Acrylic coating composition for beverage can end cap, beverage can and method

The acrylic-based coating composition with a carboxyl-reactive crosslinker addresses the balance of flexibility, toughness, and corrosion resistance in beverage can end caps, ensuring high-speed manufacturing and effective adhesion, while avoiding formaldehyde and other undesirable compounds.

CN119095922APending Publication Date: 2024-12-06SWIMC LLC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380036079.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-08
Filing Date
2023-04-07
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing coatings for beverage can end caps face challenges in achieving a balance between flexibility, toughness, and corrosion resistance, particularly when subjected to high-speed manufacturing processes and short cure times, while also ensuring safety for food contact and resistance to harsh environments.

Method used

A coating composition comprising an acrylic latex and a carboxyl-reactive nitrogen-containing crosslinker, free from formaldehyde and certain undesirable compounds, is applied to a metal substrate, allowing for high-speed curing and forming beverage can end caps with improved flexibility, toughness, and corrosion resistance.

Benefits of technology

The composition achieves robust performance in beverage can end caps, providing sufficient flexibility, toughness, and corrosion resistance, even under demanding conditions, without the need for melamine and formaldehyde crosslinkers, and exhibits excellent adhesion and resistance to feathering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095922A_ABST
    Figure CN119095922A_ABST
Patent Text Reader

Abstract

Acrylic coating composition for beverage can end caps, in particular easy-to-open beverage can end caps, beverage cans and coating methods. The beverage can includes a metal substrate at least partially coated with a coating prepared from the acrylic coating composition. The composition comprises an acrylic latex, a crosslinker, and optionally a lubricant.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of U.S. Provisional Application No. 63 / 362,707, filed on April 8, 2020, the disclosure of which is incorporated herein by reference in its entirety. Background Art

[0003] Beverage can end caps, such as easy-open can end caps, are often the most challenging coating applications in the beverage container coating industry. In some cases, this challenge is due to the rigorous manufacturing levels that the coating and substrate must withstand in the formation of beverage can end caps. For example, beverage can end caps are formed by first applying a coating composition to a flat metal coil (usually aluminum or steel coil), typically in a high-speed application process with a short cure time. The beverage can end caps are then stamped from the coated metal coil. If easy-open cans are required, rivets with pull tabs attached are also formed from the substrate, and such rivets have very demanding profiles.

[0004] Many packaging coatings, including many coatings suitable for use on the sidewalls of beverage containers, do not have the toughness and flexibility to accommodate the stamping process used to form can ends and / or rivets, while still exhibiting sufficient corrosion resistance for end use. With existing coatings, there is often a trade-off between flexibility / toughness and corrosion resistance of the coating. That is, one type of coating composition may have sufficient flexibility to accommodate stamping and rivet formation, but such performance comes at the expense of corrosion resistance.

[0005] Not only do coating compositions need to be flexible, tough, and corrosion resistant when hardened to perform in the demanding end use of beverage can end caps, but such coating compositions should preferably be capable of being applied to substrates at high speeds. For example, the compositions and hardened coatings should also be safe for food contact, have good adhesion to substrates, and resist degradation for long periods of time even when exposed to harsh environments. Many current packaging coatings suffer from one or more performance deficiencies and / or contain extractable amounts of one or more undesirable compounds, particularly when the coatings are exposed to short cure times.

[0006] Existing coatings for achieving the high level of performance required for beverage can end caps are typically bisphenol A based (BPA) and / or epoxy based compositions in combination with melamine or phenolic crosslinkers. Melamine and phenolic resins are based on formaldehyde monomers. In addition, in latex, historically both styrene and glycidyl methacrylate (GMA) have been used, for example, for internal crosslinking and other special properties in the packaging industry. For a variety of reasons, such components have become less desirable in the packaging field. However, when used in the context of coating operations for beverage can end caps, non-epoxide and non-formaldehyde alternatives often have disadvantages in terms of handling and / or performance.

[0007] Acrylic-based coatings are an alternative to epoxy coatings. Acrylic-based coating compositions have been used as spray coatings for the interior body of food or beverage containers; however, when existing acrylic-based compositions are used in the demanding and challenging processing of beverage can end caps that are subject to short cure times, the cure process and existing acrylic chemistry often do not achieve the desired performance. Moreover, acrylic-based coatings have historically not been sufficiently flexible, tough, and corrosion resistant. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 is a schematic diagram of a coil substrate coating line suitable for applying the liquid polymer coating composition of the present disclosure.

[0009] Figure 2 is a photograph of an exemplary easy-open can end.

[0010] Figures 3 to 6 are exemplary plan and perspective views of a metal sheet having a simulated pull tab formed thereon for feathering evaluation as described in the Examples. Summary of the invention

[0011] The present invention provides a coating composition suitable for beverage can end caps, preferably easy open end caps for beverage cans (in alternative embodiments, the coating composition can be an aqueous coating composition or a powder coating composition). The coating composition comprises an acrylic latex and a carboxyl-reactive nitrogen-containing crosslinker that is not derived from formaldehyde. In a preferred embodiment, the acrylic copolymer comprises acid (preferably carboxylic acid) or anhydride groups, some or all of which can be neutralized with a base.

[0012] In one embodiment, a beverage can end cover coil coating composition comprises: an acid or anhydride functional acrylic latex comprising an emulsion polymerized polymer; a carboxyl reactive crosslinker, the carboxyl reactive crosslinker being nitrogen-containing and not derived from formaldehyde; and an optional lubricant. The coating composition: (i) comprises less than 2 wt% of a crosslinker derived from formaldehyde, if any, based on the weight of the total solids; (ii) is free of bisphenol A, bisphenol F, and bisphenol S; (iii) is optionally free of styrene; (iv) when applied to a cleaned and chromium-free, zirconium pretreated aluminum panel and cured for 12 seconds to a peak metal temperature of 249°C to achieve a dry film thickness of about 11 (i.e., 10-12) grams per square meter, having a glass transition temperature (Tg) of 10°C to 50°C. ), as determined by differential scanning calorimetry (DSC); and (v) when applied to a cleaned and chromium-free, zirconium pretreated aluminum panel and cured for 12 seconds to a peak metal temperature of 249°C to achieve a dry film thickness of approximately 11 (i.e., 10-12) grams per square meter, and formed into a fully converted (typically 206) standard opening beverage can end, with less than 5 mA of current passed while exposed to an electrolyte solution containing 1 weight percent NaCl dissolved in deionized water for 4 seconds.

[0013] In another embodiment, a method is provided, comprising: providing a coating composition as described herein; applying the coating composition (e.g., via roller coating) to a substrate comprising a beverage can end cap steel or aluminum coil; heating the coated substrate in an oven for 6 seconds to 30 seconds, preferably 8 seconds to 15 seconds of oven residence time, to achieve a peak metal temperature of 200° C. to 260° C.; and optionally forming (e.g., stamping) the coated coil to form an easy-open beverage can end cap. Preferably, in the method, applying the coating composition to the surface of the substrate comprises applying the coating composition to a continuously moving surface traveling at a line speed of 50 m / min to 400 m / min.

[0014] In yet another embodiment, a coated article is provided, the coated article comprising a beverage can end cap having an interior or exterior coating, or both, formed from a coating composition described herein or obtained by a method described herein. In yet further aspects or embodiments, an article is described herein, wherein the article comprises a metal substrate having a riveted beverage can end cap, the riveted beverage can end cap having a coating disposed on at least a portion of the riveted beverage can end cap, wherein the coating is formed from an aqueous coating composition described herein.

[0015] definition

[0016] The term "easy open end" refers to a can end (usually an end of a beverage can) that includes (i) a frangible opening portion (which, for some beverage can ends, serves as a drinking opening) and (ii) a rivet portion for attaching a pull tab thereto so as to open the frangible opening portion to gain access to the product contained in the can or container.

[0017] The term "chrome-free" means free of chrome. Historically, pretreatment of aluminum sheet for beverage cans was based on chrome 6 or chrome 3. Neither is used herein.

[0018] The term "food contact surface" refers to a surface of an article (eg, a beverage can) that comes in contact with, or is intended to come in contact with, a food or beverage product.

[0019] The term "organic" or "organic group" means a hydrocarbon group (it has optional elements other than carbon and hydrogen, such as oxygen, nitrogen, sulfur and silicon), which is classified as aliphatic groups, cyclic groups or aliphatic groups and cyclic groups The combination of groups (for example, alkylaryl groups and aralkyl groups). The term "aliphatic group" means a saturated or unsaturated straight or branched hydrocarbon group. For example, the term is used to cover alkyl, alkenyl and alkynyl groups. The term "alkyl group" means a saturated straight or branched hydrocarbon group, including, for example, methyl, ethyl, isopropyl, tert-butyl, heptyl, dodecyl, octadecyl, amyl, 2-ethylhexyl, etc. The term "alkenyl group" means an unsaturated, straight or branched hydrocarbon group with one or more carbon-carbon double bonds, such as a vinyl group. The term "alkynyl group" means an unsaturated, straight or branched hydrocarbon group with one or more carbon-carbon triple bonds.

[0020] In the context of water-dispersible polymers, the term "water-dispersible" means that the polymer can be mixed into water (or an aqueous carrier) to form a stable mixture. For example, a mixture that easily separates into immiscible layers is not a stable mixture. The term "water-dispersible" is intended to include the term "water-soluble". In other words, by definition, water-soluble polymers are also considered water-dispersible polymers. As used herein, "water-dispersible" means that the components (e.g., polymer components) do not significantly separate after 4 months at room temperature (25°C) or 1 month at elevated temperature (40°C).

[0021] In the context of a dispersible polymer, the term "dispersion" refers to a mixture of a dispersible polymer and a carrier fluid. The term "dispersion" is intended to include the term "solution".

[0022] The group that can be identical or different is referred to as "independently" something. It is expected that the organic group of the compounds of the present invention is substituted. Therefore, when the term "group" is used to describe a chemical substituent, the chemical substance includes an unsubstituted group, and for example, in a chain (such as in an alkoxy group) there is an O, N, Si or S atom and a carbonyl group or other conventionally substituted group. For example, the phrase "alkyl group" is intended to include not only pure open-chain saturated hydrocarbon alkyl substituents, such as methyl, ethyl, propyl, tert-butyl, etc., but also includes the alkyl substituents carrying other substituents known in the art (such as hydroxyl, alkoxy, alkyl sulfonyl, halogen atom, cyano, nitro, amino, carboxyl, etc.). Therefore, for example, "alkyl group" includes ether groups, haloalkyl, nitroalkyl, carboxyalkyl, hydroxyalkyl, sulfoalkyl, etc.

[0023] As used herein, "acrylic latex" means a dispersion of polymer particles (prepared from ethylenically unsaturated monomers including (meth)acrylic acid and / or (meth)acrylate monomers) in water.

[0024] As used herein, "(meth)acrylate" is a shorthand reference to acrylate, methacrylate, or a combination thereof, and "(meth)acrylic" is a shorthand reference to acrylic, methacrylic, or a combination thereof.

[0025] As used herein, "cross-linker" refers to a molecule capable of forming a covalent bond between polymers or between two different regions of the same polymer.

[0026] As used herein, the terms "polymer" and "copolymer" are interchangeable and may refer to homopolymers formed from repeating units of one structural unit or monomer as well as copolymers that may be formed from different types of structural units or monomers.

[0027] As used herein, "monomer" or reactant generally refers to a compound in a reaction mixture prior to polymerization, and a monomer unit or (alternatively) a repeating unit or structural unit refers to a monomer or reactant in a polymer. Preferably, the various monomers or reactants herein are randomly polymerized monomer units, structural units or repeating units. If the discussion herein relates to a monomer or reactant, it also means the resulting monomer units, structural units or repeating units thereof in a polymer. Similarly, if the discussion relates to a monomer unit, structural unit or repeating unit, it also means a mixture of monomers or reactants used to form a polymer having associative units therein.

[0028] As used herein, the term "substantially free," when used with respect to a composition that may contain a particular compound, means that the composition contains less than 1,000 parts per million (ppm) of the compound, regardless of the context of the compound in the composition (e.g., regardless of whether the compound is present in an unreacted form, in a reacted form as a structural unit of another material, or a combination thereof). The term "completely free," when used with respect to a composition that may contain a particular compound, means that the composition contains less than 100 parts per million (ppm) of the compound, regardless of the context of the compound in the composition (e.g., regardless of whether the compound is present in an unreacted form, in a reacted form as a structural unit of another material, or a combination thereof). As will be understood by one of ordinary skill in the art, the amount of a compound in an ingredient, polymer, formulation, or other component can generally be calculated based on the amount of starting materials employed and the yield obtained when preparing such ingredient, polymer, formulation, or other component.

[0029] When the phrases "free of" (outside the context of the above phrases), "not containing", "not including any", etc. are used herein, such phrases are not intended to exclude the presence of trace amounts of related structures or compounds that may be present but not intentionally used, such as the presence of environmental contaminants.

[0030] When used herein in the context of a polymer, the term "epoxide-free" refers to a polymer that does not include any "epoxide backbone segments" (i.e., segments formed by the reaction of an epoxy group and a group reactive with the epoxy group). For example, a polymer made from an ingredient including an epoxy resin would not be considered to be epoxide-free. Similarly, a polymer having a backbone segment that is a reaction product of a bisphenol (e.g., bisphenol A, bisphenol F, bisphenol S, 4,4'-dihydroxybisphenol, etc.) and a halogenated alcohol (e.g., epichlorohydrin) would not be considered to be epoxide-free. However, a vinyl polymer (e.g., glycidyl methacrylate) formed from a vinyl monomer or oligomer including a pendant epoxy moiety would be considered to be epoxide-free because the vinyl polymer would not contain an epoxy backbone segment. A coating composition referred to as "epoxide-free" is not prepared using any polymer or other material having an epoxy backbone segment.

[0031] Feathering is a term used to describe the loss of adhesion of a coating on a pull tab of a beverage can end cap. When the beverage can is opened, if the coating loses adhesion on the pull tab, a portion of free film may be present on the opening of the container or can. This portion of free film is considered feathered.

[0032] The terms "preferred" and "preferably" refer to embodiments of the present invention that may provide certain benefits in certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are unusable, and is not intended to exclude other embodiments from the scope of the present invention.

[0033] As used herein, the term "comprising" and variations thereof do not have a limiting meaning when they appear in the specification and claims. As used herein, "a," "an," "the," "at least one," and "one or more" are used interchangeably. Thus, for example, a coating composition comprising "an" amino crosslinking agent can be interpreted to mean that the coating composition comprises "one or more" amino crosslinking agents.

[0034] As used herein, the term "or" is generally employed in its conventional sense, including "and / or," unless the content clearly dictates otherwise. The term "and / or" means one or all of the listed elements or a combination of any two or more of the listed elements.

[0035] Also herein, all numbers are assumed to be modified by the term "about," and in certain embodiments, preferably by the term "exactly." As used herein in conjunction with measured amounts, the term "about" refers to the variation in the measured amount as would be expected by a skilled artisan making the measurements and applying a level of care commensurate with the purpose of the measurement and the precision of the measuring device being used.

[0036] It should be noted that, as used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless expressly and unambiguously limited to one referent. Thus, for example, reference to "an antioxidant" includes two or more different antioxidants. As used herein, the term "comprising" and its grammatical variations are intended to be non-limiting, such that recitation of items in a list does not exclude other like items that can be substituted or added to the listed items.

[0037] For the purposes of this specification and the appended claims, unless otherwise indicated, all numbers used in the specification and claims expressing quantities, percentages or ratios, and other numerical values, are to be understood in all cases as being modified by the term "about". Therefore, unless otherwise indicated, the numerical parameters listed in the following specification and the appended claims are approximate values ​​that may vary depending on the desired properties sought to be obtained by the present disclosure. At a minimum, and without attempting to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should at least be interpreted in light of the number of reported significant digits and by applying customary rounding techniques.

[0038] It should be understood that each component, compound, substituent or parameter disclosed herein should be interpreted as being disclosed for use alone or in combination with one or more of each and every other component, compound, substituent or parameter disclosed herein.

[0039] It should also be understood that each range disclosed herein will be interpreted as a disclosure of each specific value with the same number of significant digits within the disclosed range. Thus, for example, a range of 1 to 4 will be interpreted as an explicit disclosure of the values ​​1, 2, 3, and 4, as well as any range of such values.

[0040] It should also be understood that each lower limit of each scope disclosed herein should be understood to be disclosed in conjunction with each upper limit in each scope disclosed herein for the same component, compound, substituent or parameter and each specific value in each scope. Therefore, the disclosure is interpreted as the disclosure of all scopes obtained by combining each lower limit of each scope with each upper limit of each scope or with each specific value in each scope, or by combining each upper limit of each scope with each specific value in each scope. That is, it should also be understood that any scope between the end values ​​in a wide range is also discussed herein. Therefore, the scope of 1 to 4 also means the scope of 1 to 3, 1 to 2, 2 to 4, 2 to 3, etc.

[0041] In addition, specific amounts / values ​​of components, compounds, substituents or parameters disclosed in the specification or examples should be understood as a disclosure of the lower or upper limit of the range, and can therefore be combined with any other lower or upper limit or specific amount / value of a range for the same component, compound, substituent or parameter disclosed elsewhere in the application to form a range for a component, compound, substituent or parameter.

