Abrasive article, method of manufacture and use thereof
Precisely shaped abrasive particles with a coating weight of over 300 particles per square inch address performance inconsistencies by maintaining high cut rates and low abrasive wear across diverse pressure ranges, enhancing abrasive article efficiency.
Patent Information
- Application Number
- CN202380036453.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-26
- Filing Date
- 2023-04-21
- Publication Date
- 2024-12-06
AI Technical Summary
Existing abrasive particles and articles face challenges in achieving optimal performance across a wide range of pressures due to the expected trade-offs between coating weight and pressure distribution, leading to suboptimal performance at low, medium, or high pressures.
The development of precisely shaped abrasive particles with a coating weight of greater than 300 particles per square inch, which exhibit improved performance across a wide range of pressures, including high cut rates and low abrasive weight loss, by using a multi-step process involving ceramic precursor dispersions and controlled mold formation.
The shaped abrasive particles demonstrate superior cutting performance and reduced abrasive wear across varying pressures, exceeding expectations in both high and low coating weight applications.
Smart Images

Figure CN119095931A_ABST
Abstract
Description
Background Art
[0001] Abrasive particles and abrasive articles including abrasive particles can be used to grind, polish or grind a variety of materials and surfaces during product manufacturing. Therefore, there is always a need to improve the cost, performance or life of abrasive particles or abrasive articles. Summary of the invention
[0002] An abrasive article is provided, the abrasive article comprising a backing, a make coat applied to the backing, and a plurality of shaped abrasive particles embedded in the make coat. The coating weight of the plurality of shaped abrasive particles is greater than 300 particles per square inch. According to Grinding Test 1, the abrasive article exhibits a GT1 Total Cut LP of at least 975 grams, a GT1 Total Cut MP of at least 4250 grams, and a GT1 Total Cut HP of at least 5075 grams when used to grind a substrate.
[0003] Shaped abrasive particles can generally have better performance than randomly crushed abrasive particles. However, there are general expectations about how shaped abrasive particles of different coating weights will perform at different applied pressures. Generally speaking, the higher the coating weight, the lower the expected performance at low or medium pressures because the pressure is distributed over a greater number of particle tips and the tips do not break off and create new sharp tips. Conversely, low coating weight tapes are not expected to perform well at high pressures because the unit pressure on each tip is too high and the particles break off and break apart too quickly.
[0004] Surprisingly, a construction has been discovered that performs well over a wide range of pressures and over a wider range of coating weights. BRIEF DESCRIPTION OF THE DRAWINGS
[0005] Figure 1A to Figure 1B is a schematic perspective view of shaped abrasive particles that can be used in exemplary articles described herein.
[0006] 2A-2C illustrate different shaped abrasive particles that can be used to form abrasive articles.
[0007] Figure 3 Methods of forming abrasive articles according to embodiments herein are shown.
[0008] Figure 4 A cross-sectional view of an exemplary abrasive article according to embodiments herein is shown.
[0009] FIG. 5A to FIG. 5C Example thickness measurements of the abrasive particles herein are shown.
[0010] FIG. 6A to FIG. 6B Example edge length measurements of the abrasive particles herein are shown.
[0011] Figures 7 and 8The grinding data described in detail in the examples are shown.
[0012] Although the above-mentioned drawings show several embodiments of the present disclosure, other embodiments are also contemplated, for example, as noted in the discussion. In all cases, the present disclosure is presented in an exemplary and non-restrictive manner. It should be understood that those skilled in the art can design many other modifications and embodiments that fall within the scope and spirit of the principles of the present disclosure. The accompanying drawings may not be drawn to scale. In all drawings, the same reference numerals may be used to represent the same parts. DETAILED DESCRIPTION
[0013] The following definitions apply throughout the specification and claims.
[0014] The term "aspect ratio" refers to the side length (as defined herein) divided by the thickness (as defined herein). To determine the aspect ratio of shaped abrasive particles according to the present specification, the thickness and side length measurements of the same 20 randomly selected shaped abrasive particles (see below) are used.
[0015] The term "length" refers to the maximum extent of an object along its largest dimension.
[0016] The term "width" refers to the maximum extent of something along the dimension orthogonal to its length.
