising an impact modifier and a fibrous filler dispersed in a polymer matrix is disclosed. The polymer matrix comprises a high performance thermoplastic polymer exhibiting a load deflection temperature of about 40°C or higher and a melting temperature of about 140°C or higher measured at a load of 1.8 MPa according to ISO 75-2:2013. The polymer composition exhibits a thermal shock resistance value of about 800 or higher.
[0006] Other features and aspects of the invention are described in more detail below. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] A full and enabling disclosure of the present invention including the best mode of carrying out the invention known to those skilled in the art is more particularly set forth in the remainder of the specification including reference to the accompanying drawings, in which:
[0008] Figure 1 An electric vehicle including a component that may include a polymer composition disclosed herein is shown;
[0009] Figure 2 One embodiment of a busbar that may include a polymer composition disclosed herein is shown;
[0010] Figure 3 Battery components that may employ components that may include the polymer compositions disclosed herein are shown;
[0011] Figure 4 An electronic system that may include a component that may include a polymer composition disclosed herein is shown;
[0012] Figure 5 shows that it may be included in Figure 4 Current sensors in electronic systems;
[0013] Figure 6 An inverter system that may be present in an electric vehicle is shown, which includes components that may include the polymer composition disclosed herein;
[0014] Figure 7 is a perspective view of one embodiment of a connector that may include a polymer composition disclosed herein;
[0015] Figure 8 yes Figure 7 A plan view of the connector wherein the first connector portion and the second connector portion are disengaged;
[0016] Fig. 9 yes Figure 7 a plan view of the connector wherein the first connector portion and the second connector portion are engaged;
[0017] Fig.10 Examples of parts that may include the polymer compositions disclosed herein are shown;
[0018] Fig.11 Other components that may include the polymer compositions disclosed herein are shown;
[0019] Fig.12 A low temperature thermal circuit is shown which may include components that may include a polymer composition disclosed herein;
[0020] Fig.13 A high temperature thermal circuit is shown which may include components that may include a polymer composition disclosed herein;
[0021] Fig.14 One embodiment of a water pump that may include the polymer composition disclosed herein is shown; and
[0022] Figures 15 to 18 Sample components that can be used to perform the thermal shock resistance testing described herein are shown.
[0023] In the present specification and drawings, repeated use of reference characters is intended to represent the same or analogous features or elements of the present invention. DETAILED DESCRIPTION
[0024] Those skilled in the art will appreciate that the discussion herein is merely to describe exemplary embodiments and is not intended to limit the broader aspects of the invention.
[0025] In general, the present invention relates to a polymer composition comprising an impact modifier and a fibrous filler dispersed in a polymer matrix. The polymer matrix also comprises a high-performance thermoplastic polymer having a load deflection temperature of about 40°C or higher measured at a load of 1.8 MPa according to ISO 75-2:2013, and a melting temperature of about 140°C or higher. By selectively controlling the specific components of the composition and their relative concentrations, it has been found that the resulting composition can exhibit enhanced thermal shock resistance, which is useful for forming components of electric vehicles, such as battery-powered electric vehicles, fuel cell-powered electric vehicles, plug-in hybrid electric vehicles (PHEVs), mild hybrid electric vehicles (MHEVs), full hybrid electric vehicles (FHEVs), etc. More specifically, the polymer composition can exhibit a thermal shock resistance value of about 800 or higher, in some embodiments about 1000 or higher, in some embodiments about 1200 or higher, in some embodiments about 1500 or higher, in some embodiments about 1800 or higher, in some embodiments about 2000 or higher, and in some embodiments about 3000 or higher. As used herein, "thermal shock resistance value" is determined according to the test described below, and generally refers to the number of heating cycles that a set of sample parts can withstand without visual cracking. High thermal shock resistance can be achieved even at relatively small thickness values, such as about 4 mm or less, in some embodiments about 0.2 mm to about 3.2 mm or less, in some embodiments about 0.4 mm to about 3.0 mm, and in some embodiments about 0.5 mm to about 2.8 mm (e.g., 1.2 mm or 2.5 mm).
[0026] In addition to exhibiting high thermal shock resistance, the polymer composition can also exhibit good insulation performance even at relatively small thickness values such as those described above. The insulation performance of the polymer composition can be characterized by a high comparative tracking index ("CTI"), such as about 150 volts or more, in some embodiments about 200 volts or more, in some embodiments about 300 volts or more, in some embodiments about 550 volts or more, in some embodiments about 580 volts or more, and in some embodiments about 600 volts or more, as measured according to IEC 60112:2003 at a part thickness such as those described above (e.g., 3 mm).
[0027] While exhibiting good thermal shock resistance and high CTI values, the polymer composition can still exhibit good flow properties reflected by relatively low melt viscosity, for example at a temperature of about 310° C. and 400 s according to ISO 11443:2021. -1 The polymer composition may have a shear rate of about 30 kP or less, in some embodiments about 20 kP or less, in some embodiments about 10 kP or less, in some embodiments about 5 kP or less, and in some embodiments about 2 kP to about 50 kP. Despite the low melt viscosity, the polymer composition may still maintain high impact strength and tensile strength, which may provide enhanced flexibility to the resulting part. For example, the polymer composition may exhibit a shear rate of about 5 kJ / m 2 measured at a temperature of 23 ° C according to ISO 180:2019. 2 or greater, such as about 6 kJ / m 2 About 50 kJ / m 2 , and in some embodiments about 7 kJ / m 2 About 30 kJ / m 2 , and about 6 kJ / m measured at 23 °C according to ISO 179-1:2010 2 or greater, for example, about 8 kJ / m 2 About 50 kJ / m 2 , and in some embodiments about 10 kJ / m 2 About 30 kJ / m 2. For example, the composition may exhibit: a tensile stress at break of about 100 MPa or more, in some embodiments about 100 MPa to about 200 MPa, in some embodiments about 110 MPa to about 180 MPa, in some embodiments about 120 MPa to about 170 MPa; a tensile strain at break of about 1% or more, in some embodiments about 1% to about 10%; and / or a tensile modulus of about 15,000 MPa or less, in some embodiments about 1000 MPa to about 12,000 MPa, in some embodiments about 5000 MPa to about 11,000 MPa. The tensile properties may be determined according to ISO Test No. 527:2019 at a temperature of 23°C. The composition may also exhibit a flexural strength of about 50 MPa or greater, in some embodiments about 100 MPa to about 350 MPa, and in some embodiments about 150 MPa to about 300 MPa, and / or a flexural modulus of about 5000 MPa to about 20000 MPa, in some embodiments about 8000 MPa to about 18000 MPa, and in some embodiments about 10000 MPa to about 16000 MPa. Flexural properties may be measured according to ISO 178:2019 at a temperature of 23°C.
[0028] It is noteworthy that the inventors have also found that the polymer composition is not highly sensitive to aging at high temperatures. For example, parts formed by the composition can be aged for about 100 hours or more in an atmosphere at a temperature of about 100°C or higher, about 150°C to about 200°C in some embodiments, and about 200°C to about 260°C (e.g., 240°C) in some embodiments, about 300 hours to about 3000 hours in some embodiments, and about 400 hours to about 2500 hours (e.g., about 1000 hours) in some embodiments. Even after aging, mechanical properties (e.g., impact strength, tensile properties, and / or bending properties) can also be maintained within the above range. For example, the ratio of specific mechanical properties (e.g., simple beam unnotched impact strength, tensile modulus, tensile strength, tensile strain at break, etc.) after "aging" for 1000 hours at 240°C to the initial mechanical properties before such aging can be about 0.4 or greater, about 0.5 or greater in some embodiments, and about 0.6 to 1.0 in some embodiments. For example, in one embodiment, after aging for 1000 hours at an elevated temperature (e.g., 240° C.), the part may exhibit a thermal conductivity greater than about 5 kJ / m 2 as measured at a temperature of 23° C. according to ISO 179-1:2010. 2 , in some embodiments about 6 kJ / m 2 About 30 kJ / m 2 , and in some embodiments about 7 kJ / m 2 About 20 kJ / m 2The part may also exhibit a tensile strength of about 50 MPa to about 300 MPa, about 80 MPa to about 200 MPa, and about 100 MPa to about 150 MPa in some embodiments after aging for 1000 hours in a high temperature atmosphere (e.g., 240°C); a tensile modulus of about 5000 MPa to about 25000 MPa, about 8000 MPa to about 22000 MPa in some embodiments, and about 10000 MPa to about 20000 MPa in some embodiments; and / or a tensile strain at break of about 0.4% to about 8% measured at a temperature of 23°C according to ISO527-2 / 1A:2019, about 0.6% to about 5%, and about 0.8% to about 3% in some embodiments.
[0029] The polymer composition may also exhibit good flame retardant properties. For example, the polymer composition may meet the V-0 flammability standard at a thickness of 0.8 mm. The flame retardant effect may be determined according to the UL 94 vertical burning test procedure of "Tests for the flammability of plastic materials for parts of equipment and appliances", 5th edition (October 29, 1996). The ratings tested according to UL 94 are listed in the following table:
[0030] Table 1
[0031]
[0032] "Afterflame time" is an average value determined by dividing the total afterflame time (total value of all tested samples) by the number of samples. The total afterflame time is the sum of the time (in seconds) that all samples remain ignited after two separate applications of flame, as described in the UL-94 VTM test. The shorter the time, the better the flame retardancy, i.e., the faster the flame is extinguished. For a V-0 rating, the total afterflame time of five (5) samples (each sample with two flames applied) must not exceed 50 seconds. Using the flame retardant of the present invention, the polymer composition can achieve at least a V-1 rating, and typically a V-0 rating, for a specimen having a thickness of 0.8 mm.
[0033] Various embodiments of the present invention will be described in more detail below.
[0034] I. Polymer composition
[0035] A. Thermoplastic polymers
[0036] As described above, the polymer matrix comprises one or more high-performance thermoplastic polymers. "High performance" generally refers to that the polymer has a high degree of heat resistance, such as by measuring about 40 ° C or higher, about 50 ° C or higher, about 60 ° C or higher, about 80 ° C to about 250 ° C, and about 100 ° C to about 200 ° C under a load of 1.8 MPa according to ISO 75-2:2013. The load deflection temperature ("DTUL") of about 100 ° C to about 200 ° C in some embodiments can also be semi-crystalline or crystalline, and exhibit a high melting temperature, such as about 140 ° C or higher, about 150 ° C to about 400 ° C in some embodiments, and about 200 ° C to about 380 ° C in some embodiments. The melting temperature can be measured according to ISO 11357-3:2018 using differential scanning calorimetry ("DSC") . Of course, in addition to exhibiting a high degree of heat resistance and a high melting temperature, the thermoplastic polymer may also exhibit a high glass transition temperature, for example, about 10° C. or higher, in some embodiments about 20° C. or higher, in some embodiments about 30° C. or higher, in some embodiments about 40° C. or higher, in some embodiments about 50° C. or higher, and in some embodiments from about 60° C. to about 320° C. The glass transition temperature may be determined using differential scanning calorimetry according to ISO 11357-2:2020.
[0037] Suitable thermoplastic polymers for this purpose may include, for example, polyolefins (e.g., ethylene polymers, propylene polymers, etc.), polyamides (e.g., aliphatic, semi-aromatic or aromatic polyamides), polyesters, polyarylene sulfides, liquid crystal polymers (e.g., fully aromatic polyesters, polyesteramides, etc.), polyethers (e.g., polyoxymethylene), etc., and blends thereof. The exact choice of polymer system will depend on a variety of factors, such as the nature of other fillers included in the composition, the manner in which the composition is formed and / or processed, and the specific requirements of the intended application.
[0038] For example, aromatic polymers are particularly suitable for certain applications. For example, one example of a suitable semi-crystalline aromatic polymer is an aromatic polyester, which can be a condensation product of at least one diol (e.g., aliphatic and / or alicyclic) and at least one aromatic dicarboxylic acid (e.g., those having 4 to 20 carbon atoms, and in some embodiments, 8 to 14 carbon atoms). Suitable diols can include, for example, neopentyl glycol, cyclohexanedimethanol, 2,2-dimethyl-1,3-propanediol, and a diol having the formula HO(CH2) nThe aliphatic diol of OH, wherein n is an integer from 2 to 10. Suitable aromatic dicarboxylic acids may include, for example, isophthalic acid, terephthalic acid, 1,2-di(p-carboxyphenyl)ethane, 4,4'-dicarboxydiphenyl ether, etc. and combinations thereof. Condensed rings may also be present, such as 1,4-naphthalene dicarboxylic acid or 1,5-naphthalene dicarboxylic acid or 2,6-naphthalene dicarboxylic acid. Specific examples of such aromatic polyesters may include, for example, poly(ethylene terephthalate) (PET), poly(1,4-butylene terephthalate) (PBT), poly(1,3-propylene terephthalate) (PPT), poly(1,4-butylene 2,6-naphthalene dicarboxylate) (PBN), poly(2,6-naphthalene dicarboxylate) (PEN), poly(1,4-cyclohexylene dimethylene terephthalate) (PCT) and mixtures thereof.
