Sealing gasket for crown cap with reduced sheet metal hardness

Through halogen-free polymer composite materials and optimized tin-white molding process, the health hazards and sealing performance of halogen-containing materials are solved, and a high-sealing and cost-effective container closure is achieved, suitable for high-demand crown covers application.

CN119095929APending Publication Date: 2024-12-06ACTEGA DS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035628.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-12
Filing Date
2023-05-02
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, halogen-containing materials used for container closures have health hazards and legal constraints, and in crown covers made of thinner metal plates, the sealing performance is degraded, making it difficult to meet the high-demand sealing and cost-effectiveness requirements. .

Method used

Use halogen-free polymer composite materials as sealing gaskets to produce disc-shaped or annular sealing gaskets through in-shell molding processes, and combine with the optimized tin-shaped molding process to improve the hardness and elasticity of the seals to accommodate thinner metals Use of plates and optimize material properties through additives to improve sealing performance.

Benefits of technology

Achieves improved sealing performance and cost-effectiveness of container closures without halogen, especially in thinner metal plate crown caps, which ensure high sealing and internal pressure resistance. It is suitable for bulk-made containers such as beer bottles wait.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095929A_ABST
    Figure CN119095929A_ABST
Patent Text Reader

Abstract

A crown cap for a container for containing beverages and foodstuffs, the container having an access opening to be closed by means of the crown cap, the crown cap having a sealing gasket arranged in the crown cap such that the sealing gasket sealingly closes the access opening when the crown cap is placed at the container, wherein the crown cap together with the sealing gasket does not comprise a halogen-containing material, the metal plate used by the crown cap has a thickness of 0.10 mm to 0.19 mm, and the sealing gasket comprises at least 20% by weight, based on the total weight of the sealing gasket, of at least one preferably fully hydrogenated styrene triblock copolymer, in particular a styrene-ethylene-butylene-styrene copolymer (SEBS), SEEPS and / or SEPS, or a mixture of a plurality of said copolymers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention generally relates to a container closure, in particular a crown cap, made of metal and / or plastic, with a polymer-based sealing liner for bottles or other containers for beverages and foods. In particular, the invention relates to a container closure, in particular a crown cap, which is provided with a sealing liner. The container closure does not contain halogen-containing substances and is also suitable for demanding use, in particular in crown caps with reduced sheet metal thickness. Background Art

[0002] Beverages and foods are filled in different types of containers for transport and storage or preservation. Usually, these containers must be closable so that the contents do not flow out and also prevent the entry of unwanted substances that could contaminate or damage the contents. In many applications, this involves not only solid or liquid contaminants. If the contents are sensitive to gaseous substances, the entry of these gaseous substances must also be prevented. This is caused by correspondingly designed container closures.

[0003] Container closures made of metal and / or plastic have long been known. For example, they are used in the form of screw closures, twist closures and crown caps for sealing containers such as bottles, jars and the like. Such containers have an access opening that must be sealed by the container closure. In this case, a sufficiently tight closure of the container must be ensured in order to prevent the container contents from flowing out and, on the other hand, to protect the container contents from the ingress of undesirable materials, including gaseous substances such as oxygen, trichloroanisole and the like.

[0004] The necessary tightness is usually achieved by a sealing liner which consists of a material which is on the one hand sufficiently strong but on the other hand also elastic and is arranged in the container closure in such a way that it contacts the access opening of the container when the container closure is arranged on the container. The sealing liner is usually arranged in a disc-shaped or annular manner on the inner side of the container closure. In the closed state of the container, the sealing liner rests on the container access opening and is pressed against the access opening by the container closure, wherein the hardness of the sealing liner together with its elasticity brings about a seal. A good sealing liner hereby compensates for the unevenness of the container access opening which is always present. Therefore, the more uneven the container access opening is, the higher the requirements placed on the sealing liner.

[0005] A major factor in meeting such requirements is the appropriate selection of the material of the sealing gasket. A large number of known materials are well suited for relatively simple applications, but are less or not at all suitable for more demanding seals.

[0006] The sealing liner must also meet other requirements here, so it should be pasteurizable or even sterilizable for various purposes of use. It should withstand significant internal pressures (for example in carbonated beverages) but yield in a controlled manner when the internal pressure is exceeded (overpressure valve action).

[0007] If the container closure is a twist closure (for example a twist crown, also known as a “twist crown”), the sealing liner does not have to resist the twisting of the container closure on the access opening with excessive resistance during opening.