[0017] The term "thickness" refers to the greatest extent of something along a dimension orthogonal to both length and width. To determine the thickness of shaped abrasive particles according to the present specification, 20 shaped abrasive particles are randomly selected from a larger batch of similar particles, and three thickness measurements (T1, T2, and T3) are taken for each of the 20 particles at the following locations along the sidewall: (i) each end of the sidewall; and (ii) the center of the sidewall (e.g., FIG. 5A to FIG. 5C The resulting 60 individual thickness measurements were then averaged to determine the thickness of the shaped abrasive particles.
[0018] The term "major surface" refers to a surface that is larger than at least half of the surface of the object in question.
[0019] The term "perimeter" refers to the closed boundary of a surface, which may be a flat surface or a non-flat surface.
[0020] The term "precisely shaped" means that the shape is replicated from a mold cavity used during the preparation of the ceramic abrasive particles. The term "precisely shaped" excludes random shapes obtained by mechanical comminution operations or explosive comminution.
[0021] The term "side length" refers to the straight-line distance from tip to tip of a shaped abrasive particle along one of its side walls (e.g., FIG. 5A to FIG. 6B). To determine the side length of the shaped abrasive particles according to the present specification, 20 shaped abrasive particles are randomly selected from a larger batch of similar particles, and the side length of each of the 20 particles is measured along the side wall. The 20 individual side length measurements are then averaged to determine the side length of the shaped abrasive particles.
[0022] The features and advantages of the present invention will be further understood by considering the detailed description and the appended claims.
[0023] Figure 1A to Figure 1B is a schematic perspective view of exemplary shaped abrasive particles that may be used in abrasive articles according to the present disclosure. Figure 1A Particles of the shape shown are described in more detail in U.S. Patent No. 10,301,518 B2 issued on May 28, 2019, which is incorporated herein by reference (e.g., see Figure 3 to Figure 5 and related description). Figure 1B Particles of the shape shown are described in more detail in published PCT application WO 2021 / 245492 (Liu et al.), published on December 9, 2021 (see, e.g., FIG. 6A to FIG. 6B and related descriptions, which are incorporated herein by reference) and published PCT application No. WO 2021 / 245494 (Liu et al.) published on December 9, 2021 (see, e.g., Figure 4 A to Figure 4 B and related descriptions, incorporated herein by reference). Reference is now made to Figure 1A , the exemplary shaped ceramic abrasive particle 1 includes a first surface 10 having a perimeter 20. The perimeter 20 includes a first edge 30, a second edge 32, and a third edge 34. The first edge 30 is a concave monotonic curve, while the second edge 32 and the third edge 34 are substantially straight edges. However, it is expressly contemplated that in some embodiments, the second edge and / or the third edge or all three edges may be concave monotonic curves. The second surface 70 is opposite to the first major surface 10 and does not contact the first major surface. The peripheral surface 80 has a predetermined shape and is disposed between the first surface 10 and the second surface 70 and connects the first surface and the second surface. The peripheral surface 80 includes a first wall 82, a second wall 84, and a third wall 86. The first edge 30, the second edge 32, and the third edge 34 represent the intersection of the first wall 82, the second wall 84, and the third wall 86 with the perimeter 20, respectively. The first region 90 of the perimeter 20 includes the first edge 30 that extends inwardly and terminates at the first corner 50 and the second corner 52 , thereby defining respective first and second acute interior angles 60 , 62 .
[0024] like Figure 1AAs shown, the first region of the perimeter may include a single curved inwardly extending edge, however, it is also contemplated that the first region of the perimeter may include multiple edges (e.g., 2, 3, 4, 5, 6, 7, 8, 9, 10 or more edges), any or all of which may include a curvature extending inwardly.