[0042] The above-mentioned summary of the invention and definition of the present disclosure are not intended to describe each disclosed embodiment or its every kind of implementation. The following description more specifically illustrates exemplary embodiments, aspects or embodiments. In some places of the full text of this application, guidance is provided by lists of examples, which can be used in various combinations. In each case, the cited lists are only used as representative groups and should not be interpreted as exclusive enumeration. DETAILED DESCRIPTION

[0043] The present invention provides a coating composition (aqueous or powder coating composition) for beverage can ends, especially easy open ends of beverage cans. Thus, such a composition is intended for use in forming can end coatings, especially easy open can end coatings, and especially internal such coatings (e.g., internal coatings on riveted internal steel or aluminum beverage can ends).

[0044] In one aspect, the aqueous coating composition is an acrylic coating composition comprising an acrylic latex, a carboxyl reactive crosslinking agent, and an optional lubricant. This aqueous coating composition of the present disclosure is a "coil coating composition" because it is applied using a coil coating process. On the other hand, the present disclosure provides a beverage can comprising a metal substrate thereof, at least a portion of which is coated with an aqueous coil coating composition (or a powder coil coating composition). In yet other aspects, the present disclosure provides a method for coil coating a beverage can and / or a metal substrate suitable for a beverage can, particularly an easy-open end cap of a beverage can. The method may include forming an aqueous coil coating composition as described herein (or a powder coil coating composition as described herein), and applying the composition to a metal substrate using a coil coating method.

[0045] The composition herein preferably comprises a crosslinking agent, which is preferably derived from a composition that does not contain formaldehyde. Nitrogen-containing carboxyl reactive crosslinking agents are preferred crosslinking agents. In a preferred embodiment, the crosslinking agent can be a hydroxyalkylamide crosslinking agent. Such crosslinking agents allow the production of preferred formaldehyde-free coating compositions, which have sufficient flexibility and corrosion resistance while being used as an internal or external coating for beverage can end caps including rivets (e.g., for attaching a pull tab thereto, so as to approach the interior of the can, such as via a drinking port). The crosslinking agent can have any suitable combination of one or more carboxyl reactive functional groups, and more preferably includes two or more such groups. Hydroxyl groups are preferred carboxyl reactive groups. In some embodiments, the crosslinking agent includes two or more, three or more, or four or more hydroxyl groups.

[0046] The coil coating compositions herein are suitable for use with metal substrates and coil coating conditions and application methods. In a preferred embodiment, the metal substrate is a metal commonly used in the beverage packaging industry. In one embodiment, the metal substrate comprises steel, aluminum, or a combination thereof. Preferably, the metal substrate is aluminum, and more preferably aluminum without chromium pretreatment. The metal substrate may be formed into a beverage can end cap and may include a riveted beverage can end cap.

[0047] The unique combination of acrylic latex binder system and crosslinker herein enables the preferred non-formaldehyde and non-epoxy binder system to achieve the robust performance required for beverage can end cap application even when using a short curing cycle. Among other features, this unique combination of components unexpectedly achieves the high level of product tolerance and flexibility generally required for the interior coating of beverage metal packaging (and especially easy-open end caps) at the same time. In some embodiments, this performance can be obtained without the need for melamine and / or formaldehyde crosslinkers. In addition, the resulting coating can exhibit such beneficial coating properties while also exhibiting excellent feathering properties.

[0048] For coil coating applications and beverage can end closures, the curing process for coil coating applications is typically very short (e.g., a flash peak metal temperature of 200°C to 260°C (in other embodiments, 230°C to 260°C) is achieved within a 6 second to 30 second oven cure time, preferably an 8 second to 20 second oven cure time, more preferably an 8 second to 15 second oven cure time, even more preferably an 8 second to 14 second oven cure time, and still more preferably a 10 second to 12 second oven cure time).

[0049] Additional details of the compositions and methods are provided below.

[0050] Acrylic latex

[0051] The coating composition disclosed herein is an acrylic-based coating composition. Therefore, the coating composition comprises an acrylic latex. The acrylic latex comprises polymer particles that can be stably dispersed in water. The acrylic latex is an acid or anhydride functional acrylic latex (i.e., a latex comprising a polymer having an acid group (usually a carboxylic acid group) and / or anhydride group).

[0052] Acrylic latex comprises an emulsion polymerized polymer, preferably formed by polymerization of an ethylenically unsaturated monomer component comprising two or more different monomers, more typically three or more different monomers. Preferably, the acrylic latex is polymerized in water, and at least a majority of the acrylic latex (e.g., at least 50% by weight based on the total non-volatile weight (i.e., total solid weight) of the acrylic latex) is an emulsion polymerized latex (e.g., using an emulsion polymerization process to polymerize the ethylenically unsaturated monomer component). In certain embodiments, the acrylic latex comprises at least 50% by weight, at least 60% by weight, at least 70% by weight, at least 80% by weight, at least 90% by weight, at least 95% by weight, or at least 98% by weight of an emulsion polymerized polymer, based on the total solid weight of the acrylic latex.

[0053] In certain embodiments, the acrylic latex preferably has an acid value of at least 40, at least 100 or at least 150 mg KOH / gram of latex. In certain embodiments, the acid value is less than 400, less than 300, less than 200, less than 150 or less than 100 mg KOH / gram of latex. Acid value (also referred to as acid value or acidity) is the mass (in milligrams) of potassium hydroxide (KOH) required to neutralize one gram of chemical. Acid value can be measured according to BS EN ISO 3682-1998 standard. In certain preferred embodiments, the acrylic latex has an acid value from 100 mg KOH / gram of latex to 200 mg KOH / gram of latex. Typically, due to the functionality of the monomer, the acid value is provided by the acrylic polymer particles of the acrylic latex; however, in some embodiments, at least a portion of the acid value is provided by a surfactant (e.g., a polymer surfactant having a carboxylic acid group).

[0054] In certain embodiments, the ethylenically unsaturated monomer component used to prepare the acrylic latex is a monomer mixture, more preferably a monomer mixture comprising at least one (meth)acrylate monomer, more typically a plurality of (meth)acrylate monomers. In a preferred embodiment, the ethylenically unsaturated monomer component used to prepare the acrylic latex is a monomer mixture, more preferably a monomer mixture comprising at least one ethylenically unsaturated acid or anhydride functional monomer or salt thereof and at least one (meth)acrylate monomer, more typically a plurality of (meth)acrylate monomers. Any combination of one or more (meth)acrylates may be included in the ethylenically unsaturated monomer component, optionally in combination with one or more non-(meth)acrylate monomers.

[0055] Examples of useful ethylenically unsaturated acid or anhydride functional monomers or their salts include acids such as, for example, acrylic acid, methacrylic acid, α-chloroacrylic acid, α-cyanoacrylic acid, crotonic acid, α-phenylacrylic acid, β-acryloxypropionic acid, fumaric acid, maleic acid, sorbic acid, α-chlorosorbic acid, angelic acid, cinnamic acid, p-chlorocinnamic acid, β-stearoylacrylic acid, citraconic acid, mesaconic acid, glutaconic acid, aconitic acid, tricarboxyethylene, 2-methylmaleic acid, itaconic acid, 2-methylitaconic acid, methyleneglutaric acid, their salts or mixtures thereof. Preferred unsaturated acid functional monomers include acrylic acid, methacrylic acid, crotonic acid, fumaric acid, maleic acid, 2-methylmaleic acid, itaconic acid, 2-methylitaconic acid, their salts or mixtures thereof. Most preferred unsaturated acid functional monomers include acrylic acid, methacrylic acid, their salts or mixtures thereof.

[0056] In a preferred embodiment, ethylenically unsaturated acid or anhydride functional monomers, including salts thereof, account for at least 5 weight % or at least 10 weight % of the ethylenically unsaturated monomer component used to prepare the acrylic latex. In a preferred embodiment, ethylenically unsaturated acid or anhydride functional monomers, including salts thereof, account for no more than 20 weight % or no more than 15 weight % of the ethylenically unsaturated monomer component used to prepare the acrylic latex.

[0057] In order to obtain the desired total Tg, the ethylenically unsaturated monomer component generally includes one or more "low" Tg monomers (e.g., ethyl acrylate, butyl acrylate, etc.) and one or more "high" Tg monomers (e.g., methyl methacrylate, cyclohexyl methacrylate, etc.). In certain embodiments, useful (meth)acrylate monomers (e.g., "high" Tg (meth)acrylate monomers) have a Tg greater than 50°C, greater than 60°C, greater than 70°C, greater than 80°C, greater than 90°C, or greater than 100°C. Typically, such monomers are cyclic and / or branched (meth)acrylate monomers. Although the upper limit of Tg is not limited, in some embodiments, useful (meth)acrylate monomers have a Tg of less than 130°C or less than 120°C. For the (meth)acrylate monomers specifically mentioned herein, any Tg value provided herein for such monomers should be used for comparison relative to the above-mentioned Tg threshold value. For (meth)acrylate monomers that do not have Tg values ​​reported herein, in the absence of a reliable Tg value reported by the manufacturer of the monomer, the Tg of the monomer can be determined by preparing a homopolymer having a number average molecular weight of at least 4,000 and a suitable polydispersity index (e.g., preferably less than 3 and ideally as low as possible) and measuring the Tg of the homopolymer using a suitable procedure (such as the procedures included in the Test Methods section below).

[0058] Suitable (meth)acrylate monomers include those having the following structure (Formula I):

[0059] CH 2 =C(R 1 )-CO-OR 2 (I)

[0060] Where R 1 is hydrogen or methyl, and R 2 It is an alkyl group (preferably containing 1 to 22 carbon atoms, and more preferably 1 to 16 or 1 to 12 or 1 to 10 carbon atoms), an alicyclic group (preferably containing 4 to 12 carbon atoms or 6 to 10 carbon atoms), an aryl group (preferably containing 4 to 15 carbon atoms or 6 to 10 carbon atoms) or a combination thereof.

[0061] If necessary, in formula (I), R 2The (meth)acrylates of formula (I) may be optionally substituted with one or more (e.g., one to three) moieties such as hydroxyl, halogen, phenyl, and alkoxy. Examples of suitable (meth)acrylates of formula (I) (including, for example, suitable alkyl (meth)acrylates) include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, Esters, decyl (meth)acrylate, isodecyl (meth)acrylate, tridecyl (meth)acrylate, lauryl (meth)acrylate (also known as dodecyl (meth)acrylate), cyclohexyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, isobornyl (meth)acrylate, norbornenyl (meth)acrylate, tricyclodecenyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and the like, substituted variants thereof (e.g., ring-substituted variants of benzyl (meth)acrylate or phenyl (meth)acrylate), and isomers and mixtures thereof.

[0062] Typically, (meth)acrylate monomers will comprise a majority (e.g., 50% by weight or more) of the ethylenically unsaturated monomer component. In preferred embodiments, (meth)acrylate monomers comprise at least 70% by weight, at least 80% by weight, or at least 85% by weight of the ethylenically unsaturated monomer component used to prepare the acrylic latex. In preferred embodiments, (meth)acrylates comprise no more than 95% by weight, or no more than 90% by weight, of the ethylenically unsaturated monomer component used to prepare the acrylic latex. If an acid or anhydride functional polymeric surfactant is used in an amount sufficient to prepare the latex, the ethylenically unsaturated monomer component may comprise more than 95% by weight of (meth)acrylate, or even up to 100% by weight of (meth)acrylate.

[0063] In a preferred embodiment, the ethylenically unsaturated monomer component comprises at least one "linear" (meth) alkyl ester monomer of formula (I) having a linear (e.g., unbranched) alkyl group (preferably, a (C1-C4) alkyl group). Examples of such linear groups include the following moieties: methyl, ethyl, n-propyl, n-butyl, and the like. Preferred such monomers include one or more of the following: methyl (meth) acrylate, ethyl (meth) acrylate, n-propyl (meth) acrylate, n-butyl (meth) acrylate, and mixtures thereof. In some embodiments, the ethylenically unsaturated monomer component comprises at least 20 weight percent, more preferably at least 30 weight percent, and even more preferably at least 40 weight percent of one or more linear (meth) alkyl esters. When present, the linear (meth) alkyl ester typically comprises no more than 80 weight percent, no more than 70 weight percent, no more than 60 weight percent, or no more than 50 weight percent of the ethylenically unsaturated monomer component.

[0064] In some embodiments, the ethylenically unsaturated monomer component for forming the acrylic latex comprises at least one cyclic and / or branched (meth) acrylate monomer of formula (I) having cyclic and / or branched groups. Examples of such groups include the following parts: isopropyl, isobutyl, sec-butyl, tert-butyl, cyclohexyl, polycyclic (e.g., bicyclic or tricyclic), etc. Preferred such monomers include one or more of the following: isopropyl (meth) acrylate, isobutyl (meth) acrylate, sec-butyl (meth) acrylate, tert-butyl (meth) acrylate, isopentyl (meth) acrylate, 2-ethylhexyl (meth) acrylate, isooctyl (meth) acrylate, isononyl (meth) acrylate, isodecyl (meth) acrylate, tridecyl (meth) acrylate, cyclohexyl (meth) acrylate, benzyl (meth) acrylate, isobornyl (meth) acrylate, norbornene (meth) acrylate, tricyclodecene (meth) acrylate, and mixtures thereof. Preferred such monomers include cyclohexyl (meth) acrylate. In some embodiments, the ethylenically unsaturated monomer component comprises at least 10 weight percent, at least 15 weight percent, or at least 20 weight percent of one or more cyclic and / or branched alkyl (meth)acrylates. When present, cyclic and / or branched alkyl (meth)acrylates typically comprise no more than 50 weight percent, no more than 45 weight percent, no more than 40 weight percent, no more than 35 weight percent, or no more than 30 weight percent of the ethylenically unsaturated monomer component.

[0065] One or more polyethylenically unsaturated (meth)acrylate monomers may be optionally included in the ethylenically unsaturated monomer component. Typically such monomers are used for internal crosslinking of latex particles. Examples of polyethylenically unsaturated (meth)acrylates include polyol esters of acrylic acid or methacrylic acid, such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate (e.g., 1,2-propylene glycol di(meth)acrylate and 1,3-propylene glycol di(meth)acrylate), butylene glycol di(meth)acrylate (e.g., 1,3-butylene glycol di(meth)acrylate and 1,4-butylene glycol di(meth)acrylate), heptanediol di(meth)acrylate, hexanediol di(meth)acrylate, trimethylolethane, 1,4-butylene glycol di(meth)acrylate ... Tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolbutane tri(meth)acrylate, trimethylolheptane tri(meth)acrylate, trimethylolhexane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, dipropylene glycol di(meth)acrylate, trimethylolhexane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, isosorbide di(meth)acrylate, allyl(meth)acrylate, glycerol dimethacrylate, their isomers and their mixtures. Examples of polyethylenically unsaturated monomers other than (meth)acrylate include diallyl phthalate, divinylbenzene, divinyltoluene, divinylnaphthalene and their mixtures. In some embodiments, di(meth)acrylate is a preferred polyethylenically unsaturated monomer. In some embodiments (e.g., certain emulsion polymerization embodiments), the ethylenically unsaturated monomer component comprises at least 5% by weight or at least 10% by weight of one or more polyethylenically unsaturated monomers. If used, such multi-ethylenically unsaturated monomers will typically be included in the ethylenically unsaturated monomer component in an amount of no more than 25 weight percent, no more than 20 weight percent, no more than 15 weight percent, no more than 10 weight percent, or no more than 5 weight percent. In some embodiments, the ethylenically unsaturated monomer component includes no more than 1 weight percent.

[0066] In some embodiments, the ethylenically unsaturated monomer component does not include any multi-ethylenically unsaturated (meth)acrylate monomers. In some embodiments, the ethylenically unsaturated monomer component does not include any multi-functional cross-linking monomers.

[0067] The ethylenically unsaturated monomer component may optionally contain oxirane functional monomers, such as, for example, oxirane functional α, β-unsaturated monomers. Typically, the monomer is a glycidyl ester of an α, β-unsaturated acid or anhydride thereof (i.e., an α, β-ethylenically unsaturated monomer containing an oxirane group). Examples of suitable monomers containing glycidyl groups are glycidyl (meth)acrylate (i.e., glycidyl methacrylate and glycidyl acrylate), mono- and diglycidyl itaconic acid esters, mono- and diglycidyl maleate, and mono- and diglycidyl formate. It is also contemplated that allyl glycidyl ether and vinyl glycidyl ether may be used as oxirane functional monomers. Preferred oxirane functional monomers are glycidyl acrylate and glycidyl methacrylate ("GMA"), with GMA being particularly preferred in some embodiments. The ethylenically unsaturated monomer component preferably contains no more than 30 wt%, no more than 20 wt%, no more than 10 wt%, or no more than 9 wt% of monomers containing ethylene oxide groups, if any. The ethylenically unsaturated monomer component may contain at least 1 wt%, at least 2 wt%, at least 3 wt%, or at least 5 wt% of monomers containing ethylene oxide groups.

[0068] In some embodiments, the ethylenically unsaturated monomer component does not include glycidyl (meth)acrylate monomers. In some embodiments, the acrylic latex and preferably the entire coil coating composition does not contain glycidyl acrylate and glycidyl methacrylate monomers or structural units derived therefrom. In some embodiments, the ethylenically unsaturated monomer component does not include any monomers having oxirane groups.

[0069] The ethylenically unsaturated monomer component may also include any other suitable monomers. For example, suitable other ethylenically unsaturated monomers (e.g., olefinic or vinyl monomers other than (meth)acrylates) may include isoprene, diallyl phthalate, conjugated butadiene, vinyl naphthalene, acrylonitrile, (meth)acrylamide (e.g., acrylamide, methacrylamide, N-isobutoxymethylacrylamide, N-butoxymethylacrylamide, etc.), methacrylonitrile, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl stearate, etc., and variants and mixtures thereof.

