Adhesive tape for wrapping elongated articles, such as, in particular, cable harnesses, and wrapping method

By using a pressure-sensitive adhesive composed of (meth)acrylic and ethylenically unsaturated monomer, combined with emulsion polymerization method and tackifier, the problem of easy expansion of the tape at high temperature and difficult to take into account both the edge resistance of the tape, and the problem of resistance of the tape is achieved. Stability and compatibility of cable guards at high temperatures.

CN119095926APending Publication Date: 2024-12-06TESA SE
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202380036093.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-27
Filing Date
2023-04-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

When existing tapes are used for cable protection in motor vehicles, it is difficult to achieve both easy deployment and curling resistance, and common adhesive properties may increase the expansion force when the temperature rises.

Method used

Using a pressure-sensitive adhesive composed of (meth)acrylic monomer and ethylenically unsaturated monomer, prepared by emulsion polymerization, added a dried polymer dispersion, combined with a tackifier and a light stabilizer, to form an excellent peeling adhesive. Adhesive and anti-curling tape.

Benefits of technology

It realizes that the tape maintains good peeling adhesion and curling resistance at high temperatures, and is suitable for the protection of cables in motor vehicles, ensuring that the cables do not brittle or discolor for a long time, and meet the cable compatibility of high-temperature grades. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095926A_ABST
    Figure CN119095926A_ABST
Patent Text Reader

Abstract

Adhesive tape, in particular for winding cables, consists of a preferably textile carrier and a pressure-sensitive adhesive applied on at least one side of the carrier in the form of a dry polymer dispersion, said polymer being obtained by emulsion polymerization of a monomer mixture, the present invention relates to a composition comprising a monomer mixture comprising: (a) from 80.75 to 94.89 wt%, preferably from 83.85 to 93.73 wt%, of one or more than one (meth) acrylic monomer that individually produces a homopolymer having a glass transition temperature (Tg) of-40 DEG C or less; (b) from 5.00 to 14.00% by weight, preferably from 6.00 to 12.00% by weight, of one or more ethylenically unsaturated monomers, which individually produce a homopolymer having a Tg of 15 DEG C or higher; (c) 0.10 to 5.00 wt.%, preferably 0.20 to 4.00 wt.%, of one or more ethylenically unsaturated monomers having acid and / or hydroxyl functions, (d) 0.01 to 0.25 wt.%, preferably 0.07 to 0.15 wt.%, of a chain transfer agent, the monomers (a) to (d) being different from each other and the weight percentages being based on the total amount of monomers in the monomer mixture, wherein the pressure-sensitive adhesive dispersion polymer has a tan delta maximum in a temperature range of between-25 DEG C and-15 DEG C and a tan delta value of between 0.38 and 0.55 at 130 DEG C, where tan delta is determined by dynamic mechanical analysis (DMA) at an angular frequency of 10 rad / s using a parallel plate tool, and the pressure-sensitive adhesive comprises 0.00 to 10.00, preferably 2.00 to 7.50 parts by weight of a tackifier, the polymer is dispersed with respect to 100 parts by weight of the pressure sensitive adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive tape for jacketing elongated objects such as, more particularly, cable harnesses in motor vehicles, and to a method of jacketing. Background Art

[0002] Adhesive tapes have long been used in industry for the production of cable looms. The adhesive tapes are used to bundle a plurality of electrical conductors before installation or in an already assembled state, for example to reduce the space occupied by the bundle of conductors by bundling, and also to perform protective functions, for example protection from mechanical and / or thermal exposure.

[0003] Common forms of adhesive tapes include a film or textile backing, which usually has a coating of a pressure-sensitive adhesive on one side. Adhesive tapes for wrapping elongated objects are known, for example, from EP 1 848 006 A2, DE 10 2013 213 726 A1 and EP 2 497 805 A1.

[0004] In the motor vehicle industry, the testing and classification of adhesive tapes for cable sheathing is done according to an extensive body of standards, such as LV 312-1 "Protective systems for wire harnesses in motor vehicles, adhesive tapes; Test Guideline" (10 / 2009), which is a joint standard of the companies Daimler, Audi, BMW and Volkswagen, or Ford specification ES-XU5T-1A303-aa (revised 09 / 2009) "Harness Tape Performance Specification". In the following, these standards are referred to in abbreviated form as LV 312 and Ford specification, respectively.

[0005] The noise suppression, abrasion resistance and temperature stability of the adhesive tapes are determined on the basis of defined test configurations and test methods, as fully described in LV 312.

[0006] Cable wrapping tapes with film carriers and fabric carriers are common and are usually coated on one side with various pressure-sensitive adhesives.

[0007] In addition to a host of requirements imposed on adhesive tapes, such as chemical compatibility, high peel adhesion, compatibility with different substrates, in the motor vehicle industry it is also necessary to ensure that non-flat, non-homogeneous substrates are reliably bonded via cable runs, convoluted tubes and branches. Further factors are the bending and tensile stresses during production, installation and subsequent use in the engine compartment of a motor vehicle or, in the body, the continuous bending stresses during door opening.

[0008] Since the end of the tape is ideally bonded to its reverse side, there must be good instantaneous peel adhesion (tack) to the substrate so that the tape does not initially lift (warp). To durably ensure a warp-free product, both the anchoring to the substrate and the internal strength of the adhesive must be such that the adhesive bond is robust even under the influence of tension (tensile and bending stresses).

[0009] In the winding of cable bundles, the tape is bonded around the cables in a manner ranging from no overlap to complete overlap, the radius of which is usually small, meaning that the tape is bent very sharply. At the end of the wound portion (segment), the tape is typically wound mainly on its own reverse side (back side), so that the degree of overlap is almost complete, similar to the customary presentation as a roll of tape, where the adhesive is also bonded to its own reverse side. In the case of warping, static forces act, for example as a result of the bending stiffness of the carrier and the winding tension, and can cause the open end of the tape to stand up undesirably, similar to the start of automatic unfolding (unwinding). Anti-warping is then the ability of the adhesive to resist such static forces.

[0010] In the case of an adhesive tape that is wrapped around an object, warping means the tendency for one end of the tape to stand up. The cause is a combination of the holding force caused by the adhesive, the rigidity of the carrier, and the diameter of the cable bundle.

[0011] Demonstrating the warping resistance of wire harness (WH) cable wrap tapes was done via the TFT method (Threshold Warp Time) and the SWAT method (Single Wire Application Test), as explained below.

[0012] Adhesive tapes are used to protect conductors from damage, for example due to abrasion at sharp edges. Therefore, the carrier material used is particularly robust. Therefore, according to LV 312, adhesive tapes are divided into abrasion classes A to G.

[0013] The cable insulation must not become brittle over a long period of time due to the combined effects of the adhesive tape and increased temperature. Here, according to LV 312, a distinction is made between four temperature classes T1 to T4 (corresponding to 80°C (also called temperature class A), 105°C (also called temperature class B (105)), 125°C (also called temperature class C) and 150°C (also called temperature class D)), to which the wound cable needs to withstand 3000 hours without becoming brittle. It goes without saying that the requirements for the adhesive tapes of temperature classes T3 and T4 are higher than those of the lower classes T1 and T2. The classification from T1 to T4 is determined not only by the cable insulation material, but also by the type of pressure-sensitive adhesive and carrier.

[0014] Cable wrapping tapes with natural rubber-based pressure-sensitive adhesives generally exhibit good resistance to warping, but have an unwinding force (unwinding force) that increases with storage time, especially at elevated temperatures. In addition, they meet only the lower temperature classes for cable compatibility.

[0015] Adhesive tapes based on synthetic rubbers (styrene block copolymers) such as SBS / SIS show similar behavior. Even the temperature rating of the hydrogenated products is limited.

[0016] In addition, there are cable wrapping tapes with pressure-sensitive adhesives based on UV-crosslinkable polyacrylates. These do meet the high temperature ratings, but show a tendency to warp.

[0017] The realization of an adhesive tape (for cable wrapping) that is easy to unroll and at the same time maintains good technical adhesive properties constitutes a major challenge, since these two properties appear to be mutually exclusive - the basic criteria in the case of single-sided adhesive cable wrapping tapes, namely suitable unrolling forces and sufficiently high peel adhesion, are very much in opposition to each other. While good peel adhesion values ​​and the associated low tendency to lift require good conformability and anchoring behavior of the pressure-sensitive adhesive part, these criteria tend to hinder trouble-free unrolling performance. Summary of the invention

[0018] The object of the present invention is to provide an adhesive tape which, despite its ability to be easily unrolled, has good resistance to warping and at the same time exhibits good cable compatibility and which allows particularly simple, cost-effective and rapid sheathing of elongated objects, such as cable harnesses in motor vehicles.

[0019] This object is achieved by the adhesive tape as recited in the independent claim. The dependent claims provide advantageous developments of the adhesive tape and the method for using the adhesive tape.

[0020] The invention therefore relates to an adhesive tape, more particularly an adhesive tape for winding cables, comprising, preferably consisting of, a preferably textile carrier, optionally provided on the bottom side with an applied film, and a pressure-sensitive adhesive, the pressure-sensitive adhesive being applied on at least one side of the carrier in the form of a dry polymer dispersion, the polymer being obtained by emulsion polymerization of a monomer mixture comprising:

[0021] (a) 80.75 to 94.89 wt. %, preferably 83.85 to 93.73 wt. % of one or more than one (meth)acrylic monomer which alone produces a glass transition temperature (T) of -40°C or less. g )

[0022] (b) 5.00 to 14.00 wt. %, preferably 6.00 to 12.00 wt. %, of one or more ethylenically unsaturated monomers which individually produce a T of 15° C. or more g Homopolymer

[0023] (c) 0.10 to 5.00 wt. %, preferably 0.20 to 4.00 wt. %, of one or more ethylenically unsaturated monomers having acid and / or hydroxyl functionality

[0024] (d) 0.01 to 0.25 wt%, preferably 0.07 to 0.15 wt% of a chain transfer agent

[0025] wherein monomers (a) to (d) are different from each other and the weight percentages are based on the total amount of monomers in the monomer mixture,

[0026] wherein the pressure-sensitive adhesive dispersion polymer has a tan δ maximum value in the temperature range between -25°C and -15°C, and

[0027] It has a tan δ value between 0.38 and 0.55 at 130° C., wherein tan δ is determined by dynamic mechanical analysis (DMA) using a parallel plate tool at an angular frequency of 10 rad / s.

[0028] The pressure-sensitive adhesive according to the present invention contains 0 to 10 parts by weight of a tackifier (relative to 100 parts by weight of the pressure-sensitive adhesive dispersion polymer).