[0025] The term "draft angle" refers to the angle of a taper that is incorporated into the wall of a mold cavity so that the opening of the mold cavity is wider than its base. The draft angle can be varied to change the relative size of the first surface and the second surface and the side of the circumferential surface. In various embodiments of the present disclosure, the draft angle μ can be 90 degrees, or in the range of about 95 degrees to about 130 degrees, about 95 degrees to about 125 degrees, about 95 degrees to about 120 degrees, about 95 degrees to about 115 degrees, about 95 degrees to about 110 degrees, about 95 degrees to about 105 degrees, or about 95 degrees to about 100 degrees. As used herein, the term draft angle also refers to the taper angle of the wall of a molded body that corresponds to the draft angle of a mold used to prepare the molded body. For example, Figure 1A The draft angle of the exemplary shaped ceramic abrasive particle 1 in should be the angle between the second surface 70 and the wall 84 .
[0026] It should be noted that, as discussed herein, the manufacturing process can introduce variations and changes to the final particle specifications. For example, the final draft angle, side length, aspect ratio, and thickness can generally fall within the expected range.
[0027] In some embodiments, the inwardly extending regions of shaped ceramic abrasive particles according to the present disclosure can have a maximum depth that is at least 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, or even 60% of the largest dimension of the shaped ceramic abrasive particles parallel to the maximum depth. Figure 1A , the maximum dimension 18 is parallel to the maximum depth 15 .
[0028] Figure 1B Shows something like Figure 1A Another shaped abrasive particle. Particle 100 has a first surface 102, and the first surface and second surface 104 are separated by a certain thickness 106. Figure 1B As shown, surfaces 102 and 104 may each have a curvature and be separated by a substantially constant thickness such that surfaces 102 and 104 may be considered parallel, curved, planar surfaces. Figure 1BAs shown, the curvature of surfaces 102 and 104 can be used to produce an edge (e.g., edge 112) that is more stable in an upright position. As described herein, the upright orientation includes a tip 114 that is opposite to backing 108. However, it is explicitly contemplated that particles 100 can be angled relative to backing 108, as shown by angle 110. In some embodiments, making most of the shaped abrasive particles 100 angled on the backing surface will cause the abrasive article to have a first cutting rate in a first direction and a second cutting rate in a second direction. This is due to the fact that if the shaped abrasive particles 100 are pulled against a surface facing forward against a concave surface (e.g., face 104), the shaped abrasive particles look like a shovel, thereby cutting out a larger amount of material from the substrate than when facing so that surface 102 faces forward.
[0029] Typically, the precisely shaped abrasive particles according to the present disclosure have a thickness that is significantly less than their length and / or width, but this is not required. For example, the thickness of the shaped ceramic abrasive particles can be less than or equal to one-third, one-fifth, or one-tenth of their length and / or width.
[0030] Generally, the first surface and the second surface are substantially parallel, or more parallel; however, this is not required. For example, random deviations due to drying may cause one or both of the first major surface and the second major surface to be uneven. Similarly, the first major surface and / or the second major surface may have parallel grooves formed therein, for example, as described in U.S. Patent Application Publication No. 2010 / 0146867A1 (Boden et al.).
[0031] The shaped ceramic abrasive particles according to the present disclosure comprise a ceramic material. In some embodiments, they may consist essentially of or even consist of a ceramic material, but they may contain a non-ceramic phase (e.g., as in glass-ceramics). Examples of suitable ceramic materials include alpha alumina, fused alumina-zirconia, and fused oxynitride. Additional details about sol-gel derived ceramic materials suitable for use in the shaped ceramic abrasive particles according to the present disclosure can be found, for example, in U.S. Pat. No. 4,314,827 (Leitheiser et al.), U.S. Pat. No. 4,518,397 (Leitheiser et al.); U.S. Pat. No. 4,623,364 (Cottringer et al.); U.S. Pat. No. 4,744,802 (Schwabel); U.S. Pat. No. 4,770,671 (Monroe et al.); U.S. Pat. No. 4,881,951 (Wood et al.); U.S. Pat. No. 4,960,441 (Pel low et al.); U.S. Patent No. 5,139,978 (Wood); U.S. Patent No. 5,201,916 (Berg et al.); U.S. Patent No. 5,366,523 (Rowenhorst et al.); U.S. Patent No. 5,429,647 (Larmie); U.S. Patent No. 5,547,479 (Conwell et al.); U.S. Patent No. 5,498,269 (Larmie); U.S. Patent No. 5,551,963 (Larmie); U.S. Patent No. 5,725,162 (Garg et al.) and U.S. Patent No. 6,054,093 (Torre et al.).