[0039] Derivatives and / or copolymers of aromatic polyesters (e.g., polyethylene terephthalate) can also be used. For example, in one embodiment, modified acids and / or modified glycols can be used to form derivatives of such polymers. As used herein, the terms "modified acid" and "modified glycol" mean compounds that define the acid and glycol repeating unit portions that can form polyesters respectively and that can modify polyesters to reduce their crystallinity. Examples of modified acid components can include, but are not limited to, isophthalic acid, phthalic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 2,6-naphthalene dicarboxylic acid, succinic acid, glutaric acid, adipic acid, sebacic acid, suberic acid, 1,12-dodecane dioic acid, etc. In fact, it is generally preferred to use functionalized acid derivatives thereof, such as dimethyl esters, diethyl esters or dipropyl esters of dicarboxylic acids. In practice, anhydrides or acid halides of these acids can also be used. Examples of the modified diol component may include, but are not limited to, neopentyl glycol, 1,4-cyclohexanedimethanol, 1,2-propylene glycol, 1,3-propylene glycol, 2-methyl-1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, Z,8-bis((cyclohexanediol))- ... Hydroxymethyltricyclo-[5.2.1.0]-decane) (wherein Z represents 3, 4 or 5), 1,4-bis(2-hydroxyethoxy)benzene, 4,4'-bis(2-hydroxyethoxy)diphenyl ether [bis-hydroxyethyl bisphenol A], 4,4'-bis(2-hydroxyethoxy)diphenyl sulfide [bis-hydroxyethyl bisphenol S], and diols containing one or more oxygen atoms in the chain, for example, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, etc. Generally speaking, these diols contain 2 to 18 carbon atoms, and in some embodiments contain 2 to 8 carbon atoms. The cycloaliphatic diols can be used in their cis or trans configuration or a mixture of the two forms.
[0040] Aromatic polyesters, as described above, typically have DTUL values of about 40° C. to about 80° C., in some embodiments about 45° C. to about 75° C., and in some embodiments about 50° C. to about 70° C., as measured under a load of 1.8 MPa according to ISO 75-2:2013. Aromatic polyesters also typically have glass transition temperatures of about 30° C. to about 120° C., in some embodiments about 40° C. to about 110° C., and in some embodiments about 50° C. to about 100° C., and melting temperatures of about 170° C. to about 300° C., in some embodiments about 190° C. to about 280° C., and in some embodiments about 210° C. to about 260° C. Aromatic polyesters may also have, for example, an intrinsic viscosity of about 0.1 dl / g to about 6 dl / g, in some embodiments about 0.2 dl / g to about 5 dl / g, and in some embodiments about 0.3 dl / g to about 1 dl / g, as measured according to ISO 1628-5:1998.
[0041] Polyarylene sulfide is also a suitable semi-crystalline aromatic polymer. Polyarylene sulfide can be a homopolymer or a copolymer. For example, the selective combination of dihalogenated aromatic compounds can obtain a polyarylene sulfide copolymer containing not less than two different units. For example, when p-dichlorobenzene is used in combination with m-dichlorobenzene or 4,4'-dichlorodiphenyl sulfone, a polyarylene sulfide copolymer can be formed, and the polyarylene sulfide copolymer contains: a segment having the following structure:
[0042]
[0043] and a segment having the following structure:
[0044]
[0045] Or a segment having the following structure:
[0046]
[0047] Polyarylene sulfide can be linear, semi-linear, branched or cross-linked. Linear polyarylene sulfide generally contains 80 mol% or more of the repeating unit –(Ar–S)–. Such a linear polymer may also contain a small amount of branching units or cross-linking units, but the amount of branching units or cross-linking units is generally less than about 1 mol% of the total monomer units of the polyarylene sulfide. The linear polyarylene sulfide polymer may be a random copolymer or a block copolymer containing the above-mentioned repeating units. Semi-linear polyarylene sulfide may also have a cross-linked structure or a branched structure, which is introduced into the polymer by a small amount of one or more monomers having three or more reactive functional groups. For example, the monomer component used to form the semi-linear polyarylene sulfide may include a certain amount of a polyhalogenated aromatic compound having two or more halogen substituents per molecule, which can be used to prepare a branched polymer. Such a monomer may be represented by the formula R'X nRepresents, wherein each X is selected from chlorine, bromine and iodine, n is an integer from 3 to 6, and R' is an n-valent polyvalent aromatic radical which may have up to about 4 methyl substituents, and the total number of carbon atoms in R' ranges from 6 to about 16. Examples of some polyhalogenated aromatic compounds having more than two halogen substitutions per molecule that can be used to form the semi-linear polyarylene sulfide include 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, 1,3-dichloro-5-bromobenzene, 1,2,4-triiodobenzene, 1,2,3,5-tetrabromobenzene, hexachlorobenzene, 1,3,5-trichloro-2,4,6-trimethylbenzene, 2,2',4,4'-tetrachlorobiphenyl, 2,2',5,5'-tetraiodobiphenyl, 2,2',6,6'-tetrabromo-3,3',5,5'-tetramethylbiphenyl, 1,2,3,4-tetrachloronaphthalene, 1,2,4-tribromo-6-methylnaphthalene, and the like, and mixtures thereof.
[0048] If desired, polyarylene sulfide can be functionalized. For example, disulfide compounds containing reactive functional groups (such as carboxyl, hydroxyl, amine, etc.) can react with polyarylene sulfide. The functionalization of polyarylene sulfide can further provide any optional binding sites between the impact modifier and the polyarylene sulfide, which can improve the distribution of the impact modifier in the entire polyarylene sulfide and prevent phase separation. The disulfide compound can react with the polyarylene sulfide during melt processing to reduce its overall melt viscosity. When used, the disulfide compound generally constitutes about 0.01wt.% to about 3wt.% of the polymer composition, about 0.02wt.% to about 1wt.% in some embodiments, and about 0.05wt.% to about 0.5wt.% in some embodiments. The ratio of the amount of polyarylene sulfide to the amount of the disulfide compound can also be about 1000:1 to about 10:1, about 500:1 to about 20:1 or about 400:1 to about 30:1. Suitable disulfide compounds are generally those with the following formula:
[0049] R 3 –S–S–R 4
[0050] Where R 3 and R 4 can be the same or different and are independently hydrocarbon groups containing from 1 to about 20 carbon atoms. 3 and R 4 It can be an alkyl, cycloalkyl, aryl or heterocyclic group. In certain embodiments, R 3 and R 4 Typically a non-reactive functional group such as phenyl, naphthyl, ethyl, methyl, propyl, etc. Examples of such compounds include diphenyl disulfide, naphthyl disulfide, dimethyl disulfide, diethyl disulfide, and dipropyl disulfide. 3 and R 4It is also possible to include a reactive functional group at the end of the disulfide compound. For example, R 3 and R 4 At least one of the compounds may include a terminal carboxyl group, a hydroxyl group, a substituted or unsubstituted amino group, a nitro group, etc. Examples of the compound may include, but are not limited to, 2,2'-diaminodiphenyl disulfide, 3,3'-diaminodiphenyl disulfide, 4,4'-diaminodiphenyl disulfide, dibenzyl disulfide, dithiosalicylic acid (or 2,2'-dithiobenzoic acid), dithioglycolic acid, α,α'-dithiodilactate, β,β'-dithiodilactate, 3,3'-dithiodipyridine, 4,4'dithiomorpholine, 2,2'-dithiobis(benzothiazole), 2,2'-dithiobis(benzimidazole), 2,2'-dithiobis(benzoxazole), 2-(4'-morpholinodithio)benzothiazole, etc., and mixtures thereof.
[0051] The polyarylene sulfide may have a melt flow rate of about 100 grams per 10 minutes ("g / 10 min") to about 800 g / 10 min, in some embodiments about 200 g / 10 min to about 700 g / 10 min, and in some embodiments about 300 g / 10 min to about 600 g / 10 min, as measured under a load of 5 kg and a temperature of 316°C according to ISO 1133.
[0052] The polyarylene sulfide, as described above, typically has a DTUL value of about 70° C. to about 220° C., in some embodiments about 90° C. to about 200° C., and in some embodiments about 120° C. to about 180° C., as measured under a load of 1.8 MPa according to ISO 75-2:2013. The polyarylene sulfide also typically has a glass transition temperature of about 50° C. to about 120° C., in some embodiments about 60° C. to about 115° C., and in some embodiments about 70° C. to about 110° C., and a melting temperature of about 220° C. to about 340° C., in some embodiments about 240° C. to about 320° C., and in some embodiments about 260° C. to about 300° C.
[0053] In addition to the polymers mentioned above, highly crystalline aromatic polymers can also be used in the polymer composition. A particularly suitable example of such a polymer is a liquid crystal polymer, which has a high crystallinity that enables it to effectively fill small gaps in the mold. Liquid crystal polymers are generally classified as "thermotropic" because liquid crystal polymers can have a rod-like structure and exhibit crystalline behavior in their molten state (e.g., thermotropic nematic state). Such polymers typically have a DTUL value of about 120°C to about 340°C measured under a load of 1.8MPa according to ISO 75-2:2013, about 140°C to about 320°C in some embodiments, and about 150°C to about 300°C in some embodiments. The polymer also has a relatively high melting temperature, for example, about 250°C to about 400°C, about 280°C to about 390°C in some embodiments, and about 300°C to about 380°C in some embodiments. It is known in the art that such a polymer can be formed by one or more repeating units.
[0054] For example, the liquid crystal polymer may include one or more aromatic ester repeating units, typically in an amount of about 60 mol.% to 100 mol.%, in some embodiments about 70 mol.% to about 99.5 mol.%, and in some embodiments about 80 mol.% to about 99 mol.%. The aromatic ester repeating unit may generally be represented by the following formula (V):
[0055]
[0056] in,
[0057] Ring B is a substituted or unsubstituted 6-membered aryl group (e.g., 1,4-phenylene or 1,3-phenylene), a substituted or unsubstituted 6-membered aryl group fused to a substituted or unsubstituted 5-membered or 6-membered aryl group (e.g., 2,6-naphthalene), or a substituted or unsubstituted 6-membered aryl group linked to a substituted or unsubstituted 5-membered or 6-membered aryl group (e.g., 4,4-biphenylene); and
[0058] Y1 and Y2 are independently O, C(O), NH, C(O)HN or NHC(O).
[0059] Typically, at least one of Y1 and Y2 is C(O). Examples of such aromatic ester repeating units may include, for example, aromatic dicarboxyl repeating units (Y1 and Y2 in Formula V are C(O)), aromatic hydroxycarboxyl repeating units (Y1 in Formula V is O, and Y2 is C(O)), and various combinations thereof.
[0060] For example, aromatic dicarboxylic acid repeating units derived from aromatic dicarboxylic acids and their alkyl, alkoxy, aryl and halogen substitutes and combinations thereof may be used, such as terephthalic acid, isophthalic acid, 2,6-naphthalene dicarboxylic acid, diphenyl ether-4,4'-dicarboxylic acid, 1,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, 4,4'-dicarboxybiphenyl, bis(4-carboxyphenyl) ether, bis(4-carboxyphenyl) butane, bis(4-carboxyphenyl) ethane, bis(3-carboxyphenyl) ether, bis(3-carboxyphenyl) ethane, etc. Particularly suitable aromatic dicarboxylic acids may include, for example, terephthalic acid ("TA"), isophthalic acid ("IA") and 2,6-naphthalene dicarboxylic acid ("NDA"). When used, repeating units derived from aromatic dicarboxylic acids (e.g., IA, TA, and / or NDA) typically constitute from about 5 mol.% to about 60 mol.%, in some embodiments from about 10 mol.% to about 50 mol.%, and in some embodiments from about 20 mol.% to about 40 mol.% of the polymer.