[0029] One or more than one (meth)acrylic monomer (a) may individually produce a homopolymer having a glass transition temperature (Tg) in the range of -65°C to -40°C.

[0030] One or more than one (meth)acrylic monomers (a) can be selected from 2-ethylhexyl acrylate, n-butyl acrylate, 3-methylbutyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, nonyl acrylate, propyl acrylate, propylheptyl acrylate, heptadecyl acrylate, decyl methacrylate, dodecyl methacrylate, isodecyl methacrylate, octyl methacrylate, lauryl methacrylate, 2-methoxyethyl acrylate, 3-methoxypropyl acrylate, 3-ethoxypropyl acrylate, 3-methoxybutyl acrylate, hydroxybutyl acrylate, hydroxyethyl caprolactone acrylate and combinations thereof, preferably selected from 2-ethylhexyl acrylate, n-butyl acrylate and combinations thereof, more preferably n-butyl acrylate.

[0031] The monomer mixture may include (a) 83.85 to 93.73 weight percent of one or more than one (meth)acrylic monomer that individually produces a homopolymer having a glass transition temperature (Tg) of -40°C or less; wherein the weight percents are based on the total amount of monomers in the monomer mixture.

[0032] In a preferred embodiment, the (meth)acrylic monomer consists of n-butyl acrylate.

[0033] One or more than one ethylenically unsaturated monomer (b) may individually produce a homopolymer having a glass transition temperature (Tg) of 15°C or higher, preferably in the range of 15°C to 150°C, more preferably in the range of 18°C ​​to 120°C.

[0034] One or more than one ethylenically unsaturated monomers (b) may be selected from acrylonitrile, 3,3,5-trimethylcyclohexyl acrylate, cyclohexyl acrylate, isobornyl acrylate, octadecyl acrylate, tert-butyl acrylate, 2-phenylethyl methacrylate, benzyl methacrylate, n-butyl methacrylate, cyclohexyl methacrylate, ethyl methacrylate, glycidyl methacrylate, hexadecyl methacrylate, isobornyl methacrylate, isobutyl methacrylate, isopropyl methacrylate, methyl methacrylate, neopentyl methacrylate, octadecyl methacrylate, propyl methacrylate, tert-butyl methacrylate, styrene, methoxystyrene, 2-methylstyrene, 3-methylstyrene, 4-ethylstyrene, 4-isopropylstyrene, 4-methoxy-2-methylstyrene, 4-methoxystyrene, 4-methylstyrene, 2-chlorostyrene, 4-bromostyrene, 4-chlorostyrene, 4-fluorostyrene and combinations thereof, preferably selected from methyl methacrylate, n-butyl methacrylate, styrene and combinations thereof, more preferably methyl methacrylate.

[0035] The monomer mixture may include (b) 6.00 to 12.00 weight percent of one or more than one ethylenically unsaturated monomer that individually produces a homopolymer having a Tg of 15° C. or greater; wherein the weight percents are based on the total amount of monomers in the monomer mixture.

[0036] In a preferred embodiment, the ethylenically unsaturated monomer consists of methyl methacrylate.

[0037] One or more than one ethylenically unsaturated monomers (c) having an acid functionality may be selected from ethylenically unsaturated carboxylic acid monomers, ethylenically unsaturated sulfonic acid monomers, ethylenically unsaturated phosphorus-containing acid monomers, preferably selected from (meth)acrylic acid, crotonic acid, fumaric acid, itaconic acid, maleic acid, maleic anhydride, vinylacetic acid, vinyllactic acid, vinylsulfonic acid, styrenesulfonic acid, 2-carboxyethyl (meth)acrylate, vinylsulfonic acid, vinylsulfonic acid phenyl ester, sodium 4-vinylbenzenesulfonate, 2-methyl-2-propylene-1-sulfonic acid, 4-styrenesulfonic acid, 2-acrylamido-2-methyl-1-propanesulfonic acid, vinylphosphonic acid, dimethyl vinylphosphonate, diethyl vinylphosphonate, diethyl allylphosphonate, allylphosphonic acid and combinations thereof, more preferably selected from (meth)acrylic acid.

[0038] Preferred is (meth)acrylic acid of formula I,

[0039]

[0040] Where R 3 = is H or CH3; preferably, acrylic acid or methacrylic acid is optionally used in a mixture. Acrylic acid is particularly preferred.

[0041] One or more than one ethylenically unsaturated monomers (c) having a hydroxyl functional group may be selected from allyl alcohol, vinyl alcohol, N-hydroxymethyl acrylamide, 1-penten-3-ol, hydroxyalkyl esters of ethylenically unsaturated acids such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyethyl caprolactone acrylate, and combinations thereof, preferably hydroxyalkyl esters of ethylenically unsaturated acids such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyethyl caprolactone acrylate, more preferably hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and combinations thereof.

[0042] One or more than one ethylenically unsaturated monomers having acid and hydroxyl functionality (c) may be chosen from 3-allyloxy-2-hydroxy-1-propanesulfonic acid.

[0043] The monomer mixture may include (c) 0.20 to 4.00 wt%, preferably 0.50 to 3.00 wt% of one or more than one ethylenically unsaturated monomer having acid and / or hydroxyl functionality; wherein the weight percentages are based on the total amount of monomers in the monomer mixture.

[0044] In a preferred embodiment, the ethylenically unsaturated monomers consist of acrylic acid and hydroxyethyl methacrylate.

[0045] The chain transfer agent (d) can be selected from n-dodecyl mercaptan, carbon tetrachloride, carbon tetrabromide, bromotrichloromethane, 4-methylbenzenethiol, isooctyl 3-mercaptopropionate, tert-nonyl mercaptan, 4,4'-thiobisbenzenethiol, tert-dodecyl mercaptan, α-methylstyrene dimer, thioglycolic acid, 2-ethylhexyl thioglycolate, butyl 3-mercaptopropionate, 1,8-dimercapto-3,6-dioxaoctane and combinations thereof, preferably n-dodecyl mercaptan.

[0046] The monomer mixture may include (d) 0.10 to 0.20 weight percent of a chain transfer agent; wherein the weight percent is based on the total amount of monomers in the monomer mixture.

[0047] In a preferred embodiment, the chain transfer agent consists of n-dodecyl mercaptan.

[0048] According to a particularly preferred variant, the polymer has the following composition:

[0049] (a) 80.75 to 94.89% by weight, preferably 83.85 to 93.73% by weight, of n-butyl acrylate

[0050] (b) 5.00 to 14.00 wt %, preferably 6.00 to 12.00 wt % of methyl methacrylate

[0051] (c) 0.10 to 5.00 wt. %, preferably 0.20 to 4.00 wt. % of acrylic acid and methacrylate (hydroxyethyl)

[0052] (d) 0.01 to 0.25 wt. %, preferably 0.07 to 0.15 wt. % of a chain transfer agent, such as n-dodecyl mercaptan.

[0053] The pressure sensitive adhesive dispersion polymers of the present invention have a tan δ maximum in the temperature range between -25°C and -15°C and have a tan δ value of 0.38 to 0.55. Tan δ is determined by dynamic mechanical analysis (DMA) at an angular frequency of 10 rad / s using a parallel plate tool as further described in the Examples.

[0054] As used herein, the term "tan δ" is also referred to as damping coefficient, dissipation coefficient or loss coefficient, and is defined as the ratio between the loss modulus (G") and the elastic modulus (G'). According to the present invention, the tan δ value at 130°C may be between 0.40 and 0.50, preferably between 0.40 and 0.45. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein.

[0055] The glass transition temperature of the above-mentioned monomers which alone produce a certain homopolymer glass transition temperature (Tg) refers to the glass transition temperature determined by differential scanning calorimetry (DSC). The person skilled in the art realizes in this context that DSC is sufficiently decisive only when the material sample is kept at this temperature for at least 2 minutes after the initial heating cycle to a temperature at least 25°C higher than the highest glass transition temperature or melting temperature of the material but at least 20°C lower than the lowest decomposition temperature of the material. The sample is then cooled to a temperature at least 20°C lower than the lowest glass transition temperature or melting temperature to be determined, wherein the cooling rate should be a maximum of 20°C / min, preferably a maximum of 10°C / min. After a further waiting time of several minutes, the actual measurement is then carried out, during which the sample is heated to at least 20°C higher than the highest melting temperature or glass transition temperature at a heating rate of generally 10°C / min or less. The corresponding maximum and minimum limiting temperatures can be roughly specified in simple preliminary measurements using a single sample.

[0056] The pressure-sensitive adhesive dispersion polymers according to the present invention may be prepared by any emulsion polymerization process known to those skilled in the art, provided that a monomer mixture as defined herein is used.

[0057] A description of this process can be found, for example, in Peter A. Lovell and Mohamed S. "Emulsion Polymerization and Emulsion Polymers" El-Aasser-Wiley-VCH 1997-ISBN 0-471-96746-7 or in EP 1 378 527 B1.

[0058] During the polymerization, it cannot be ruled out that not all monomers undergo reaction to form polymers. It is obvious here that the residual monomer content should be as small as possible.

[0059] Preference is given to providing an adhesive comprising a polymer dispersion having a residual monomer content of less than or equal to 1% by weight, more particularly less than or equal to 0.5% by weight (relative to 100 parts by weight of the pressure-sensitive adhesive dispersion polymer).

[0060] In the emulsion polymerization used to prepare the pressure-sensitive adhesive dispersion polymer of the present invention, a seed dispersion may be used. Any seed particles known to those skilled in the art may be used.

[0061] The seed particles are preferably present in an amount of 0.01 to 10 parts by weight, preferably 0.1 to 5 parts by weight, based on 100 parts by weight of all ethylenically unsaturated monomers used in the polymer. Those skilled in the art will understand that any range formed by any explicitly disclosed lower and upper limits is expressly encompassed in this specification.

[0062] The process for preparing the above-mentioned pressure-sensitive adhesive dispersion polymers can be carried out at a temperature of 0 to 130° C., preferably 0 to 100° C., particularly preferably 20 to 95° C., very particularly preferably 40 to 90° C., in the absence of an emulsifier or in the presence of one or more emulsifiers, in the absence of a protective colloid or in the presence of one or more protective colloids and in the presence of one or more initiators.