[0032] The shaped ceramic abrasive particles according to the present disclosure are generally used as a plurality of particles, which may include shaped ceramic abrasive particles of the present disclosure, other shaped abrasive particles, and / or crushed abrasive particles. For example, a plurality of abrasive particles according to the present disclosure may include at least 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 95%, or even 99% or more of the shaped ceramic abrasive particles described herein in numerical terms. The shaped ceramic abrasive particles may have the same nominal size and shape, but in some embodiments, it may be useful to use a combination of sizes and / or shapes.
[0033] Typically, shaped ceramic abrasive particles according to the present disclosure have a relatively small maximum particle dimension; for example, less than about 1 centimeter (cm), 5 millimeters (mm), 2 mm, 1 mm, 200 microns, 100 microns, 50 microns, 20 microns, 10 microns, or even less than 5 microns, although other sizes can be used.
[0034] Any abrasive particles mentioned in this disclosure may be sized according to abrasive industry recognized and specified nominal grades. Exemplary abrasive industry recognized grading standards include those promulgated by ANSI (American National Standards Institute), FEPA (European Abrasive Manufacturers Federation) and JIS (Japanese Industrial Standards). Such industry recognized classification standards include, for example: ANSI 4, ANSI 6, ANSI 8, ANSI 16, ANSI 24, ANSI 30, ANSI 36, ANSI 40, ANSI 50, ANSI 60, ANSI 80, ANSI 100, ANSI 120, ANSI 150, ANSI 180, ANSI 220, ANSI 240, ANSI 280, ANSI320, ANSI 360, ANSI 400 and ANSI 600; FEPA P8, FEPA P12, FEPA P16, FEPA P24, FEPA P30, FEPA P36, FEPA P40, FEPA P50, FEPA P60, FEPA P80, FEPA P100, FEPA P120, FEPA P150, FEPA P180, FEPA P220, FEPA P240, P320, FEPA P400, FEPA P500, FEPA P600, FEPA P800, FEPAP1000, and FEPA P1200; and JIS 8, JIS12, JIS 16, JIS24, JIS 36, JIS 46, JIS 54, JIS 60, JIS 80, JIS100, JIS150, JIS 180, JIS220, JIS240, JIS280, JIS 320, JIS 360, JIS 400, JIS400, JIS 600, JIS 800, JIS1000, JIS1500, JIS2500, JIS 4000, JIS 6000, JIS 8000 and JIS10,000. More typically, the shaped ceramic abrasive particles are individually sized according to ANSI 60 and 80 or FEPA P60 and P80 grading standards.
[0035] The term "abrasive industry recognized specified nominal grade" also includes abrasive industry recognized specified nominal screening grade. For example, the specified nominal screening grade may be graded as a nominal screening grade using a U.S. standard test sieve that conforms to ASTM E-11-09 "Standard Specification for Wire Cloth and Sieves for Testing Purposes". ASTM E-11-09 sets forth the design and construction requirements for test sieves that utilize a woven wire cloth mounted in a frame as the medium to classify materials according to a specified particle size. A typical designation may be expressed as -18+20, meaning that the shaped ceramic abrasive particles pass through a test sieve that conforms to the specifications of ASTM E11-09 "Standard Specification for Wire Cloth and Sieves for Testing Purposes" for a No. 18 sieve and are retained on a test sieve that conforms to the specifications of ASTM E11-09 for a No. 20 sieve. In one embodiment, the shaped ceramic abrasive particles have a particle size such that at least 90% of the particles pass through an 18 mesh test sieve and can be retained on a 20 mesh, 25 mesh, 30 mesh, 35 mesh, 40 mesh, 45 mesh, or 50 mesh test sieve. In various embodiments, the shaped ceramic abrasive particles can have a nominal screen grade including -18+20, -20+25, -25+30, -30+35, -35+40, 5-40+45, -45+50, -50+60, -60+70, -70+80, -80+100, -100+120, -120+140, -140+170, -170+200, -200+230, -230+270, -270+325, -325+400, -400+450, -450+500, or -500+635.