[0070] In some embodiments, the ethylenically unsaturated monomer component, preferably the acrylic latex, and more preferably the entire coil coating composition does not contain any (meth)acrylamide-type monomers (e.g., acrylamide or methacrylamide, N-isobutoxymethylacrylamide, N-butoxymethylacrylamide) or structural units derived therefrom.

[0071] The ethylenically unsaturated monomer component may optionally contain one or more vinyl aromatic compounds, including styrene. If a vinyl aromatic monomer is used, it is preferably not styrene or a substituted styrene. In a preferred embodiment, the ethylenically unsaturated monomer component is not intentionally formulated to contain styrene.

[0072] Suitable vinyl aromatic compounds may include styrene (not preferred in some embodiments), substituted styrene compounds (not preferred in some embodiments), and / or other types of vinyl aromatic compounds (e.g., any of the ethylenically unsaturated monomers containing aromatic groups described herein, including aryl (meth)acrylates, such as benzyl (meth)acrylate). In some embodiments, the ethylenically unsaturated monomer component contains, if any, less than 20 weight percent, less than 10 weight percent, less than 5 weight percent, or less than 1 weight percent of vinyl aromatic compounds.

[0073] In some embodiments, the ethylenically unsaturated monomer component for preparing acrylic latex does not include styrene. In some such embodiments that do not contain styrene (or, alternatively, some "low" styrene embodiments), the ethylenically unsaturated monomer component includes one or more monomers containing cyclic groups, such as, for example, ethylenically unsaturated monomers including C4 rings (e.g., cyclobutane rings), C5 rings (e.g., cyclopentane rings), C6 rings (e.g., cyclohexane rings) or polycyclic groups (e.g., bicyclic groups or tricyclic groups). In some embodiments, the cyclohexane group that can optionally include one or more substituents replacing hydrogen is a preferred cyclic group. (Meth) acrylic acid esters containing cyclic groups are preferred such monomers, wherein cyclohexyl (meth) acrylic acid ester is particularly preferred. Suitable branched monomers (e.g., monomers with branched groups that do not include longer straight chains) can also be used in such embodiments that do not contain styrene to replace styrene. Although it is not desired to be bound by theory, such monomers can be used to replace styrene or other vinyl aromatic monomers to provide at least some beneficial properties of styrene without using styrene.

[0074] In some embodiments, the ethylenically unsaturated monomer component, preferably the acrylic latex, more preferably the entire coil coating composition, is substantially free of vinyl aromatic monomers or structural units derived therefrom. In some embodiments, the ethylenically unsaturated monomer component, preferably the acrylic latex, more preferably the entire coil coating composition does not contain any vinyl aromatic monomers or structural units derived therefrom. In some embodiments, the acrylic latex (e.g., emulsion-polymerized acrylic latex) is substantially free of vinyl monomers containing cyclic groups (e.g., certain embodiments, such as, for example, certain embodiments when methyl (meth)acrylate is employed).

[0075] In some embodiments, the ethylenically unsaturated monomer component, preferably the acrylic latex, and more preferably the entire coil coating composition, does not contain any halogenated monomers, such as chlorinated vinyl monomers or structural units derived therefrom.

[0076] In some embodiments, the ethylenically unsaturated monomer component forming the acrylic latex may optionally include one or more adhesion promoting monomers. Examples of such monomers may include certain ethylenically unsaturated monomers with a phosphate group or a phosphite group. Examples of such monomers are PAM-100, PAM-200 and PAM-300 monomers commercially available from Solvay. Such monomers may be used in an amount to achieve the desired result.

[0077] In some embodiments, the ethylenically unsaturated monomer component forming the acrylic latex may optionally include a hydroxyl-functional monomer (e.g., hydroxyethyl acrylate (HEA), hydroxyethyl methacrylate (HEMA), hydroxypropyl (meth)acrylate (HPMA), etc.). Generally, the amount of the hydroxyl-functional monomer will be selected to achieve the desired hydroxyl functionality. That is, when a hydroxyl-functional monomer is used, the acrylic latex may have any suitable hydroxyl value to achieve the desired result.

[0078] In some embodiments, the ethylenically unsaturated monomer component used to form the acrylic latex comprises (i) at least one of acrylic acid or methacrylic acid, preferably acrylic acid, (ii) at least one of ethyl acrylate or n-butyl acrylate, preferably ethyl acrylate, and (iii) a cyclic or branched monomer, preferably cyclic, more preferably cyclohexyl (meth)acrylate, and even more preferably cyclohexyl methacrylate (CHMA).

[0079] Any suitable method or material can be used to prepare the acrylic latex. Although the aforementioned monomers can be polymerized by standard free radical polymerization techniques (e.g., using initiators such as azoalkanes, peroxides, or peroxyesters) to form acrylic polymers, at least a portion (e.g., at least 50 wt%, at least 60 wt%, at least 70 wt%, at least 80 wt%, at least 90 wt%, at least 95 wt%) of the acrylic latex is an emulsion polymerized polymer.

[0080] The ethylenically unsaturated monomer component is typically emulsion polymerized in an aqueous medium in the presence of at least one surfactant (or emulsifier), which may be polymeric, non-polymeric, or a blend thereof. In embodiments where one or more surfactants are used to prepare the latex polymer, the surfactant may be anionic, cationic, or zwitterionic surfactants, or mixtures thereof, and preferably also includes one or more salt groups. In a preferred embodiment, the surfactant includes one or more neutralized acid or anhydride groups. Examples of suitable neutralized acid groups may include carboxylate groups (-COO-), sulfate groups (-OSO-), and thiocyanate groups (-S-O-). 3 -), sulfinate group (-SOO-), sulfonate group (–SO 2 O–), phosphate group (-OPO 3 -), phosphite group (-POO-), phosphonate group (-PO 3 -) and their combinations.

[0081] In some embodiments, anionic surfactants are preferred. Examples of suitable anionic surfactants include any of the following surfactants, preferably at least partially neutralized with a suitable base (e.g., any of the bases disclosed herein): any of the acid or anhydride functional polymeric surfactants disclosed herein, dodecylbenzenesulfonic acid, dinonylnaphthalenesulfonic acid, dinonylnaphthylene disulfonic acid, di(2-ethylhexyl)sulfosuccinic acid, dioctylsulfosuccinic acid, sodium lauryl sulfate, sodium dodecyl sulfate, sodium lauryl polyoxyethylene sulfate, fatty acid (ester) acid esters, polyarylether phosphate acid or sulfonic acid ester acid, etc., including mixtures thereof.

[0082] In some embodiments, it may be useful to use a surfactant that is a "strong acid" surfactant prior to neutralization.

[0083] Although any suitable base can be used to neutralize or partially neutralize the polymer or non-polymer surfactant to form anionic salt groups, amines are preferred bases, and tertiary amines are particularly preferred. Some examples of suitable tertiary amines are trimethylamine, dimethylethanolamine (also known as dimethylethanolamine), methyldiethanolamine, triethanolamine, ethylmethylethanolamine, dimethylethylamine, dimethylpropylamine, dimethyl 3-hydroxy-1-propylamine, dimethylbenzylamine, dimethyl 2-hydroxy-1-propylamine, diethylmethylamine, dimethyl 1-hydroxy-2-propylamine, triethylamine, tributylamine, N-methylmorpholine and mixtures thereof. Most preferably, triethylamine or dimethylethanolamine is used as the tertiary amine.

[0084] Some additional examples of neutralizing bases for forming anionic salt groups include inorganic and organic bases such as sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonium hydroxide, and mixtures thereof.

[0085] Some examples of neutralizing compounds useful for neutralizing the base groups present on the surfactant and forming cationic salt groups include organic and inorganic acids, such as formic acid, acetic acid, hydrochloric acid, sulfuric acid, and combinations thereof.

[0086] Although the surfactant may optionally include one or more ethylenically unsaturated groups (e.g., if the surfactant is a polymerizable non-polymeric surfactant), in some embodiments, the surfactant is a saturated surfactant. By way of example, amine-neutralized dodecylbenzenesulfonic acid is considered a saturated surfactant. Although amine-neutralized dodecylbenzenesulfonic acid includes an aromatic group containing a carbon-carbon double bond, it does not include any ethylenically unsaturated groups.

[0087] The surfactant can be any suitable type of surfactant, and can, for example, be a "lower" molecular weight surfactant (e.g., a surfactant that is non-polymeric and / or has a number average molecular weight of less than about 1,000 Daltons, more typically less than about 750 Daltons, and even more typically less than about 500 Daltons).

[0088] In some embodiments, a polymeric surfactant having a number average molecular weight of, for example, greater than about 2,000 Daltons or even greater than about 4,000 Daltons is used. Examples of suitable polymeric surfactants may include water-dispersible polymers of acrylic acid, alkyd, polyester, polyether, polyolefin, or polyurethane type, including copolymers thereof (e.g., polyether-acrylic acid copolymers) and mixtures thereof. Typically, such water-dispersible polymers include one or more salt groups to facilitate stable dispersion into water. Examples of suitable such polymer salts are disclosed in the following documents: U.S. Pat. No. 8,092,876 (O'Brien); International Publication No. WO 2018 / 013766 (O'Brien et al.); and U.S. Pat. No. 9,404,006 (Li) (which describes the use of certain (poly)ethylene (meth)acrylic acid copolymers).

[0089] Examples of specific water-dispersible polymers useful as "polymeric surfactants" are acid-functional polymers of "higher" acid values ​​(e.g., acid values ​​greater than about 40, more preferably greater than about 100 mg KOH / g polymer). In some embodiments, an acrylic polymer having such an acid value is solution polymerized in an organic solvent and then poured into water (e.g., via at least partial neutralization with a suitable base such as, for example, an amine or any other base disclosed herein) and used to support the emulsion polymerization of an ethylenically unsaturated monomer component. In some embodiments, the acid- or anhydride-functional organic solution-polymerized acrylic polymer is formed from an ethylenically unsaturated monomer component that includes an acid- or anhydride-functional monomer, a branched and / or cyclic monomer, and optionally any other suitable ethylenically unsaturated monomer. In some such embodiments, the acrylic polymer is free of styrene.

[0090] Examples of suitable polymerizable surfactants include those disclosed in U.S. Patent Publication No. 2002 / 0155235 (Taylor et al.); those disclosed in U.S. Patent No. 10,800,941 (Gibanel et al.), and those available under the trade name REASOAP from Adeka Corporation, Tokyo, Japan; NOIGEN and HITENOL available from Da-Ichi Kogyo Siyyaku Co., Ltd. (Tokyo, Japan), and SIPOMER available from Solvay Rhodia (Brussels, Belgium).

[0091] In some embodiments, nonionic surfactants are included in the reaction mixture for preparing the latex polymer. Any suitable nonionic surfactant can be used. Examples of suitable nonionic surfactants include ethoxylated compounds. In some embodiments, the nonionic compound is a sucrose ester, a sorbitan ester, an alkyl glycoside, a glyceride, or a mixture thereof. In some embodiments, nonionic surfactants containing hydroxyl groups are used. Nonionic surfactants containing or derived from polysorbate compounds can be used in some embodiments.

[0092] In some embodiments, a surfactant or a mixture of surfactants as described in U.S. Publication No. 2020 / 0385601 (Gibanel et al.). For example, one or more anionic or zwitterionic surfactants (e.g., non-polymeric surfactants) having acid groups neutralized with a metal base (e.g., a metal base including aluminum, calcium, lithium, magnesium, sodium, or potassium) can be used. An example of such a surfactant is sodium dioctyl sulfosuccinate.

[0093] In a preferred embodiment, a single-stage or multi-stage emulsion polymerization process is used to prepare the latex polymer (not counting any emulsion polymerization step that may be used to prepare a "seed" that is optionally used to promote the overall emulsion polymerization). The emulsion polymerization process can be carried out in a variety of ways. For example, the emulsion polymerization reaction of the ethylenically unsaturated monomer component can be carried out in the form of a batch, intermittent or continuous operation.

[0094] In some embodiments, the emulsion polymerization process uses an optional pre-emulsion monomer mixture, wherein some or all of the reactant components and one or more surfactants are dispersed in an aqueous carrier under agitation to form a stable pre-emulsion. In other embodiments, the ethylenically unsaturated monomer component is polymerized without using a pre-emulsion step.

[0095] A portion of the surfactant and a portion of the aqueous carrier may also be introduced into the reactor and preferably heated, stirred and maintained under nitrogen aeration to aid in the subsequent polymerization reaction. Preferred temperatures for heating the surfactant dispersion include temperatures greater than 65°C, more preferably from 70°C to 90°C.

[0096] The monomer pre-emulsion or non-pre-emulsified ethylenically unsaturated monomer component can be fed incrementally or continuously over time to the heated aqueous dispersion in the reactor. Alternatively, in certain embodiments, a batch or semi-batch process can be used to polymerize the reactant monomers in the aqueous dispersion, as described in, for example, U.S. Patent No. 8,092,876 (O'Brien). In further embodiments, the polymerization process can be carried out in a classic two-stage (or multi-stage) "core-shell" arrangement. Alternatively, the polymerization process can be carried out in a multi-stage "reverse core-shell" arrangement, as discussed in International Publication No. WO 2015 / 002958 (Gibanel et al.).

[0097] Regarding the conditions of the emulsion polymerization, the ethylenically unsaturated monomer component is preferably polymerized in an aqueous medium with a water-soluble free radical initiator.

[0098] The temperature of the polymerization is generally from 0°C to 100°C, preferably from 50°C to 90°C, more preferably from 70°C to 90°C, even more preferably from 80°C to 85°C. The pH of the aqueous medium is generally maintained at a pH of 5 to 12.

[0099] Typically, the free radical initiator can be selected from one or more water-soluble peroxides known to be used as free radical initiators. Examples include hydrogen peroxide and tert-butyl hydroperoxide. Redox initiator systems well known in the art (e.g., tert-butyl hydroperoxide, erythrosonic acid, and ferrous complexes) can also be used.

[0100] Further examples of polymerization initiators that may be employed include polymerization initiators that thermally decompose at the polymerization temperature to generate free radicals. Examples include both water-soluble and water-insoluble substances. Further examples of free radical initiators that may be used include persulfates such as ammonium or alkali metal (potassium, sodium or lithium) persulfates; azo compounds such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile) and 1-tert-butylazocyanocyclohexane; hydroperoxides such as tert-butyl hydroperoxide, hydrogen peroxide, tert-amyl hydroperoxide, methyl hydroperoxide and cumene hydroperoxide; peroxides such as peroxides; Benzoyl oxide, octanoyl peroxide, di-tert-butyl peroxide, ethyl 3,3'-di(tert-butylperoxy)butyrate, ethyl 3,3'-di(tert-amylperoxy)butyrate, tert-amylperoxy-2-ethylhexanoate and tert-butylperoxypivalate; peresters such as tert-butyl peracetate, tert-butyl perphthalate, tert-butyl perbenzoate; and percarbonates such as di(1-cyano-1-methylethyl)peroxydicarbonate; perphosphates, etc.; and combinations thereof.

[0101] The polymerization initiator can be used alone or can be used as the oxidizing component of a redox system which also preferably includes a reducing component such as ascorbic acid, malic acid, glycolic acid, oxalic acid, lactic acid, thioglycolic acid or an alkali metal sulfite, more specifically a bisulfite, dithionite or metabisulfite such as sodium bisulfite, potassium dithionite and potassium metabisulfite, or sodium formaldehyde sulfoxylate, benzoin, and combinations thereof. The reducing component is commonly referred to as an accelerator or catalyst activator.

[0102] Initiators and accelerators (if any) are preferably used in a proportion of from 0.001% to 5% each, based on the weight of the monomers to be copolymerized. If desired, promoters such as chlorides and sulfates of cobalt, iron, nickel or copper may be used in small amounts. Examples of redox catalyst systems include tert-butyl hydroperoxide / sodium formaldehyde sulfoxylate / Fe(II) and ammonium persulfate / sodium bisulfite / sodium bisulfite / Fe(II).

[0103] If desired, chain transfer agents may be used to control polymer molecular weight.

[0104] After polymerization is complete, at least a portion of the carboxylic acid groups and / or anhydride groups (or other salt-forming groups, such as other neutralizable acid groups and / or neutralizable base groups) of the latex polymer can be neutralized or partially neutralized with a suitable alkaline compound (or other suitable neutralizing compound) to produce water-dispersible groups. The alkaline compound used for neutralization can be a metal base, a fugitive base (e.g., ammonia and primary, secondary and / or tertiary amines), or a mixture thereof. In a preferred embodiment, the base is a fugitive base, more preferably an amine. The degree of neutralization can vary significantly depending on the amount of acid or base groups included in the latex polymer and the desired degree of dispersion.

[0105] Although any suitable base can be used to neutralize or partially neutralize the acid groups of the latex to form anionic salt groups, amines are preferred bases, with tertiary amines being particularly preferred. Some examples of suitable tertiary amines are trimethylamine, dimethylethanolamine (also referred to as dimethylethanolamine), methyldiethanolamine, triethanolamine, ethylmethylethanolamine, dimethylethylamine, dimethylpropylamine, dimethyl 3-hydroxy-1-propylamine, dimethylbenzylamine, dimethyl 2-hydroxy-1-propylamine, diethylmethylamine, dimethyl 1-hydroxy-2-propylamine, triethylamine, tributylamine, N-methylmorpholine and mixtures thereof. Most preferably, triethylamine or dimethylethanolamine is used as the tertiary amine. Some other examples of neutralizing bases for forming anionic salt groups include inorganic and organic bases, such as sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonium hydroxide and mixtures thereof. In a preferred embodiment, the base is a short-acting base, more preferably an amine. The degree of neutralization can vary significantly depending on the amount of the acid or base groups included in the latex polymer and the desired degree of dispersion.