[0008] Furthermore, the sealing liner must be able to be produced and inserted into the container closure as inexpensively as possible. It is known to cut a disk-shaped sealing liner out of a web or film and then fasten it into the container closure ("out-shell molding") or to introduce it into the container closure, where it is shaped and cured ("in-shell molding"). In-shell molding also allows the production of sealing liners that are not disk-shaped but rather annular.

[0009] In polymer-based sealing liners, this conventionally takes place by introduction as a plastisol with subsequent shaping and drying, or in thermoplastic materials by introduction in a heated, flowable state with subsequent shaping and cooling.

[0010] Previously, PVC-containing sealing liners were widely used, but PVC and other halogen-containing materials are now causing great concern. They are considered to be potentially harmful to health and are not easy to remove. In many countries, the use of such halogen-containing materials is restricted or even prohibited by law or regulations.

[0011] Therefore, there is a significant need for container closures that are also capable of being made of halogen-free materials without having to give up the advantages that sealing liners containing PVC, for example, have in terms of processing, sealing properties, cost, etc.

[0012] To this end, various proposals have been made in the prior art.

[0013] Thus, it has been known for decades to produce sealing liners based on halogen-free polymers (both for twist-off closures and for pry-open closures such as conventional crown caps). These sealing liners are always "composite materials", i.e. a mixture of one or (mostly) several polymers with additives which adapt the properties of the sealing liners to the intended purpose of use, simplify their processing or use, etc.

[0014] Typical polymers in composite materials are thermoplastics, especially polyolefins, thermoplastic elastomers, elastomeric thermoplastics and synthetic rubbers. Typical additives are plasticizers, oils, lubricants, antioxidants, stabilizers, pigments, fillers, etc.

[0015] Polymer-based sealing liners have varying degrees of permeability to foreign matter, depending on the choice of their components. If the sealing liners do not rest optimally on the access opening, such foreign matter can, for example, pass between the sealing liners and the access opening. They can also dissolve in the material of the sealing liners and diffuse into the container. Therefore, the mechanical properties (especially hardness and elasticity) and the chemical properties (solubility of foreign matter) of the sealing liners must be optimized.

[0016] It is known to add one or more substances to the material of the sealing liner which chemically bind the incoming oxygen and thus "capture" it - hence also called "scavengers". An example of this is sodium sulfite, which is incorporated into the sealing liner in the form of solid particles of a suitable particle size.

[0017] However, there is still a need for sealing gaskets which do not contain halogen-containing materials and which can improve the sealing effect particularly in problematic and demanding applications, in particular in the applications which will be explained in more detail below by way of example:

[0018] A more specific problem that can be solved by means of the invention arises in the case of container closures that can be pried open or twisted open, in particular crown caps.

[0019] The containers that are common here, usually beer bottles and bottles for carbonated soft drinks and mineral water, are mass-produced products whose quality in the access area varies in terms of unevenness, microcracks, etc. Beverages such as beer, soft drinks and mineral water are very sensitive to taste changes, which can be caused by oxidation after the ingress of oxygen and / or by the ingress of taste-changing substances such as trichloroanisole.

[0020] However, the storage time is usually short.

[0021] Sealing gaskets exist in the prior art which ensure an adequate seal in conventional crown caps.

[0022] However, there is an increasing demand from manufacturers to use thinner tinplate for such crown caps.

[0023] In Europe, conventional crown corks have a sheet metal thickness of 0.20 mm to 0.23 mm, whereas there is a desire to work with sheet metal thicknesses of 0.19 mm and below (up to 0.15 mm) in order to save material.

[0024] However, a crown cap made of thinner tinplate with the same yield limit cannot reliably press the sealing gasket inserted into the crown cap toward the container access opening with the same force as a conventional crown cap made of thicker metal plate. A reduction in the thickness of the tinplate leads to an overall decrease in sealing performance (resistance to internal pressure).

[0025] This effect can be counteracted on the one hand by using seals which are optimized with regard to hardness and elasticity or mechanically improved tinplates with a higher yield point.

[0026] A seal with an optimized ratio of hardness and elasticity is only one important component in order to be able to use thinner tinplate for the crown cork. In addition, tinplate with a higher yield strength should be used.

[0027] For standard crown corks, tinplate alloys with a maximum yield strength of 415 MPa are used, while for crown corks with a thickness of 0.18 mm, tinplate with a yield strength of 415 MPa to 620 MPa should be used, and for crown corks with a thickness of 0.15 mm, tinplate with a yield strength>620 MPa should be used.