[0036] In some embodiments, shaped ceramic abrasive particles can be prepared according to a multi-step process. The process can be performed using a ceramic precursor dispersion (eg, a dispersion (eg, sol-gel) comprising a ceramic precursor material.
[0037] Briefly, the method includes the following steps: preparing a seeded or unseeded ceramic precursor dispersion that can be converted into a corresponding ceramic (e.g., a boehmite sol-gel that can be converted into alpha alumina); filling one or more mold cavities having the desired outer shape of shaped abrasive particles with the ceramic precursor dispersion, drying the ceramic precursor dispersion to form shaped ceramic precursor particles; removing the shaped ceramic precursor particles from the mold cavities; calcining the shaped ceramic precursor particles to form calcined shaped ceramic precursor particles, and then sintering the calcined shaped ceramic precursor particles to form shaped ceramic abrasive particles.
[0038] In some embodiments, the calcining step is omitted and the shaped ceramic precursor particles are sintered directly after being removed from the mold. In some embodiments, the mold can be made of a sacrificial material (e.g., a polyolefin material) that burns out during calcining or sintering, thereby eliminating the need to separate the ceramic precursor particles from the mold during processing.
[0039] The process will now be described in more detail in the context of shaped ceramic abrasive particles containing alpha-alumina.
[0040] The first process step involves providing a seeded or seedless dispersion of a ceramic precursor material (i.e., a ceramic precursor dispersion) that can be converted into a ceramic material. Ceramic precursor dispersions often contain a volatile liquid component. In one embodiment, the volatile liquid component is water. The ceramic precursor dispersion should contain enough liquid to make the viscosity of the dispersion low enough to fill the mold cavity and replicate the mold surface, but the amount of liquid should not be too much, so that the cost of subsequently removing the liquid from the mold cavity is too high. In one embodiment, the ceramic precursor dispersion contains 2% to 90% by weight of particles that can be converted into ceramics (such as particles of aluminum oxide monohydrate (boehmite) or another aluminum oxide precursor), and at least 10% to 98% by weight, or 50% to 70% by weight, or 50% to 60% by weight of volatile components (such as water). Conversely, in some embodiments, the ceramic precursor dispersion contains 30% to 50% by weight, or 40% to 50% by weight of solids.
[0041] Examples of useful ceramic precursor dispersions include zirconium oxide sols, vanadium oxide sols, cerium oxide sols, aluminum oxide sols, and combinations thereof. Useful aluminum oxide dispersions include, for example, boehmite dispersions and other aluminum oxide hydrate dispersions. Boehmite can be prepared by known techniques or can be commercially obtained. Examples of commercially available boehmite include products under the trade names "DISPERAL" and "DISPAL", both from Sasol North America, Inc., or products under the trade name "HIQ-40" from BASF. These monohydrated aluminum oxides are relatively pure; that is, they contain relatively few (if any) other hydrate phases in addition to the monohydrate and have a high surface area.
[0042] Other examples of suitable ceramic precursor materials include non-colloidal alumina slurries as described in U.S. Pat. No. 10,400,146 (Rosenflanz et al.), issued Sept. 3, 2019.
[0043] The physical properties of the resulting shaped ceramic abrasive particles will generally depend on the types of materials used in the ceramic precursor dispersion.As used herein, a "gel" is a three-dimensional network of solids dispersed in a liquid.
[0044] The ceramic precursor dispersion may contain a modifying additive or a precursor of a modifying additive. The modifying additive may be used to enhance certain desired properties of the abrasive particles, or to improve the efficiency of a subsequent sintering step. The modifying additive or a precursor of a modifying additive may be in the form of a soluble salt, typically a water-soluble salt. They are typically composed of metal-containing compounds and may be precursors to oxides of magnesium, zinc, iron, silicon, cobalt, nickel, zirconium, hafnium, chromium, yttrium, praseodymium, samarium, ytterbium, neodymium, lanthanum, gadolinium, cerium, dysprosium, erbium, titanium, and mixtures thereof. The specific concentrations of these additives that may be present in the ceramic precursor dispersion may be adjusted by one skilled in the art.