[0061] Aromatic hydroxycarboxylic acid repeating units derived from aromatic hydroxycarboxylic acids and their alkyl, alkoxy, aryl and halogen substitutes and combinations thereof may also be used, such as 4-hydroxybenzoic acid; 4-hydroxy-4'-biphenylcarboxylic acid; 2-hydroxy-6-naphthoic acid; 2-hydroxy-5-naphthoic acid; 3-hydroxy-2-naphthoic acid; 2-hydroxy-3-naphthoic acid; 4'-hydroxyphenyl-4-benzoic acid; 3'-hydroxyphenyl-4-benzoic acid; 4'-hydroxyphenyl-3-benzoic acid, etc. Particularly suitable aromatic hydroxycarboxylic acids are 4-hydroxybenzoic acid ("HBA") and 6-hydroxy-2-naphthoic acid ("HNA"). When used, repeating units derived from hydroxycarboxylic acids (e.g., HBA and / or HNA) typically constitute from about 10 mol.% to about 75 mol.%, in some embodiments from about 20 mol.% to about 60 mol.%, and in some embodiments from about 30 mol.% to about 50 mol.% of the polymer.
[0062] Other repeating units may also be used in the polymer. In certain embodiments, for example, repeating units derived from aromatic diols and their alkyl, alkoxy, aryl and halogen substituents and combinations thereof may be used, such as hydroquinone, resorcinol, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 4,4'-dihydroxybiphenyl (or 4,4'-biphenol), 3,3'-dihydroxybiphenyl, 3,4'-dihydroxybiphenyl, 4,4'-dihydroxybiphenyl ether, bis(4-hydroxyphenyl)ethane, etc. Particularly suitable aromatic diols may include, for example, hydroquinone ("HQ") and 4,4'-biphenol ("BP"). When used, repeating units derived from aromatic diols (e.g., HQ and / or BP) typically constitute about 1 mol.% to about 50 mol.%, in some embodiments about 5 mol.% to about 45 mol.%, and in some embodiments about 10 mol.% to about 40 mol.%. Repeating units derived from, for example, aromatic amides (e.g., acetaminophen ("APAP")) and / or aromatic amines (e.g., 4-aminophenol ("AP"), 3-aminophenol, 1,4-phenylenediamine, 1,3-phenylenediamine, etc.) may also be used. When used, repeating units derived from aromatic amides (e.g., APAP) and / or aromatic amines (e.g., AP) typically constitute from about 0.1 mol.% to about 20 mol.%, in some embodiments from about 0.5 mol.% to about 15 mol.%, and in some embodiments from about 1 mol.% to about 10 mol.% of the polymer. It should also be understood that various other monomer repeating units may be incorporated into the polymer. For example, in certain embodiments, the polymer may contain one or more repeating units derived from non-aromatic monomers (e.g., aliphatic or alicyclic hydroxycarboxylic acids, dicarboxylic acids, diols, amides, amines, etc.). Of course, in other embodiments, if the polymer lacks repeating units derived from non-aromatic (e.g., aliphatic or alicyclic) monomers, the polymer may be "all aromatic".
[0063] In a particular embodiment, the liquid crystal polymer may be a "high naphthalene" polymer in that it contains relatively high levels of repeating units derived from naphthalene hydroxycarboxylic acid and naphthalene dicarboxylic acid (e.g., NDA, HNA) or a combination thereof. That is, the total amount of repeating units derived from naphthalene hydroxycarboxylic acid and / or naphthalene dicarboxylic acid (e.g., NDA, HNA, or a combination of HNA and NDA) is typically about 10 mol.% or more of the polymer, in some embodiments about 12 mol.% or more, in some embodiments about 15 mol.% or more, and in some embodiments about 18 mol.% to about 35 mol.%. In one embodiment, for example, repeating units derived from NDA may constitute 10 mol.% or more of the polymer, in some embodiments about 12 mol.% or more, in some embodiments about 15 mol.% or more, and in some embodiments about 18 mol.% to about 35 mol.%. When used, the molar ratio of repeating units derived from HBA to repeating units derived from naphthalene units (e.g., NDA, HNA, or NDA and HNA) can be selectively controlled within a specific range to help achieve the desired properties, such as from about 1 to about 20, in some embodiments from about 1.5 to about 15, and in some embodiments from about 2 to about 10. The polymer may also contain repeating units derived from: aromatic dicarboxylic acids (e.g., IA and / or TA) in an amount of from about 1 mol.% to about 20 mol.%, in some embodiments from about 2 mol.% to about 15 mol.%; and / or aromatic diols (e.g., BP and / or HQ) in an amount of from about 20 mol.% to about 50 mol.%, in some embodiments from about 30 mol.% to about 45 mol.%. However, in some cases, it may be desirable to minimize the presence of such monomers in the polymer to help achieve the desired properties. For example, the total amount of repeating units derived from aromatic dicarboxylic acids (e.g., IA and / or TA) and / or aromatic diols (e.g., BP and / or HQ) can be about 5 mol.% or less, in some embodiments about 4 mol.% or less, and in some embodiments, from about 0.1 mol.% to about 3 mol.% of the polymer.
[0064] In certain embodiments, all liquid crystal polymers are "high naphthalene" polymers as described above. However, in other embodiments, "low naphthalene" liquid crystal polymers may also be used in the composition, wherein the total amount of repeating units derived from naphthalene hydroxycarboxylic acid and / or naphthalene dicarboxylic acid (e.g., NDA, HNA, or a combination of HNA and NDA) is less than 10 mol.%, in some embodiments about 8 mol.% or less, in some embodiments about 6 mol.% or less, and in some embodiments about 1 mol.% to about 5 mol.%. When used, it is generally desirable that this low naphthalene polymer exists only in a relatively low amount. For example, when used, low naphthalene liquid crystal polymers generally constitute about 1 wt.% to about 50 wt.% of the total amount of liquid crystal polymers in the composition, about 10 wt.% to about 45 wt.% in some embodiments, and about 15 wt.% to about 40 wt.% in some embodiments, and constitute about 0.5 wt.% to about 45 wt.% of the entire composition, about 2 wt.% to about 35 wt.% in some embodiments, and about 5 wt.% to about 25 wt.% in some embodiments. In contrast, high naphthalene liquid crystal polymers typically constitute from about 50 wt.% to about 99 wt.%, in some embodiments from about 55 wt.% to about 95 wt.%, and in some embodiments from about 60 wt.% to about 85 wt.% of the total amount of liquid crystal polymers in the composition, and from about 25 wt.% to about 65 wt.%, in some embodiments from about 30 wt.% to about 60 wt.%, and in some embodiments from about 35 wt.% to about 55 wt.% of the entire composition.
[0065] Of course, in addition to aromatic polymers, aliphatic polymers may also be suitable as high-performance thermoplastic polymers in the polymer matrix. For example, in one embodiment, polyamides may be used, which typically have CO-NH linkages in the main chain and are obtained by condensation of aliphatic diamines and aliphatic dicarboxylic acids, by ring-opening polymerization of lactams, or by self-condensation of aminocarboxylic acids. For example, polyamides may contain aliphatic repeating units derived from aliphatic diamines, which typically have 4 to 14 carbon atoms. Examples of such diamines include: linear aliphatic alkylene diamines, such as 1,4-tetramethylethylenediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, etc.; branched aliphatic alkylene diamines, such as 2-methyl-1,5-pentanediamine, 3-methyl-1,5-pentanediamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, 2,4-dimethyl-1,6-hexanediamine, 2-methyl-1,8-octanediamine, 5-methyl-1,9-nonanediamine, etc.; and combinations thereof. Aliphatic dicarboxylic acids may include, for example, adipic acid, sebacic acid, etc. Specific examples of such aliphatic polyamides include, for example, nylon-4 (poly-α-pyrrolidone), nylon-6 (polycaproamide), nylon-11 (polyundecamide), nylon-12 (polydodecanamide), nylon-46 (polytetramethylene adipamide), nylon-66 (polyhexamethylene adipamide), nylon-610 and nylon-612. Particularly suitable are nylon-6 and nylon-66.
[0066] It should be understood that aromatic monomer units may also be included in the polyamide, so that it is considered aromatic (only aromatic monomer units are both aliphatic monomer units and aromatic monomer units). Examples of aromatic dicarboxylic acids may include, for example, terephthalic acid, isophthalic acid, 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,4-benzenedioxy-diacetic acid, 1,3-benzenedioxy-diacetic acid, biphenyl dicarboxylic acid, 4,4'-oxydibenzoic acid, diphenylmethane-4,4'-dicarboxylic acid, diphenyl sulfone-4,4'-dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, and the like. Particularly suitable aromatic polyamides may include: poly(nonylene terephthalamide) (PA9T), poly(nonylene terephthalamide / nonylene sebacamide) (PA9T / 910), poly(nonylene terephthalamide / nonylene dodecanamide) (PA9T / 912), poly(nonylene terephthalamide / 11-aminoundecaneamide) (PA9T / 11), poly(nonylene terephthalamide / 12-aminododecaneamide) (PA9T / 12), poly(decylene terephthalamide / 11-aminoundecaneamide) (PA10T / 11), poly(decylene terephthalamide / 12-aminododecaneamide) (PA10T / 12), poly(decylene terephthalamide / decylene dodecanamide) (PA10T / 12), poly(decylene terephthalamide / decylene dodecanamide) (PA10T / 12), poly(decylene terephthalamide / decylene dodecanamide) (PA10T / 12), poly(decylene terephthalamide / decylene dodecanamide) (PA10T / 12), poly(decylene terephthalamide / decylene dodecanamide) (PA10T / 12).
[0013] Poly(decylene terephthalamide / decylene dodecanamide) (PA10T / 1010), Poly(decylene terephthalamide / decylene dodecanamide) (PA10T / 1012), Poly(decylene terephthalamide / butylene adipamide) (PA10T / 46), Poly(decylene terephthalamide / caprolactam) (PA10T / 6), Poly(decylene terephthalamide / hexylene hexane diamide) (PA10T / 66), Poly(dodecylene terephthalamide / dodecylene dodecanamide) (PA12T / 1212), Poly(dodecylene terephthalamide / caprolactam) (PA12T / 6), Poly(dodecylene terephthalamide / hexylene hexane diamide) (PA12T / 66), etc.
[0067] Polyamides suitable for use in polymer matrices are generally crystalline or semi-crystalline in nature and therefore have a measurable melting temperature. The melting temperature can be relatively high so that the composition can provide a considerable degree of heat resistance to the resulting part. For example, the melting temperature of the polyamide can be about 220°C or higher, in some embodiments about 240°C to about 325°C, and in some embodiments about 250°C to about 335°C. The polyamide may also have a relatively high glass transition temperature, for example, about 30°C or higher, in some embodiments about 40°C or higher, and in some embodiments about 45°C to about 140°C.
[0068] The propylene polymer can also be an aliphatic high-performance polymer suitable for use in a polymer matrix. Any of a variety of propylene polymers or combinations of propylene polymers, such as propylene homopolymers (e.g., syndiotactic, atactic, isotactic, etc.), propylene copolymers, etc., can generally be used in the polymer matrix. In one embodiment, for example, a propylene polymer that is an isotactic or syndiotactic homopolymer can be used. The term "syndiotactic" generally refers to a stereoregularity in which a considerable portion of the methyl groups, if not all, alternate on opposite sides along the polymer chain. On the other hand, the term "isotactic" generally refers to a stereoregularity in which a considerable portion of the methyl groups, if not all, are located on the same side of the polymer chain. In yet other embodiments, copolymers of propylene and α-olefin monomers can be used. Specific examples of suitable α-olefin monomers include: ethylene; 1-butene; 3-methyl-1-butene; 3,3-dimethyl-1-butene; 1-pentene; 1-pentene with one or more methyl, ethyl or propyl substituents; 1-hexene with one or more methyl, ethyl or propyl substituents; 1-heptene with one or more methyl, ethyl or propyl substituents; 1-octene with one or more methyl, ethyl or propyl substituents; 1-nonene with one or more methyl, ethyl or propyl substituents; 1-decene substituted with ethyl, methyl or dimethyl; 1-dodecene; and styrene. The propylene content of such copolymers may be from about 60 mol.% to about 99 mol.%, in some embodiments from about 80 mol.% to about 98.5 mol.%, and in some embodiments from about 87 mol.% to about 97.5 mol.%. The α-olefin content may also be from about 1 mol.% to about 40 mol.%, in some embodiments from about 1.5 mol.% to about 15 mol.%, and in some embodiments from about 2.5 mol.% to about 13 mol.%.
[0069] Suitable propylene polymers generally have DTUL values of about 80° C. to about 250° C., in some embodiments about 100° C. to about 220° C., and in some embodiments about 110° C. to about 200° C., as measured under a load of 1.8 MPa according to ISO 75-2:2013. The glass transition temperature of such polymers may likewise be from about 10° C. to about 80° C., in some embodiments from about 15° C. to about 70° C., and in some embodiments from about 20° C. to about 60° C. In addition, the melting temperature of such polymers may be from about 50° C. to about 250° C., in some embodiments from about 90° C. to about 220° C., and in some embodiments from about 100° C. to about 200° C.