[0028] The maximum possible yield strength or stiffness of the tinplate is determined by the forming process during the deep drawing of the crown corks.

[0029] In order to achieve an optimal ratio of tensile strength to strength, thinner (<0.20 mm) tinplate is preferably produced by means of the "double reduction" method, otherwise the risk of damage (premature cracking) during the forming of the crown cap increases significantly.

[0030] For the production of packaging steel, in particular tinplate, so-called hot-rolled strip having a thickness of approximately 1.5 mm to 4.0 mm is used in the process.

[0031] First, the hot rolled strip is pickled and then cold rolled.

[0032] The first thickness reduction of the tinplate takes place during cold rolling.

[0033] In order to be able to achieve high deformations due to thickness reduction, the nip is lubricated with a mixture of water and rolling oil.

[0034] The tinplate must also be cooled with water because the rolling process generates heat.

[0035] The cold work hardening must then be eliminated by an annealing process, since the strong thickness reduction makes the tinplate very hard and brittle and thus may not be suitable as a packaging material. However, before annealing can be carried out, the cold-rolled tinplate must be degreased.

[0036] Annealing of tinplate ensures restoration of its deformability.

[0037] The thickness of the tinplate is then further reduced by dry re-rolling without any lubrication or cooling.

[0038] The "double-reduced" material thus produced enables the production of tinplates whose greater strength compensates for their smaller thickness. The tinplates are then tinned or chromed for corrosion protection purposes until they are finally adjusted to different packaging sizes.

[0039] Tinplate for packaging steel and crown caps produced therefrom are specified in accordance with DIN EN 10202 or EN 17177.

[0040] That is, there is a need for improved container closures. Summary of the invention

[0041] The object of the present invention is to create an improved closure which can be used not only generally but also for the particularly demanding applications discussed here.

[0042] Against this background, an important object of the present invention is to provide an improved crown cork with a sealing liner which does not contain halogen-containing materials and which can be designed both as a twist-off closure and as a pry-open closure and which can be produced more simply and thus more cost-effectively.

[0043] Another important object of the invention is to create such a crown cap with improved tightness, in particular with respect to outflow, even in the case of mass-produced containers such as beer bottles or the like.

[0044] The good barrier effect of the known sealing gaskets should be retained here.

[0045] The objects of the present invention consist in realizing such a container closure having a sealing liner which can be produced by means of shell in-molding.

[0046] The sealing liner should be designed to be very soft in order to be able to reliably seal the bottle even in the event of microcracks and similar access defects.

[0047] Other objects and advantages of the present invention are obtained from the following description including the embodiments.

[0048] The invention achieves these and other objects with the feature combination of the independent claims.

[0049] Advantageous embodiments are defined in the dependent claims.

[0050] In the following detailed description of the present invention, the following definitions and features are discussed first, which are independent of the various embodiments that are generally significant for the present invention and its optional design solutions. The definitions given above should be considered and do not contradict the following embodiments. Unless otherwise specified in the specification, technical terms have their usual meanings.

[0051] Next, the present invention is explained according to various embodiments.

[0052] Definition and measurement:

[0053] The container closures for the purposes of this application are crown caps, which are preferably designed as conventional crown caps to be pried open or as twist crown caps of conventional size. The crown caps are formed by a body made of metal and / or plastic and a sealing liner arranged therein. The container closures can be twist closures (with threaded elements including bumps etc.) or closures that can be removed (without twisting the container closure) and then usually pried open ("pry-off" closures), including crown caps, snap caps etc. A stopper is not a container closure in this respect.

[0054] The sealing gasket according to the invention is in principle a disk-shaped or annular (optionally contoured) shaped part which either consists entirely of a homogeneous polymer composite material or comprises at least two different, respectively homogeneous materials, at least one of which is a homogeneous polymer composite material.

[0055] "In-shell forming" is understood not only as the known method in which a heat-flowable polymer composite is introduced into the body of the closure and imprinted there into a disc-shaped sealing gasket (SACMI method or Zapata method), but also as the following method in which the polymer composite is introduced by injection (optionally only in the edge area of ​​the sealing surface) and formed into an annular sealing gasket.

[0056] The polymer composite material for the purposes of the present invention is a mixture of one or (in most cases) more polymers with additives (such as plasticizers, anti-blocking agents, lubricants, antioxidants, stabilizers, fillers, pigments, etc.), which additives adapt the properties of the composite material to the intended use and simplify the processing or use of the composite material.