[0045] Typically, the introduction of a modifying additive or a modifying additive precursor will result in gelling of the ceramic precursor dispersion. The ceramic precursor dispersion may also be gelled by heating for a period of time to reduce the liquid content of the dispersion by evaporation. The ceramic precursor dispersion may also contain a nucleating agent. Nucleating agents suitable for use in the present disclosure may include fine particles of alpha alumina, alpha iron oxide or its precursors, titanium dioxide and titanates, chromium oxide, or any other substance that nucleates the conversion. If a nucleating agent is used, the amount should be sufficient to convert the alpha-alumina. Methods for nucleating alpha alumina precursor dispersions are disclosed in U.S. Pat. No. 4,744,802 (Schwabel).
[0046] Peptizing agents can be added to the ceramic precursor dispersion to produce a more stable hydrosol or colloidal ceramic precursor dispersion. Suitable peptizing agents are monoprotic acids or acidic compounds such as acetic acid, hydrochloric acid, formic acid and nitric acid. Polyprotic acids can also be used, but they may cause the ceramic precursor dispersion to gel rapidly, making it difficult to handle or introduce additional components to it. Some commercial sources of boehmite contain acid titers (e.g., absorbed formic acid or nitric acid) that help form stable ceramic precursor dispersions.
[0047] The ceramic precursor dispersion may be formed by any suitable means; for example, in the case of a sol-gel alumina precursor, simply mixing alumina monohydrate with water containing a peptizing agent, or forming a slurry of alumina monohydrate to which a peptizing agent is added.
[0048] Defoamers or other suitable chemicals may be added to reduce the tendency to form bubbles or entrap air during mixing. Other chemicals such as wetting agents, alcohols or coupling agents may be added if necessary.
[0049] The second process step involves providing a mold having at least one mold cavity, and preferably a plurality of cavities formed in at least one major surface of the mold.
[0050] In some embodiments, the mold is formed as a production tool, which can be, for example, a coating roller such as a belt, a sheet, a continuous fiber web, a rotary gravure roller, a sleeve mounted on a coating roller, or a die. In one embodiment, the production tool comprises a polymer material. Examples of suitable polymer materials include thermoplastics, such as polyesters, polycarbonates, poly(ether sulfones), poly(methyl methacrylate), polyurethanes, polyvinyl chloride, polyolefins, polystyrene, polypropylene, polyethylene, or a combination thereof, or a thermosetting material. In one embodiment, the entire mold is made of a polymer material or a thermoplastic material. In another embodiment, the surface of the mold that contacts the ceramic precursor dispersion when drying (such as the surface of a plurality of cavities) comprises a polymer material or a thermoplastic material, and the other parts of the mold can be made of other materials. By way of example, a suitable polymer coating can be applied to a metal mold to change its surface tension properties.
[0051] Polymer or thermoplastic production tools can be replicated from metal master tools. The master tool will have the reverse pattern desired for the production tool. The master tool can be made in the same way as the production tool. In one embodiment, the master tool is made of metal, such as nickel, and is diamond turned. In one embodiment, the master tool is formed at least in part using stereolithography technology. The polymer sheet material can be heated together with the master tool so that the master tool pattern is embossed on the polymer material by pressing the two together. The polymer or thermoplastic material can also be extruded or cast onto the master tool and then pressed. The thermoplastic material is cooled to harden it, thereby making the production tool. If a thermoplastic production tool is utilized, care should be taken not to generate too much heat, which can deform the thermoplastic production tool, thereby limiting its life. More information on the design and manufacture of production molds or master tools can be found in U.S. Pat. Nos. 5,152,917 (Pieper et al.); 5,435,816 (Spurgeon et al.); 5,672,097 (Hoopman et al.); 5,946,991 (Hoopman et al.); 5,975,987 (Hoopman et al.); and 6,129,540 (Hoopman et al.).
[0052] The cavity may be accessible from an opening in either the top or bottom surface of the mold. In some cases, the cavity may extend through the entire thickness of the mold. Alternatively, the cavity may extend only a portion of the thickness of the mold. In one embodiment, the top surface is generally parallel to the bottom surface of the mold, wherein the mold cavity has a generally uniform depth. At least one edge of the mold, i.e., the edge in which the cavity is formed, may remain exposed to the ambient atmosphere during the step in which the volatile components are removed.