[0106] The emulsion polymerized polymer of the acrylic latex can have any suitable molecular weight. The latex polymer can have any suitable molecular weight. In some embodiments, the latex polymer has a number average molecular weight (M) greater than 20,000, greater than 30,000, greater than 100,000, greater than 200,000, or greater than 300,000. n ). n The upper range of M is not limited and may be 1,000,000 or greater. However, in certain embodiments, M n Less than 1,000,000, less than 600,000, or less than 400,000. Gel permeation chromatography (GPC) using polystyrene standards is a useful method for determining Mn. Because the molecular weight may be too large to measure (e.g., via GPC analysis using polystyrene standards) in some embodiments, it may be necessary to determine the number average molecular weight via theoretical calculations.

[0107] The acrylic latex may have any suitable glass transition temperature (Tg). In preferred embodiments, the acrylic latex has a Tg of at least 0°C, at least 5°C, at least 10°C, at least 15°C, at least 20°C, or at least 25°C. In embodiments intended for use in forming easy-open end cap coatings, particularly interior such coatings (e.g., interior coatings located on riveted interior steel or aluminum beverage can end caps), the acrylic latex preferably exhibits a Tg of no greater than 50°C, no greater than 45°C, or no greater than 40°C. In some embodiments, the acrylic latex exhibits a Tg of no greater than 35°C, no greater than 30°C, or no greater than 25°C. Differential scanning calorimetry (DSC) is an example of a useful method for determining the Tg of a latex, using the representative DSC method provided in the Test Methods section described below.

[0108] The coating composition of the present disclosure preferably comprises at least a film-forming amount of the acrylic latex described herein. In a preferred embodiment, the coating composition comprises at least 50 wt%, at least 65 wt%, at least 80 wt%, or at least 90 wt% of the acrylic latex based on the total solid weight of the coating composition. The coating composition preferably comprises less than 99 wt% or less than 95 wt% of the acrylic latex described herein based on the total solid weight of the coating composition.

[0109] Crosslinking agent

[0110] In a preferred embodiment, one or more curing agents or crosslinking resins (sometimes referred to simply as crosslinkers) are used to formulate aqueous coil coating compositions. The choice of a particular crosslinker generally depends on the particular product being formulated. For coating compositions, it is preferred to use carboxyl-reactive crosslinkers, particularly certain nitrogen-containing carboxyl-reactive crosslinkers.

[0111] The carboxyl-reactive cross-linking agent may contain any suitable number of nitrogen atoms, although it will typically contain one or more or two or more nitrogen atoms.Such cross-linking agents are not derived from formaldehyde.

[0112] The carboxyl reactive cross-linking agent can have any suitable combination of one or more carboxyl reactive functional groups, and more preferably includes two or more such groups. Hydroxyl groups are preferred carboxyl reactive groups. Other suitable carboxyl reactive groups can include, for example, carbodiimide, oxazoline and aziridine groups. In some embodiments, the carboxyl reactive cross-linking agent includes two or more, three or more or four or more hydroxyl groups.

[0113] In some embodiments, the crosslinking agent (eg, hydroxyalkylamide) has a hydroxyl number of at least 100, at least 200, at least 300, at least 400, or at least 500 mg KOH / g resin.

[0114] In certain embodiments of the coating composition, the acrylic latex and the crosslinking agent are present in a molar equivalent ratio of carboxyl groups in the acrylic latex to hydroxyl groups in the crosslinking agent of at least 1.5:1, preferably at least 2:1 (e.g., COOH groups to OH groups). In certain embodiments of the coating composition, the acrylic latex and the crosslinking agent are present in a molar equivalent ratio of carboxyl groups in the acrylic latex to hydroxyl groups in the crosslinking agent of at most 6:1 or at most 5:1 (e.g., COOH groups to OH groups). If the ratio is lower than 1.5:1 (latex carboxyl groups to crosslinker hydroxyl groups), in certain embodiments, the flexibility of the coil coating composition is too low for effective stamping of can end caps. If the ratio is higher than 6:1 (latex carboxyl groups to crosslinker hydroxyl groups), other properties of the coil coating composition (such as solvent resistance, chemical resistance, and adhesion) may be adversely affected.

[0115] Herein, "carboxyl equivalents" and "carboxyl groups" include carboxylic acid groups as well as neutralized acid groups (i.e., carboxylate groups) and anhydride groups (anhydride groups count as two carboxyl equivalents). The molar equivalent ratio of carboxyl groups in the acrylic latex to hydroxyl groups in the crosslinker is calculated as shown.

[0116] The equivalent number of COOH groups in acrylic latex is based on the measured acid value of the latex (i.e., resin). The acid value (also known as acid number or acidity) is the mass (in milligrams) of potassium hydroxide (KOH) required to neutralize one gram of the chemical. The acid value is used to calculate the number of COOH groups per unit mass of resin:

[0117]

[0118] in:

[0119] AV(resin): measured acid value of latex (in mg / g)

[0120] AE: Acid equivalent = eAc = eCOOH = Equivalent weight of COOH groups in latex (in moles)

[0121] M(KOH): Molecular weight of potassium hydroxide (KOH) = 56.1 g / mol

[0122] m (dry resin): dry mass of latex (in g) (=weight % of latex in formulation x dry content % in latex).

[0123] The equivalent number of hydroxyl groups in a crosslinker (e.g., PRIMID crosslinker) is based on the same principle as the calculation of COOH groups in latex. The hydroxyl value is the mass of potassium hydroxide (KOH) required to neutralize the acetic acid absorbed when one gram of a chemical containing free hydroxyl groups is acetylated. The hydroxyl value measured on a PRIMID crosslinker using, for example, the ISO 4629 test method allows the calculation of the number of OH groups per unit mass of the crosslinker (e.g., PRIMID crosslinker) (i.e., resin):

[0124]

[0125] in:

[0126] HV(resin): Measured hydroxyl value of the crosslinker (in mg / g)

[0127] HE: Hydroxyl equivalent weight = eOH = equivalent weight of OH groups in the crosslinker (in moles)

[0128] M(KOH): Molecular weight of potassium hydroxide (KOH) = 56.1 g / mol

[0129] m (dry resin): dry mass of crosslinker in g (= % by weight of dry crosslinker in the formulation).

[0130] The coating compositions herein preferably contain at least 0.5 wt%, at least 1 wt%, at least 1.5 wt%, at least 2 wt%, at least 2.5 wt%, or at least 3 wt% of a crosslinker, based on the total solid weight of the coating composition. Although the upper limit of the amount of the crosslinker may vary depending on the specific embodiment, typically the coating composition will contain less than 30 wt%, less than 20 wt%, less than 15 wt%, less than 10 wt%, or less than 7 wt% of a crosslinker, based on the total solid weight of the coating composition.

[0131] The coating compositions of the present disclosure may include a crosslinker mixture, wherein the crosslinker mixture includes greater than 50 wt%, greater than 66 wt%, or greater than 80 wt% of the nitrogen-containing carboxyl-reactive crosslinker described herein, based on the total weight of the crosslinker.

[0132] In some embodiments, the carboxyl reactive crosslinking agent includes two or more nitrogen atoms, and in some embodiments includes a total of two nitrogen atoms. In other embodiments, one or more (and more preferably two or more) nitrogen atoms are present in an amide group, an aziridine group, an imide group, a diimide group, an oxazoline group, a carbamate group, or a combination thereof. In certain embodiments, the crosslinking agent includes at least one amide group, at least one imide group, or a combination thereof.

[0133] In some embodiments, the nitrogen-containing carboxyl-reactive crosslinking agent includes two or more amide groups. In yet other embodiments, the nitrogen-containing carboxyl-reactive crosslinking agent may contain a single amide group, such as, for example, a multi-substituted amide group with two or more hydroxyl groups. In a preferred embodiment, the nitrogen-containing carboxyl-reactive crosslinking agent includes a β-hydroxyl group relative to the nitrogen atom of the amide bond.

[0134] Suitable nitrogen-containing carboxyl-reactive crosslinkers include hydroxyalkylamide crosslinkers. These allow the production of preferably formaldehyde-free aqueous coating compositions comprising the acrylic latex described above and having sufficient flexibility to be used as an interior or exterior coating for easy-open beverage can end caps. By way of example, the preferred hydroxyalkylamide crosslinker PRIMID QM1260 from EMS-GRILTECH has a hydroxyl value of 550 to 650 mgKOH / g, according to the manufacturer.

[0135] In certain preferred embodiments, the nitrogen-containing carboxyl-reactive crosslinking agent comprises one or more, more preferably two or more groups having the structure of the following formula (III):

[0136] HO-R 5 -N(R 6 )-C(=O)-(III)

[0137] Each R 5 are independently organic groups, and each R 6 As shown in formula (III), the hydroxyl group depicted can be a primary hydroxyl group, a secondary hydroxyl group or a tertiary hydroxyl group, depending on R 5 In some embodiments, the hydroxyl group is a primary hydroxyl group.

[0138] In formula (III), R 5 Any suitable number of carbon atoms may be included, but will typically include from 2 to 10 carbon atoms, more typically from 2 to 8 carbon atoms, more typically from 2 to 6 carbon atoms, and even more typically from 2 to 4 carbon atoms. In formula (III), R 5 Typically at least two carbon atoms will be included in the chain, with one end of the carbon atom being connected to the depicted nitrogen atom and the other end being connected to the depicted hydroxyl group. In one embodiment, the depicted hydroxyl group is directly attached to a first carbon atom, which is directly attached to a second carbon, which in turn is directly attached to the depicted nitrogen atom. In some embodiments of formula (III), R 5 Yes – (CH 2 ) 2 In yet other embodiments of formula (III), R 5It is an alkylene group preferably having 1 to 5 carbon atoms (e.g., methylene, ethylene, n-propylene, sec-propylene, n-butyl, sec-butylene, tert-butylene, pentylene, etc.).

[0139] In some embodiments of Formula (III), R 6 is an organic group including a hydroxyl group. In some such embodiments of Formula (III), R 6 With structure HO-R 5 -, where R 5 is as described above. 6 Examples of groups include hydroxyalkyl groups preferably having from 1 to 5 carbon atoms (e.g., hydroxymethyl, hydroxy-methyl, hydroxy-ethyl, 3-hydroxy-propyl, 2-hydroxy-propyl, 4-hydroxy-butyl, 3-hydroxy-butyl, 2-hydroxy-2-propyl-methyl, 5-hydroxy-pentyl, 4-hydroxy-pentyl, 3-hydroxy-pentyl, 2-hydroxy-pentyl and pentyl isomers). Such R 6 An example of a nitrogen-containing carboxyl-reactive crosslinking agent of the group is provided in the following formula (IV) (which is believed to be the structure of the PRIMID XL-552 product commercially available from EMS):

[0140]

[0141] In certain preferred embodiments, the nitrogen-containing carboxyl-reactive crosslinking agent is a compound having the structure of the following formula (V):

[0142] (HO-R 5 -N(R 6 )-C(=O)) n -X(V)

[0143] Where R 5 and R 6 is as described above for formula (III), n is an integer of 2 or greater, and X is a polyvalent organic group.

[0144] In yet other embodiments, the nitrogen-containing carboxyl-reactive crosslinking agent is a compound having the structure of Formula (VI):

[0145] HO-R 5 -N(R 6 )-C(=O)-XC(=O)-N(R 6 )-(R 5 )-OH(VI)

[0146] Wherein R 5 and R 6is independently an organic group, X is a divalent organic group, and wherein the hydroxyl groups are independently primary hydroxyl groups or secondary hydroxyl groups. In some embodiments of Formula (VI), X is an alkylene group. In other embodiments of Formula (VI), X is -(CH 2 ) m -group, wherein (i) m is an integer of 1 or greater, 2 or greater, 3 or greater, 4 or greater, and more typically 2 to 10, and (ii) one or more hydrogens may be replaced by a substituent group (e.g., an organic substituent group). In one embodiment, X is -(CH 2 ) 4 –.

[0147] In certain embodiments, R attached to Formula (V) or (VI) 5 Part or R 6 Some of the hydroxyl groups are secondary hydroxyl groups or are located relative to the nitrogen atom, more preferably the β position of the nitrogen atom of the amide bond. Thus, for example, in certain embodiments, the nitrogen-containing carboxyl reactive crosslinking agent is a β-hydroxyalkylamide compound. Some examples of such compounds include: bis[N,N-bis(β-hydroxy-ethyl)]adipamide, bis[N,N-bis(β-hydroxy-propyl)]succinamide, bis[N,N-bis(β-hydroxy-ethyl)]azelamide, bis[N,N-bis(β-hydroxy-propyl)]adipamide, bis[N-methyl-N-(β-hydroxy-ethyl)]oxalamide and mixtures thereof. The PRIMID QM-1260 product commercially available from EMS is an example of a preferred β-hydroxyalkylamide crosslinking agent. It is believed that the structure corresponding to the PRIMID QM-1260 product is provided by the following formula (VII):

[0148]

[0149] Without wishing to be bound by theory, in some embodiments, hydroxyalkylamides, particularly β-hydroxyalkylamides, such as those of formula (V), (VI) or (VII) are preferably used, because oxazolinium intermediates are formed, which are believed to occur and result in enhanced reactivity of the crosslinking agent with the carboxyl group (e.g., on acrylic copolymers). Therefore, in some embodiments, nitrogen-containing carboxyl reactive crosslinking agents are preferably capable of forming oxazolinium intermediates or other carbon-nitrogen heterocyclic intermediates with enhanced reactivity with the carboxyl group. Preferably, such reactive intermediates are formed under short curing times of typical beverage can end cap coating heat curing conditions. For example, for coating curing conditions, in some embodiments, such reactive intermediates can be formed even under oven baking conditions with a peak metal temperature from 200°C to 260°C (in some embodiments, 230°C to 260°C) and during a relatively short oven residence time of only 8 seconds to 20 seconds, 8 seconds to 15 seconds, 8 seconds to 12 seconds, or even 10 seconds to 12 seconds.

[0150] In a preferred embodiment, the nitrogen-containing carboxyl-reactive crosslinking agent is formed from reactants that do not include formaldehyde. The preferred carboxyl-reactive crosslinking agent is also substantially free of, completely free of, and preferably free of any structural units derived from BPA and aromatic glycidyl ether compounds (e.g., BADGE, BFDGE, and epoxy novolac).

[0151] In yet other embodiments, the crosslinking agent may include a carbodiimide polymer or a carbodiimide moiety. Exemplary such carbodiimide crosslinking agents or portions thereof may include, but are not limited to, aliphatic and / or alicyclic dinitrogen derivatives of carbonic acid. Such crosslinking agents have a general structure: R'N=C=NR', wherein R' is independently an aliphatic or alicyclic group. The aliphatic group of R' may be a carbon chain of 1 to 6 carbon atoms. Suitable examples of carbodiimide moieties or crosslinking agents include dibutylcarbodiimide and dicyclohexylcarbodiimide. Polymeric or oligomeric carbodiimide crosslinking agents may also be used. Water-dispersible carbodiimide crosslinkers may be prepared by incorporating a small amount of amines (such as dimethylaminopropylamine) and alkyl sulfonates or sulfates into the carbodiimide structure. Suitable water-dispersible carbodiimides may also be prepared by incorporating polyethylene oxide or polypropylene oxide into the carbodiimide structure. Exemplary carbodiimide cross-linkers are disclosed in International Publication No. WO 2019 / 118697 (PPG Industries, Ohio, Inc.).

[0152] In other embodiments, the carboxyl reactive crosslinking agent comprises an oxazoline crosslinking agent, particularly a polyoxazoline crosslinking agent. As used herein, the term "polyoxazoline" means a compound containing at least two (2) oxazoline groups. The compound may be monomeric or polymeric. Suitable monomeric polyoxazolines include bisoxazoline and / or trioxazoline. Exemplary oxazoline crosslinking agents are disclosed in International Publication Nos. WO 2014 / 139972 (Akzo Nobel Coatings International BV) and WO 2019 / 116328 (PPG Industries, Ohio, Inc.).

[0153] In some embodiments, the coating composition as disclosed herein may optionally include one or more catalysts at a suitable level to produce the desired result (e.g., to increase the curing rate and / or the degree of crosslinking). Non-limiting examples of catalysts include, but are not limited to, strong acids (e.g., dodecylbenzenesulfonic acid (DDBSA, which can be obtained from Cytec under the trade name CYCAT600), methanesulfonic acid (MSA), p-toluenesulfonic acid (pTSA), dinonylnaphthalene disulfonic acid (DNNDSA), and trifluoromethanesulfonic acid), quaternary ammonium compounds, phosphorus compounds, titanium compounds (e.g., titanium acetylacetonate, tetraalkyl titanate, isopropyl orthotitanate, water-soluble titanium chelate, triethanolamine chelate of titanium, tetrakis(triethanolamine) chelate of titanium, lactic acid titanate chelate), zinc compounds, and combinations thereof. Specific examples include, but are not limited to, tetraalkylammonium halides, tetraalkyl or tetraaryl phosphonium iodides or phosphonium acetates, zinc octoate, triphenylphosphine, and similar catalysts known to those skilled in the art. If used, the catalyst is preferably present in an amount of at least 0.01 wt % or at least 0.1 wt % based on the weight of non-volatile materials in the coating composition. If used, the catalyst is preferably present in an amount of no greater than 3 wt % or no greater than 1 wt % based on the weight of non-volatile materials in the coating composition. In a preferred embodiment, any such curing catalyst used does not include tin.