[0070] The oxymethylene polymer may also be an aliphatic high-performance polymer suitable for use in a polymer matrix. The oxymethylene polymer may be one or more homopolymers, copolymers, or mixtures thereof. Homopolymers are prepared by polymerizing formaldehyde or formaldehyde equivalents (e.g., cyclic oligomers of formaldehyde). Copolymers may contain one or more comonomers commonly used to prepare polyoxymethylene compositions. Commonly used comonomers include alkylene oxides of 2 to 12 carbon atoms. If a copolymer is selected, the amount of the comonomer is generally no more than 20 wt.%, no more than 15 wt.% in some embodiments, and about 2 wt.% in some embodiments. Comonomers may include ethylene oxide and butylene oxide. Preferably, homopolymers and copolymers are: 1) those whose terminal hydroxyl groups are terminated by chemical reaction to form ester groups or ether groups; or 2) copolymers that are not fully terminated but have some free hydroxyl ends from the comonomer units. In either case, typical end groups are acetate and methoxy.
[0071] B. Impact modifier
[0072] As described above, impact modifiers may also be used in the polymer composition. Typically, the impact modifier comprises about 1 to about 20 parts by weight per 100 parts by weight of the polyarylene sulfide, in some embodiments about 2 to about 15 parts by weight, and in some embodiments about 5 to about 10 parts by weight. For example, the impact modifier may comprise about 0.1 wt.% to about 20 wt.%, in some embodiments about 0.5 wt.% to about 15 wt.%, and in some embodiments about 1 wt.% to about 10 wt.% of the polymer composition.
[0073] Examples of suitable impact modifiers can include, for example, polyepoxides, polyurethanes, polybutadienes, acrylonitrile-butadiene-styrene, polyamides, block copolymers (e.g., polyether-polyamide block copolymers), etc., and mixtures thereof. In one embodiment, "epoxy-functionalized" olefin copolymers are used because they contain an average of two or more epoxy functional groups per molecule. The copolymers typically contain olefin monomer units derived from one or more alpha-olefins. Examples of such monomers include, for example, linear and / or branched alpha-olefins having 2 to 20 carbon atoms and typically 2 to 8 carbon atoms. Specific examples include: ethylene, propylene, 1-butene; 3-methyl-1-butene; 3,3-dimethyl-1-butene; 1-pentene; 1-pentene with one or more methyl, ethyl or propyl substituents; 1-hexene with one or more methyl, ethyl or propyl substituents; 1-heptene with one or more methyl, ethyl or propyl substituents; 1-octene with one or more methyl, ethyl or propyl substituents; 1-nonene with one or more methyl, ethyl or propyl substituents; 1-decene substituted with ethyl, methyl or dimethyl; 1-dodecene; and styrene. Particularly desirable α-olefin monomers are ethylene and propylene. The copolymer may also contain epoxy-functionalized monomer units. An example of such a unit is an epoxy-functionalized (meth)acrylic acid monomer component. As used herein, the term "(meth)acrylic acid" includes acrylic and methacrylic acid monomers, as well as salts or esters thereof, such as acrylate and methacrylate monomers. For example, suitable epoxy-functional (meth)acrylic monomers may include, but are not limited to, those containing 1,2-epoxy groups, such as glycidyl acrylate and glycidyl methacrylate. Other suitable epoxy-functional monomers include allyl glycidyl ether, glycidyl ethacrylate, and glycidyl itaconate. Other suitable monomers may also be used to help achieve the desired molecular weight.
[0074] Of course, the copolymer may also contain other monomer units known in the art. For example, another suitable monomer may include a non-epoxy functional (meth)acrylic monomer. Examples of such (meth)acrylic monomers may include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, sec-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-pentyl acrylate, isopentyl acrylate, isobornyl acrylate, n-hexyl acrylate, 2-ethylbutyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, n-decyl acrylate, methylcyclohexyl acrylate, cyclopentyl acrylate, cyclohexyl acrylate, methyl methacrylate, ethyl methacrylate, 2-hydroxyethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, isopropyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, isopentyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, 2-ethylbutyl methacrylate, methylcyclohexyl methacrylate, cinnamyl methacrylate, crotonyl methacrylate, cyclohexyl methacrylate, cyclopentyl methacrylate, 2-ethoxyethyl methacrylate, isobornyl methacrylate, and the like, and combinations thereof. For example, in a particular embodiment, the copolymer can be a terpolymer formed from an epoxy-functional (meth) acrylic monomer component, an α-olefin monomer component, and a non-epoxy-functional (meth) acrylic monomer component. The copolymer can be, for example, poly(ethylene-co-butyl acrylate-co-glycidyl methacrylate) having the following structure:
[0075]
[0076] where x, y, and z are 1 or greater.
[0077] The corresponding parts of the monomer components can be selected to achieve a balance between epoxy reactivity and melt flow rate. More specifically, high epoxy monomer content can lead to good reactivity with polyarylene sulfide, but too high a content may reduce the melt flow rate to the extent that the copolymer adversely affects the melt strength of the polymer blend. Therefore, in most embodiments, epoxy-functional (meth) acrylic monomers constitute about 1wt.% to about 20wt.% of the copolymer, about 2wt.% to about 15wt.% in some embodiments, and about 3wt.% to about 10wt.% in some embodiments. Similarly, alpha-olefin monomers can constitute about 55wt.% to about 95wt.% of the copolymer, about 60wt.% to about 90wt.% in some embodiments, and about 65wt.% to about 85wt.% in some embodiments. When used, other monomer components (e.g., non-epoxy-functional (meth) acrylic monomers) can constitute about 5wt.% to about 35wt.% of the copolymer, about 8wt.% to about 30wt.% in some embodiments, and about 10wt.% to about 25wt.% in some embodiments. The resulting melt flow rate is typically from about 1 gram / 10 minutes to about 30 grams / 10 minutes ("g / 10 min"), in some embodiments from about 2 g / 10 min to about 20 g / 10 min, and in some embodiments from about 3 g / 10 min to about 15 g / 10 min, as measured in accordance with ASTM D1238-13 under a 2.16 kg load and a temperature of 190°C.
[0078] If desired, other impact modifiers can also be used in combination with epoxy functionalized impact modifiers. For example, other impact modifiers can include block copolymers, at least one of which is made of a material that is hard at room temperature but fluid when heated, and another is a softer material that is rubbery at room temperature. For example, the block copolymer can have an AB or ABA block copolymer repeating structure, wherein A represents a hard segment and B is a soft segment. The non-limiting strength of the impact modifier with an AB repeating structure includes polyamide / polyether, polysulfone / polydimethylsiloxane, polyurethane / polyester, polyurethane / polyether, polyester / polyether, polycarbonate / polydimethylsiloxane and polycarbonate / polyether. The triblock copolymer can also include polystyrene as a hard segment and polybutadiene, polyisoprene or polyethylene-to-polybutylene as a soft segment. Similarly, styrene butadiene repeating copolymers and polystyrene / polyisoprene repeating polymers can be used. In a specific embodiment, the block copolymer can have alternating polyamide blocks and polyether blocks. Such materials are commercially available, for example from Atofina as PEBAX TMThe polyamide blocks may be derived from copolymers of a diacid component and a diamine component, or may be prepared by homopolymerization of a cyclic lactam. The polyether blocks may be derived from homopolymers or copolymers of cyclic ethers such as ethylene oxide, propylene oxide, and tetrahydrofuran.
[0079] C. Fiber filler
[0080] The polymer composition may also use fibrous fillers. Such fibrous fillers generally constitute about 10 to about 80 parts by weight per 100 parts by weight of polyarylene sulfide, in some embodiments about 20 to about 75 parts by weight, and in some embodiments about 25 to about 60 parts by weight. For example, the fibrous filler may constitute about 10 wt.% to about 60 wt.%, in some embodiments about 15 wt.% to about 50 wt.%, and in some embodiments about 20 wt.% to about 45 wt.% of the polymer composition.
[0081] Generally, any of a variety of different types of fibers may be used: such as those inorganic fibers derived from glass; silicates, such as neosilicates, tantalum silicates, inosilicates (e.g., calcium inosilicates, such as wollastonite; calcium magnesium inosilicates, such as tremolite; calcium magnesium iron inosilicates, such as actinolite; magnesium iron inosilicates, such as anthophyllite; etc.), phyllosilicates (e.g., aluminum phyllosilicates, such as palygorskite), reticular silicates, etc.; sulfates, such as calcium sulfate (e.g., dehydrated or anhydrite); mineral wool (e.g., rock wool or slag wool); etc. Glass fibers are particularly suitable for the present disclosure, such as those formed from E-glass, A-glass, C-glass, D-glass, AR-glass, R-glass, S1-glass, S2-glass, etc., and mixtures thereof. If desired, the glass fibers may be provided with a sizing agent or other coating known in the art.
[0082] The fiber can have any desired cross-sectional shape, such as round, flat, etc. In certain embodiments, it may be desirable to use fibers with relatively flat cross-sectional dimensions, whose aspect ratio (i.e., cross-sectional width divided by cross-sectional thickness) is about 1.5 to about 10, in some embodiments about 2 to about 8, and in some embodiments about 3 to about 5. When such flat fibers are used at a certain concentration, they can further improve the mechanical properties of molded parts without having a significant adverse effect on the melt viscosity of the polymer composition. For example, the fiber can have a nominal width of about 1 micron to about 50 microns, in some embodiments about 5 microns to about 50 microns, and in some embodiments about 10 microns to about 35 microns. The fiber can also have a nominal thickness of about 0.5 microns to about 30 microns, in some embodiments about 1 micron to about 20 microns, and in some embodiments about 3 microns to about 15 microns. In addition, the fiber can have a narrow size distribution. That is, at least about 60 vol.% of the fiber, in some embodiments at least about 70 vol.% of the fiber, and in some embodiments at least about 80 vol.% of the fiber can have a width and / or thickness within the above range. In the molded part, the volume average length of the fibers may be from about 10 microns to about 500 microns, in some embodiments from about 100 microns to about 400 microns, and in some embodiments from about 150 microns to about 350 microns.
[0083] D. Optional components
[0084] In addition to the above components, the polymer composition can also include various other optional components to help improve its overall performance. For example, in one embodiment, a siloxane polymer can be used in the polymer composition. This siloxane polymer generally constitutes about 0.05 weight part to about 10 weight parts per 100 weight parts of polyarylene sulfide, about 0.1 weight part to about 8 weight parts in some embodiments, and about 0.5 weight part to about 5 weight parts in some embodiments. For example, the siloxane polymer can constitute about 0.05wt.% to about 15wt.% of the polymer composition, about 0.5wt.% to about 10wt.% in some embodiments, and about 1wt.% to about 8wt.% in some embodiments. Not limited by theory, it is believed that the siloxane polymer can, for example, improve the processing of the composition by providing better mold filling, internal lubrication, demoulding, etc. In addition, it is believed that the siloxane polymer is unlikely to migrate or diffuse to the surface of the composition, which further minimizes the possibility of phase separation and further contributes to damping impact energy. The siloxane polymers generally have a high molecular weight, such as a weight average molecular weight of about 100,000 grams per mole or greater, in some embodiments about 200,000 grams per mole or greater, and in some embodiments, from about 500,000 grams per mole to about 2,000,000 grams per mole. The siloxane polymers may also have a relatively high kinematic viscosity at 25° C., such as about 10,000 centistokes or greater, in some embodiments about 30,000 centistokes or greater, and in some embodiments, from about 50,000 centistokes to about 50×10 6 Centistokes, for example about 1×10 6 Centistokes to 50×10 6 Centistokes. The viscosity of silicone polymers can be measured according to ASTM D445-21.
[0085] Any of a variety of high molecular weight siloxane polymers can generally be used in the polymer composition. High molecular weight siloxane polymers generally include repeating units of siloxane-based monomer residues. As used herein, "siloxane" refers to repeating units of monomer residues having the following structure:
[0086]
[0087] Where R 1 and R 2 Independently hydrogen or a hydrocarbyl moiety, referred to as an "M" group in silicone chemistry.
[0088] Silicone resins may include branch points, e.g.
[0089]
[0090] It is known in silicone chemistry as the "Q" group, or
[0091]
[0092] It is known as the "T" group in silicone chemistry.