[0053] The cavities have a specific three-dimensional shape to produce shaped ceramic abrasive particles. The depth dimension is equal to the vertical distance from the top surface to the lowest point on the bottom surface. The depth of a given cavity can be uniform or can vary along its length and / or width. The cavities of a given mold can have the same shape or different shapes.
[0054] The third process step involves filling the cavity in the mold with the ceramic precursor dispersion (e.g., by conventional techniques). In some embodiments, a knife roll coater or a vacuum slot die coater may be used. If necessary, a release agent may be used to aid in removing the particles from the mold. Typical release agents include oils (such as peanut oil or mineral oil, fish oil), silicones, polytetrafluoroethylene, zinc stearate, and graphite. Generally, a release agent such as peanut oil in a liquid such as water or alcohol is applied to the surface of the production tool in contact with the ceramic precursor dispersion so that when demolding is required, there is about 0.1 mg / in per unit area of the mold. 2(0.02mg / cm 2 ) to about 3.0 mg / in 2 (0.5mg / cm 2 ) or about 0.1 mg / in 2 (0.02mg / cm 2 ) to about 5.0 mg / in 2 (0.8mg / cm 2 ) between the mold release agent. In some embodiments, the top surface of the mold is coated with a ceramic precursor dispersion. The ceramic precursor dispersion can be sucked onto the top surface.
[0055] Next, a scraper or leveling bar (i.e., a scraper) can be used to completely press the ceramic precursor dispersion into the cavity of the mold. The remaining portion of the ceramic precursor dispersion that has not entered the cavity can be removed from the top surface of the mold and recycled. In some embodiments, a small portion of the ceramic precursor dispersion can be retained on the top surface, and in other embodiments, the top surface is substantially free of dispersion. The pressure applied by the scraper or leveling bar is typically less than 100 psi (0.7 MPa), less than 50 psi (0.3 MPa), or even less than 10 psi (69 kPa). In some embodiments, the exposed surface of the ceramic precursor dispersion does not substantially extend beyond the top surface.
[0056] In those embodiments where it is desired to form substantially planar faces of shaped ceramic abrasive particles using exposed surfaces of the cavities, it may be necessary to overfill the cavities (eg, using a micronozzle array) and slowly dry the ceramic precursor dispersion.
[0057] The fourth process step involves removing the volatile components to dry the dispersion. Advantageously, the volatile components are removed at a rapid evaporation rate. In some embodiments, the operation of removing the volatile components by evaporation is carried out at a temperature above the boiling point of the volatile components. The upper limit of the drying temperature generally depends on the material from which the mold is made. For polypropylene molds, the temperature should be below the melting point of the plastic. In one embodiment, for an aqueous dispersion containing between about 40% and 50% solids and a polypropylene mold, the drying temperature may be between about 90°C and about 165°C, or between about 105°C and about 150°C, or between about 105°C and about 120°C. Higher temperatures can result in improved production speeds, but can also result in degradation of the polypropylene mold, thereby limiting its useful life as a mold.
[0058] The fifth process step involves removing the resulting shaped ceramic precursor particles from the mold cavity. The shaped ceramic precursor particles can be removed from the cavity by using the following processes alone or in combination on the mold: gravity, vibration, ultrasonic vibration, vacuum or pressurized air to remove the particles from the mold cavity.
[0059] The shaped ceramic precursor particles may also be dried outside of the mold. If the ceramic precursor dispersion is dried to the desired extent in the mold, this additional drying step is not required. However, in some cases, it may be economical to employ this additional drying step to minimize the time that the ceramic precursor dispersion resides in the mold. Typically, the shaped ceramic precursor particles will be dried at a temperature of 50° C. to 160° C., or at 120° C. to 150° C., for 10 minutes to 480 minutes, or 120 minutes to 400 minutes.