[0154] Optional Ingredients

[0155] The beverage can end cover coil coating composition of the present disclosure (whether it is an aqueous coating composition or a powder coating composition) comprises at least 80% by weight of an acid or anhydride functional acrylic latex, which comprises an emulsion polymerized polymer, based on the weight of total resin solids. The beverage can end cover coil coating composition of the present disclosure may also include other optional (secondary) polymers, which do not adversely affect the coating composition or the cured coating composition produced therefrom. Such secondary polymers are usually included in the coating composition as filler materials, although they can be included as cross-linked materials, or provide desired properties. One or more optional polymers (secondary polymers) can be included in an amount sufficient for the intended purpose, but not in an amount that adversely affects the coating composition or the cured coating composition produced therefrom. Examples of such other optional polymers may include polyolefins, polyesters, polyurethanes, polyethers (i.e., epoxy polymers) and their copolymers.

[0156] Although the coating composition may optionally include one or more polyester polymers, in preferred embodiments, the coating composition includes no more than 20 weight percent, no more than 10 weight percent, no more than 5 weight percent, or no more than 1 weight percent of a polyester polymer, if any, based on total resin solids.

[0157] Similarly, while the coating composition may optionally include one or more polyolefin polymers, in preferred embodiments, the coating composition includes no more than 20 weight percent, no more than 10 weight percent, no more than 5 weight percent, or no more than 1 weight percent polyolefin polymer, if any, based on total resin solids.

[0158] Similarly, while the coating composition may optionally include one or more polyurethane polymers, in preferred embodiments, the coating composition includes no more than 20 weight percent, no more than 10 weight percent, no more than 5 weight percent, or no more than 1 weight percent polyurethane polymer, if any, based on total resin solids.

[0159] Although the coating composition may optionally include one or more polyether polymers, in preferred embodiments, the coating composition includes no more than 20 weight percent, no more than 10 weight percent, no more than 5 weight percent, or no more than 1 weight percent of a polyether polymer, if any, based on total resin solids.

[0160] In preferred embodiments, the coating compositions of the present disclosure are "epoxide-free" and are not prepared using any polymers or other materials having epoxy backbone segments.

[0161] When using, optional composition is usually included in the coating composition to enhance the composition aesthetics, promote the manufacture, processing, handling and application of the composition, and / or further improve the coating composition or the specific functional properties of the cured coating composition produced therefrom. Suitable optional composition can include for example pigment, extender, filler, lubricant, corrosion inhibitor, flow control agent, thixotropic agent, dispersant, antioxidant, tackifier, light stabilizer, surfactant and their mixture. Every kind of optional composition is preferably with the amount that is enough to be used for its intended purpose, but is not included with the such amount of the coating composition that adversely affects coating composition or the cured coating composition produced therefrom.

[0162] Particularly useful optional ingredients may be lubricants (e.g., waxes) that facilitate the manufacture of easy-open end caps by imparting lubricity and flexibility to the coated metal substrate sheet or coil. Examples of lubricants include, for example, carnauba wax, Fischer-Tropsch wax, fatty acid ester wax, silicone wax, lanolin wax, hydroxyl-functional polysiloxane wax (such as, for example, described in U.S. Pat. No. 9,169,406 (Wilbur et al.), polytetrafluoroethylene (PTFE) wax, polyolefin wax (e.g., polyethylene (PE) wax, polypropylene (PP) wax, and high-density polyethylene (HDPE) wax), amide wax (e.g., micronized ethylene bis stearamide (EBS) wax), combinations thereof, and modified forms thereof (e.g., amide-modified PE wax, PTFE-modified PE wax, etc.). The lubricant may be a micronized wax that may optionally be spherical.

[0163] Examples of suitable commercially available lubricants include the CERETAN series of products from Munzing (e.g., CERETAN MA 7020, MF 5010, MM 8015, MT 9120 and MXD 3920 products); the LUBA-PRINT series of products from Munzing (e.g., LUBA-PRINT 255 / B, 276 / A (ND), 351 / G, 501 / S-100, 749 / PM and CA30 products); the SST-52, S-483, FLUOROSLIP 893-A, TEXTURE 5347W and SPP-10 products from Shamrock; the CERAFLOUR series of products from BYK (e.g., CERAFLOUR 981, 988, 996, 258 and 970 products); and the CERACOL 607 product from BYK.

[0164] In some embodiments, PTFE-free lubricants (i.e., those that do not contain polytetrafluoroethylene) are preferred. In some embodiments, the coating composition does not contain any lubricant prepared using fluorine-containing ingredients. In some embodiments, the coating composition does not contain any fluorine-containing ingredients.

[0165] If used, one or more lubricants can be present in the coating composition in an amount of at least 0.1 wt%, at least 0.25 wt%, at least 0.5 wt%, or at least 0.75 wt%, based on the total weight of the coating composition. In other embodiments, the lubricant can be present in the coating composition in an amount of no greater than 3 wt%, no greater than 2 wt%, no greater than 1.5 wt%, no greater than 1.25 wt%, or no greater than 1 wt%, based on the total weight of solids in the coating composition.

[0166] The lubricant may be present in (i.e., incorporated into) the coating composition of the present disclosure. The lubricant may also be applied to the coating composition after the coating composition is applied to the substrate. That is, the lubricant may be present in a second coating composition that is applied as a separate layer over the layer of the coating composition of the present disclosure.

[0167] Another useful optional ingredient is a pigment, such as titanium dioxide. If used, one or more pigments may be present in the coating composition in an amount of no greater than 25 wt % and typically in an amount of 15 wt % to 25 wt %, based on the total weight of the coating composition.

[0168] Surfactants can be optionally added to the coating composition to assist in the flow and wetting of the substrate. Examples of surfactants include, but are not limited to, nonylphenol polyethers and salts and similar surfactants known to those skilled in the art. If used, one or more surfactants can be present in an amount of at least 0.01 % by weight and at least 0.1 % by weight based on the total weight of resin solids. If used, one or more surfactants can be present in an amount of no more than 10 % by weight and no more than 5 % by weight in certain embodiments based on the total weight of resin solids. In some embodiments, the coating composition does not include any surfactant.

[0169] Carrier fluid

[0170] The aqueous coating composition herein may include any suitable amount of water, optionally (and preferably) in combination with one or more organic solvents. In some embodiments, the amount of the liquid carrier is selected so that the total non-volatile solid content of the coating composition is based on the total weight of the composition, preferably in the range of from 10 wt % to 50 wt %, more preferably 20 wt % to 40 wt %. For example, and more preferably, the composition may have a total non-volatile solid content of 30 wt % to 40 wt % based on the total weight of the composition.

[0171] The carrier fluid (eg, aqueous carrier) may make up the remainder of the weight of the coating composition.In certain embodiments, the coating compositions of the present disclosure have a viscosity at 25°C measured via ASTM D-1200 of 30 to 80 seconds or 35 to 60 seconds using a Ford #2 cup.

[0172] In preferred embodiments, the carrier fluid is water.In certain embodiments, the coating composition comprises at least 10 wt%, at least 20 wt%, at least 25 wt%, at least 35 wt%, or at least 50 wt% water, based on the total weight of the coating composition.

[0173] In other embodiments, the carrier fluid may include one or more organic solvents, preferably one or more water-miscible organic solvents. In some embodiments, the organic solvent may include one or more of the following: isopropanol, ethanol, methanol, butanol, amyl alcohol, glycol, glycol ether (i.e., butanediol), glycol ester, glycol ether ester, mineral spirits, aromatic solvents, acetone, ketones (such as methyl ethyl ketone) or tetrahydrofuran or mixtures thereof.

[0174] In some embodiments, the coating composition is an aqueous coating composition comprising at least 5% by weight of one or more organic solvents. In a preferred embodiment, the coating composition comprises at least some organic solvents, more preferably at least 5%, at least 10%, or at least 15% by weight of one or more organic solvents, based on the total coating weight. Typically, at least some, if not all, of the one or more organic solvents are water miscible.

[0175] Coil coating compositions and their properties

[0176] The coil coating compositions of the present disclosure are typically water-based, i.e., contain water as part or all of the carrier fluid. However, if desired, the coil coating composition can be spray dried and in the form of powder particles. Examples of such powder coating compositions and methods for packaging are described in International Publication Nos. WO 2021 / 097308 and WO 2022 / 246120, both of which are granted to SWIMC LLC.

[0177] In some embodiments, the coil coating composition has a glass transition temperature (Tg) of from 10°C to 50°C, preferably from 15°C to 45°C and more preferably from 20°C to 40°C when cured in a beverage can end coil baking. Differential scanning calorimetry (DSC) is an example of a useful method for determining the Tg of a coil coating composition, and a representative DSC method is employed. Although not wishing to be bound by theory, it is believed that if the Tg of the cured coating is too low, one or more properties (such as, for example, flavor stripping or corrosion resistance) may be unsuitable. Similarly, if the Tg is too high, one or more properties (such as flexibility (e.g., as indicated by porosity values ​​before and / or after pasteurization or retorting)) may be unsuitable.

[0178] Although the coating compositions of the present disclosure do not require the use of any formaldehyde-derived crosslinking agents to exhibit good beverage can end performance, a certain amount of such crosslinking agents may be employed if desired. In some embodiments, the coil coating composition comprises less than 2 wt % or less than 1 wt % of a formaldehyde-derived crosslinking agent, if any, based on the weight of the total solids. In some embodiments, the coil coating composition is substantially free, completely free, or free of a formaldehyde-derived crosslinking agent. In some embodiments, the coil coating composition herein is formaldehyde-free.

[0179] In a preferred embodiment, no formaldehyde-containing compounds or formaldehyde-derived compounds are used to prepare the coating composition, although trace amounts may be present due to, for example, environmental contamination. Because phenolic plastic crosslinker resins are typically prepared from reactants that include formaldehyde, in a preferred embodiment, the coating composition does not include any phenolic plastic crosslinkers. Similarly, in a preferred embodiment, the coating composition also does not include any benzoguanamine formaldehyde, melamine formaldehyde, or urea formaldehyde crosslinkers. In a presently preferred embodiment, the coating composition also does not include any isocyanate crosslinkers.

[0180] In some embodiments, the coil coating composition is free of bisphenol A, bisphenol F, and bisphenol S. In some embodiments, the coil coating composition does not include any intentionally added bisphenol components (such as bisphenol A, bisphenol S, or bisphenol F).

[0181] In certain embodiments, the aqueous coating compositions herein are substantially free of all bisphenol compounds. In certain embodiments, the aqueous coating compositions are completely free of all bisphenol compounds. For example, hydroquinone, resorcinol, catechol, etc. are not bisphenols because these phenol compounds include only one phenylene ring.

[0182] The amount of bisphenol compounds (e.g., bisphenol A, bisphenol F, and bisphenol S) and structural units derived therefrom can be determined based on the starting ingredients; the test method is not necessary, and considering the small amounts of these compounds, parts per million (ppm) can be used instead of weight percentages for convenience. In certain preferred embodiments, bisphenol compounds are not used (i.e., they are not intentionally added), although trace amounts may be present due to, for example, environmental contamination.

[0183] In some such embodiments, the coil coating composition is epoxide-free.

[0184] "Epoxide-free" coating compositions are prepared without the use of any polymers or other materials having epoxy backbone segments.

[0185] In some embodiments, the acrylic latex, and preferably the entire coil coating composition, is substantially free, completely free, or free of glycidyl acrylate monomers and glycidyl methacrylate monomers, whether free or polymerized.

[0186] In some embodiments, the acrylic latex, and preferably the entire coil coating composition, is substantially free, completely free, or free of (meth)acrylamide-type monomers (e.g., acrylamide or methacrylamide, N-isobutoxymethylacrylamide, N-butoxymethylacrylamide) or structural units derived therefrom.

[0187] In some embodiments, the acrylic latex, and more preferably the entire coil coating composition, is substantially free, completely free, or free of vinyl aromatic monomers, whether free or polymerized.

[0188] In some embodiments, the coil coating composition is styrene-free.

[0189] In some embodiments, the acrylic latex, and more preferably the entire coil coating composition, is substantially free, completely free, or free of halogenated monomers, whether free or polymerized.

[0190] In some embodiments, the coating composition does not contain any fluorine-containing ingredients.

[0191] In a preferred embodiment, the aqueous coating composition herein, when applied to a cleaned and chrome-free pretreated aluminum panel and cured for a 12 second oven cure time to a peak metal temperature of 249°C to achieve a dry film thickness of approximately 11 grams per square meter (i.e., 10 gsm-12 gsm), and formed into a fully converted (typically 206) standard opening beverage can end, passes less than 5 mA of current, preferably less than 2 mA of current, even more preferably less than 1 mA of current, while exposed to an electrolyte solution containing 1 wt. % NaCl dissolved in deionized water for 4 seconds.

[0192] Exemplary coatings of the present invention exhibit one or more of the properties described in the Examples section. In some embodiments, the coatings of the present disclosure, when applied to cleaned and chromium-free, zirconium pretreated aluminum panels and cured for 12 seconds to a peak metal temperature of 249°C to achieve a dry film thickness of about 11 (i.e., 10-12) grams per square meter, and preferably formed into fully converted (typically 206) standard opening beverage can end caps, exhibit one or more of the following properties (and in some embodiments, all or various combinations of such properties):

[0193] MEK solvent resistance of at least 30 double rubs;

[0194] The blush rating after water pasteurization is at least 6;

[0195] Adhesion grade is GT0 or GT1; and

[0196] Feathering, if any, is 0.5 mm or less, 0.4 mm or less, 0.3 mm or less, 0.2 mm or less, or 0.1 mm or less, or there is no feathering.

[0197] Here, MEK solvent resistance, blush and adhesion are tested on flat panels. The values ​​of these parameters will not change if a fully converted (eg, 206) standard opening beverage can end is then formed and then tested.

[0198] Beverage can and method

[0199] As described above, the coating compositions herein are particularly suitable for beverage cans, particularly can end caps, which are subjected to short curing cycles. Two-piece cans are manufactured by joining a can body (usually a drawn metal body) to a can end cap (usually an easy-open can end cap formed of aluminum or steel or sheet material). The coatings of the present invention are suitable for coating coil substrates used to prepare beverage can end caps.

[0200] The coating process is a continuous coating consisting of metal such as steel or aluminum. The metal substrate is in the form of a coil substrate that allows a continuous coating process. Figure 1Depicts a coil substrate W of an embodiment suitable for receiving a liquid (or powder) polymer coating composition. The coil substrate has a selected width and thickness and has sufficient length to allow the substrate to be wound into a coil. The coil substrate allows a continuous coating process. For example, the surface 12 of the coil substrate 10 is usually exposed to receive the coating. The placement of the coating on the surface 12 of the coil substrate 10 can be carried out in a continuous manner, involving an unwinding station 14, a coating station 16 for applying a coating 18, a curing station 20, and a coiling station 22 for rewinding the coated coil 24 at the end cap. As presented in the present disclosure, the modification of the liquid polymer coating composition reduces or alleviates the edge accumulation and edge blister formation on the coated coil.

[0201] Once applied, the coating is subjected to a short heat, UV and / or electromagnetic curing cycle for hardening (e.g., drying and curing) the coating. The coating provides a coated metal (e.g., steel and / or aluminum) substrate that can be processed to form a beverage can end, particularly an easy-open can end, an example of which is shown in Figure 2 middle.

[0202] Metal substrates used in typical coating processes typically have an average thickness of 175 microns to 250 microns. Typically, the surface of the metal substrate is pretreated with a chrome-based or non-chrome-based pretreatment (e.g., zirconium-based and acrylic-based pretreatments) prior to coating with the coating composition.

[0203] In one example of a coating process, coating can be performed by first providing a substrate (such as aluminum or steel) for forming a beverage can end cap. Next, an aqueous coating composition as described herein can be applied to the surface of the substrate (e.g., by roller coating or any other suitable technology). Then, the applied aqueous coating composition is cured at the peak metal temperature for a period of time to form a cured coating on the surface of the substrate. Finally, the applied aluminum or steel substrate is then shaped (e.g., stamped) into a suitable beverage can or can end cap.

[0204] In some embodiments, conventional roller coating process can be used to apply aqueous coating composition on substrate sheet material continuously online or in batches.In some embodiments, in continuous process, the moving surface of substrate advances with a linear speed of at least 50 m / min, at least 100 m / min, at least 200 m / min or at least 300 m / min.Usually, the linear speed will be less than 400 m / min.For such surface moving continuously, aqueous coating composition is applied usually with coating weight and relative thickness, to obtain the average coating thickness of expectation after solidification.In certain embodiments, the average dry film thickness of the gained on substrate can be at least 7 microns, at least 8 microns or at least 9 microns, and can be at most 11 microns, at most 12 microns or at most 15 microns (usually for inner coating) or even thinner for outer coating.Once applied to substrate, any suitable curing mechanism can be adopted.For example, coating composition can be subjected to thermal convection, ultraviolet radiation, electromagnetic magnetic radiation or their combination in curing cycle, and this curing cycle provides the fully drying and curing of coating composition to form the final coating of expectation.

[0205] In some embodiments, the curing time of the coating composition of the present disclosure is at least 6 seconds, at least 10 seconds or at least 12 seconds, and at most 15 seconds, at most 20 seconds, at most 25 seconds or at most 30 seconds. Preferably, the curing time is 8 seconds to 15 seconds, 8 seconds to 12 seconds or 10 seconds to 12 seconds. In the case of thermal baking to cure the coating, such curing time refers to the residence time in the oven. In such embodiments, the curing process is generally carried out to achieve a peak metal temperature (PMT) of 200°C to 260°C and 230°C to 255°C in other methods.