[0063] Initiators that can be used when practicing the present invention may include water-soluble and / or oil-soluble initiators that are effective for polymerization purposes. Representative initiators are well known in the art and include, for example, azo compounds (e.g., AIBN, AMBN, and cyanovaleric acid) and inorganic peroxy compounds, such as hydroperoxides, sodium peroxydisulfate, potassium peroxydisulfate, and ammonium peroxydisulfate, percarbonates, and perborates, and organic peroxy compounds, such as alkyl hydroperoxides, dialkyl peroxides, acyl hydroperoxides, and diacyl peroxides, and esters, such as tert-butyl perbenzoate, and combinations of inorganic and organic initiators.Suitable initiators may be selected from 2,3-dimethyl-2,3-diphenylbutane, tert-butyl hydroperoxide, tert-amyl hydroperoxide, cumyl hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, isopropyl cumyl hydroperoxide, p-menthane hydroperoxide, 2,5-di(tert-butylperoxy)-2,5-dimethyl-3-hexyne, 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane, di(tert-butyl) peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, di(tert-butylperoxy-isopropyl)benzene, tert-butylcumyl peroxide, di(tert-amyl) peroxide, diperoxide Isopropylbenzene, 4,4-di(tert-butylperoxy)butyl valerate, tert-butyl peroxybenzoate, 2,2-di(tert-butylperoxy)butane, tert-amyl peroxybenzoate, tert-butyl peroxyacetate, tert-butyl peroxycarbonate (2-ethylhexyl), tert-butyl peroxycarbonate isopropyl, tert-butyl peroxyhexanoic acid 3,5,5-trimethyl ester, 1,1-di(tert-butylperoxy)cyclohexane, tert-amyl peroxyacetate, tert-amyl peroxycarbonate (2-ethylhexyl), 1,1-di(tert-butylperoxy)-3,5,5-trimethylcyclohexane, 1,1-di(tert-butylperoxy)cyclohexane, tert-butyl monoperoxymaleate, 1,1'-azobis(tert-butylperoxy) (Hexahydrobenzonitrile), tert-butyl peroxyisobutyrate, tert-butyl peroxydiethylacetate, tert-butyl peroxy-2-ethylhexanoate, dibenzoyl peroxide, tert-amyl peroxy-2-ethylhexanoate, di(4-methylbenzoyl)peroxide, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, ammonium peroxydisulfate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(isobutyronitrile), didecanoyl peroxide, potassium persulfate, dilauroyl peroxide, di(3,5,5-trimethylhexanoyl)peroxide, tert-amyl peroxypivalate, tert-butyl peroxyneoheptanoate Peroxydicarbonate, bis(2-ethylhexyl)peroxydicarbonate, bis(4-tert-butylcyclohexyl)peroxydicarbonate, diisopropyl peroxydicarbonate, tert-butyl peroxyneodecanoate, di-sec-butyl peroxydicarbonate, tert-amyl peroxyneodecanoate, diisopropyl peroxyneodecanoate, tert-amyl peroxyneodecanoate, diisopropyl peroxyneoheptanoate, tert-amyl peroxyneodecanoate, cumyl peroxyneoheptanoate, di(3-methoxybutyl)peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, cumyl peroxyneodecanoate, diisobutyryl peroxide, and mixtures thereof.

[0064] Initiator can be used in an amount sufficient to initiate polymerization at a desired rate. Typically, 0.01 to 5 wt %, preferably 0.1 to 4 wt %, of initiator is sufficient, based on the total weight of the monomers in the monomer mixture. Most preferably, the amount of initiator is 0.01 to 2 wt %, based on the total weight of the monomers in the monomer mixture.

[0065] The above-mentioned inorganic and organic peroxy compounds can also be used alone or in combination with one or more suitable reducing agents, as known in the art. Examples of such reducing agents can include sulfur dioxide, alkali metal disulfites, alkali metal bisulfites and ammonium bisulfites, thiosulfates, dithionites and formaldehyde sulfoxylates, as well as hydroxylamine hydrochloride, hydrazine sulfate, iron (II), cuprous naphthanate, glucose, sulfonic acid compounds such as sodium methanesulfonate, amine compounds such as dimethylaniline and ascorbic acid. The amount of the reducing agent is preferably 0.03 to 10 parts by weight per part by weight of the polymerization initiator.

[0066] Surfactants or emulsifiers suitable for stabilizing dispersion polymers may include those conventional surfactants used in polymerization processes. One or more surfactants may be added to the aqueous phase and / or the monomer phase. The effective amount of the surfactant in the seeding process is the amount selected to support stabilization of the particles as a colloid, minimize contact between the particles, and prevent coagulation. In non-seed methods, the effective amount of the surfactant is the amount selected to determine the particle size.

[0067] Representative surfactants include saturated and ethylenically unsaturated sulfonic acids or their salts, including, for example, unsaturated hydrocarbon sulfonic acids, such as vinyl sulfonic acid, allyl sulfonic acid and methallyl sulfonic acid and their salts; aromatic hydrocarbon acids, such as p-styrene sulfonic acid, isopropenylbenzenesulfonic acid and vinyloxybenzenesulfonic acid and their salts; sulfoalkyl esters of acrylic acid and methacrylic acid, such as sulfoethyl methacrylate and sulfopropyl methacrylate and their salts, and 2-acrylamido-2-methylpropanesulfonic acid and its salts; alkylated diphenyl oxide disulfonates, sodium dodecylbenzenesulfonate and the dihexyl or dioctyl esters of sodium sulfosuccinate, sodium alkyl esters of sulfonic acid, ethoxylated alkylphenols and ethoxylated alcohols; fatty alcohol sulfates and fatty alcohol (poly) ether sulfates.

[0068] The type and amount of surfactant is generally determined by the number of particles, their size and their composition. Typically, the amount of surfactant is 0 to 20 wt %, preferably 0 to 10 wt %, more preferably 0 to 5 wt %, based on the total weight of the monomers in the monomer mixture. The amount of surfactant includes all values ​​and subvalues ​​therebetween based on the total weight of the monomers in the monomer composition. Polymerization can be carried out without the use of a surfactant.

[0069] Alternatively, protective colloids may also be used to replace the above-mentioned surfactants or to use protective colloids in addition to the above-mentioned surfactants. As used herein, the term "protective colloid" generally refers to a water-soluble polymer compound that is used to stabilize finely dispersed polymer particles. The protective colloid can surround the particles with a film, and due to its, for example, spatial expansion, prevent the particles from approaching each other and thus prevent flocculation or coagulation. Suitable colloids include polyhydroxy compounds, such as polyvinyl alcohol, partially acetylated polyvinyl alcohol, casein, hydroxyethyl starch, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polysaccharides and degraded polysaccharides, polyethylene glycol, polyvinyl pyrrolidone, ethylene glycol-propylene glycol block copolymers and gum arabic. Preferred protective colloids are carboxymethyl cellulose, hydroxyethyl cellulose and hydroxypropyl cellulose. Typically, the amount of these protective colloids is 0-10 parts by weight, preferably 0-5 parts by weight, more preferably 0-3 parts by weight, based on the total weight of the monomers. Based on the total weight of the monomers, the amount of the protective colloid includes all values ​​and subvalues ​​therebetween.

[0070] The adhesive is a pressure-sensitive adhesive (PSA), in other words an adhesive which allows permanent bonding to almost all substrates even with relatively weak applied pressure and which can be detached (separated) from the substrate again after use in a manner that leaves essentially no residue. The PSAs have a permanent pressure-sensitive adhesive effect at room temperature, in other words have sufficiently low viscosity and high tack, and therefore the surface of the adhesive substrate in question is wetted even with low applied pressure. The adhesive's bondability derives from its adhesive properties, and its re-detachability derives from its cohesive properties.

[0071] In order to obtain pressure-sensitive adhesive properties, the adhesive must be above its glass transition temperature at the processing temperature in order to have viscoelastic properties. Since cable bundle winding takes place at normal ambient temperature (approximately 15°C to 25°C), the glass transition temperature of the PSA formulation is preferably below +15°C (determined by DSC (differential scanning calorimetry) at a heating rate of 10 K / min according to DIN 53765).

[0072] The glass transition temperature of the acrylate copolymer can be estimated from the glass transition temperature of the homopolymer and their relative proportions according to the Fox equation.

[0073] To obtain polymers having a desired glass transition temperature, for example pressure-sensitive adhesives or heat-sealing compounds, the quantitative composition of the monomer mixture is advantageously selected so that equation (E1) analogous to the Fox equation (see TG Fox, Bull. Am. Phys. Soc. 1956, 1, 123) yields the desired Tg of the polymer.

[0074]

[0075] The addition of a possible adhesion promoter automatically increases the glass transition temperature by about 5 to 40 K, depending on the amount added, the compatibility and the softening temperature.

[0076] Therefore, an acrylate copolymer having a glass transition temperature of at most 0°C is preferred.

[0077] According to ASTM D3330 (for 30 g / m on 23 μm polyester film carrier 2 The adhesive of the present invention has a peel adhesion on steel of at least 2.0 N / cm with an adhesive coating weight of at least 1.0 N / cm.

[0078] According to the present invention, the pressure-sensitive adhesive composition may further include a tackifier resin in addition to the pressure-sensitive adhesive dispersion polymer of the present invention.

[0079] According to the general understanding of those skilled in the art, "tackifier resin" is understood to mean an oligomeric or polymeric resin that increases the self-adhesion (tack, inherent adhesion) of a PSA compared to an otherwise identical PSA without the tackifier resin.

[0080] The use of tackifiers to increase the peel adhesion values ​​of PSAs is known in principle. This effect also occurs if the adhesive is admixed with 0.00 to 10.00 parts by weight (relative to 100 parts by weight of the pressure-sensitive adhesive dispersion polymer), preferably 2.00 to 7.50 parts by weight, more preferably 2.50 to 5.50 parts by weight of tackifier.

[0081] As tackifier resins, one, two or more substances selected from the known various tackifier resins can be used. In principle, all known classes of compounds have suitability as tackifiers (also referred to as tackifier resins). Tackifiers are, for example, hydrocarbon resins (e.g., polymers based on unsaturated C5 or C9 monomers), terpene phenolic resins, polyterpene resins based on raw materials such as α- or β-pinene, aromatic resins such as coumarone-indene resins or resins based on styrene or α-methylstyrene such as rosin and its derivatives, such as disproportionated, dimerized or esterified rosin, for example reaction products with glycols, glycerol or pentaerythritol, to name a few.

[0082] Preferred resins are those based on terpene phenols and rosin esters.