[0093] As used herein, the term "hydrocarbyl" refers to a monovalent group formed by removing a hydrogen atom from a hydrocarbon (e.g., an alkyl group such as ethyl, or an aryl group such as phenyl). In one or more embodiments, the siloxane monomer residue can be any dialkylsiloxane, diarylsiloxane, dialkylarylsiloxane, or diaralkylsiloxane having the same or different alkyl, aryl, alkaryl, or aralkyl moieties. In one embodiment, R 1 and R 2 Each independently is C1 to C 20 , C1 to C 12 or C1 to C6 alkyl (e.g., methyl, ethyl, propyl, butyl, etc.), aryl (e.g., phenyl), alkaryl, aralkyl, cycloalkyl (e.g., cyclopentyl), arylene (arylenyl), alkenyl, cycloalkenyl (e.g., cyclohexenyl), alkoxy (e.g., methoxy), etc., and combinations thereof. In various embodiments, R 1 and R 2 Can have the same or different number of carbon atoms. In various embodiments, R 1 and R 2 Each hydrocarbon group is a saturated and optionally linear alkyl group. In addition, the alkyl group in this embodiment is not limited to the R of the polymer chain. 1 and R 2 Each of can be the same. Applicable to R 1 and R 2 Non-limiting examples of the alkyl group include methyl, ethyl, 1-propyl, 2-propyl, 1-butyl, isobutyl, tert-butyl, or a combination of two or more thereof.
[0094] In addition, the siloxane polymers may contain various terminal groups as R 1 and / or R 2 Groups such as vinyl, hydroxyl, hydride, isocyanate, epoxy, acidic group, halogen atom, alkoxy, acyloxy, ketoxime, amino, amide, acidamide, aminooxy, sulfhydryl, alkenyloxy, alkoxyalkoxy, or aminooxy, and combinations thereof. In addition, the polymer composition may include a mixture of two or more siloxane polymers.
[0095] In some embodiments, high molecular weight siloxane polymers may be increased by copolymerizing a plurality of siloxane polymers having a low weight average molecular weight (e.g., a molecular weight of less than 100,000 g / mole) with a polysiloxane linker. For example, in one particular embodiment, a resin may be formed by copolymerizing one or more low molecular weight siloxane polymers with a linear polydiorganosiloxane linker, as described in U.S. Pat. No. 6,072,012 to Juen et al. The substantially linear polydiorganosiloxane linker may have the following general formula:
[0096] (R 3 (3-p) R 4 p SiO 1 / 2 )(R 3 2SiO 2 / 2 ) x ((R 3 R 4 SiO 2 / 2 )(R 3 2SiO 2 / 2 ) x ) y (R 3 (3-p) R 4 p SiO 1 / 2 )
[0097] in,
[0098] Each R 3 is a monovalent group independently selected from alkyl, aryl and aralkyl;
[0099] Each R 4 is a monovalent group independently selected from hydrogen, hydroxyl, alkoxy, oxime, alkyloxime and aryloxime, wherein at least two R 5 The groups are usually present in each molecule and bonded to different silicon atoms;
[0100] p is 0, 1, 2, or 3;
[0101] x is 0 to 200, and in some embodiments 0 to 100; and
[0102] y is 0 to 200, and in some embodiments 0 to 100.
[0103] In certain embodiments, the siloxane polymer can be provided in the form of a masterbatch including a carrier resin. For example, the carrier resin can constitute about 0.05wt.% to about 15wt.%, in some embodiments about 0.1wt.% to about 10wt.%, and in some embodiments about 0.5wt.% to about 8wt.% of the polymer composition. Any of a variety of carrier resins can be used, such as polyolefins (ethylene polymers, propylene polymers, etc.), polyamides, etc. For example, in one embodiment, the carrier resin is an ethylene polymer. The ethylene polymer can be ethylene and α-olefins (e.g., C3-C 20 α-olefins or C3-C 12 Copolymers of α-olefins (e.g., α-olefins) are preferably copolymers of 1-butylene, 1-butylene, 1-hexene, 1-octene, 1-octene, 1-nonene, 1-decene substituted with ethyl, methyl or dimethyl; 1-dodecene, and styrene. Particularly desirable α-olefin comonomers are 1-butylene, 1-hexene, and 1-octene. The ethylene content of such copolymers may be from about 60 mol.% to about 99 mol.%, in some embodiments from about 80 mol.% to about 98.5 mol.%, and in some embodiments from about 87 mol.% to about 97.5 mol.%. The alpha-olefin content may likewise be from about 1 mol.% to about 40 mol.%, in some embodiments from about 1.5 mol.% to about 15 mol.%, and in some embodiments from about 2.5 mol.% to about 13 mol.%. The density of the ethylene polymer may vary depending on the type of polymer used, but is generally from about 0.85 g / cm3 to about 0.96 g / cm3 (g / cm 3 ). For example, the density of a polyethylene "plastomer" may be about 0.85 g / cm 3 To about 0.91g / cm 3 Similarly, the density of "linear low density polyethylene" (LLDPE) can be about 0.91 g / cm 3 To about 0.940g / cm 3 ; The density of "low density polyethylene" (LDPE) can be about 0.910 g / cm 3 To about 0.940g / cm 3 ; while the density of "high-density polyethylene" (HDPE) can be about 0.940 g / cm 3To about 0.960g / cm 3 , such as determined according to ASTM D792. Some non-limiting examples of high molecular weight siloxane polymer masterbatches that can be used include, for example, those available from Dow Corning under the trade names MB50-001, MB50-002, MB50-313, MB50-314, and MB50-321.
[0104] If desired, an organosilane compound may be used in the polymer composition, for example, in an amount of about 0.1 to about 8 parts by weight, in some embodiments about 0.3 to about 5 parts by weight, and in some embodiments about 0.5 to about 3 parts by weight per 100 parts by weight of polyarylene sulfide. For example, the organosilane compound may constitute about 0.01 wt.% to about 3 wt.%, in some embodiments about 0.02 wt.% to about 2 wt.%, and in some embodiments about 0.05 wt.% to about 1 wt.% of the polymer composition. For example, the organosilane compound may be any alkoxysilane known in the art, such as vinyl alkoxysilane, epoxy alkoxysilane, amino alkoxysilane, mercapto alkoxysilane, and combinations thereof. In one embodiment, for example, the organosilane compound may have the following general formula:
[0105] R 5 -Si-(R 6 )3,
[0106] in,
[0107] R 5 is a sulfide group (e.g. -SH), an alkyl sulfide containing 1 to 10 carbon atoms (e.g. mercaptopropyl, mercaptoethyl, mercaptobutyl, etc.), an alkenyl sulfide containing 2 to 10 carbon atoms, an alkynyl sulfide containing 2 to 10 carbon atoms, an amino group (e.g. NH2), an aminoalkyl group containing 1 to 10 carbon atoms (e.g. aminomethyl, aminoethyl, aminopropyl, aminobutyl, etc.), an aminoalkenyl group containing 2 to 10 carbon atoms, an aminoalkynyl group containing 2 to 10 carbon atoms, etc.;
[0108] R 6 It is an alkoxy group having 1 to 10 carbon atoms, for example, methoxy, ethoxy, propoxy and the like.
[0109] Some representative examples of organosilane compounds that may be included in the mixture include mercaptopropyl trimethoxysilane, mercaptopropyl triethoxysilane, aminopropyl triethoxysilane, aminoethyl triethoxysilane, aminopropyl trimethoxysilane, aminoethyl trimethoxysilane, vinyl trimethoxysilane, vinyl triethoxysilane, acetylene trimethoxysilane, acetylene triethoxysilane, aminoethyl aminopropyl trimethoxysilane, 3-aminopropyl triethoxysilane, 3-aminopropyl trimethoxysilane, 3-aminopropyl methyl dimethoxysilane or 3-aminopropyl methyl diethoxysilane, N-(2-aminoethyl)-3-aminopropyl Trimethoxysilane, N-methyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, bis(3-aminopropyl)tetramethoxysilane, bis(3-aminopropyl)tetraethoxydisiloxane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropylmethyldiethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-diallylaminopropyltrimethoxysilane, γ-diallylaminopropyltrimethoxysilane, and the like, and combinations thereof. Particularly suitable organosilane compounds are 3-aminopropyltriethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0110] The polymer composition may also include a heat stabilizer. For example, the heat stabilizer may be a phosphite stabilizer, such as an organic phosphite. For example, suitable phosphite stabilizers include monophosphites and diphosphites, wherein the diphosphites have a molecular configuration that inhibits moisture absorption and / or have a relatively high spirocyclic isomer content. For example, a diphosphite stabilizer having a spirocyclic isomer content greater than 90%, such as greater than 95%, such as greater than 98% may be selected. Specific examples of such diphosphite stabilizers include, for example, bis(2,4-dicumylphenyl) pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, mixtures thereof, etc. When used, the heat stabilizer generally constitutes about 0.1wt.% to about 3wt.% of the composition, and in some embodiments about 0.2wt.% to about 2wt.%.
[0111] Nucleating agents can also be used to further enhance the crystallinity of the composition. An example of this nucleating agent is an inorganic crystalline compound, such as a boron-containing compound (such as boron nitride, sodium tetraborate, potassium tetraborate, calcium tetraborate, etc.), alkaline earth metal carbonate (such as calcium magnesium carbonate), oxide (such as titanium oxide, aluminum oxide, magnesium oxide, zinc oxide, antimony trioxide, etc.), silicate (such as talc, sodium aluminum silicate, calcium silicate, magnesium silicate, etc.), alkaline earth metal salt (such as calcium carbonate, calcium sulfate, etc.) and the like. It has been found that boron nitride (BN) is particularly advantageous when used in the polymer composition of the present invention. Boron nitride exists in a variety of different crystalline forms (such as h-BN-hexagonal, c-BN-cubic or sphalerite and w-BN-wurtzite), any of which can be used for the present invention generally. Due to its stability and flexibility, hexagonal crystal is particularly suitable.
[0112] If desired, the crosslinking system can also be used in combination with any optional impact modifier to help further improve the strength and flexibility of the composition under various conditions. In this case, a crosslinked product can be formed by a crosslinkable polymer composition comprising polyarylene sulfide and one or more impact modifiers, a siloxane polymer, a filler and a crosslinking system, and any other additives. When used, such a crosslinking system (which may include one or more crosslinking agents) generally constitutes about 0.1 to about 15 parts per 100 parts of polyarylene sulfide, about 0.2 to about 10 parts in some embodiments, and about 0.5 to about 5 parts in some embodiments, and about 0.05wt.% to about 15wt.% of the polymer composition, about 0.1wt.% to about 10wt.% in some embodiments, and about 0.2wt.% to about 5wt.% in some embodiments. By using such a crosslinking system, the compatibility and distribution of polyarylene sulfide and impact modifier can be significantly improved. For example, the impact modifier can be dispersed in the polymer composition in the form of discrete domains of nanometer size. For example, the average cross-sectional size of the domains is from about 1 nanometer to about 1000 nanometers, in some embodiments from about 5 nanometers to about 800 nanometers, and in some embodiments from about 10 nanometers to about 500 nanometers. The domains can have a variety of different shapes, such as ellipsoidal, spherical, cylindrical, plate-like, tubular, etc. This improved dispersion can lead to better mechanical properties, or allow equivalent mechanical properties to be achieved with a smaller amount of impact modifier.
[0113] Any crosslinking agent among various crosslinking agents can be generally used in the crosslinking system. For example, in one embodiment, the crosslinking system can include metal carboxylates. Without being limited by theory, it is believed that the metal atom in the carboxylates can act as a Lewis acid, which receives electrons from oxygen atoms in the functional groups (e.g., epoxy functional groups) of the impact modifier. Once reacted with carboxylates, the functional groups can become activated and can be easily attacked at any carbon atom in the three-membered ring by nucleophilic substitution, thereby causing crosslinking between the chains of the impact modifier. Metal carboxylates are generally metal salts of fatty acids. The metal cations used in the salts can vary, but are generally divalent metals, such as calcium, magnesium, lead, barium, strontium, zinc, iron, cadmium, nickel, copper, tin, etc., and mixtures thereof. Zinc is particularly suitable. Fatty acids can generally be any saturated or unsaturated acid having a carbon chain length of about 8 to 22 carbon atoms and about 10 to about 18 carbon atoms in some embodiments. If desired, the acid can be substituted. Suitable fatty acids can include, for example, lauric acid, myristic acid, behenic acid, oleic acid, palmitic acid, stearic acid, ricinoleic acid, capric acid, neodecanoic acid, hydrogenated tallow fatty acid, hydroxystearic acid, hydrogenated castor oil fatty acid, erucic acid, coconut oil fatty acid, etc., and mixtures thereof. The metal carboxylates typically constitute from about 0.05 wt.% to about 5 wt.%, in some embodiments from about 0.1 wt.% to about 2 wt.%, and in some embodiments from about 0.2 wt.% to about 1 wt.% of the polymer composition.