[0206] In any of the above-mentioned application methods, the coating composition herein can be applied to the substrate using any suitable procedure, including, for example, spraying, roller coating, coating, curtain coating, dip coating, meniscus coating, conformal coating, blade coating, knife coating, dip coating, slot coating, slide coating, vacuum coating, etc., as well as other types of predetermined amount coating. Other commercial coating application and curing methods are also contemplated, including, for example, electrocoating, extrusion coating, lamination, powder coating (e.g., after spray drying to form a powder), etc.

[0207] Depending on the particular application and article, the coating compositions herein can be applied to a substrate before or after the substrate is formed into an article. In some embodiments, at least a portion of a planar metal substrate (e.g., a metal coil) is coated with a layer of the coating composition of the present invention and then cured before the planar substrate is formed (e.g., stamped) into a can end (e.g., an easy-open can end).

[0208] After the coating composition is applied to the substrate, various methods can be used to cure the composition, including, for example, oven baking conventional methods, or any other method that provides a high temperature suitable for curing the coating. The curing process can be carried out in discrete or combined steps. For example, the substrate can be dried at ambient temperature so that the coating composition remains in a mostly uncrosslinked state. The coated substrate can then be heated to fully cure the composition. In some cases, the coating composition of the present invention can be dried and cured in one step.

[0209] Embodiments of liquid polymer coating compositions (or alternatively, powder coating compositions) related to beverage can end caps should preferably exhibit sufficient flexibility in the cured coating composition to accommodate the extreme profile of the rivet portion of the easy-open can end cap. In some embodiments, the tests conducted to determine whether a particular coating can be used as an easy-open can end cap can be the porosity test and feathering test set forth herein. The porosity test indicates the level of flexibility of the coating, and measures the ability of the coating to maintain its integrity and substrate adhesion when undergoing the forming process required to produce the beverage can end cap. In particular, it is a measure of the presence or absence of cracks or fractures in the inner coating of the formed end cap. Feathering refers to the adhesion loss of the coating adjacent to the drinking port of the beverage can end cap, and when present, indicates that a portion of the free film can remain on the opening of the can when opened.

[0210] The present disclosure also provides methods including making an aqueous coating composition for use on a metal substrate of a metal package (e.g., a metal coil or sheet for forming a beverage can end cap). In some cases involving multiple parties, a first party (e.g., a party that manufactures and / or supplies an aqueous coating composition) may provide a second party (e.g., a metal coater (e.g., a coil coater for an easy-to-open beverage can end cap), a can manufacturer, or a brand owner) with instructions, suggestions, or other disclosures about the final use of the packaging coating. Such disclosures may include, for example, instructions for coating a metal substrate for subsequent use in forming a packaging can or portion thereof, coating a metal substrate of a preformed can or portion thereof, preparing an aqueous coating composition for such use, curing conditions or process-related conditions for such coatings, or instructions, suggestions, or other disclosures for a suitable type of packaging product for the resulting coating. Such disclosures may appear, for example, in a technical data sheet (TDS), a safety data sheet (SDS), a regulatory disclosure, a warranty or warranty limitation statement, marketing materials, or a presentation, or appear on a company website. A first party who makes such a disclosure to a second party shall be deemed to have caused the aqueous coating composition to be used on a metal substrate for metal packaging (e.g., a can or an easy open end cap) even if the second party actually applies the composition to a commercial metal substrate, uses such coated substrate in commerce on a metal substrate for packaging cans, and / or fills such coated cans with product.

[0211] Implementation

[0212] Embodiment 1 is a beverage can end cap coil coating composition, the beverage can end cap coil coating composition comprising: an acid or anhydride functional acrylic latex, the acid or anhydride functional acrylic latex comprising an emulsion polymerized polymer; a carboxyl reactive crosslinking agent, the carboxyl reactive crosslinking agent is nitrogen-containing and not derived from formaldehyde; and an optional lubricant; wherein the coating composition:

[0213] (i) contains less than 2% by weight, based on the weight of total solids, of a crosslinking agent derived from formaldehyde,

[0214] If any;

[0215] (ii) does not contain bisphenol A, bisphenol F and bisphenol S;

[0216] (iii) optionally free of styrene;

[0217] (iv) has a glass transition temperature (Tg) of 10°C to 50°C when applied to a cleaned and chromium-free, zirconium pretreated aluminum panel and cured for 12 seconds to a peak metal temperature of 249°C to achieve a dry film thickness of about 11 (i.e., 10-12) grams per square meter, as determined by differential scanning calorimetry (DSC); and

[0218] (v) when applied to a cleaned and chromium-free, zirconium pretreated aluminum panel and cured for 12 seconds to a peak metal temperature of 249°C to achieve a dry film thickness of approximately 11 (i.e., 10-12) grams per square meter, and formed into a fully converted (typically 206) standard opening beverage can end, with less than 5 mA of current passed while exposed to an electrolyte solution containing 1 wt. % NaCl dissolved in deionized water for 4 seconds.

[0219] Embodiment 2 is a coating composition according to embodiment 1, wherein the acrylic latex has an acid value of at least 40, at least 100, or at least 150 mg KOH / gram of latex. Embodiment 3 is a coating composition according to embodiment 1 or 2, wherein the acrylic latex has an acid value of less than 400, less than 300, less than 200, less than 150, or less than 100 mg KOH / gram of latex. Embodiment 4 is a coating composition according to embodiment 2 or 3, wherein the acrylic latex has an acid value of 100 mg KOH / g latex to 200 mg KOH / g latex.

[0220] Embodiment 5 is a coating composition according to any of the preceding embodiments, wherein the acrylic latex comprises at least 50 wt%, at least 60 wt%, at least 70 wt%, at least 80 wt%, at least 90 wt%, at least 95 wt%, or at least 98 wt% of an emulsion polymerized polymer, based on the total solid weight of the acrylic latex.

[0221] Embodiment 6 is a coating composition according to any of the preceding embodiments, wherein the acrylic latex is formed from the polymerization of an ethylenically unsaturated monomer component comprising two or more different monomers, more typically three or more different monomers.

[0222] Embodiment 7 is a coating composition according to embodiment 6, wherein the ethylenically unsaturated monomer component comprises a (meth)acrylate monomer, preferably having a Tg of greater than 50°C, greater than 60°C, greater than 70°C, greater than 80°C, greater than 90°C, or greater than 100°C. Embodiment 8 is a coating composition according to embodiment 6 or 7, wherein the ethylenically unsaturated monomer component comprises at least one ethylenically unsaturated acid or anhydride functional monomer, including salts thereof, preferably in an amount of at least 5 wt% or at least 10 wt%, based on the total weight of the ethylenically unsaturated monomer component. Embodiment 9 is a coating composition according to any one of embodiments 6 to 8, wherein the ethylenically unsaturated monomer component comprises at least one ethylenically unsaturated acid or anhydride functional monomer, including salts thereof, preferably in an amount of no more than 20 wt% or no more than 15 wt%, based on the total weight of the ethylenically unsaturated monomer component.

[0223] Embodiment 10 is a coating composition according to any one of embodiments 6 to 9, wherein the ethylenically unsaturated acid or anhydride functional monomer, including its salt, comprises an acid selected from the group consisting of acrylic acid, methacrylic acid, α-chloroacrylic acid, α-cyanoacrylic acid, crotonic acid, α-phenylacrylic acid, β-acryloxypropionic acid, fumaric acid, maleic acid, sorbic acid, α-chlorosorbic acid, angelic acid, cinnamic acid, p-chlorocinnamic acid, β-stearoylacrylic acid, citraconic acid, mesaconic acid, glutaconic acid, aconitic acid, tricarboxyethylene, 2-methylmaleic acid, itaconic acid, 2-methylitaconic acid, methyleneglutaric acid, their salts, and mixtures thereof. Embodiment 11 is a coating composition according to embodiment 10, wherein the ethylenically unsaturated acid or anhydride functional monomer, including its salt, comprises an acid selected from the group consisting of acrylic acid, methacrylic acid, crotonic acid, fumaric acid, maleic acid, 2-methylmaleic acid, itaconic acid, 2-methylitaconic acid, their salts, and mixtures thereof. Embodiment 12 is a coating composition according to embodiment 11, wherein the ethylenically unsaturated acid or anhydride functional monomer, including salts thereof, comprises an acid selected from the group consisting of acrylic acid, methacrylic acid, salts thereof, and mixtures thereof.

[0224] Embodiment 13 is a coating composition according to any one of embodiments 6 to 12, wherein the ethylenically unsaturated monomer component comprises at least one (meth)acrylate monomer in an amount of preferably at least 70 wt%, at least 80 wt%, or at least 85 wt%, based on the total weight of the ethylenically unsaturated monomer component. Embodiment 14 is a coating composition according to any one of embodiments 6 to 13, wherein the ethylenically unsaturated monomer component comprises at least one (meth)acrylate monomer in an amount of preferably no more than 95 wt%, or no more than 90 wt%, based on the total weight of the ethylenically unsaturated monomer component.

[0225] Embodiment 15 is a coating composition according to any one of embodiments 6 to 14, wherein the ethylenically unsaturated monomer component comprises at least one (meth)acrylate monomer having structural formula (I):

[0226] CH 2 =C(R 1 )-CO-OR 2 (I)

[0227] Where R 1 is hydrogen or methyl, and R 2is an alkyl group (preferably containing 1 to 22 carbon atoms, more preferably 1 to 16 or 1 to 12 or 1 to 10 carbon atoms), an alicyclic group (preferably containing 4 to 12 carbon atoms or 6 to 10 carbon atoms), an aryl group (preferably containing 4 to 15 carbon atoms or 6 to 10 carbon atoms), or a combination thereof. Embodiment 16 is a coating composition according to embodiment 15, wherein the (meth)acrylate monomer of (Formula I) is selected from methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, tridecyl (meth)acrylate, lauryl (meth)acrylate (also known as dodecyl (meth)acrylate), cyclohexyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, isobornyl (meth)acrylate, norbornene (meth)acrylate, tricyclodecenyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and the like, substituted variants thereof (e.g., ring-substituted variants of benzyl (meth)acrylate or phenyl (meth)acrylate), and isomers and mixtures thereof.

[0228] Embodiment 17 is a coating composition according to embodiment 15 or 16, wherein the ethylenically unsaturated monomer component comprises at least one linear (meth) alkyl ester monomer of formula (I) having a linear alkyl group. Embodiment 18 is a coating composition according to embodiment 17, wherein the ethylenically unsaturated monomer component comprises at least one linear (meth) alkyl ester monomer of formula (I) having a linear (C1-C4) alkyl group. Embodiment 19 is a coating composition according to embodiment 18, wherein the linear (meth) alkyl ester monomer is selected from methyl (meth) acrylate, ethyl (meth) acrylate, n-propyl (meth) acrylate, n-butyl (meth) acrylate, and mixtures thereof.

[0229] Embodiment 20 is a coating composition according to embodiment 19, wherein the linear alkyl (meth)acrylate monomer is selected from ethyl (meth)acrylate.

[0230] Embodiment 21 is a coating composition according to any one of embodiments 17 to 20, wherein the ethylenically unsaturated monomer component comprises one or more linear alkyl (meth)acrylate monomers in an amount of at least 20 weight percent, at least 30 weight percent, or at least 40 weight percent, based on the total weight of the ethylenically unsaturated monomer component. Embodiment 22 is a coating composition according to any one of embodiments 17 to 21, wherein the ethylenically unsaturated monomer component comprises one or more linear alkyl (meth)acrylate monomers in an amount of no more than 80 weight percent, no more than 70 weight percent, no more than 60 weight percent, or no more than 50 weight percent, based on the total weight of the ethylenically unsaturated monomer component.

[0231] Embodiment 23 is a coating composition according to any one of embodiments 15 to 22, wherein the ethylenically unsaturated monomer component comprises at least one cyclic and / or branched (meth)acrylate monomer of formula (I) having cyclic and / or branched groups. Embodiment 24 is a coating composition according to embodiment 23, wherein the cyclic and / or branched (meth)acrylate monomer is selected from isopropyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, isopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, tridecyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, norbornene (meth)acrylate, tricyclodecenyl (meth)acrylate, and mixtures thereof. Embodiment 25 is a coating composition according to embodiment 24, wherein the cyclic and / or branched (meth)acrylate monomer is selected from cyclohexyl (meth)acrylate.

[0232] Embodiment 26 is a coating composition according to any one of embodiments 23 to 25, wherein the ethylenically unsaturated monomer component comprises one or more cyclic and / or branched alkyl (meth)acrylate monomers in an amount of at least 10 weight percent, at least 15 weight percent, or at least 20 weight percent, based on the total weight of the ethylenically unsaturated monomer component. Embodiment 27 is a coating composition according to any one of embodiments 23 to 26, wherein the ethylenically unsaturated monomer component comprises one or more cyclic and / or branched alkyl (meth)acrylate monomers in an amount of no more than 50 weight percent, no more than 45 weight percent, no more than 40 weight percent, no more than 35 weight percent, or no more than 30 weight percent, based on the total weight of the ethylenically unsaturated monomer component.

[0233] Embodiment 28 is a coating composition according to any one of embodiments 6 to 27, wherein the acrylic latex is formed by polymerization of an ethylenically unsaturated monomer component comprising at least one multi-ethylenically unsaturated (meth)acrylate monomer. Embodiment 29 is a coating composition according to embodiment 28, wherein the ethylenically unsaturated monomer component comprises one or more multi-ethylenically unsaturated (meth)acrylate monomers in an amount of at least 5 weight percent or at least 10 weight percent based on the total weight of the ethylenically unsaturated monomer component. Embodiment 30 is a coating composition according to embodiment 28 or 29, wherein the ethylenically unsaturated monomer component comprises one or more multi-ethylenically unsaturated (meth)acrylate monomers in an amount of no more than 25 weight percent, no more than 20 weight percent, no more than 15 weight percent, no more than 10 weight percent, no more than 5 weight percent, or no more than 1 weight percent based on the total weight of the ethylenically unsaturated monomer component.

[0234] Embodiment 31 is a coating composition according to any one of embodiments 6 to 27, wherein the ethylenically unsaturated monomer component does not contain any multi-ethylenically unsaturated (meth)acrylate monomers. Embodiment 32 is a coating composition according to embodiment 31, wherein the ethylenically unsaturated monomer component does not contain any multi-functional cross-linking monomers.

[0235] Embodiment 33 is a coating composition according to any one of embodiments 6 to 32, wherein the acrylic latex is formed by polymerization of an ethylenically unsaturated monomer component further comprising at least one ethylene oxide functional monomer. Embodiment 34 is a coating composition according to embodiment 33, wherein the ethylene oxide functional monomer is not glycidyl acrylate or glycidyl methacrylate. Embodiment 35 is a coating composition according to embodiment 33 or 34, wherein the ethylenically unsaturated monomer component comprises one or more ethylene oxide functional monomers in an amount of no more than 30 weight percent, no more than 20 weight percent, no more than 10 weight percent, or no more than 9 weight percent, based on the total weight of the ethylenically unsaturated monomer component. Embodiment 36 is a coating composition according to any one of embodiments 33 to 35, wherein the ethylenically unsaturated monomer component comprises one or more ethylene oxide functional monomers in an amount of at least 1 weight percent, at least 2 weight percent, at least 3 weight percent, or at least 5 weight percent, based on the total weight of the ethylenically unsaturated monomer component.

[0236] Embodiment 37 is a coating composition according to any one of embodiments 6 to 32, wherein the ethylenically unsaturated monomer component does not contain any monomers having ethylene oxide groups. Embodiment 38 is a coating composition according to any of the preceding embodiments, wherein the acrylic latex and preferably the entire coating composition is substantially free of, completely free of, or free of glycidyl acrylate monomers and glycidyl methacrylate monomers (whether free or polymerized). Embodiment 39 is a coating composition according to any of the preceding embodiments, wherein the acrylic latex and preferably the entire coating composition is substantially free of, completely free of, or free of any (meth)acrylamide-type monomers (e.g., acrylamide or methacrylamide, N-isobutoxymethylacrylamide, N-butoxymethylacrylamide) or structural units derived therefrom.

[0237] Embodiment 40 is a coating composition according to any one of embodiments 6 to 39, wherein the ethylenically unsaturated monomer component is free of styrene. Embodiment 41 is a coating composition according to any of the preceding embodiments, wherein the coating composition is free of styrene. Embodiment 42 is a coating composition according to any of the preceding embodiments, wherein the acrylic latex, and preferably the entire coating composition, is substantially free of, completely free of, or free of vinyl aromatic monomers, whether free or polymerized.

[0238] Embodiment 43 is a coating composition according to any one of embodiments 6 to 43, wherein the ethylenically unsaturated monomer component does not contain any halogenated monomers, such as chlorinated vinyl monomers. Embodiment 44 is a coating composition according to any of the preceding embodiments, wherein the acrylic latex, and preferably the entire coating composition, is substantially free of, completely free of, or free of halogenated monomers, whether free or polymerized.

[0239] Embodiment 45 is a coating composition according to any one of embodiments 6 to 44, wherein the ethylenically unsaturated monomer component comprises one or more adhesion promoting monomers. Embodiment 46 is a coating composition according to any one of embodiments 6 to 45, wherein the ethylenically unsaturated monomer component comprises one or more hydroxyl functional monomers.

[0240] Embodiment 47 is a coating composition according to any one of embodiments 6 to 46, wherein the ethylenically unsaturated monomer component comprises: (i) at least one of acrylic acid or methacrylic acid; (ii) at least one of ethyl acrylate or n-butyl acrylate; and (iii) a cyclic monomer. Embodiment 48 is a coating composition according to embodiment 47, wherein the ethylenically unsaturated monomer component comprises acrylic acid, ethyl acrylate, and cyclohexyl methacrylate (CHMA).