[0083] The term "rosin-based resin" refers to both rosin and rosin-derived resins. Examples of rosin may include unmodified rosin (raw rosin), such as gum rosin, wood rosin or tall oil rosin, and modified rosin obtainable from unmodified rosin by modification such as hydrogenation, disproportionation or polymerization. Suitable examples of rosin-derived resins include rosin esters, such as unmodified rosin ester (which is an ester of unmodified rosin and alcohol) and modified rosin ester (which is an ester of modified rosin and alcohol); unsaturated fatty acid-modified rosin obtainable by modifying rosin with unsaturated fatty acids; unsaturated fatty acid-modified rosin ester obtainable by modifying rosin ester with unsaturated fatty acids; rosin alcohol obtainable by reducing carboxyl groups in rosin or the above-mentioned various rosin derivatives (including rosin ester, unsaturated fatty acid-modified rosin and unsaturated fatty acid-modified rosin ester); metal salts of rosin or the above-mentioned various rosin derivatives. Suitable examples of terpene resins include terpenes (typically monoterpenes), such as α-pinene, β-pinene, d-limonene, l-limonene and dipentene. Suitable examples of modified terpene resins include resins obtainable by modifying terpene resins, such as styrene-modified terpene resins or hydrogenated terpene resins. Suitable examples of phenolic resins include terpene phenol resins, hydrogenated terpene phenol resins, alkylphenol resins and rosin phenol resins.

[0084] Preferred tackifier resins are those having an ASTM E28-99 (2009) softening point greater than 90°C, more preferably greater than 100°C, according to ASTM E29-99 (2009).

[0085] Particularly preferred are resins based on terpene phenols and rosin esters having a softening point of more than 100° C. according to ASTM E2899 (2009). The resins are effectively used in the form of dispersions. In this way, they can be easily mixed with the polymer dispersion in finely divided form.

[0086] Preferably, the pressure-sensitive adhesive composition of the present invention may not contain any tackifier resin. The pressure-sensitive adhesive composition of the present invention may be substantially free of any tackifier resin. As used herein, the term "substantially free of" means that a tackifier resin (if any) exists as an incidental impurity, for example, based on the gross weight of the pressure-sensitive adhesive composition, in an amount less than 0.04% by weight. According to the present invention, the pressure-sensitive adhesive composition of the present invention may be completely free of any tackifier resin. As used herein, the term "completely free of" refers to the absence of a tackifier resin at all in the pressure-sensitive adhesive composition.

[0087] To further improve cable compatibility, the adhesive formulation can optionally be blended with light stabilizers or with primary and / or secondary (auxiliary) aging inhibitors.

[0088] The aging inhibitors used may be products based on sterically hindered phenols, phosphites, thiosynergists, sterically hindered amines or UV absorbers.

[0089] It is preferred to use a primary antioxidant, such as Irganox 1010 or Irganox 254, alone or in combination with a secondary antioxidant, such as Irgafos TNPP or Irgafos 168.

[0090] The aging inhibitors here can be used in any desired combination with one another, with mixtures of primary and secondary antioxidants in combination with light stabilizers such as Tinuvin 213 showing particularly good aging-inhibiting effects.

[0091] It has been shown that aging inhibitors in which the primary antioxidant is combined with the secondary antioxidant in one molecule are particularly advantageous. These aging inhibitors include cresol derivatives whose aromatic ring is substituted by a thioalkyl chain at two arbitrarily different positions, preferably in the ortho and meta positions relative to the OH group, and the sulfur atom can also be connected to the aromatic ring of the cresol building unit via one or more alkyl chains. The number of carbon atoms between the aromatic part and the sulfur atom can be between 1 and 10, preferably between 1 and 4. The number of carbon atoms in the alkyl side chain can be between 1 and 25, preferably between 6 and 16. In this context, the following types of compounds are particularly preferred: 4,6-bis(dodecylthiomethyl)-o-cresol, 4,6-bis(undecylthiomethyl)-o-cresol, 4,6-bis(decylthiomethyl)-o-cresol, 4,6-bis(nonylthiomethyl)-o-cresol or 4,6-bis(octylthiomethyl)-o-cresol. Ageing inhibitors of this type are obtainable, for example, under the name Irganox 1726 or Irganox 1520 from the company Ciba Geigy.

[0092] The amount of the added aging inhibitor or aging inhibitor package should be in the range of 0.10 to 10.00 wt. %, preferably in the range of 0.20 to 5.00 wt. %, very preferably in the range of 0.50 to 3.00 wt. %, based on the total solids content of the pressure-sensitive adhesive composition.

[0093] The pressure-sensitive adhesive composition may also include rheological additives (thickeners), defoamers, deaerators, wetting agents, flow control agents, and combinations thereof. The pressure-sensitive adhesive composition of the present invention may include rheological additives (thickeners), defoamers, deaerators, wetting agents, flow control agents, and combinations thereof in an amount ranging from 0.1 to 5% by weight, based on the total solids content of the pressure-sensitive adhesive composition.

[0094] A basic distinction is made here between organic and inorganic rheological additives.

[0095] Organic thickeners are then divided into two basic modes of action: (i) thickening of the aqueous phase, i.e. non-associative, and (ii) association between thickener molecules and particles, partly with the introduction of stabilizers (emulsifiers). Representatives of the first (i) group of compounds are water-soluble polyacrylic acids and polyco-acrylic acids, which form polyelectrolytes with high hydrodynamic volume in alkaline media. The technicians also refer to these as ASE (alkali swellable emulsions). They are characterized by high static shear viscosity and strong shear thinning. Another class of compounds are modified polysaccharides, especially cellulose ethers such as carboxymethylcellulose, 2-hydroxyethylcellulose, carboxymethyl-2-hydroxyethylcellulose, methylcellulose, 2-hydroxyethylmethylcellulose, 2-hydroxyethylethylcellulose, 2-hydroxypropylcellulose, 2-hydroxypropylmethylcellulose, 2-hydroxybutylmethylcellulose. Also included in this class of compounds are less commonly used polysaccharides such as starch derivatives and specific polyethers.

[0096] In principle, the active group (group) of (ii) associative thickeners is a block copolymer with a water-soluble middle block and hydrophobic end blocks, which interact with the particles or with themselves and thus form a three-dimensional network with the incorporated particles. The following are familiar to the skilled person as typical representatives: HASE (hydrophobically modified alkali swellable emulsion), HEUR (hydrophobically modified ethylene oxide urethane) or HMHEC (hydrophobically modified hydroxyethyl cellulose). In the case of HASE thickeners, the middle block is ASE and the end blocks are usually long hydrophobic alkyl chains connected via polyethylene oxide bridges. In the case of HEUR, the water-soluble middle block is a polyurethane and in the case of HMHEC it is 2-hydroxyethyl cellulose. In particular, nonionic HEUR and HMHEC are essentially insensitive to pH.

[0097] Depending on their structure, associative thickeners lead to a more or less Newtonian (independent of shear rate) or pseudoplastic (shear-liquefaction) flow behavior. Occasionally they also exhibit thixotropic properties, meaning that the viscosity depends not only on shear force but also on time.

[0098] Inorganic thickeners are usually phyllosilicates of natural or synthetic origin, examples being hectorites and montmorillonites. When in contact with water, the individual layers separate from one another. Due to the different charges on the faces and edges of the flakes, they form a space-filling house-of-cards structure when stationary, resulting in a high static shear viscosity up to the yield point. When sheared, the house-of-cards structure collapses and a significant drop in shear viscosity is observed. Depending on the charge, concentration and geometry of the flakes, the formation of the structure can take some time, so that thixotropy can also be achieved with such inorganic thickeners.

[0099] The thickener may in some cases be stirred directly into the adhesive dispersion, or in some cases may be advantageously pre-dispersed or pre-diluted in water beforehand.

[0100] Suppliers of thickeners are, for example, OMG Borchers, Omya, Byk Chemie, Dow Chemical Company, Evonik or Münzing Chemie.

[0101] The pressure-sensitive adhesive composition may also include fillers such as silica, glass in the form of solid or hollow beads, microspheres, calcium carbonate, zinc oxide, titanium dioxide, aluminum oxide, aluminum oxide hydroxide, and combinations thereof. According to the present invention, the pressure-sensitive adhesive composition of the present invention may include fillers in an amount in the range of 0.1 to 20 wt %, based on the total solid content of the pressure-sensitive adhesive composition.

[0102] Suitable supports include in principle all support materials, preferably textile supports and more preferably woven textiles, more particularly woven polyester textiles.

[0103] As carrier materials for the adhesive tape, all known textile carriers can be used, for example knitted fabrics, scrims, tapes, braids, tufted textiles (needle pile textiles), felts, woven fabrics (including plain, twill and satin weaves), knitted fabrics (including warp knits and other knitted fabrics) or non-woven webs, the term "non-woven web" including at least sheet-like textile structures according to EN 29092 (1988) as well as stitchbonded webs and similar systems.

[0104] Particularly advantageous are adhesive tapes in which woven, nonwoven or knitted fabrics are used as carriers. Carriers of these kinds are described, for example, in WO 2015 / 004190 A1.

[0105] Woven and knitted spacer fabrics with lamination can likewise be used.

[0106] These kinds of spacer fabrics are disclosed in EP 0 071 212 B1. Spacer fabrics are mat-like layer structures which comprise an overlying layer of fiber or wire web, a base layer and between these layers individual retaining fibers or bundles of such fibers which are distributed over the area of ​​the layer structure, are needled through the particle layer and connect the overlying layer and the base layer to one another. As a further but not mandatory feature, the retaining fibers according to EP 0 071 212 B1 contain particles of an inert mineral, such as sand, gravel, etc.

[0107] The retaining fibers needled through the particle layer hold the cover and base layers at a distance from each other and connect the cover and base layers.

[0108] The nonwovens under consideration particularly include consolidated staple fiber webs and filament webs, meltblown webs and spunbond webs, which generally require additional consolidation. Possible consolidation methods known for webs include mechanical consolidation, thermal consolidation and chemical consolidation. If mechanical consolidation is used to hold the fibers together purely mechanically (generally by the entanglement of individual fibers, by the mutual looping of fiber bundles or by sewing in additional threads), adhesive (using adhesives) or cohesive (adhesive-free) fiber-fiber bonds can be obtained by heat and by chemical techniques. Given suitable formulations and suitable process schemes, these bonds can be limited to or at least mainly limited to fiber nodes, so that a stable three-dimensional network is formed, but at the same time a loose open structure is maintained in the web.

[0109] Webs which have proven to be particularly advantageous are those which are consolidated, in particular, by sewing with individual threads or by looping with each other.

[0110] Such consolidated webs are produced, for example, on a "Malimo" type stitchbonding machine from the company Karl Mayer (formerly Malimo) and can be obtained from companies including Techtex GmbH. Stitchbonded nonwoven fabrics are formed by a nonwoven material having a plurality of stitches extending parallel to each other. These stitches are formed by sewing or stitching continuous textile threads. For this type of nonwoven (also known as Maliwatt). Malifleece is characterized in that cross-laid webs are consolidated by forming loops from the fibers of the web.