[0057] Thermoplastic elastomers are industrially produced polymers having elastic properties which are based on the molecular structure. Typical thermoplastic elastomers are (block) copolymers of styrene and butadiene, with the addition of other monomers (ethylene, isoprene, ...).

[0058] The percentage statements in this context are percentages by weight, based on the total weight, as long as the percentage statement relates to the share of an ingredient in a product composed of a plurality of ingredients.

[0059] The melt flow rate (MFR) describes the flowability of a substance or substance mixture at 190° C. and a weight load of 5 kg. The melt flow rate is determined in accordance with DIN EN ISO 1133-1 and is specified in g / 10 min and is determined using a customary commercial melt indexer, such as the one from ZwickRoell.

[0060] The Shore hardness D specifies the hardness of a substance or a mixture of substances. The Shore hardness D is determined according to ASTM D2240 at a press plate at least 6 mm thick. The measuring time is 5 s. The corresponding specimens are produced at 180° C. by melting under pressure and subsequently cooling to 23° C. (maintenance time 30 minutes).

[0061] The Shore hardness A is determined analogously to the Shore hardness D in accordance with ASTM D 2240. Here too, the measuring time is 5 s.

[0062] The compression set test ("compression set", DVR) is a measure of the resetting behavior (permanent deformation) of a substance or a mixture of substances. The samples are manufactured similarly to the samples for Shore hardness measurement at temperatures between 170°C and 230°C. The samples have a diameter of 13 mm and a thickness of 6.3 mm. The measurement tolerances correspond to DIN ISO 815-1. The relevant samples are adjusted and siliconized according to the same standard. In the DVR, the corresponding samples are subjected to a compression of 25% within 22 hours at the respectively given temperature. After the load duration of 22 hours, the samples are released and the thickness of the samples is remeasured or the permanent deformation is determined after 30 minutes. The thickness or permanent deformation of the samples is also measured according to DIN ISO 815-1 at the respectively given temperatures after more than 22 hours of load and is stated as a percentage of the permanent compression according to the sample before compression.

[0063] That is, a DVR of 25% corresponds to a permanent "compression" of the sample by one-quarter of the original height (thickness).

[0064] A composite material is processable for the purposes of the present invention if it is processable in a conventional manner on general facilities for producing container closures having polymer-based sealing liners.

[0065] A material according to the invention is pasteurizable if it allows a gas-tight seal at 60° C. to 85° C. during industrial pasteurization without losing its usability properties for the intended application.

[0066] For the closure test also with the crown cap according to the invention, the following parameters were selected:

[0067] The bottle access opening consists of glass according to DIN EN ISO 12821CC 26H180.

[0068] The closing rings have corresponding inner diameters of 28.25 mm and 28.3 mm (if the steel through-port is taken into account).

[0069] The closing force was 300 kg. The closing speed was 15 mm / s. Pasteurization was carried out at 68° C. in a spray pasteurizer for 20 minutes (hold time). BRIEF DESCRIPTION OF THE DRAWINGS

[0070] The attached figure gives an overview of the experiments performed and their results:

[0071] Figure 1 An overview of the parameters of the sealing compound and crown cap blank used is shown.

[0072] Figure 2 The closure technique used is shown schematically.

[0073] Figure 3 Shown is the pressure checking equipment used.

[0074] Figure 4 The results of closure tests with different sealing composites are shown.

[0075] Figure 5 Shows similar Figure 4 result.

[0076] Figure 6 The results of a test on the side impact resistance are shown.

[0077] Figure 7 The results are shown for the tightness of different crown corks, only material C being according to the invention.

[0078] Figure 8 Shows in detail similar Figure 7 result.

[0079] Fig. 9 is an overview of the research findings.

[0080] Fig.10 The results for internal pressure resistance in different materials are shown. DETAILED DESCRIPTION

[0081] It has been shown that the crown cap according to the invention is superior in its technical properties to crown caps having a lower SEBS content.