[0241] Embodiment 49 is a coating composition according to any of the preceding embodiments, comprising less than 1 weight percent, if any, of a crosslinker derived from formaldehyde, based on the weight of total solids. Embodiment 50 is a coating composition according to embodiment 49, substantially free of, completely free of, or free of a crosslinker derived from formaldehyde. Embodiment 51 is a coating composition according to any of the preceding embodiments, the coating composition being free of formaldehyde.

[0242] Embodiment 52 is a coating composition according to any of the preceding embodiments, the coating composition not comprising any intentionally added bisphenol components such as bisphenol A, bisphenol S, or bisphenol F. Embodiment 53 is a coating composition according to any of the preceding embodiments, the coating composition being free of epoxides.

[0243] Embodiment 54 is a coating composition according to any of the preceding embodiments, wherein the emulsion-polymerized polymer of the acrylic latex has a number average molecular weight (M) greater than 20,000, greater than 30,000, greater than 100,000, greater than 200,000, or greater than 300,000. n Embodiment 55 is a coating composition according to any of the preceding embodiments, wherein the emulsion-polymerized polymer of the acrylic latex has an M of less than 1,000,000, less than 600,000, or less than 400,000. n .

[0244] Embodiment 56 is a coating composition according to any of the preceding embodiments, wherein the acrylic latex has a Tg of at least 0°C, at least 5°C, at least 10°C, at least 15°C, at least 20°C, or at least 25°C as determined by DSC, and a Tg of no higher than 50°C, no higher than 45°C, no higher than 40°C, no higher than 35°C, no higher than 30°C, or no higher than 25°C as determined by DSC.

[0245] Embodiment 57 is a coating composition according to any of the preceding embodiments, wherein the coating composition forms a cured coating having a Tg as determined by DSC from 15° C. to 45° C. Embodiment 58 is a coating composition according to any of the preceding embodiments, wherein the coating composition forms a cured coating having a Tg as determined by DSC from 20° C. to 40° C.

[0246] Embodiment 59 is a coating composition according to any of the preceding embodiments, comprising at least 50%, at least 65%, at least 80%, or at least 90% by weight of the acrylic latex based on the total weight of the coating composition. Embodiment 60 is a coating composition according to any of the preceding embodiments, comprising less than 99% or less than 95% by weight of the acrylic latex based on the total weight of the coating composition.

[0247] Embodiment 61 is a coating composition according to any of the preceding embodiments, wherein the nitrogen-containing carboxyl-reactive crosslinking agent comprises two or more carboxyl-reactive functional groups. Embodiment 62 is a coating composition according to any of the preceding embodiments, wherein the carboxyl-reactive crosslinking agent comprises hydroxyl groups. Embodiment 63 is a coating composition according to embodiment 62, wherein the carboxyl-reactive crosslinking agent comprises two or more, three or more, or four or more hydroxyl groups. Embodiment 64 is a coating composition according to embodiment 63, wherein the carboxyl-reactive crosslinking agent comprises at least four hydroxyl groups.

[0248] Embodiment 65 is a coating composition according to any one of embodiments 62 to 64, wherein the crosslinker has a hydroxyl value of at least 100 mg KOH / g resin, at least 200 mg KOH / g resin, at least 300 mg KOH / g resin, at least 400 mg KOH / g resin, or at least 500 mg KOH / g resin.

[0249] Embodiment 66 is a coating composition according to any of the preceding embodiments, wherein the acrylic latex and the carboxyl-reactive crosslinker are present in the coating composition in an amount to provide an excess of carboxyl (-COOH and neutralized such groups) equivalents in the acrylic latex relative to the hydroxyl (-OH) equivalents in the crosslinker. Embodiment 67 is a coating composition according to embodiment 66, wherein the acrylic latex and the carboxyl-reactive crosslinker are present in the coating composition in a molar equivalent ratio of carboxyl groups in the acrylic latex to hydroxyl groups in the crosslinker of at least 1.5:1 or preferably at least 2:1 (e.g., COOH groups and / or salts thereof to OH groups). Embodiment 68 is a coating composition according to embodiment 66 or 67, wherein the acrylic latex and the carboxyl-reactive crosslinker are present in the coating composition in a molar equivalent ratio of carboxyl groups in the acrylic latex to hydroxyl groups in the crosslinker of at most 6:1 or at most 5:1 (e.g., COOH groups and / or salts thereof to OH groups).

[0250] Embodiment 69 is a coating composition according to any of the preceding embodiments, comprising at least 0.5 wt%, at least 1 wt%, at least 1.5 wt%, at least 2 wt%, at least 2.5 wt%, or at least 3 wt% of the carboxyl-reactive crosslinker, based on the total solid weight of the coating composition. Embodiment 70 is a coating composition according to any of the preceding embodiments, comprising less than 30 wt%, less than 20 wt%, less than 15 wt%, less than 10 wt%, or less than 7 wt% of the crosslinker, based on the total solid weight of the coating composition.

[0251] Embodiment 71 is a coating composition according to any of the preceding embodiments, wherein the carboxyl-reactive crosslinker comprises two or more nitrogen atoms, and in some embodiments comprises a total of two nitrogen atoms. Embodiment 72 is a coating composition according to embodiment 71, wherein the carboxyl-reactive crosslinker comprises at least one amide group, at least one imide group, or a combination thereof. Embodiment 73 is a coating composition according to embodiment 72, wherein the carboxyl-reactive crosslinker comprises a β-hydroxy group relative to the nitrogen atom of the amide bond. Embodiment 74 is a coating composition according to embodiment 73, wherein the carboxyl-reactive crosslinker comprises one or more, and more preferably two or more, groups having a structure of formula (III):

[0252] HO-R 5 -N(R 6 )-C(=O)-(III)

[0253] Each R 5 are independently organic groups, and each R 6 is independently hydrogen or an organic group. Embodiment 75 is a coating composition according to embodiment 74, wherein the carboxyl-reactive crosslinking agent is a compound having a structure of formula (V):

[0254] (HO-R 5 -N(R 6 )-C(=O)) n -X(V)

[0255] Where R 5 and R 6 is as described for formula (III), n is an integer of 2 or greater, and X is a multivalent organic group. Embodiment 76 is a coating composition according to embodiment 74, wherein the carboxyl-reactive crosslinking agent is a compound having a structure of formula (VI):

[0256] HO-R 5 -N(R 6)-C(=O)-XC(=O)-N(R 6 )-(R 5 )-OH(VI)

[0257] Wherein R 5 and R 6 is independently an organic group, X is a divalent organic group, and wherein the hydroxyl groups are independently primary hydroxyl groups or secondary hydroxyl groups. Embodiment 77 is a coating composition according to embodiment 74, wherein the carboxyl-reactive crosslinking agent comprises a compound of formula (VII):

[0258]

[0259] Embodiment 78 is a coating composition according to any one of Embodiments 1 to 70, wherein the carboxyl-reactive crosslinker comprises a carbodiimide crosslinker. Embodiment 79 is a coating composition according to any one of Embodiments 1 to 70, wherein the carboxyl-reactive crosslinker comprises an aziridine crosslinker. Embodiment 80 is a coating composition according to any one of Embodiments 1 to 70, wherein the carboxyl-reactive crosslinker comprises an oxazoline crosslinker.

[0260] Embodiment 81 is a coating composition according to any of the preceding embodiments, comprising a mixture of crosslinkers, wherein the mixture of crosslinkers comprises greater than 50 weight percent, greater than 66 weight percent, or greater than 80 weight percent of the nitrogen-containing carboxyl-reactive crosslinker, based on the total weight of the crosslinkers.

[0261] Embodiment 82 is a coating composition according to any of the preceding embodiments, wherein the coating composition further comprises a lubricant, wherein the lubricant is incorporated into the coating composition, or the lubricant is applied to the coating composition after the coating composition is applied to a substrate. Embodiment 83 is a coating composition according to embodiment 82, wherein the lubricant is selected from carnauba wax, Fischer-Tropsch wax, fatty acid ester wax, silicone wax, lanolin wax, hydroxyl-functional polysiloxane wax, polytetrafluoroethylene (PTFE) wax, polyolefin wax (e.g., polyethylene (PE) wax, polypropylene (PP) wax, and high-density polyethylene (HDPE) wax), amide wax (e.g., micronized ethylene-bisstearamide (EBS) wax), combinations thereof, and modified forms thereof (e.g., amide-modified PE wax, PTFE-modified PE wax, etc.). Embodiment 84 is a coating composition according to embodiment 82 or 83, wherein the lubricant is a PTFE-free lubricant (i.e., a polytetrafluoroethylene-free lubricant). Embodiment 85 is a coating composition according to embodiment 84, wherein the coating composition does not contain any lubricant prepared using a fluorine-containing component. Embodiment 86 is a coating composition according to any one of embodiments 82 to 85, wherein one or more lubricants are present in the coating composition in an amount of at least 0.1 wt%, at least 0.25 wt%, at least 0.5 wt%, or at least 0.75 wt%, based on the total weight of solids in the coating composition. Embodiment 87 is a coating composition according to any one of embodiments 82 to 86, wherein one or more lubricants are present in the coating composition in an amount of no greater than 3 wt%, no greater than 2 wt%, no greater than 1.5 wt%, no greater than 1.25 wt%, or no greater than 1 wt%, based on the total weight of solids in the coating composition.

[0262] Embodiment 88 is a coating composition according to any of the preceding embodiments, the coating composition comprising one or more ingredients selected from the group consisting of pigments, extenders, fillers, corrosion inhibitors, flow control agents, thixotropic agents, dispersants, antioxidants, adhesion promoters, light stabilizers, surfactants, and mixtures thereof. Embodiment 89 is a coating composition according to any of the preceding embodiments 88 (except embodiment 53), the coating composition further comprising one or more secondary polymers selected from the group consisting of polyolefins, polyesters, polyurethanes, polyethers, and copolymers thereof. Embodiment 90 is a coating composition according to embodiment 89, wherein the one or more secondary polymers (if present) are present (if present) in an amount of no more than 20 weight percent, no more than 10 weight percent, no more than 5 weight percent, or no more than 1 weight percent based on total resin solids.

[0263] Embodiment 91 is a coating composition according to any of the preceding embodiments, comprising 10 wt % to 50 wt %, preferably 20 wt % to 40 wt %, and more preferably 30 wt % to 40 wt % total non-volatile solids, based on the total weight of the coating composition.

[0264] Embodiment 92 is a coating composition according to any preceding embodiment, the coating composition having a viscosity at 25° C. measured via ASTM D-1200 of 30 to 80 seconds or 35 to 60 seconds using a Ford #2 cup.

[0265] Embodiment 93 is a coating composition according to any of the preceding embodiments, further comprising a carrier fluid. Embodiment 94 is a coating composition according to any of the preceding embodiments, comprising at least 10 wt%, at least 20 wt%, at least 25 wt%, at least 35 wt%, or at least 50 wt% water, based on the total weight of the coating composition. Embodiment 95 is a coating composition according to Embodiment 93 or 94, wherein the carrier fluid comprises one or more organic solvents, preferably one or more water-miscible organic solvents. Embodiment 96 is a coating composition according to Embodiment 95, wherein the organic solvent comprises isopropanol, ethanol, methanol, butanol, pentanol, glycol, glycol ether, glycol ester, acetone, methyl ethyl ketone, or tetrahydrofuran, or a mixture thereof.

[0266] Embodiment 97 is a beverage can end cover coil coating composition according to any of the preceding embodiments, wherein the coating composition is an aqueous coating composition comprising at least 5 weight percent of one or more organic solvents. Embodiment 98 is a coating composition according to Embodiment 97, wherein the coating composition comprises at least 5 weight percent, at least 10 weight percent, or at least 15 weight percent of one or more organic solvents based on the total weight of the coating composition.

[0267] Embodiment 99 is a coating composition according to any of the preceding embodiments, wherein the coating composition: comprises a lubricant; comprises at least 50 weight percent of the acrylic latex, based on the total solid weight of the coating composition; comprises at least 5 weight percent of one or more organic solvents, based on the total weight of the coating composition; and has a total non-volatile solids content of 30 weight percent to 40 weight percent, based on the total weight of the composition.

[0268] Embodiment 100 is a coating composition according to any of the preceding embodiments, wherein when applied to a cleaned and chromium-free pretreated aluminum panel and cured for 12 seconds to a peak metal temperature of 249°C to achieve a dry film thickness of approximately 11 g / m2, and formed into a fully converted (typically 206) standard opening beverage can end, less than 2 mA of current or less than 1 mA of current is passed while exposed to an electrolyte solution containing 1 wt% NaCl dissolved in deionized water for 4 seconds.

[0269] Embodiment 101 is a coating composition according to any of the preceding embodiments, wherein a coating prepared from such a composition, when applied to a cleaned and chromium-free, zirconium pretreated aluminum panel and cured for 12 seconds to a peak metal temperature of 249° C. to achieve a dry film thickness of about 11 (i.e., 10-12) grams per square meter, and preferably formed into a fully converted (typically 206) standard opening beverage can end, exhibits one or more of the following properties (and in some embodiments all or various combinations of such properties): MEK solvent resistance of at least 30 double rubs; a blush rating of at least 6 after water pasteurization; an adhesion rating of GT0 or GT; and feathering (if any) of 0.5 mm or less, 0.4 mm or less, 0.3 mm or less, 0.2 mm or less, or 0.1 mm or less, or no feathering.

[0270] Embodiment 102 is a coating composition according to any preceding embodiment, wherein the coating composition is spray dried and is in the form of a powder coating composition.

[0271] Embodiment 103 is a method comprising: providing a coating composition according to any of the preceding embodiments; applying the coating composition (e.g., via roller coating) to a substrate comprising a beverage can end cap steel or aluminum coil; heating the coated substrate in an oven for an oven residence time of 6 seconds to 30 seconds to achieve a peak metal temperature of 200°C to 260°C; and optionally forming (e.g., stamping) the coated coil to form an easy-open beverage can end cap.

[0272] Embodiment 104 is a method according to embodiment 103, wherein applying the coating composition to the surface of the substrate comprises applying the coating composition to a continuously moving surface traveling at a line speed of 50 meters / minute to 400 meters / minute.

[0273] Embodiment 105 is a coated article comprising a beverage can end cap having an interior or exterior coating, or both, formed from a coating composition according to any one of Embodiments 1 to 104 or obtained by a method according to Embodiments 105 or 106.

[0274] Embodiment 106 is a method or article according to any one of embodiments 103 to 105, wherein the coating has an average dry coating thickness of 7 micrometers to 15 micrometers.

[0275] Embodiment 107 is a method or article according to any one of embodiments 103 to 106, wherein the metal substrate has an average thickness of 175 to 250 microns. Embodiment 108 is a method or article according to any one of embodiments 103 to 107, wherein the surface of the metal substrate is pre-treated with a chromium-based or non-chromium-based (e.g., zirconium-based and acrylic-based) treatment prior to coating with the coating composition.

[0276] Embodiment 109 is a method comprising applying the aqueous coating composition of any one of Embodiments 1 to 102 to a metal substrate of a metal packaging.

[0277] Example

[0278] The following examples are given to illustrate but not to limit the scope of the present invention. Unless otherwise stated in the examples and throughout this disclosure, all parts, ratios and percentages are by weight, and all molecular weights are weight average molecular weights. Unless otherwise stated, all chemicals used are commercially available from, for example, Sigma-Aldrich (St. Louis, MO). One or more of the following test methods are used in the following examples.

[0279] Test Method

[0280] Solvent resistance : The "curing" or cross-linking degree of the coating is measured as solvent resistance, such as methyl ethyl ketone (MEK). The test is performed as described in ASTM D 5402-93. The number of double rubs (i.e., one back and forth motion) is reported. Preferably, the MEK solvent resistance is at least 30 double rubs, preferably at least 50 double rubs, and more preferably at least 100 double rubs.

[0281] Anti-whitening : Whitening resistance measures the ability of a coating to resist attack by various solutions after pasteurization or retort. Typically, whitening is measured by the amount of water absorbed into the coated film. When the film absorbs water, it typically becomes cloudy or appears white. Whitening is typically visually assessed using a scale of 0 to 10, with a rating of "10" indicating no whitening and a rating of "0" indicating complete whitening of the film. The whitening rating after retort (as described herein) is preferably at least 6, and more preferably 7 or higher, and most preferably 9 or higher.

[0282] Adhesion Adhesion testing is performed to assess whether a coating adheres to the coated substrate. Adhesion testing is performed using a SCOTCH 610 tape according to DIN 53151 (German Institute for Standardization eV10772 Berlin, Germany). Adhesion is typically graded on a scale of GT0-GT5, with a grade of "GT0" indicating no adhesion failure, a grade of "GT2" indicating 85% of the coating remains adhered, a grade of "GT3" indicating 65%-85% of the coating remains adhered, and so on. Commercially viable coatings typically require an adhesion grade of GT0 or GT1.

[0283] Water distillation : For the evaluation herein, the coated substrates were immersed in deionized water and subjected to heat and corresponding pressure of 121°C for a period of 90 minutes to achieve such temperature. The coatings were then subjected to blush resistance and adhesion tests.

[0284] Glass Transition Temperature ("Tg") : To evaluate the Tg of acrylic latex, samples for differential scanning calorimetry ("DSC") testing can be prepared by measuring 40 mg of liquid sample into a DSC pan and heating to 150°C in an oven for 1 hour. All samples were analyzed by DSC under the following experimental conditions: 1-equilibrium temperature at -50°C; 2-temperature ramp: 20°C / min to 150°C (end of cycle 1); 3-equilibrium temperature at -50°C; 4-temperature ramp: 20°C / min to 200°C (end of cycle 2); 5-equilibrium temperature at -50°C; 6-temperature ramp: 20°C / min to 200°C (end of cycle 3).