[0114] Crosslinking systems can also use "multifunctional" crosslinking agents, which contain at least two reactive functional groups. Such multifunctional crosslinking agents can be used as weak nucleophiles, which can react with activated functional groups (e.g., epoxy functional groups) on impact modifiers. The multifunctional nature of such molecules enables them to bridge two functional groups on impact modifiers, thereby effectively acting as curing agents. Multifunctional crosslinking agents typically include two or more reactive functional end portions connected by a bond or non-polymeric (non-repetitive) linking component. For example, crosslinking agents can include diepoxides, multifunctional epoxides, diisocyanates, polyisocyanates, polyols, water-soluble carbodiimides, diamines, diols, diaminoalkanes, multifunctional carboxylic acids, diacyl halides, etc. Multifunctional carboxylic acids and amines are particularly suitable. The specific examples of multifunctional carboxylic acid crosslinking agents may include but are not limited to isophthalic acid, terephthalic acid, phthalic acid, 1,2-di(p-carboxylphenyl)ethane, 4,4'-dicarboxyl diphenyl ether, 4,4'-bisbenzoic acid, 1,4-naphthalene dicarboxylic acid or 1,5-naphthalene dicarboxylic acid, decahydronaphthalene dicarboxylic acid, norbornene dicarboxylic acid, bicyclooctane dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid (cis and trans), 1,4-hexane dicarboxylic acid, adipic acid, azelaic acid, dicarboxyl dodecanoic acid, succinic acid, maleic acid, glutaric acid, suberic acid, azelaic acid and sebacic acid. Corresponding dicarboxylic acid derivatives may also be used, such as carboxylic acid diesters, carboxylic anhydrides or carboxylic acid halides having 1 to 4 carbon atoms in alcohol radicals. In certain embodiments, aromatic dicarboxylic acids are particularly suitable, such as isophthalic acid or terephthalic acid.
[0115] When used, the multifunctional crosslinking agent generally constitutes about 50 wt.% to about 95 wt.%, in some embodiments about 60 wt.% to about 90 wt.%, and in some embodiments about 70 wt.% to about 85 wt.%, of the crosslinking system, while the metal carboxylate generally constitutes about 5 wt.% to about 50 wt.%, in some embodiments about 10 wt.% to about 40 wt.%, and in some embodiments about 15 wt.% to about 30 wt.%. For example, the multifunctional crosslinking agent may constitute about 0.1 wt.% to about 10 wt.%, in some embodiments about 0.2 wt.% to about 5 wt.%, and in some embodiments about 0.5 wt.% to about 3 wt.% of the polymer composition. Of course, in some embodiments, the composition may generally be free of a multifunctional crosslinking agent, or the crosslinking system may generally be free of a metal carboxylate.
[0116] Other components that may be included in the composition may also include, for example, particulate fillers (e.g., talc, mica, etc.), antimicrobial agents, pigments (e.g., black pigments), antioxidants, stabilizers, surfactants, waxes, flow promoters, solid solvents, flame retardants, and other materials added to enhance performance and processability.
[0117] II. Melt Processing
[0118] As known in the art, the combination of thermoplastic polymers, impact modifiers, fiber fillers and various other optional additives can vary. For example, materials can be provided to the melt processing device of the dispersed blending material simultaneously or sequentially. Batch and / or continuous melt processing techniques can be adopted. For example, mixer / kneader, Banbury mixer, Farrel continuous mixer, single screw extruder, twin screw extruder, roller mill, etc. can be used to blend and melt process materials. A particularly suitable melt processing device is a co-rotating twin screw extruder (e.g., Leistritz co-rotating fully meshing twin screw extruder). This extruder can include a feed port and a discharge port, and provides high-intensity distribution and dispersed mixing. For example, components can be fed to the same or different feed ports of a twin screw extruder and melt blended to form a substantially uniform molten mixture. Melt blending can occur under high shear / pressure and heat to ensure sufficient dispersion. For example, melt processing may be performed at a temperature of about 100° C. to about 500° C., and in some embodiments, about 150° C. to about 300° C. Likewise, the apparent shear rate during melt processing may be about 100 seconds -1 to about 10,000 seconds -1 , and in some embodiments about 500 seconds -1 to about 1500 seconds -1 Of course, other variables, such as residence time during melt processing (which is inversely proportional to throughput rate), can also be controlled to achieve the desired uniformity.
[0119] If desired, one or more distribution and / or dispersive mixing elements can be used in the mixing section of the melt processing unit. Suitable distribution mixers can include, for example, Saxon, Dulmage, Cavity Transfer Mixer, etc. Similarly, suitable dispersive mixers can include Blister rings, Leroy / Maddock, CRD mixers, etc. It is well known in the art that the aggressiveness of mixing can be further improved by using pins that produce folding and redirection of the polymer melt in the barrel, such as those used for Buss kneader extruders, cavity transfer mixers, and vortex intermeshing pin mixers. The speed of the screw can also be controlled to improve the properties of the composition. For example, the screw speed can be about 400rpm or lower, in one embodiment, for example, about 200rpm to about 350rpm, or about 225rpm to about 325rpm. In one embodiment, the compounding conditions can be balanced to provide a polymer composition showing improved performance. For example, the compounding conditions can include a screw design to provide a mild, moderate or aggressive screw condition. For example, a system can have a mildly aggressive screw design in which the screw has a single melting section in the downstream half of the screw that is designed to achieve gentle melting and distributive melt homogenization. A moderately aggressive screw design can have a stronger melting section upstream of the filler feed barrel that is more focused on stronger dispersing elements to achieve uniform melting. In addition, it can have another gentle mixing section downstream to mix the filler. Although this section is weaker, it can still increase the shear strength of the screw, making it stronger overall than the mildly aggressive design. A highly aggressive screw design can have the strongest shear strength of the three. The main melting section can consist of a long series of highly dispersed kneading blocks. The downstream mixing section can utilize a mixture of distributing elements and dense dispersing elements to achieve uniform dispersion of all types of fillers. The shear strength of the highly aggressive screw design can be significantly higher than the other two designs. In one embodiment, the system can include a moderate to aggressive screw design with a relatively gentle screw speed (e.g., about 200 rpm to about 300 rpm).
[0120] The resulting polymer composition may have a crystallization temperature (before forming a molded part) of about 250° C. or less, in some embodiments from about 100° C. to about 245° C., and in some embodiments from about 150° C. to about 240° C. The polymer composition may also have a melting temperature of 140° C. to about 380° C., in some embodiments from about 200° C. to about 360° C., in some embodiments from about 250° C. to about 320° C., and in some embodiments from about 260° C. to about 300° C. Melting and crystallization temperatures may be determined using differential scanning calorimetry as known in the art according to ISO Test No. 11357-3:2018.
[0121] III. Molded parts
[0122] A variety of different techniques can be used to form molded parts from polymer compositions. Suitable techniques may include, for example, injection molding, low-pressure injection molding, extrusion compression molding, gas injection molding, foam injection molding, low-pressure gas injection molding, low-pressure foam injection molding, gas extrusion compression molding, foam extrusion compression molding, extrusion molding, foam extrusion molding, compression molding, foam compression molding, gas compression molding, etc. For example, an injection molding system including a mold can be used, in which the polymer composition can be injected. The time inside the syringe can be controlled and optimized so that the polymer matrix is not pre-cured. When the cycle time is reached and the barrel is full to discharge, the composition can be injected into the mold cavity using a piston. A compression molding system can also be used. Like injection molding, molding the polymer composition into the desired article also occurs in the mold. Any known technology can be used such as placing the composition in a compression mold by picking up the composition by an automated robot arm. The temperature of the mold can be maintained at the solidification temperature of the polymer composition or higher than the solidification temperature for a desired period of time to allow solidification. Then the molded product can be solidified by making it reach a temperature lower than the melting temperature. The resulting product can be demoulded. The cycle time of each molding process can be adjusted to suit the polymer composition to achieve adequate bonding and improve overall process yield.
[0123] IV. Composite structure
[0124] As mentioned above, the unique properties of the polymer composition can make it easier to be integrally molded with metal parts with very different thermal expansion coefficients. Therefore, if necessary, the polymer composition can be applied to a composite structure, which includes a metal part integrally molded and contacted with a resin part including the polymer composition of the present invention. This can be achieved using a variety of techniques, such as by an insert molding process, wherein the polymer composition is molded (e.g., injection molded) onto a portion or the entire surface of the metal part. The metal part can include any number of different metals, such as aluminum, stainless steel, magnesium, nickel, chromium, copper, titanium and alloys thereof. Due to its unique performance, the polymer composition can adhere to the metal part by flowing in and / or around the surface indentations or pores of the metal part. In order to improve adhesion, the metal part can be optionally pretreated to increase the degree and surface area of the surface indentations. This can be achieved using mechanical techniques (e.g., sandblasting, grinding, flaring, punching, molding, etc.) and / or chemical techniques (e.g., etching, anodizing, etc.). In addition to pretreating the surface, the metal part can also be preheated at a temperature close to but lower than the melting temperature of the polymer composition. This can be achieved using a variety of techniques, such as contact heating, radiant gas heating, infrared heating, convection or forced convection air heating, induction heating, microwave heating or a combination thereof. Regardless, the polymer composition is typically injected into a mold containing an optionally preheated metal part.
[0125] V. Electric Vehicles
[0126] As mentioned above, the polymer composition, molded part and / or composite structure is particularly suitable for use as a component of an electric vehicle. Figure 1 , for example, one embodiment of an electric vehicle 112 including a power system 110 is shown. The power system 110 includes one or more electric motors 114 connected to a transmission 116, which in turn is mechanically connected to a drive shaft 120 and drive wheels 122. Although not required, the transmission 116 in this particular embodiment is also connected to an engine 118, although the description herein is equally applicable to pure electric vehicles. The electric motor 114 may be capable of operating as a motor or a generator to provide propulsion and deceleration capabilities. The power system 110 also includes a propulsion source, such as a battery assembly 124 that stores and provides energy used by the electric motor 114. The battery assembly 124 typically provides a high voltage current output (e.g., a DC current having a voltage of about 400 volts to about 800 volts) from one or more battery cell arrays that may include one or more battery cells.
[0127] The power system 110 may also include at least one power electronics module 126, which is connected to the battery assembly 124 (also commonly referred to as a battery pack) and may include a power converter (e.g., a converter, etc., and a combination thereof). The power electronics module 126 is generally connected to the motor 114 and provides the ability to bidirectionally transmit electrical energy between the battery assembly 124 and the motor 114. For example, the battery assembly 124 may provide a DC voltage, while the motor 114 may require a three-phase AC voltage to operate. The power electronics module 126 may convert the DC voltage into the three-phase AC voltage required by the motor 114. In regenerative mode, the power electronics module 126 may convert the three-phase AC voltage from the motor 114 as a generator into the DC voltage required by the battery assembly 124. The battery assembly 124 may also provide energy for other vehicle electrical systems. For example, the power system may use a DC / DC converter module 128, which converts the high-voltage DC output from the battery assembly 124 into a low-voltage DC power supply compatible with other vehicle loads (such as compressors and electric heaters). In a typical vehicle, the low voltage system is electrically connected to an auxiliary battery 130 (e.g., a 12V battery). There may also be a battery energy control module (BECM) 133 in communication with the battery assembly 124, which serves as a controller for the battery assembly 124 and may include an electronic monitoring system that manages the temperature and state of charge of each battery cell. The battery assembly 124 may also have a temperature sensor 131, such as a thermistor or other thermometer. The temperature sensor 131 may communicate with the BECM 133 to provide temperature data about the battery assembly 124. The temperature sensor 131 may also be located on or near a battery cell within the traction battery 124. It is also contemplated that more than one temperature sensor 131 may be used to monitor the temperature of a battery cell.
[0128] In certain embodiments, the battery assembly 124 can be recharged by an external power source 136 (e.g., an electrical outlet). The external power source 136 can be electrically connected to an electric vehicle supply equipment (EVSE), which regulates and manages the transfer of electrical energy between the power source 136 and the vehicle 112. The EVSE 138 can have a charging connector 140 for plugging into a charging port 134 of the vehicle 112. The charging port 134 can be any type of port configured to transfer power from the EVSE 138 to the vehicle 112, and can be electrically connected to a charger or an on-board power conversion module 132. The power conversion module 132 can condition the power supplied by the EVSE 138 to provide the appropriate voltage and current levels to the battery assembly 124. The power conversion module 132 can interact with the EVSE 138 to coordinate the delivery of power to the vehicle 112.