[0111] The carrier used may be a web of the Kunit or Multiknit type. The Kunit web is characterized in that it originates from a process of forming a sheet-like structure of a longitudinally oriented fiber web, which has loops on one side and loop feet or pile fiber folds on the other side, but has neither a line nor a prefabricated sheet-like structure. Such a web has also been produced for a relatively long time, for example on a "Malimo" type stitching machine from the company Karl Mayer. Another characteristic feature of this web is that, as a longitudinal fiber web, it is able to absorb high tensile forces in the longitudinal direction. The characteristic feature of the Multiknit web relative to the Kunit web is that, by double-sided needling, the web is consolidated on both the top side and the bottom side. The starting product for Multiknit is usually one or two single-sided pile fiber nonwovens that are looped with each other produced by the Kunit process. In the final product, both top surfaces of the nonwoven are formed by looping the fibers with each other to form a closed surface, and are connected to each other by fibers that stand almost vertically. A further possibility is the introduction of further needle-seamable sheetlike structures and / or dispersible media.

[0112] Finally, the stitchbonded web as an intermediate is also suitable for forming the covering of the present invention and the adhesive tape of the present invention. The stitchbonded web is formed by a nonwoven material having a plurality of sutures extending parallel to each other. These sutures are formed by stitchbonding or sewing continuous textile threads. For this type of web, a "Malimo" type stitchbonding machine from Karl Meyer is known.

[0113] Needle felt webs are also particularly suitable. In needle felt webs, the fibers are tufted into a sheet-like structure by means of needles provided with barbs. By alternating the introduction and withdrawal of the needles, the material is consolidated on the needle bar, wherein the individual fibers are looped with each other to form a solid sheet-like structure. The number and arrangement of the needling points (needle shape, penetration depth, double-sided needling) determine the thickness and strength of the fiber structure, which is generally lightweight, air-permeable and elastic.

[0114] Also particularly advantageous are staple fiber webs which are mechanically preconsolidated in a first step or hydraulically laid wet laid webs in which 2 to 50% by weight of the web fibers, more particularly 5 to 40% by weight of the web fibers are fusible fibers.

[0115] Such webs are characterized in that the fibers are wet laid or, for example, a staple fiber web is preconsolidated by forming loops from the fibers of the web by needling, stitching or air jet and / or water jet treatment.

[0116] In a second step, heat setting takes place, wherein the strength of the web is increased again by melting or partial melting of the fusible fibers.

[0117] For the use of the nonwoven according to the invention, the adhesive consolidation of mechanically pre-consolidated or wet-laid webs is particularly interesting, which can be carried out via the addition of a binder in solid, liquid, foamed or pasty form. A wide variety of theoretical presentation forms are possible: for example, a solid binder as a powder for dripping; as a sheet or as a web; or in the form of adhesive fibers. The liquid binder can be applied as a solution in water or an organic solvent, or as a dispersion. For adhesive consolidation, adhesive dispersions are mainly selected: thermosetting materials in the form of phenolic or melamine resin dispersions, elastomers as dispersions of natural or synthetic rubbers, or generally dispersions of thermoplastic materials (e.g., acrylates, vinyl acetate, polyurethanes, styrene-butadiene systems, PVC, etc., and copolymers thereof). Typically, the dispersion is anionic or nonionic stabilized, but in some cases, cationic dispersions can also be advantageous.

[0118] The adhesive can be applied in a manner according to the prior art and for which reference is made, for example, to standard works on coating or nonwoven technology, such as “Vliesstoffe” (Georg Thieme Verlag, Stuttgart, 1982) or “Textiltechnik-Vliesstofferzeugung” (Arbeitgeberkreis Gesamttextil, Eschborn, 1996).

[0119] For mechanically pre-consolidated nonwovens that already have sufficient composite strength, one-sided jet application of adhesive is suitable for producing specific changes in surface properties.

[0120] Such a procedure not only saves the use of its adhesive, but also greatly reduces the energy requirement for drying. Since no squeezing rollers are required and since the dispersion remains mainly in the upper region of the nonwoven, undesirable hardening and stiffening of the web can be largely prevented.

[0121] For adequate adhesive consolidation of the web carrier it is generally necessary to add binder in an amount of the order of 1% to 50% by weight, more particularly 3% to 20% by weight, based on the weight of the fiber web.

[0122] The adhesive can be added as early as during the production of the web, during mechanical preconsolidation, or in a separate process step, which can be carried out in-line or off-line. After the addition of the adhesive, conditions must be temporarily created for the adhesive in which the adhesive becomes adhesive and adhesively connects the fibers, which can be achieved, for example, during the drying of the dispersion or by heating, with further variant possibilities by applying pressure over the entire surface or in parts. The adhesive can be activated in known drying tunnels (given a suitable choice of adhesive) or by means of infrared radiation, UV radiation, ultrasound, high-frequency radiation, etc. For the subsequent end use, it is reasonable, although not absolutely necessary, for the adhesive to lose its tack after the end of the web production process. Advantageously, as a result of the heat treatment, volatile components such as fiber auxiliaries are removed, resulting in a web with a favorable fogging value, so that when low-fogging adhesives are used, adhesive tapes with particularly favorable fogging values ​​can be produced; therefore, the covering also has a very low fogging value.

[0123] Fogging (see DIN 75201A) refers to the effect in which, under adverse conditions, low molecular weight compounds can be released from the adhesive tape (outgassing) and condense on cold parts. Thus, for example, the view through the windshield can be adversely affected.

[0124] Another special form of adhesive consolidation involves activating the binder by partial dissolution or partial swelling. In this case, in principle, the fibers themselves or admixed special fibers can also assume the function of the binder. However, since such solvents are objectionable for environmental reasons and / or are problematic in terms of their handling, this method is not often used for most polymeric fibers.

[0125] Advantageously and at least in regions, the carrier can have a single-sided or double-sided polished surface, preferably in each case a surface polished over the entire region. As described in detail in, for example, EP 1 448 744 A1, the polished surface can be embossed (calendered, chintzed).

[0126] Furthermore, the carrier can be compacted by calendering on a roller mill. The two rollers preferably run in opposite directions and at the same peripheral speed, so that the carrier is pressed and compacted.

[0127] If there are differences in the peripheral speed of the rollers, the support is additionally polished.

[0128] The carrier is preferably a woven fabric, more preferably a woven polyester fabric. Particularly preferred is a fabric having the following structure:

[0129] ·The number of threads in the warp is 10 to 60 / cm

[0130] ·The number of threads in the weft is 10 to 40 / cm

[0131] The warp yarns have a yarn weight of 40 dtex to 400 dtex, more particularly 44 dtex to 330 dtex, very preferably 167 dtex.

[0132] The weft yarns have a yarn weight of 40 dtex to 660 dtex, more preferably 44 dtex to 400 dtex, very preferably 167 dtex.

[0133] According to a further advantageous embodiment of the invention, the number of threads in the warp is 40 to 50 / cm, preferably 44 / cm.

[0134] According to a further advantageous embodiment of the invention, the number of threads in the weft thread is 18 to 22 / cm, preferably 20 / cm.

[0135] According to another advantageous embodiment of the invention, the woven fabric is a woven polyester fabric.Other possibilities are woven polyamide fabrics, woven viscose fabrics and / or woven blends comprising said materials.

[0136] Further preferably, the thickness of the woven fabric is at most 300 μm, more preferably 170 to 230 μm, very preferably 190 to 210 μm. According to another advantageous embodiment of the invention, the carrier has a maximum of 200 g / m 2 , preferably 100 to 150 g / m 2 The basis weight.

[0137] The starting materials for the carrier material of the adhesive tape are more particularly (artificial) fibers (staple fibers or continuous filaments) made of synthetic polymers, also called synthetic fibers, made of polyester, polyamide, polyimide, aramid, polyolefin, polyacrylonitrile or glass; (artificial) fibers made of natural polymers, for example cellulose fibers (viscose, modal, lyocell, cupro, acetate, triacetate, celluloid), for example rubber fibers, for example vegetable protein fibers and / or for example animal protein fibers and / or natural fibers made of cotton, sisal, flax, silk, hemp, flax, coconut or wool. However, the invention is not limited to the materials mentioned; on the contrary, a variety of further fibers can be used to produce the carrier, as is clear to the person skilled in the art without taking an inventive step. In addition, yarns made of the specified fibers are also suitable.

[0138] In the case of woven fabrics or scrims, the individual threads may be produced from blended yarns and may therefore have both synthetic and natural components. In general, however, the warp and weft threads are each formed from a single species. The warp and / or weft threads here may in each case consist only of synthetic threads or only of threads made of natural raw materials, in other words, of a single species.

[0139] The yarn or thread of the woven fabric can be in the form of a filament. For the purposes of the present invention, a filament refers to a bundle of parallel single linear fibers / filaments, also often referred to as multifilament in the literature. The fiber bundle can optionally be given inherent reinforcement by twisting, which is then referred to as spun or folded filament. Alternatively, the fiber bundle can be given inherent reinforcement by entanglement using compressed air or water jets. Hereinafter, for all these embodiments, only the term "filament" will be used in a generalized manner. The filament can be textured or smooth and can have point reinforcement or no reinforcement.

[0140] A preferred material for the textile carrier is polyester, due to its excellent ageing resistance and excellent media resistance with respect to chemicals and working fluids such as oil, gasoline, antifreeze, etc. In addition, polyester has the advantage of resulting in a highly wear-resistant and temperature-stable carrier, which is particularly important for specific end uses in motor vehicles and, for example, cable bundling in the engine compartment. According to one embodiment of the invention, the carrier used is a PET nonwoven or a woven PET fabric.

[0141] The basis weight of the fabric carrier is advantageously 30 g / m 2 and 300g / m 2 between 50 g / m 2 and 200g / m 2 between 50 g / m 2 and 150g / m 2 between 70 g / m 2 and 130g / m 2 between.

[0142] According to a preferred embodiment of the invention, the adhesive has been absorbed into the carrier to an extent of more than 10%, preferably more than 25%, more preferably more than 50% after being applied to the carrier. For example, the value 25% here means that the adhesive has penetrated the thickness of the textile carrier by 25% of the layer thickness, i.e., in the case of a carrier with a thickness of 100 μm, has penetrated a layer thickness of 25 μm in the carrier (starting from the surface of the carrier on which the adhesive was applied and in a direction perpendicular to the planes generated by the longitudinal and transverse directions, respectively).

[0143] Likewise suitable for the adhesive tapes are carrier materials consisting of paper, laminates, films (eg PP, PE, PET, PA, PU), foams or foam films.