[0082] The formulation used can be found in Table 1:

[0083] Table I:

[0084] A B C SEBS - 16.0 35.0 Medical white oil - 16.0 35.0 PE-LD 84.8 52.8 14.8 PP-CoPo 15 15.0 15.0 Stabilizer 0.2 0.2 0.2 Oil / SEBS 0 1.00 1.00 Shore Hardness A 95 90 61 Shore hardness D 45 30 15 DVR (23℃, 25% compression) - 25.6 15.9 DVR (70℃, 25% compression) - 58.4 40.2

Claims

1. A crown cap for a container for containing beverages and foods, the container having an access opening to be closed by means of the crown cap, the crown cap having a sealing liner which is arranged in the crown cap so that when the crown cap is placed on the container, the sealing liner seals the access opening in a sealing manner, wherein the crown cork together with the sealing liner does not contain any halogen-containing material, wherein the metal sheet used for the crown cork has a thickness of 0.10 mm to 0.19 mm, The sealing liner comprises at least twenty percent by weight of at least one preferably fully hydrogenated styrene triblock copolymer, especially styrene-ethylene-butylene-styrene copolymer (SEBS), SEEPS and / or SEPS, or a mixture of multiple copolymers of the above copolymers, based on the total weight of the sealing liner. 2 . The crown cork according to claim 1 , wherein the metal sheet used has a thickness of at most 0.20 mm, in particular at most 0.19 mm, preferably 0.14 mm to 0.17 mm and particularly preferably 0.15 mm to 0.16 mm.

3. The crown cork according to claim 1 or 2, wherein the metal sheet is tinplate with a thickness of at most 0.19 mm, preferably produced by means of the "double reduction" process and having a yield strength of at least 415 MPa, preferably having a yield strength of more than 415 MPa. 4 . The crown cork according to claim 3 , wherein the metal sheet has a thickness of at most 0.18 mm at a yield strength between 415 MPa and 620 MPa and preferably has a thickness of at most 0.15 mm at a yield strength above 620 MPa.

5. The crown according to claim 1, wherein the sealing liner contains between 20% and 50% by weight, preferably between 25% and 45% by weight, particularly preferably between 30% and 40% by weight, of a styrene triblock copolymer, in particular SEBS. 6 . The crown according to claim 1 , wherein the sealing liner contains between 33% and 38% by weight, preferably between 33% and 37% by weight, of a styrene triblock copolymer, in particular SEBS.

7. The crown according to claim 1, wherein the sealing liner comprises at least 20% by weight of oil, preferably white oil, wherein the oil content (in % by weight) is preferably as high as the content of the styrene triblock copolymer. 8 . The crown according to claim 1 , wherein the sealing liner comprises at least one olefin polymer or olefin copolymer, in particular PE-LD or PP-CoPo. 9 . The crown according to claim 1 , wherein the sealing liner has a Shore A hardness of 40 to 75, preferably 50 to 70, particularly preferably 55 to 65 at room temperature (23° C.).

10. The crown according to claim 1, wherein the sealing gasket has a compression set determined according to DIN ISO 815-1 of 10% to 25%, preferably 15% to 20% at 23°C, and a compression set determined according to DIN ISO 815-1 of 30% to 50%, preferably 35% to 45% at 70°C. 11 . The crown cap according to claim 1 , wherein the SEBS component of the sealing liner has a solution viscosity in toluene (15% by weight, 25° C.) of ≥50 mPa.s, preferably ≥100 mPa.s and particularly preferably ≥500 mPa.s.

12. The crown according to claim 1, wherein the sealing liner has a SEBS composition with a styrene alcohol content of between 27% and 35% by weight, preferably between 29% and 33% by weight. 13 . The crown cap according to claim 1 , wherein the ratio of oil to SEBS of the sealing gasket is between 0.7:1 and 1.3:1, preferably between 0.8:1 and 1.2:1, particularly preferably between 0.9:1 and 1.1:

1.

14. The crown according to any one of the preceding claims, wherein the sealing liner has at least 14% of a plasticizer, i.e. a white oil, whose kinematic viscosity at 40°C is between 60 cSt and 350 cSt, and / or a liquid polyalphaolefin (C2-C20) with the same viscosity.

15. The crown according to any one of the preceding claims, wherein the sealing liner comprises 15 to 60% by weight of polyolefins, namely PE and PP and copolymers of the polyolefins having C4-C8 and mixtures thereof. 16 . The crown as claimed in claim 1 , wherein the sealing liner comprises up to 20% by weight of polybutene (and copolymers with C2 / C3) or polystyrene. 17 . The crown cap according to claim 1 , wherein the sealing liner has up to 20% by weight of fillers, preferably calcium carbonate, talc and / or sodium sulfite also as a scavenger. 18 . The crown cork as claimed in claim 1 , which is designed as a twist-off crown cork. 19 . The crown cork as claimed in claim 1 , the metal sheet of which at least partially consists of tinplate and / or of steel, in particular stainless steel or aluminum.