[0129] The polymer compositions described herein may include Figure 1For example, a busbar (one example of which is shown in FIG. Figure 2 ) can be used to electrically connect the cells of the battery assembly 124. Figure 3 For example, the battery assembly 124 may include a plurality of battery cells 158. The battery cells 158 may be stacked side by side to form a battery cell group, sometimes referred to as a battery array. In one embodiment, the battery cells 158 are prismatic lithium-ion batteries. However, battery cells having other geometries (cylindrical, pouch, etc.) and / or chemical compositions (nickel metal hydride, lead acid, etc.) may alternatively be used within the scope of the present disclosure. Each battery cell 158 includes a positive terminal (represented by the symbol (+)) and a negative terminal (represented by the symbol (-)). The battery cells 158 are arranged so that the terminals of each battery cell 158 are arranged adjacent to the terminals of an adjacent battery cell 158 of opposite polarity. As used herein, the terms "battery," "monocell," and "battery cell" are used interchangeably to refer to any type of single battery element used in a battery system. The batteries described herein generally include lithium-based batteries, but may include a variety of chemistries and configurations, including iron phosphate, metal oxide, lithium-ion polymer, nickel metal hydride, nickel cadmium, nickel-based batteries (hydrogen, zinc, cadmium, etc.), and any other battery type compatible with electric vehicles. For example, some embodiments may use batteries from The 6831NCR 18650 battery cell, or some variant of the 18650 form factor that is 6.5cm x 1.8cm and about 45g.
[0130] As is known in the art, busbars are connected to the battery assembly 124 (eg Figure 3 The manner of each battery cell shown in FIG. 1 may vary. Figure 2 , shows an embodiment of a busbar 10 including a conductor 12. The conductor 12 includes a conductive material 18, such as copper, aluminum, aluminum alloy, etc., and can generally be in the form of a solid rod, a hollow tube, etc. The busbar 10 includes a connector portion 14 at either end, which is configured to match the corresponding terminals of two or more batteries. An insulating portion 16 (e.g., a coating material or a molding material) including a polymer composition as described herein can cover a portion of the conductive material of the conductor 12. In order to form the busbar 10, the insulating portion 16 can be applied to the surface of the conductive material 18. For example, a rod or tube of the conductive material 18 can be inserted into a preformed tube of the insulating coating 16, such as an extruded tube of a specific size and cut to the correct proportions, and then the busbar 10 can be formed into any suitable form. In another embodiment, the insulating coating can be applied to the surface of the conductive material 18 in the melt, and can be solidified on the surface of the conductive material in the applied area.
[0131] Of course, busbars of any suitable shape and size may be provided. For example, the busbar may be used as a template for placing the individual battery cells so that the battery cells are uniform in each prepared battery assembly. In such an embodiment, the busbar may hold the individual batteries of the battery assembly 124 in place during the manufacturing process, and may add insulation pads or injection shells that may be formed from the polymer composition described herein without causing the individual battery cells to deviate from their positions.
[0132] In addition to busbars, other components may also use the polymer composition of the present invention. For example, Figure 4 A block diagram of a battery electronics device for an electric vehicle 112 is shown. The battery electronics system shown includes a battery assembly 124 and a current sensor 142. As shown, the current sensor 142 is connected between the battery assembly 124 and the load / source 144. When the load / source 144 is a load such as one or more motors 114, the current sensor 142 can be configured to measure the current flowing from the battery assembly 124 to the load / source 144. Similarly, when the load / source 144 is a source such as an external power source 136, the current sensor 142 can be configured to measure the current flowing from the load / source 144 to the battery assembly 124. The (BECM) 133 can be configured to power the current sensor 142 to enable it to operate. The BECM 133 can also be configured to read an output generated by the current sensor 142, which indicates the current flowing between the battery assembly 124 and the load / source 144.
[0133] Figure 5 One embodiment of a current sensor 142 is shown. The current sensor 142 may include a current input port 141 and a current output port 143 as well as a standard ground 145, a common collector voltage (VCC) 146, and an output port 147. The current sensor 142 may also include a housing 148 comprising a polymer composition as described above, which may house other components of the current sensor 142, such as resistors, capacitors, converters, processing chips, etc.
[0134] Another component of an electric vehicle that may include the polymer composition is an inverter system, an exemplary embodiment of which is as follows Figure 6As shown. The system includes an inverter module 320 and an interconnection system 335. The interconnection system 335 includes an electromagnetic interference (EMI) core 330 and an EMI filter device 325. The inverter module 320 is coupled to the interconnection system 335 through a pair of busbars 310. The EMI core 330 is located between the EMI filter device 325 and the inverter module 320 and is in communication with the busbar 310. The EMI filter device 325 includes an EMI filter card 340 and a pair of bolts 350, 352, and the bolts 350, 352 include a positive terminal (+) bolt 350 and a negative terminal (-) bolt 352 for coupling to a power source, such as a battery assembly 124. The EMI core 330 is coupled to the bolts 350, 352 through the busbar 310. The EMI filter card 340 is also coupled between the ground and the busbar 310 through a pair of wires 334. The inverter module 320 includes a plurality of transistors (not shown). The transistors in the inverter module 320 turn on and off relatively quickly (e.g., 5kHz to 20kHz). This switching tends to generate electrical switching noise. Ideally, the electrical switching noise should be contained within the inverter module 320 and prevented from entering the rest of the electrical system to prevent interference with other electrical components in the vehicle.
[0135] The inverter system may include several components that may include the disclosed polymer composition, including but not limited to EMI filter device 325 (e.g., as a housing and / or internal support structure), EMI filter card 340, busbar 310, and connectors used within the system. For example, an electrical connector including the polymer composition described herein may be used Figure 7 In the inverter system shown or in another part of the electric vehicle. The electrical connector can generally include a first connector part containing at least one electrical contact and an insulating member surrounding at least a portion of the connector part. The insulating member may include the polymer composition of the present invention. The first connector part can be configured to match with an opposite second connector part, and the second connector part includes a socket for receiving the electrical contact. In this embodiment, the second connector part may include at least one socket configured to receive the electrical contact of the first connector part and an insulating member surrounding at least a portion of the second connector part. The insulating member of the second connector part may also include the polymer composition of the present invention.
[0136] Reference Figure 7 , Figure 8 and Fig. 9, shows a specific embodiment of a connector 200 for an electric vehicle (e.g., an electric vehicle power system). The connector 200 includes a first connector portion 202 and a second connector portion 204. The first connector portion 202 may include one or more electrical pins 206, and the second connector portion 204 may include one or more sockets 208 for receiving the electrical pins 206. The first insulating member 212 may extend from the bottom 203 of the first connector portion 202 to surround the pins 206, and similarly, the second insulating member 218 may extend from the bottom 201 of the second connector portion 204 to surround the sockets 208. In some cases, the periphery of the first insulating member 212 may extend beyond the ends of the electrical pins 203, and the periphery of the second insulating member 218 may extend beyond the ends of the sockets 208. The bottom 203 and / or the first insulating member 212 of the first connector portion 202, and the bottom 201 and / or the second insulating member 218 of the second connector portion 204 may be formed from the polymer composition of the present invention.
[0137] Although not required, the first connector portion 202 may also include an identification mark 210 that is fixed to or defined by the first protective member 212. The second connector portion 204 may also optionally define an alignment window 220 that is sized based on the identification mark 210 to more easily determine when the parts are fully mated. For example, unless the barrier 221 covers a portion of the identification mark 210, the identification mark 210 may not be readable. Optionally, the second connector portion 204 may include a supplemental mark 224 proximate the alignment window 220.
[0138] Fig.10 and Fig.11 Other embodiments of parts in which the polymer composition of the present invention can be used are shown, for example Fig.10 Gaskets, connectors, insulators and supports that may be formed from the polymer composition are shown. Fig.11 The components shown that may include the polymer composition include: quick connectors, tees and interconnects, wherein a plurality of Fig.11 The top of the brushless DC motor ( Fig.11 The left side of the middle part), such as the sealing ring, housing, support, etc. of the motor; guide rail ( Fig.11 Other examples of busbars in the image are also shown in the middle right of ); and battery sealing ring ( Fig.11 at the bottom of the ).
[0139] Systems that can employ the polymer compositions of the present invention are by no means limited to electrical systems. For example, thermal management systems can also advantageously include polymer compositions. The thermal management system of an electric vehicle can typically include a plurality of different subsystems, such as, but not limited to, a powertrain subsystem, a refrigeration subsystem, a battery cooling subsystem, and a heating, ventilation, and cooling (HVAC) subsystem. In some embodiments, one or more subsystems of the thermal management system can be fluidly connected to each other, thereby allowing a hot heat transfer medium to flow from a high temperature circuit into a low temperature circuit, and allowing a cooler heat transfer medium to flow from a low temperature circuit into a high temperature circuit.
[0140] For example, Fig.12 shows a first temperature control loop that may be found in an electric vehicle, Fig.13 A second temperature control loop that may be found in an electric vehicle is shown, each loop being designed for a different subsystem and each loop including one or more components that may employ the polymer composition of the present invention. For example, the first temperature control loop ( Fig.12 ) may include a heat transfer medium (e.g., water) that is pumped through the loop by a suitable pump 160 (e.g., an electric water pump) and cooled by heat transfer with a heat exchanger 162 (e.g., an energy storage system (ESS) heat exchanger) and a refrigerant in a radiator / reservoir 164. In addition, the loop may include a heater 166 (e.g., a positive temperature coefficient (PTC) heater) and the battery assembly 124, which can ensure that the temperature of the system can be maintained within its preferred operating range regardless of the ambient temperature. Second temperature control loop ( Fig.13 ) may also include a heat transfer medium, which may be the same as or different from the heat transfer medium of another subsystem. The heat transfer medium of the second temperature control loop may be pumped through the loop by an appropriate pump 161, heat exchanger 162, and radiator reservoir 165. The high temperature control loop may be used to cool the power electronics 167 of the vehicle as well as the motor 114.
[0141] One example of a thermal management system component that may include the polymer composition of the present invention is a coolant pump, such as an electric water pump, exemplified by Fig.14As shown. As shown, the electric water pump 401 includes an electric motor 410 as a driving source, and a hydraulic part 420 for generating coolant suction and discharge force. The motor 410 and related components are retained in a motor housing 411. The hydraulic part 420 includes a volute 421, which generally includes a spiral flow space, an inlet 422 and an outlet 423, and an impeller (not shown) rotated by the electric motor 410. The pump 401 has an interface including a mechanical seal (not shown) for sealing and separating the water flow space and the motor chamber. Typically, a mounting portion 412 is provided on the motor housing 411 to install the pump 401 in a vehicle. The components (e.g., housing, sleeve, interface, etc.) of the electric pump 401 may include the polymer composition of the present invention.
[0142] The present invention may be better understood with reference to the following examples.
[0143] Test Method
[0144] Melt viscosity: Melt viscosity (Pa-s) can be measured according to ISO 11443:2021 in 400s -1 The Dynisco LCR7001 capillary rheometer is used to measure the shear rate of 1.5 % to 2.5 %. The rheometer orifice (die) can have a diameter of 1 mm, a length of 20 mm, an L / D ratio of 20.1, and an inlet angle of 180°. The diameter of the barrel can be 9.55 mm + 0.005 mm, and the length of the rod is 233.4 mm. The melt viscosity is usually measured at a temperature of 310°C.
[0145] Tensile modulus, tensile stress at break, and tensile strain at break: Tensile properties can be tested according to ISO 527-2 / 1A:2019 (technically equivalent to ASTM D638-14). Modulus and strength measurements can be performed on the same test strip sample with a length of 80 mm, a thickness of 10 mm, and a width of 4 mm. The test temperature can be 23°C, and the test speed for tensile strength and tensile strain at break can be 5 mm / min, and the test speed for tensile modulus can be 1 mm / min.
[0146] Flexural modulus and flexural stress: Flexural properties can be tested according to ISO 178:2019 (technically equivalent to ASTM D790-10). The test can be performed on a 64 mm support span. The test can be performed on the center portion of an uncut ISO 3167 multipurpose bar. The test temperature can be 23°C and the test speed can be 2 mm / min.
[0147] Izod notched impact strength can be measured according to ISO 180:2019. The specimens are cut from the center of the multi-purpose bar using a single-tooth milling machine. The test temperature is 23°C.
[0148] Charpy notched impact strength: Charpy properties can be tested according to ISO test No. ISO 179-1:2010 (technically equivalent to ASTM D256-10, Method B). This test can be performed using Type 1 specimen dimensions (80 mm length, 10 mm width, and 4 mm thickness). When testing notched impact strength, the notch can be a Type A notch (0.25 mm base radius). The specimens can be cut from the center of a multipurpose bar using a single tooth milling machine. The test temperature can be 23°C or -30°C.