[0144] These non-textile sheet materials are particularly suitable when specific requirements require such modifications to the invention. For example, compared to textiles, the membranes are generally thinner and, due to the non-porous layer, offer additional protection against the penetration of chemicals and working fluids such as oil, gasoline, antifreeze, etc. into the actual cable area, and can be adapted to the requirements in principle by appropriate choice of the material constituting the membrane: for example, using polyurethane or polyolefin copolymers, flexible and elastic sheaths can be produced; using polyesters and polyamides, good abrasion resistance and temperature stability are achieved.

[0145] Foam or foamed film, on the other hand, has greater space-filling and good sound-insulating properties - where, for example, a length of cable is being laid in a duct- or tunnel-like area in a vehicle, a suitably thick and sound-insulating sheathing tape can prevent damaging flapping and vibrations from the outset.

[0146] Preferred is a laminate of a textile carrier and a polymer layer or film applied to at least one side of the textile carrier. In addition, the film and / or polymer layer can be applied to the top and bottom sides of the textile carrier. The application can be carried out by lamination or by extrusion.

[0147] In a preferred variant, the textile carrier is provided on its underside with a film which is provided on the other side with a pressure-sensitive adhesive.

[0148] Suitable materials for the film or polymeric material include films such as PP, PE, polyester, PA, PU or PVC. The film itself may in turn consist of a plurality of individual plies, for example plies that are coextruded to form the film.

[0149] Polyolefins are preferred, but also include copolymers of ethylene and polar monomers such as styrene, vinyl acetate, methyl methacrylate, butyl acrylate or acrylic acid. It can be a homopolymer such as HDPE, LDPE, MDPE or a copolymer of ethylene with another olefin such as propylene, butene, hexene or octene (e.g. LLDPE, VLDPE). Polypropylene (e.g. polypropylene homopolymer, random polypropylene copolymer or polypropylene block copolymer) is also suitable.

[0150] The film preferably has a thickness of 12 to 100 μm, more preferably 28 to 50 μm, more particularly 35 μm.The film may be coloured and / or transparent.

[0151] The adhesive tape may finally have a backing material with which one or both layers of adhesive are lined before use. Suitable backing materials also include all the materials described above in their entirety.

[0152] Preferably, a non-linting material is used, such as a polymer film or a long-fiber paper of suitable size.

[0153] If the adhesive tape described is to have low flammability, this quality can be achieved by adding flame retardants to the carrier and / or the adhesive. These flame retardants can be organic bromine compounds, if necessary, together with synergists such as antimony trioxide, although in view of the absence of halogens in the adhesive tape, it is preferred to use red phosphorus, organic phosphorus compounds, inorganic compounds or swelling compounds such as ammonium polyphosphate alone or in combination with synergists.

[0154] In a preferred embodiment, the adhesive tape is a single-sided tape, ie the adhesive is applied to one side of the carrier.

[0155] The adhesive coating weight is preferably between 40 and 160 g / m 2 Between, more preferably between 60 and 130 g / m 2 Between 80 and 100 g / m 2 Between, based on the tape area.

[0156] In the context of the present invention, the general expression "adhesive tape" covers all sheet-like structures, such as two-dimensionally extending sheets or sheet portions, tapes with extended length and limited width, tape portions etc., and finally also die-cuts or labels.

[0157] Thus, the adhesive tape has a longitudinal extent and a transverse extent. The adhesive tape also has a thickness extending perpendicularly to the two extents, wherein the transverse extent and the longitudinal extent are several times greater than the thickness. Over the entire surface extent of the adhesive tape defined by the length and the width, the thickness is very largely the same, preferably completely the same.

[0158] The adhesive tape is present in particular in the form of a sheet web. A sheet web is an article whose length is several times greater than its width, wherein the width is approximately the same and preferably identical along the entire length. The adhesive tape can be produced in the form of a roll, in other words wound onto itself in the form of an Archimedean spiral.

[0159] What is applied to the reverse side of the adhesive tape may be a reverse varnish, so as to exert a favorable influence on the unwinding performance of the adhesive tape wound into an Archimedean spiral. For this purpose, the reverse varnish may be equipped with silicone compounds or fluorosilicone compounds and polyethylene stearyl urethane, polyethyleneimine stearyl urea or organic fluorine compounds as anti-adhesion substances.

[0160] Functional layers such as films and / or polymer layers to be applied on the top and bottom side of the (textile) carrier or varnish layer are part of the carrier, these layers do not define further layers which are included in the term "carrier".

[0161] The adhesive may be applied in the form of a strip in the longitudinal direction of the adhesive tape, the width of the strip being less than the width of the carrier of the adhesive tape.

[0162] Depending on the specific application, there may also be a plurality of parallel strips of adhesive applied to the carrier material.

[0163] The position of the strip on the carrier is freely selectable, preference being given to an arrangement directly at one edge of the carrier.

[0164] The adhesive is preferably applied to the carrier over the entire area.

[0165] At least one strip of a covering may be provided on the adhesive coating of the carrier, which strip of covering extends in the longitudinal direction of the adhesive tape and covers 20% to 90% of the adhesive coating.

[0166] The strips preferably cover a total of 50% to 80% of the adhesive coating. The degree of coverage is selected depending on the application and the diameter of the cable harness. The percentage figures indicated relate to the width of the strips of the covering relative to the width of the carrier.

[0167] According to a preferred embodiment of the invention, there is exactly one strip of the covering on the adhesive coating.

[0168] The position of the strip on the adhesive coating is freely selectable and is preferably arranged directly at one of the longitudinal edges of the carrier. In this way, an adhesive strip is produced which extends in the longitudinal direction of the adhesive tape and ends at the other longitudinal edge of the carrier. In the case of using the adhesive tape for jacketing a cable harness (by guiding the adhesive tape in a spiral motion around the cable harness), the winding of the cable harness can be achieved by bonding the adhesive of the adhesive tape only to the adhesive tape itself, wherein the substrate is not in contact with any adhesive.

[0169] Since the cables are not fixed by any adhesive, the cable bundle sheathed in this way has a very high flexibility. Therefore, the flexibility of the cables during installation (especially in narrow passages or sharp bends) is significantly increased.

[0170] If it is necessary to fix the tape to the substrate to some extent, the sheathing can be done by bonding a portion of the adhesive strip to the tape itself and another portion to the substrate.

[0171] According to a further advantageous embodiment, the strip is applied centrally to the adhesive coating, whereby two adhesive strips are produced which extend in the longitudinal direction of the adhesive tape on the longitudinal edges of the carrier.

[0172] In order to apply the tape securely and economically in said spiral motion around the cable harness, and in order to counteract the slipping of the resulting protective wrap, two adhesive strips, each present on the longitudinal edge of the tape, are advantageous, especially if one strip (which is usually narrower than the second strip) serves as a fixing aid and the second, wider strip serves as a fastener. In this way, the tape is bonded to the cables in such a way that the cable harness is fixed against slipping but is flexible in design.

[0173] In addition, there are embodiments in which more than one strip of covering is applied on the adhesive coating. Where only one strip is mentioned, the skilled person conceptually reads it to accommodate the possibility that two or more strips covering the adhesive coating may also be present simultaneously.

[0174] The procedure for producing the adhesive tape of the invention involves only direct coating of the support with the dispersion in one or more operations performed in succession. In the case of a textile support, the untreated textile can be coated directly or by a transfer process. Alternatively, the textile can be pretreated with a coating (using any desired film-forming substance, cured from solution, dispersion, melt and / or radiation) and then provided with the PSA in a downstream operation directly or by a transfer process.

[0175] The application components used are the customary ones: wire blade, coating rod, roller application, nozzle coating, double-chamber blade, multi-stage cascade die.

[0176] The pressure-sensitive adhesive composition can be directly applied to the supporting substrate and dried to form a pressure-sensitive adhesive layer. Alternatively, the pressure-sensitive adhesive composition can be applied to a highly removable surface, such as the surface of a release liner, the back side of a supporting layer treated with reagents, and dried to form a PSA layer from the outward appearance, and the pressure-sensitive adhesive layer is transferred to the supporting substrate. The pressure-sensitive adhesive layer can be applied with any known method and a coating machine commonly used, such as a gravure coater, a reverse roll coater, a lick coater, a dip roll coater, a bar coater, a knife coater, a spray coater, a curtain coater, etc. Pressure-sensitive adhesive layer of the present invention is formed continuously usually. According to purpose and application, the pressure-sensitive adhesive layer can be formed with the rule or random pattern of a point, a strip, etc.

[0177] On the basis of the positive properties outlined, adhesive tapes can be significantly used for insulating and wrapping wires or cables.

[0178] Furthermore, it is advantageously suitable for the jacketing of elongated objects, more particularly cable harnesses in motor vehicles, wherein the adhesive tape is passed in a helical line around the elongated object or the elongated object is wrapped with the adhesive tape in an axial direction.

[0179] Finally, the concept of the invention also includes an elongated object sheathed with the adhesive tape of the invention. The elongated material is preferably a cable harness.

[0180] Due to the excellent suitability of the adhesive tape, it can be used in a sheath (sheath) which consists of a covering, in which at least in one edge region of the covering a self-adhesive tape is present and is bonded to the covering in such a way that the adhesive tape extends over one of the longitudinal edges of the covering and preferably in an edge region which is narrower than the width of the covering.

[0181] Such a product and its optimized embodiments are disclosed in EP 1 312 097 A1. EP 1 300 452 A2, DE 102 29 527 A1 and WO 2006 / 108871 A1 show further developments for which the adhesive tape according to the invention is also very suitable. The adhesive tape according to the invention can also find use in a method of the type disclosed by EP 1 367 608 A2.

[0182] Finally, EP 1 315 781 A1 and DE 103 29 994 A1 describe possible embodiments of adhesive tapes of the kind for the adhesive tape according to the invention.

[0183] The inventive concept also encompasses elongated objects, such as, in particular, cable harnesses, which are sheathed with the adhesive tape according to the invention, and vehicles which comprise elongated objects sheathed in this manner.

[0184] According to one embodiment of the invention, the elongated object is a cable run comprising a bundle of a plurality of cables, such as 3 to 1000 cables, preferably 10 to 500 cables, more particularly 50 to 300 cables. BRIEF DESCRIPTION OF THE DRAWINGS

[0185] The purpose of the following text is to explain the adhesive tape in more detail using a number of figures, without wishing to bring about any kind of limitation thereby.

[0186] Figure 1 Shows the tape in cross section,

[0187] Figure 2 A detail showing a cable harness consisting of a bundle of individual cables and sheathed with the adhesive tape of the invention, and

[0188] Figure 3 Displays beneficial applications of adhesive tape. DETAILED DESCRIPTION

[0189] The cross section (cross section) is shown in Figure 1 In FIG. 8 , there is an adhesive tape consisting of a woven textile carrier 1 , which on one side carries an applied self-adhesive coating 2 based on an acrylate dispersion.