[0285] To evaluate the Tg of the cured coating, the aqueous coating composition was applied to a cleaned and chromium-free, zirconium pretreated aluminum panel and cured for 12 seconds of oven cure time to a peak metal temperature of 249°C to achieve a dry film thickness of approximately 11 grams per square meter (i.e., 10 gsm-12 gsm). After cooling to room temperature, the sample was scraped off the panel, weighed into a standard sample pan and analyzed using a standard DSC hot-cold method. The sample for testing was scraped off the panel and analyzed by DSC under the following experimental conditions: 1-equilibrium temperature at -50°C; 2-heating: 20°C / min to 150°C (end of cycle 1); 3-equilibrium temperature at -50°C; 4-heating: 20°C / min to 200°C (end of cycle 2); 5-equilibrium temperature at -50°C; 6-heating: 20°C / min to 200°C (end of cycle 3).

[0286] The glass transition is calculated from the thermogram of the last thermal cycle. The glass transition is measured at the inflection point of the transition.

[0287] Feathering :like Figures 3 to 6As shown in , feathering is measured using a 0.226 mm gauge coated aluminum reference sheet 10, a scoring tool (or equivalent) with a 60 micron scoring width set in a Carver press, a 7X magnifying glass (or equivalent) graded in 0.005 inch increments, an optional 6 inch vise, a 2000 mL beaker (or equivalent), and a thermometer. The sample to be tested is prepared by cutting a 2 inch x 6 inch sheet 10 from the area to be tested. The 2 inch cut must be in the rolling direction (with the metal grain). Using a permanent marker, a straight line can be made along the entire 6 inch edge of the side of the product as a reference for forming a simulated pull tab. Using a permanent marker, make a 1 / 4 inch straight line mark on the side of the product 1 / 2 inch from the top edge of the test sample, and then make five additional 1 / 4 inch straight line marks at 1 inch intervals along the 6 inch width of the sample to help space the simulated pull tabs apart.

[0288] To test, place the sheet 10 (coated or product side up) between the scoring tool and the anvil in the Carver Press. The first 1 / 4 inch line on the sample matches the black line on the scoring tool. The bottom edge of the sample should be aligned flush with the guide block on the inside of the press. The press rod is manually raised until a force of 5 metric tons is registered on the hydraulic pressure gauge to form a score line 11 that creates a simulated pull tab 12. The sheet 10 is then indexed to the second black line at the top edge of the sample. The press rod is raised again until a force of 5 metric tons is registered on the hydraulic pressure gauge to form another score line 11 that creates a second simulated pull tab 12. Figure 3 As shown generally in FIG. 1 , a total of five simulated pull tabs 12 are repeated along a 6-inch width. Next, a portion 14 of the simulated pull tab 12 is cut or torn approximately 1 / 4 inch by hand or by using a pair of small scissors, such as Figure 4 The pull tab portion 14 can be bent upwardly by 90 degrees.

[0289] Next, the sheet 10 is conditioned, such as by immersing the test sample upright (i.e., with the "legs" facing upward) in a water bath as needed to perform the appropriate test selected, such as immersing a beaker and thermometer in a water bath as needed. Typically, it is conditioned in deionized (DI) water at 85°C for 45 minutes, followed by cooling with tap water before further testing. Other processing conditions may be used as required for a specific application. For feathering evaluation, one sheet 10 is evaluated at a time by drying each sheet before testing. First, the sheet 10 is turned over so that the coated side 13 faces the operator. The scored leg 14 of each simulated pull tab is facing away from the operator at a 90° angle. The sheet 10 is then placed on a flat surface (if necessary, tape or other fastening methods (i.e., a vise) can be used to fix the edge of the plate on the surface). Each simulated pull tab 12 is then pulled straight 15 away from the operator (parallel to the floor) using a pair of pliers or other devices (not shown) to completely remove the pull tab from the test sample. Figure 5 The simulated tab 12a is shown in the process of being pulled and the simulated tab 12b is removed from the sheet 10. After all five simulated tabs are pulled, the feathering is measured on the end cap 18 of the formed opening 16 of the sample 10 using, for example, a 7X eyepiece marked in 0.005 inch increments, as shown in FIG. Figure 6 The feathering is determined by calculating the average of all five values ​​for each sheet 10.

[0290] Coatings for easy-open beverage can end caps preferably exhibit feathering of less than 0.5 mm, more preferably less than 0.4 mm, most preferably less than 0.3 mm, and optimally 0.2 mm or even less. When properly cured, certain preferred films of the present disclosure exhibit feathering of 0.1 mm or less when tested as described above and when subjected to the short cure cycles noted herein.

[0291] Porosity Beverage can ends were prepared by applying the aqueous coating composition to a cleaned and chromium-free, zirconium pretreated aluminum panel and curing for 12 seconds oven cure time to a peak metal temperature of 249°C to achieve a dry film thickness of approximately 11 grams per square meter (i.e., 10 gsm-12 gsm) and forming into a fully converted 206 gauge opening beverage can end.

[0292] The porosity test is carried out by placing the coated beverage can end cap on a cup filled with an electrolyte solution. The cup is inverted to expose the inner coated surface of the can end cap to the electrolyte solution. The amount of current passing through the end cap is then measured. If the coating remains intact (no cracks or breaks) after manufacturing, the minimum current will pass through the end. For this evaluation, the fully converted standard open can end cap (which is a "riveted" aluminum beverage can end cap) is exposed to an electrolyte solution containing a deionized water solution of 1 wt % NaCl for 4 seconds. The WACO Enamel Rater II purchased from the Wilkens-Anderson Company, Chicago, IL, with an output voltage of 6.3 volts is used to measure metal exposure. The measured current is reported in milliamperes. Usually the end cap continuity is initially tested, and then the end cap is tested after pasteurization or retorting. When tested as described above, if the coating passes less than 10 milliamperes (mA) of current (after the end cap is formed), it is considered that the coating meets the porosity test. Preferred coatings pass the initial test at less than 5 milliamps (mA), more preferably less than 2 mA, and even more preferably less than 1 mA. Preferred coatings pass the porosity test after pasteurization at less than 10 mA, more preferably less than 8 mA, and even more preferably less than 5 mA.

[0293] Viscosity test : This test measures the viscosity of a coating composition for rheological purposes such as for defect-free, efficient roller application and other coating application properties. The test is conducted according to ASTM D1200-88 using a Ford Viscosity Cup #2 at 25°C. The results are measured in seconds.

[0294] Example 1

[0295] The materials included in Table 1 were used to prepare an acrylic latex seed polymer.

[0296] Table 1

[0297]

[0298]

[0299] Seed preparation process

[0300] Seeds were prepared as follows.

[0301] A monomer premix was prepared by mixing raw materials 7 to 9 in a conical flask and stirring for 10 minutes. Monomers from 10 to 12 were added sequentially under stirring, keeping 5 minutes between each monomer addition. The final premix was kept under stirring for 45 minutes before use.

[0302] Raw materials 1 to 3 were loaded in a round bottom vessel equipped with a condenser, mechanical stirrer and temperature probe and heated to 80° C. Raw materials 5 and 6 were premixed and added to the vessel together with raw material 4 while the temperature was maintained at 80° C.

[0303] Simultaneously and separately, a monomer premix (including raw materials 7 to 12) and an initiator premix (raw materials 13 to 15) were added to the vessel over 180 minutes. Both feed lines were flushed with raw materials 16 and 17. The reaction mixture was maintained at 80°C for 60 minutes. At the end of the maintenance, raw material 18 was added to the vessel, and then the spike premix (raw materials 19 to 21) was added over 60 minutes. The reaction mixture was again maintained at 80°C for 60 minutes. At the end of the maintenance, the reaction mixture was cooled to 35°C.

[0304] The final properties of the seed polymer were: non-volatile material (NVM) (at 180°C) = 31%; acid value (AV) = 37.7; pH = 3; viscosity at 25°C (Ford #4 cup) = 15 seconds; particle size distribution (PSD) (Microtrac) = 70 nm.

[0305] Example 2

[0306] The materials included in Table 2 were used to prepare acrylic latex.

[0307] Table 2

[0308]

[0309]

[0310] Method for preparing acrylic latex

[0311] Acrylic latex was prepared as follows.

[0312] A monomer premix was prepared by mixing raw materials 6 to 8 in a conical flask and stirring for 10 minutes. Monomers from 9 to 11 were added sequentially under stirring, keeping 5 minutes between each monomer addition. The final premix was kept under stirring for 45 minutes before use.

[0313] Raw materials 1 and 2 were loaded in a round bottom vessel equipped with a condenser, mechanical stirrer and temperature probe and heated to 80° C. Raw materials 4 and 5 were premixed and added to the vessel together with raw material 3 while the temperature was maintained at 80° C.

[0314] Simultaneously and separately, a monomer premix (including raw materials 6 to 11) and an initiator premix (raw materials 12 to 14) were added to the vessel over 180 minutes. Both feed lines were flushed with raw materials 15 and 16. The reaction mixture was maintained at 80°C for 60 minutes. At the end of the maintenance, raw material 17 was added to the vessel, and then the spike premix (raw materials 18 to 20) was added over 60 minutes. The reaction mixture was again maintained at 80°C for 60 minutes. At the end of the maintenance, the reaction mixture was cooled to 35°C.

[0315] The final properties of the acrylic latex were: NVM (at 180°C) = 41.6%; AV = 86; pH = 2.8; Viscosity at 25°C (Ford #2 cup) = 37 seconds; PSD (Microtrac) = 136 nm; and Tg by DSC = 22°C.

[0316] Example 3

[0317] The acrylic latex of Example 2 was formulated into an aqueous coil coating composition using the ingredients indicated in Table 3.

[0318] Table 3

[0319]

[0320] Preparation method

[0321] A coil coating composition including a 3:1 molar equivalent ratio of acrylic latex COOH to crosslinker OH was prepared using a 15% neutralization rate (which is the percentage of COOH groups that can be neutralized with the amount of neutralizer added) as follows.

[0322] A crosslinker premix was prepared by adding PRIMID crosslinker (40 wt % solution) and deionized water (60 wt %) in a beaker and mixing until the crosslinker was completely dissolved (approximately 45 minutes).

[0323] A neutralizer premix was prepared by mixing the DMEA neutralizer and all of the deionized water (17.72%) with stirring for 30 seconds (giving a 3.2% solution of DMEA in DI water).

[0324] The acrylic latex was loaded in a container and the neutralizer premix was added dropwise under vigorous stirring. The mixture was then kept for 15 minutes.

[0325] The crosslinker premix was added under stirring, followed by the solvent under stirring. The lubricant was then added under vigorous stirring and the composition was then held for 10 minutes.

[0326] Example 4

[0327] The coating composition was then applied to a beverage can end cap substrate (chrome-free, zirconium-pretreated aluminum beverage can end cap sheet (alloy 5182 / temperature H39) from Elval, the aluminum rolling division of Elval Halcor SA, Athens, Greece, which had been pretreated with a Permatreat 1903 zirconium-containing pretreatment product from CHEMETALL, Main, Germany) having a beverage can end cap thickness of 0.2 mm to 0.3 mm using a rod applicator to obtain a dry film weight of 10 g / m2 to 12 g / m2. The coated panels were then baked in a coil oven under rapid curing conditions at 249°C PMT (peak metal temperature) for a 12 second dwell time. After the rapid curing process, the coated panels were cooled in an air environment and basic film properties were checked as indicated in Table 4.

[0328] Table 4

[0329]

[0330] Standard = a non-latex aqueous epoxy novolac coil coating composition having commercially acceptable properties for use on the interior of beverage can end closures.

[0331] The glass transition temperature of the cured film was measured by DSC and was determined to be 30° C. After forming of the easy-open beverage can end cap, the coating exhibited very good rivet flexibility. After forming of the easy-open beverage can end cap, the coating showed particularly low porosity values, less than 5 mA.

[0332] The complete disclosures of the patents, patent documents and publications cited herein are incorporated herein by reference as a whole, as if each is separately incorporated. In the case of any conflict or difference between the disclosures in this specification written and any document incorporated herein by reference, the written specification will be used as the standard. Without departing from the scope and spirit of the present disclosure, various modifications and changes to the present disclosure will become apparent to those skilled in the art. It should be understood that the present disclosure is not intended to be unduly limited to the illustrative embodiments and embodiments set forth herein, and such embodiments and embodiments are presented only by way of example, and the scope of the present disclosure is intended to be limited only to the embodiments set forth herein as follows.

Claims

1. A beverage can end cover coil coating composition, the beverage can end cover coil coating composition comprising: an acid or anhydride functional acrylic latex comprising an emulsion polymerized polymer; a carboxyl-reactive crosslinking agent that is nitrogen-containing and not derived from formaldehyde; and optional lubricant; The coating composition: (i) contains less than 2 weight percent, if any, of a crosslinking agent derived from formaldehyde, based on the weight of total solids; (ii) does not contain bisphenol A, bisphenol F and bisphenol S; (iii) optionally free of styrene; (iv) has a glass transition temperature (Tg) of 10°C to 50°C when applied to a cleaned and chromium-free, zirconium pretreated aluminum panel and cured for 12 seconds to a peak metal temperature of 249°C to achieve a dry film thickness of about 11 (i.e., 10-12) grams per square meter, as determined by differential scanning calorimetry (DSC); and (v) when applied to a cleaned and chromium-free, zirconium pretreated aluminum panel and cured for 12 seconds to a peak metal temperature of 249°C to achieve a dry film thickness of approximately 11 (i.e., 10-12) grams per square meter, and formed into a fully converted (typically 206) standard opening beverage can end, with less than 5 mA of current passed while exposed to an electrolyte solution containing 1 wt. % NaCl dissolved in deionized water for 4 seconds.

2. The coating composition of claim 1, wherein the acrylic latex has an acid value of at least 40 mg KOH / gram of latex.

3. The coating composition of claim 1 or 2, wherein the acrylic latex has an acid value of less than 400 mg KOH / gram of the latex.

4. The coating composition of any preceding claim, wherein the acrylic latex comprises at least 50 wt% of an emulsion polymerized polymer, based on the total solids weight of the acrylic latex.

5. A coating composition according to any preceding claim, wherein the acrylic latex is formed from the polymerization of an ethylenically unsaturated monomer component comprising two or more different monomers.

6. The coating composition of claim 5, wherein the ethylenically unsaturated monomer component comprises at least one ethylenically unsaturated acid or anhydride functional monomer and at least one (meth)acrylate monomer, the at least one ethylenically unsaturated acid or anhydride functional monomer including salts thereof.

7. The coating composition of claim 5 or 6, wherein the ethylenically unsaturated monomer component comprises a (meth)acrylate monomer having a Tg greater than 50°C.

8. The coating composition of any one of claims 5 to 7, wherein the ethylenically unsaturated monomer component comprises acrylic acid, ethyl acrylate, and cyclohexyl methacrylate (CHMA).

9. A coating composition according to any preceding claim comprising less than 1 wt% of a crosslinker, if any, derived from formaldehyde, based on the weight of total solids.

10. The coating composition of claim 9, being substantially free, completely free, or free of a crosslinker derived from formaldehyde.

11. A coating composition according to any preceding claim, wherein the coating composition: Contains lubricant; Based on the total solid weight of the coating composition, comprising at least 50% by weight of the acrylic latex; comprising at least 5 wt % of one or more organic solvents, based on the total weight of the coating composition; and The total non-volatile solids content is 30 wt % to 40 wt % based on the total weight of the composition.

12. A coating composition according to any preceding claim, wherein the crosslinker has a hydroxyl value of at least 100 mg KOH / g resin.

13. A coating composition according to any preceding claim, wherein the acrylic latex and the carboxyl-reactive crosslinker are present in the coating composition in amounts to provide an excess of carboxyl equivalents in the acrylic latex relative to the hydroxyl equivalents in the crosslinker.

14. The coating composition of claim 13, wherein the acrylic latex and the carboxyl-reactive crosslinking agent are present in the coating composition in a molar equivalent ratio of carboxyl groups in the acrylic latex to hydroxyl groups in the crosslinking agent of at least 1.5:

1.

15. The coating composition according to claim 13 or 14, wherein the acrylic latex and the carboxyl-reactive crosslinking agent are present in the coating composition in a molar equivalent ratio of carboxyl groups in the acrylic latex to hydroxyl groups in the crosslinking agent of at most 6:

1.

16. A coating composition according to any preceding claim, comprising at least 0.5 wt% and less than 30 wt% of the carboxyl-reactive crosslinker, based on the total solids weight of the coating composition.

17. A coating composition according to any preceding claim which is spray dried and is in the form of a powder coating composition.

18. A method, the method comprising: include: Providing a coating composition according to any preceding claim; applying the coating composition (e.g., via roller coating) to a substrate comprising a beverage can end steel or aluminum coil; heating the coated substrate in an oven for an oven residence time of 6 seconds to 30 seconds, preferably 8 seconds to 15 seconds, to achieve a peak metal temperature of 200°C to 260°C; and optionally forming the coated web to form an easy-open beverage can end.

19. A coated article comprising a beverage can end having an interior or exterior coating, or both, formed from a coating composition according to any one of claims 1 to 17 or obtained by the method according to claim 18.

20. A method comprising applying the aqueous coating composition of any one of claims 1 to 17 to a metal substrate of a metal packaging.

Citation Information

Patent Citations

  • Acrylic polymers and compositions containing such polymers

    CN109844016A