[0149] Comparative Tracking Index ("CTI"): The Comparative Tracking Index (CTI) can be determined in accordance with International Standard IEC 60112-2003 to provide a quantitative indication of the performance of a composition as an electrical insulating material under conditions of moisture and / or contamination. In determining the CTI rating of a composition, two electrodes are placed on a molded test specimen. When a 0.1% aqueous solution of ammonium chloride is dropped onto the test specimen, a voltage difference is then established between the electrodes. The maximum voltage at which five (5) specimens withstand 50 drops without failure during the test period is determined. The test voltage range is 100V to 600V, in increments of 25V. The voltage value that causes failure when fifty (50) drops of electrolyte are applied is the "Comparative Tracking Index". This value provides an indication of the relative resistance of the material to tracking. According to UL746A, a nominal part thickness of 3mm is considered to be representative of performance at other thicknesses.
[0150] Thermal shock resistance: To test thermal shock resistance, first use Figures 15 to 18 The molds and inserts shown were used to form four (4) types of sample parts. Fig.15 As shown, the first mold 100 is molded to produce a plastic thickness of 1.2 mm and a part size of 63.8 mm×20 mm×10.4 mm; the second mold 200 is molded to produce a plastic thickness of 2.5 mm and a part size of 65.1 mm×22.6 mm×13 mm; the third mold 300 is molded to produce a plastic thickness of 1.2 mm and a part size of 40 mm×20 mm×10.4 mm; the fourth mold 400 is molded to produce a plastic thickness of 42.6 mm×22.6 mm×13 mm. Two circular holes 402 are formed on the cavity side of each of the molds 300 and 400, parallel to the longitudinal edges of the molds. The diameter of the hole 402 is 3.5 mm and is recessed into the cavity side of the mold. The first mold 100 and the second mold 200 respectively include metal inserts 105 and 205 (see Fig.16), the metal inserts 105, 205 are formed of AISI H13 / 440C stainless steel plates having dimensions of 62.6 mm×18 mm×18 mm and are embedded in the mold in a manner that no weld is formed. The inserts 105, 205 have a single circular hole 502 at their respective ends, which has a diameter of 5 mm. The third mold 300 and the fourth mold 400 also include metal inserts 305, 405, respectively (see Fig.16 ), the metal inserts 305, 405 are formed of AISI H13 / 440C stainless steel plates with a size of 37.6 mm × 18 mm × 18 mm. Fig.16 As shown, each of the metal inserts 305, 405 includes two circular holes 602 that are aligned parallel to the lateral edges of the inserts and recessed into the core side of each respective insert. The holes 602 have a diameter of 2.0 mm and are recessed into the core side of the insert to a depth of 5 mm. When inserted into the mold 300, 400, a weld is formed at the line where the two flow fronts meet, so that the flow fronts cannot be "braided" or "welded" together during the molding process.
[0151] Reference Fig.15 , Fig.17 and Fig.18 , a sample part can be formed using the above mold by first passing the polymer composition through a gate 702 having an upper end 704 with a small diameter (i.e., 6 mm) and a lower end 706 with a diameter greater than the upper end 704 (i.e., 8 mm). The polymer composition can flow into a first flow channel 802 (with a diameter of 7 mm) through the gate 702 and flow through a gate 804 for the third mold 300 with a size of 0.8 mm×10 mm and a gate 806 for the fourth mold 400 with a size of 1.7×10 mm. The polymer composition can also flow into a second flow channel 902 (with a diameter of 6 mm) through the gate 702 and flow through a gate 904 for the first mold 100 with a size of 0.8 mm×10 mm and a gate 906 for the fourth mold 400 with a size of 1.7 mm×10 mm. The draft angle on each side of the mold is 1.5°. When forming a molded part, processing conditions can be selected in a manner known to those skilled in the art. For example, the melt temperature and nozzle temperature can be 320°C, the injection pressure can be 1250 bar, the peak pressure can be 1146 bar (e.g., for mold 100) and 1120 bar (e.g., for mold 300), the injection speed can be 80 mm / s and the injection time can be about 0.25 s, the holding pressure can be about 800 bar, the cooling time can be about 15 s, and the total cycle time can be about 23 s.
[0152] A set of twenty (20) sample parts can be formed using each of the above molds. The sample parts can then be subjected to a first heating cycle in a thermal shock chamber having a hot zone and a cold zone, such as the thermal shock chamber commercially available from Weisstechnik under the name "ShockEvent T / 120 / V2". The hot zone can be heated to a temperature of 140°C and the cold zone can be cooled to a temperature of -40°C. To initiate the first heating cycle, the sample parts are placed in the hot zone for 30 minutes, and then the product carrier in the chamber moves the sample parts from the hot zone to the cold zone for another 30 minutes. In this manner, the total time for the first cycle is 1 hour. 24 cycles are performed per day, each cycle lasting 1 hour. The sample parts are visually inspected for cracking once a day for the first two weeks and twice a week thereafter until all twenty (20) samples have cracked or a full set of cycles has been completed, which can be 1500 or 3000 cycles depending on the test protocol. When the first specimen cracks, the number of cycles achieved before cracking is recorded as the "Thermal Shock Resistance Value". If a full set of cycles (1500 or 3000) is completed without any specimens cracking, the "Thermal Shock Resistance Value" is simply recorded as ">1500" or ">3000", depending on the specific test protocol.
[0153] Comparative Example 1-2
[0154] Comparative Examples 1 and 2 were melt compounded using a 32 mm Coperion co-rotating fully intermeshing twin screw extruder and included various concentrations of polyarylene sulfide, glass fiber, lubricant (Glycolube P) and colorant. The following table lists the formulation of each comparative example in more detail.
[0155]
[0156] Example 1-2
[0157] Examples 1 to 2 were melt mixed using a 32 mm Coperion co-rotating fully intermeshing twin screw extruder, including various concentrations of polyarylene sulfide, impact modifier, glass fiber, siloxane polymer, organosilane, lubricant (Glycolube) and colorant. The impact modifier is a random copolymer of ethylene and glycidyl methacrylate, wherein the glycidyl methacrylate content is 8 wt.%, and the melt flow index at 190°C is 5 g / 10 min. The siloxane polymer is a UHMW functionalized siloxane polymer provided in the form of a masterbatch with a siloxane content of 50% and a resin content of 50%. The organosilane is 3-aminopropyltriethoxysilane. The following table lists the formulation of each example in more detail.
[0158]
[0159] After forming, the samples were tested for various thermal shock resistance, CTI and various other physical properties. The results are shown below.
[0160] Comparative Example 1 Comparative Example 2 Example 1 Example 2 Thermal shock resistance value (weld, 1.2mm) 300 200 >1,500 >1,500 Thermal shock resistance value (weld, 2.5mm) 720 480 >1,500 >1,500 Thermal shock resistance value (without weld, 1.2mm) 624 336 >1,500 >1,500 Thermal shock resistance value (without weld, 2.5mm) 1,392 840 >1,500 >1,500 <![CDATA[400s -1 Melt viscosity at (kpoise)]]> 3.3 3.7 3.5 3.6 Tensile modulus (MPa) 11,760 15,220 10,725 14,700 Tensile breaking stress (MPa) 168.2 202.6 167.4 186.3 Tensile strain at break (%) 1.8 1.8 2.3 2.1 Flexural modulus (MPa) 11,360 15,010 10,765 14,610 Bending strength(MPa) 256 291 250 283 <![CDATA[Izod notched impact strength at 23 °C (kJ / m 2 )]]> 8.8 9.3 13.5 13.7 CTI(V) 150 150 175 175 Flammability at 0.8mm V-0 V-0 V-0 V-0
[0161] Example 1 was reformulated (Example 1a) and tested again for various physical properties before and after heat aging in air at 240°C for 1000 hours.
[0162]
[0163] Without departing from the spirit and scope of the present invention, those of ordinary skill in the art may make these and other modifications and variations to the present invention. In addition, it should be understood that the aspects of each embodiment may be fully interchangeable or partially interchangeable. In addition, those of ordinary skill in the art will appreciate that the foregoing description is exemplary only and is not intended to limit the present invention as further described in the appended claims.
Claims
1. A polymer composition comprising an impact modifier and a fibrous filler dispersed in a polymer matrix, wherein: The polymer matrix comprises a high performance thermoplastic polymer exhibiting a load deflection temperature of about 40°C or higher and a melting temperature of about 140°C or higher measured at a load of 1.8 MPa according to ISO 75-2:2013, wherein the polymer composition also exhibits a thermal shock resistance value of about 800 or higher.
2. The polymer composition according to claim 1, wherein The high performance thermoplastic polymer includes polyolefin, polyamide, polyester, polyarylene sulfide, liquid crystal polymer, polyether, polyoxymethylene or a combination thereof.
3. The polymer composition according to claim 1, wherein The high performance thermoplastic polymer includes polyarylene sulfide.
4. The polymer composition of claim 1, further comprising an ultra high molecular weight siloxane polymer having a weight average molecular weight of about 100,000 g / mole or greater.
5. The polymer composition according to claim 4, wherein The siloxane polymer is functionalized.
6. The polymer composition according to claim 4, wherein The siloxane polymer includes one or more of vinyl, hydroxyl, hydride, isocyanate, epoxy, acidic group, halogen atom, alkoxy, acyloxy, ketoxime, amino, amide, acidamide, aminooxy, thiol, alkenyloxy, alkoxyalkoxy or aminooxy groups.
7. The polymer composition according to claim 1, further comprising an organosilane compound.
8. The polymer composition according to claim 7, wherein The organosilane compound includes aminoalkoxysilane.
9. The polymer composition according to claim 1, wherein The polymer composition comprises about 10 to about 80 parts by weight of the fibrous filler and about 1 to about 20 parts by weight of the impact modifier per 100 parts by weight of the polymer matrix.
10. The polymer composition according to claim 1, wherein The fibrous filler includes glass fibers.
11. The polymer composition according to claim 1, wherein The impact modifier includes epoxy-functional monomer units.
12. The polymer composition according to claim 11, wherein The epoxy-functional monomer units include epoxy-functional (meth)acrylic monomer components.
13. The polymer composition according to claim 12, wherein The epoxy-functional (meth)acrylic monomer component is formed from glycidyl acrylate, glycidyl methacrylate or a combination thereof.
14. The polymer composition according to claim 11, wherein The impact modifier also includes an alpha-olefin monomer component.
15. The polymer composition according to claim 14, wherein The alpha-olefin monomer component comprises from about 55 wt.% to about 95 wt.% of the impact modifier, and the epoxy-functional monomer component comprises from about 1 wt.% to about 20 wt.% of the impact modifier.
16. The polymer composition according to claim 11, wherein The impact modifier also includes a non-epoxy functional (meth)acrylic monomer component in an amount of about 5 wt. % to about 35 wt. % of the polymer.
17. The polymer composition according to claim 1, wherein The impact modifier has a melt flow index of about 1 g / 10 minutes to about 30 g / 10 minutes as measured according to ASTM D1238-13 at a load of 2.16 kg and a temperature of 190°C.
18. The polymer composition according to claim 1, wherein The polymer matrix constitutes from about 50 wt. % to about 98 wt. % of the polymer composition.
19. The polymer composition according to claim 1, wherein According to ISO 11443:2021 at a temperature of about 310°C and 400s -1 The polymer composition exhibits a melt viscosity of about 30 kP or less measured at a shear rate of .
20. The polymer composition according to claim 1, wherein The polymer composition exhibits a comparative tracking index of about 150 volts or more measured at a part thickness of 3 mm according to IEC 60112:2003.
21. The polymer composition according to claim 1, wherein The polymer composition exhibits a V-0 rating measured according to the UL94 test at a thickness of 0.8 mm.
22. The polymer composition according to claim 1, wherein The polymer composition exhibits an impact resistance value of about 1500 or greater.
23. The polymer composition according to claim 1, wherein The polymer composition exhibits an impact resistance value of about 3000 or greater.
24. A composite structure comprising a metal component and a resin component, the metal component being in contact with the resin component, the resin component comprising the polymer composition according to claim 1.
25. The composite structure of claim 24, wherein: The structure is insert molded.
26. An electric vehicle comprising a power system including at least one electric propulsion source and a transmission connected to the propulsion source via at least one power electronics module, wherein: The electric vehicle comprises the composite structure of claim 24.
27. The electric vehicle according to claim 26, wherein: The electric vehicle includes an electrical component including the composite structure.
28. The electric vehicle according to claim 27, wherein: The electrical components include bus bars, current sensors, inverter filters, electrical connectors, brushless DC motors, guide rings, battery cell sealing rings, or combinations thereof.
29. The electric vehicle according to claim 26, wherein: The electrical component includes a quick connector, a tee, an interconnector, or a combination thereof.
30. The electric vehicle of claim 26, wherein: The electric vehicle includes a thermal management system component including the polymer composition.
31. The electric vehicle according to claim 30, wherein: The thermal management system components include a coolant pump.
Citation Information
Patent Citations
Ultra-high molecular weight, soluble siloxane resins
US6072012A