[0190] The adhesive is already absorbed to an extent of 20% into the carrier, which results in an optimized anchoring and at the same time improves the manual tearability of the carrier.

[0191] Figure 2 A detail of a cable bundle consisting of a bundle of individual cables 7 and sheathed with the adhesive tape 11 of the invention is shown. The adhesive tape is passed in a spiral motion around the cable bundle.

[0192] The detail of the cable harness shown has two turns I and II of the tape. A further turn would extend to the left, but is not shown here.

[0193] In a further embodiment for sheathing, two tapes 60 , 70 according to the invention provided with adhesive are laminated with their adhesive offset to one another (preferably by 50% in each case) to produce a product.

[0194] Evaluation Criteria

[0195] The standard for compatible tapes used for cable wrapping applications is

[0196] Peel adhesion to backing according to LV 312

[0197] Anti-warping properties according to SWAT method and TFT method

[0198] Cable compatibility test procedure for cables with T2 PVC insulation in accordance with LV 312

[0199] Unless expressly stated otherwise, the measurements were carried out under test conditions of 23±1° C. and 50±5% relative humidity.

[0200] Measurement of peel adhesion to the backing according to LV 312

[0201] The peel adhesion to the backing ("KK backing") was measured according to LV 312. Values ​​<4 N / cm or >6 N / cm are unacceptable; values ​​of 4 to 6 N / cm are according to the invention.

[0202] Measurement of warping resistance according to the SWAT method

[0203] The SWAT test was used to study the lift behavior of the tape after it was spirally wrapped around the cable.

[0204] The tests were carried out under standard conditions (23±1° C. and 50±5% relative humidity) and at 40° C. The elevated temperature simulates the intensified demands during transport.

[0205] The test used a 19 mm wide tape. It was manually wrapped four times (1440°) around a cable with an ETFE (ethylene-tetrafluoroethylene) jacket and a diameter of 1 mm without additional pressure. Scissors were used to cut the tape.

[0206] Unless the end of the tape is pressed down, an average lift of 5 mm is assumed to remain.

[0207] A total of seven wraps (seven total wraps) are created around the cable.

[0208] The warping was measured with a ruler after three, ten and 30 days under standard conditions. Figure 8 The absolute warp value was calculated by subtracting 5 mm from the actual measured warp length.

[0209] Therefore, in Figure 8 In the middle, the warping value is 23mm (28mm-5mm).

[0210] The warping value reported as result is the result of the average warping value of seven wraps.The test at 40°C was similarly carried out in a conventional drying oven.

[0211] The adhesive tapes according to the invention were evaluated below at 40° C. in a drying cabinet by the specified SWAT method.

[0212] Here, values ​​<10 mm are regarded as the lower limit for the warping resistance.

[0213] A mean value <5 mm was assigned 2 points, a mean value between 5 and 10 mm was assigned 1 point, and a mean value >10 mm was assigned 0 points.

[0214] Measurement of warping resistance according to LV 312 or TFT method (threshold warping time)

[0215] In order to determine the warping behavior by the TFT method, the following test was used, in which a test specimen prepared in flat form was applied to a 1 1 / 2" core and generate additional bending stress. The combination of tensile load and bending stress generated by the test weight causes the tape to separate from the upper end of the bond and cause the test specimen to fall and eventually fail (see Figure 4 , which also shows a schematic construction).

[0216] The time (minutes) before the drop is the result.

[0217] The key parameters for the holding time of the test specimens are weight and temperature, the weight being chosen to give a value of at least 100 minutes.

[0218] The cylindrical test mandrel is 1 1 / 2" card core, with an outer diameter of 42±2mm and a marking line 5mm adjacent to the apex line.

[0219] The adhesive base is the opposite side of the tape itself.

[0220] The hand roller has a weight of 2 kg.

[0221] The test weight is 1 kg.

[0222] The test conditions are 23±1°C and 50±5% relative humidity, or 40°C in a heating cabinet.

[0223] The test is performed on a 19 mm wide strip of tape. A strip of 400 mm in length is adhered to the release paper and cut to form 3 strips of 100 mm each. This should be done with a new cutter blade. The opposite side must not be touched.

[0224] A small piece of card was adhered under one of the ends of each strip and the assembly was perforated (see Figure 5 ).

[0225] The test strips were then individually bonded centrally to a wider strip of adhesive substrate (1 / 3 the width of the tape under test). 1 / 2 times the tape) so that the small pieces of card still just overlap at the ends (2 to 3 mm) (see Figure 6 ).

[0226] The specimen was rolled using a 2 kg hand roller at a rate of 10 m / min in 3 cycles.

[0227] The finished test sample, in other words the test strip together with the adhesive substrate, is then adhered to the core in such a way that the upper end of the test specimen overlaps the apex by 5 mm (see Figure 7 ). In this operation, pressure must be applied only to the bonding substrate and not to the test specimen.

[0228] The fully prepared test specimens are placed without weight loading in a controlled climate chamber at 40°C for 20 ± 4 hours.

[0229] A weight of 1 kg is then hung on the sample and a stopwatch is started.

[0230] The measurement ends after all three test specimens of one sample have failed.

[0231] The average of three separate measurements is reported in minutes.

[0232] The hold time is reported in minutes.

[0233] In this case, TFT values ​​of >1200 min are regarded as the lower limit with regard to the warping resistance.

[0234] Values ​​below this value received 0 points, values ​​from ≥ 1200 to 2000 minutes received 1 point, and values ​​above 2000 minutes received 2 points. These ratings reflect the increased safety against warping.

[0235] Measurement of cable compatibility of cables with T2-PVC insulation according to LV 312 ("CC")

[0236] The measurement was carried out in accordance with the measurement method specified in LV 312. The measurement was carried out in each case at 105° C. (T2).

[0237] Brittleness and discoloration

[0238] If there is no embrittlement after 3000 hours of bending at 105°C around a mandrel with a diameter of 2 mm and at the same time no discoloration or edge discoloration after 3000 hours at 105°C, cable compatibility is considered to exist and a score of "2" is given.

[0239] Clearly visible discoloration (without embrittlement), but not too dark, may be classified as sufficiently compatible and receive a score of "1".

[0240] If the sample experienced embrittlement and / or a black or dark brown discoloration was visible (the original color was no longer visible), the specimen received a score of "0".

[0241] Dynamic Mechanical Analysis (DMA)

[0242] The viscoelastic properties of the examples were characterized by dynamic mechanical analysis (DMA) on a dynamic mechanical analyzer MCR 302e equipped with a Peltier temperature controlled lower plate (P-PTD 200, 56 mm in diameter) and a Peltier hood (H-PTD 200) for good temperature control (both commercially available from Anton Paar Group AG (Austria)). The samples were prepared by diluting the dispersion to 40% solids content and placing such a large amount of the dispersion in a 30 mm diameter disk-shaped silicone mold that a film thickness of 0.6 mm to 0.8 mm was obtained after drying for two days under ambient conditions (20° C. to 25° C.). Film formation was completed by heating the dried sample in an oven at 80° C. for 5 hours and conditioning for another 24 hours under standard climatic conditions (temperature of 23±1° C. and controlled relative humidity of 50±5%). A 15 mm diameter disk was punched out of the sample film and placed between the 15 mm diameter parallel plates of the upper plate, taking care to ensure full contact between the specimen and the plates. A temperature scan with a heating rate of 2 K / min was recorded starting from -40 °C up to 130 °C at a constant angular frequency of 10 rad / s, at a constant normal force of 1 N and a logarithmic deformation slope from 0.02 to 2%.

[0243] Peel Adhesion Measured According to ASTM D3330

[0244] To measure the peel adhesion of the pure dispersion, a coated sample of the adhesive was first prepared. For this purpose, the dispersion was applied to a PET film (polyethylene terephthalate) with a thickness of 23 μm and stretched using a film stretching device so that after drying at 105° C. for 5 minutes in a forced air drying cabinet, the adhesive coating weight was 30 g / m 2 .

[0245] Using a cutting knife, strips 20 mm wide and 25 cm long were cut from the sheet.

[0246] The bond strength to steel was measured according to ASTM D3330.

[0247] Measurement of glass transition temperature

[0248] The glass transition temperature was determined on a DSC 204F1 "Phonix" dynamic differential calorimeter from Netzsch, Germany, in a 25 μL aluminum crucible with a perforated cover under a nitrogen atmosphere (20 ml / min gas flow rate). The initial sample mass was 8.1 mg. The sample was subjected to two measurements from -140° C. to 200° C. with a heating rate of 10 K / min. The subject of the analysis was the second heating curve.

[0249] The method is based on DIN 53765.

[0250] Example

[0251] Embodiment Overview

[0252] The adhesive tape of the invention is described below by way of examples in preferred embodiments, without any intention that the invention should be restricted thereby.

[0253] Furthermore, comparative examples are given which show unsuitable adhesive tapes.

[0254] To illustrate the invention, example tapes were produced according to the following protocol:

[0255] Preparation of dispersion polymers for pressure-sensitive adhesives

[0256] The pressure sensitive adhesive dispersion polymer was prepared by a free radical emulsion polymerization process combining initial reactor charge and two reactant feeds. A double walled 6 liter glass reactor connected to a cryostat capable of controlling temperature and equipped with a blade stirrer was charged with 800 g of deionized water and 40 g of a polymethyl methacrylate seed dispersion having a solid content of 20 wt% and an average particle size of 30 nm.

[0257] A monomer pre-emulsion consisting of 2.76 kg of reactants (according to Table 1.1, Table 2.1 and Table 3.1), 22.8 g of anionic surfactant (C13-C15 alkyl aryl sulfonate) and 1.2 kg of deionized water was prepared and treated with a dissolver disk for 5 min to obtain a uniform monomer emulsion. In addition, an initiator solution was prepared by dissolving 8 g of sodium persulfate in 72 g of deionized water.

[0258] After heating the initial charge to 85° C. under stirring, the monomer pre-emulsion and the initiator solution were fed continuously into the reactor over 4 hours. The reaction temperature was kept constantly at 85° C. The monomer feed port was finally rinsed with 50 g of water. The batch was stirred for another 30 min and then cooled to 60° C. For post-activation, 2.5 g of a 5 wt % solution of isoascorbic acid were fed into the batch over 1 hour and a first shot of 1.1 g of a 10 wt % solution of tert-butyl hydroperoxide was added at the start of the isoascorbic acid feed and a second shot was added 30 minutes later.

[0259] The batch was then cooled to ambient temperature (20-25° C.), neutralized to pH 7.5 with 10 wt. % sodium hydroxide solution and sieved through a 100 μm filter cloth.

[0260] Preparation of pressure sensitive adhesive formulations

[0261] If applicable, a tackifier resin (Snowtack 100G ('ST100G'), Lawter) was mixed into the PSA dispersion in the amounts given in Table 1.1, Table 2.1 and Table 3.1. The PSA dispersion was then adjusted to a 10 s thickener within 10 s by stirring in a hydrophobically modified alkali swellable emulsion (HASE) associative thickener (RHEOBYK-HV 80, BYK-Chemie GmbH). -1 15 Pa*s at a shear rate of 1.50 g (measured using an R180 viscometer (proRheo GmbH) in rotational mode using coaxial cylinder geometry).

[0262] Coating of pressure sensitive adhesive formulations

[0263] Using a film stretching apparatus, a woven polyester fabric (linear fiber density 167 dtex, warp thread count (end count) 43 1 / cm, weft thread count (fill count) 25 1 / cm) was coated with the thickened Example PSA dispersion to give an adhesive coating weight of 90 g / m after drying in a forced air oven at 105° C. for 5 minutes. 2 .

[0264]

[0265]

[0266]

[0267]

[0268]

[0269]

[0270]

[0271] The examples show that by using small amounts of chain transfer agents, good SWAT and TFT performance can be achieved.

[0272] At the same time, good compatibility with PVC cables is maintained. When the assembly consisting of cable and adhesive tape is stored at temperatures above 105° C. for up to 3000 hours in accordance with LV 312 and the cable is then bent around a mandrel, the adhesive tape does not damage the cable with the PVC sheath. The adhesive tape according to the invention shows neither embrittlement of the cable nor strong discoloration within 3000 hours at 105° C.

[0273] Furthermore, despite low tackifier concentrations in the adhesive or even no tackifier added at all, high peel adhesion to the backing and moderately high unwinding forces can be achieved, which are essential for compactness of the wrap (wrap) during harness production.

Claims

1. An adhesive tape, in particular an adhesive tape for wrapping cables, comprising, preferably consisting of, a preferably textile carrier, optionally provided on the bottom side with an applied film, and a pressure-sensitive adhesive, the pressure-sensitive adhesive being applied on at least one side of the carrier in the form of a dry polymer dispersion, the polymer being obtained by emulsion polymerization of a monomer mixture comprising: (a) 80.75 to 94.89 wt. %, preferably 83.85 to 93.73 wt. % of one or more (meth)acrylic monomers which individually produce a glass transition temperature (T) of -40°C or less. g ) (b) 5.00 to 14.00 wt. %, preferably 6.00 to 12.00 wt. %, of one or more ethylenically unsaturated monomers which individually produce a T of 15° C. or more. g Homopolymer (c) 0.10 to 5.00 wt. %, preferably 0.20 to 4.00 wt. %, of one or more ethylenically unsaturated monomers having acid and / or hydroxyl functionality (d) 0.01 to 0.25 wt%, preferably 0.07 to 0.15 wt% of a chain transfer agent wherein monomers (a) to (d) are different from each other and the weight percentages are based on the total amount of monomers in the monomer mixture, wherein the pressure-sensitive adhesive dispersion polymer has a tan delta maximum value in the temperature range between -25°C and -15°C, and having a tan δ value between 0.38 and 0.55 at 130° C., wherein tan δ is determined by dynamic mechanical analysis (DMA) using a parallel plate tool at an angular frequency of 10 rad / s, And the pressure-sensitive adhesive includes 0.00 to 10.00, preferably 2.00 to 7.50 parts by weight of a tackifier (relative to 100 parts by weight of the pressure-sensitive adhesive dispersion polymer).

2. The adhesive tape according to claim 1, It is characterized in that The one or more than one (meth)acrylic monomers (a) are selected from 2-ethylhexyl acrylate, n-butyl acrylate, 3-methylbutyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, nonyl acrylate, propyl acrylate, propylheptyl acrylate, heptadecyl acrylate, decyl methacrylate, dodecyl methacrylate, isodecyl methacrylate, octyl methacrylate, lauryl methacrylate, 2-methoxyethyl acrylate, 3-methoxypropyl acrylate, 3-ethoxypropyl acrylate, 3-methoxybutyl acrylate, hydroxybutyl acrylate, hydroxyethyl caprolactone acrylate and combinations thereof, preferably selected from 2-ethylhexyl acrylate, n-butyl acrylate and combinations thereof, more preferably n-butyl acrylate.

3. The adhesive tape according to any one of claims 1 and 2, It is characterized in that The one or more than one ethylenically unsaturated monomers (b) are selected from acrylonitrile, 3,3,5-trimethylcyclohexyl acrylate, cyclohexyl acrylate, isobornyl acrylate, octadecyl acrylate, tert-butyl acrylate, 2-phenylethyl methacrylate, benzyl methacrylate, n-butyl methacrylate, cyclohexyl methacrylate, ethyl methacrylate, glycidyl methacrylate, hexadecyl methacrylate, isobornyl methacrylate, isobutyl methacrylate, isopropyl methacrylate, methyl methacrylate, neopentyl methacrylate, octadecyl methacrylate, propyl methacrylate, tert-butyl methacrylate, styrene, methoxystyrene, 2-methylstyrene, 3-methylstyrene, 4-ethylstyrene, 4-isopropylstyrene, 4-methoxy-2-methylstyrene, 4-methoxystyrene, 4-methylstyrene, 2-chlorostyrene, 4-bromostyrene, 4-chlorostyrene, 4-fluorostyrene and combinations thereof, preferably selected from methyl methacrylate, n-butyl methacrylate, styrene and combinations thereof, more preferably methyl methacrylate.

4. The adhesive tape according to claim 1, It is characterized in that The one or more than one ethylenically unsaturated monomers (c) having an acid functional group are selected from ethylenically unsaturated carboxylic acid monomers, ethylenically unsaturated sulfonic acid monomers, ethylenically unsaturated phosphorus-containing acid monomers, preferably selected from (meth)acrylic acid, crotonic acid, fumaric acid, itaconic acid, maleic acid, maleic anhydride, vinyl acetic acid, vinyl lactic acid, vinyl sulfonic acid, styrene sulfonic acid, 2-carboxyethyl (meth)acrylate, vinyl sulfonic acid, vinyl sulfonic acid phenyl ester, sodium 4-vinylbenzenesulfonate, 2-methyl-2-propylene-1-sulfonic acid, 4-styrenesulfonic acid, 2-acrylamido-2-methyl-1-propanesulfonic acid, vinylphosphonic acid, dimethyl vinylphosphonate, diethyl vinylphosphonate, diethyl allylphosphonate, allylphosphonic acid and combinations thereof, more preferably selected from (meth)acrylic acid.

5. The adhesive tape according to at least one of claims 1 to 3, It is characterized in that The one or more than one ethylenically unsaturated monomers (c) having a hydroxyl functional group are selected from allyl alcohol, vinyl alcohol, N-hydroxymethyl acrylamide, 1-penten-3-ol, hydroxyalkyl esters of ethylenically unsaturated acids such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyethyl caprolactone acrylate and combinations thereof, preferably hydroxyalkyl esters of ethylenically unsaturated acids such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyethyl caprolactone acrylate, more preferably hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate and combinations thereof, more preferably hydroxyethyl methacrylate.

6. Adhesive tape according to at least one of the preceding claims, It is characterized in that The chain transfer agent (d) is selected from n-dodecyl mercaptan, carbon tetrachloride, carbon tetrabromide, bromotrichloromethane, 4-methylbenzenethiol, isooctyl 3-mercaptopropionate, tert-nonyl mercaptan, 4,4'-thiobisbenzenethiol, tert-dodecyl mercaptan, α-methylstyrene dimer, thioglycolic acid, 2-ethylhexyl thioglycolate, butyl 3-mercaptopropionate, 1,8-dimercapto-3,6-dioxaoctane and combinations thereof, preferably n-dodecyl mercaptan.

7. Adhesive tape according to at least one of the preceding claims, It is characterized in that The composition of the polymer is as follows: (a) 80.75 to 94.89% by weight, preferably 83.85 to 93.73% by weight, of n-butyl acrylate (b) 5.00 to 14.00 wt %, preferably 6.00 to 12.00 wt % of methyl methacrylate (c) 0.10 to 5.00 wt. %, preferably 0.20 to 4.00 wt. % of acrylic acid and methacrylate (hydroxyethyl) (d) 0.01 to 0.25 wt. %, preferably 0.07 to 0.15 wt. % of a chain transfer agent, such as n-dodecyl mercaptan.

8. Adhesive tape according to at least one of the preceding claims, It is characterized in that (For 30 g / m on 23 μm polyester film support 2 The pressure sensitive adhesive has a peel adhesion on steel of at least 2.0 N / cm according to ASTM D3330.

9. Adhesive tape according to at least one of the preceding claims, It is characterized in that The carrier is a textile carrier, preferably a nonwoven material or a woven fabric, more particularly a woven polyester fabric.

10. The adhesive tape according to at least one of the preceding claims, It is characterized in that The carrier is a woven fabric, preferably a woven polyester fabric, and more preferably has the following construction: The number of threads in the warp is 10 to 60 / cm The number of threads in the weft yarn is 10 to 40 / cm The warp yarns have a yarn weight between 40 and 400 dtex, more particularly between 44 and 330 dtex, very preferably 167 dtex The weft threads have a yarn weight of between 40 and 660 dtex, more preferably between 44 and 400 dtex, very preferably 167 dtex.

11. The adhesive tape according to claim 9, It is characterized in that The textile carrier, preferably a nonwoven, is already provided on the bottom side with an applied film (film between textile carrier and adhesive).

12. Use of the adhesive tape according to at least one of the preceding claims for covering an elongated object, the adhesive tape being guided in a helical line around the elongated object.

13. Use of an adhesive tape according to at least one of the preceding claims for sheathing elongated objects, the elongated objects being sheathed by the tape in the axial direction.

14. Elongated objects, such as, in particular, cable harnesses, sheathed with an adhesive tape according to at least one of the preceding claims.

15. A vehicle comprising a sheathed elongate article according to claim 14.

Citation Information

Patent Citations

  • Method for sheathing elongated goods such as, in particular, cables or cable sets

    DE102013213726A1

  • Band of row of sequential overlapping casing sections for elongated material, e.g. cable sets, has preferably textile covering, narrow self-adhesive band extending over longitudinal edge of covering

    DE10229527A1

  • Process for encapsulating cables with an adhesive strip comprises applying strips of adhesive material to a support material so that the support material does not adhere to the longitudinal edges

    DE10329994A1

  • Mat-like laminated article and method of producing the same

    EP0071212B1

  • Method for sheathing longitudinally extended products

    EP1300452A2