[0060] The sixth process step involves calcining the shaped ceramic precursor particles. During calcination, substantially all volatile materials are removed and the various components present in the ceramic precursor dispersion are converted into metal oxides. Typically, the shaped ceramic precursor particles are heated to a temperature of 400°C to 800°C and maintained within this temperature range until free water and more than 90% by weight of any combined volatile materials are removed. In an optional step, it may be desirable to introduce modifying additives by an impregnation process. Water-soluble salts may be introduced into the pores of the calcined shaped ceramic precursor particles by impregnation. The shaped ceramic precursor particles are then pre-calcined again. This optional step is further described in U.S. Patent No. 5,164,348 (Wood).
[0061] The seventh process step involves sintering the calcined shaped ceramic precursor particles to form ceramic particles. Prior to sintering, the calcined shaped ceramic precursor particles are not fully densified and therefore lack the desired hardness for use as shaped ceramic abrasive particles. Sintering is performed by heating the calcined shaped ceramic precursor particles to a temperature of 1000° C. to 1650° C. The length of time that the calcined shaped ceramic precursor particles must be exposed to the sintering temperature in order to achieve this degree of transformation depends on a variety of factors, but is typically from 5 seconds to 48 hours.
[0062] In another embodiment, the duration of the sintering step ranges from one minute to 90 minutes.After sintering, the shaped ceramic abrasive particles can have a Vickers hardness of 10 GPa (gigapascals), 16 GPa, 18 GPa, 20 GPa, or more.
[0063] Other steps may be used to modify the process, such as rapidly heating the material from the calcining temperature to the sintering temperature, centrifuging the ceramic precursor dispersion to remove sludge and / or waste. In addition, if desired, the method may be modified by combining two or more of these process steps. Conventional process steps that may be used to modify the process of the present disclosure are more fully described in U.S. Pat. No. 4,314,827 (Leitheiser).
[0064] Shaped ceramic abrasive particles composed of crystallites of alpha alumina, magnesium aluminum spinel, and rare earth hexaaluminate can be prepared using sol-gel alpha alumina precursor particles according to the methods described in the following patents: for example, U.S. Patent No. 5,213,591 (Celikkaya et al.) and U.S. Published Patent Application Nos. 2009 / 0165394A1 (Culler et al.) and 2009 / 0169816A1 (Erickson et al.). The alpha alumina abrasive particles may contain zirconium oxide, as disclosed in U.S. Patent No. 5,551,963 (Larmie). Alternatively, the alpha alumina abrasive particles may have microstructures or additives, for example, as disclosed in U.S. Patent No. 6,277,161 (Castro). More information about methods of making shaped ceramic abrasive particles is disclosed in co-pending U.S. Published Patent Application No. 2009 / 0165394A1 (Culler et al.).
[0065] Surface coatings on shaped ceramic abrasive particles can be used to improve adhesion between the shaped ceramic abrasive particles and the binder material in the abrasive article, or can aid in electrostatic deposition of the shaped ceramic abrasive particles. In one embodiment, a surface coating as described in U.S. Pat. No. 5,352,254 (Celikkaya) can be used in an amount of 0.1% to 2% relative to the weight of the shaped abrasive particles. Such surface coatings are described in U.S. Pat. Nos. 5,213,591 (Celikkaya et al.), 5,011,508 (Wald et al.), 1,910,444 (Nicholson), 3,041,156 (Rowse et al.), 5,009,675 (Kunz et al.), 5,085,671 (Martin et al.), 4,997,461 (Markhoff-Matheny et al.), and 5,042,991 (Kunz et al.). In addition, the surface coating can prevent the shaped abrasive particles from blocking. The term "blocking" is used to describe the phenomenon whereby metal particles from the workpiece being abraded become welded to the tops of the shaped ceramic abrasive particles. Surface coatings that perform the above functions are known to those skilled in the art.
[0066] The shaped ceramic abrasive particles of the present disclosure can generally be prepared using tools cut from diamond dies (or dies that are inverse replicas thereof), thereby providing greater feature definition than other manufacturing alternatives (e.g., stamping or punching). Typically, the cavities in the tool surface have smooth surfaces that converge along sharp edges, but this is not required. The resulting shaped ceramic abrasive particles have a corresponding nominal average shape that corresponds to the shape of the cavities in the tool surface; however, variations (e.g., random variations) from the nominal average shape can occur during manufacturing, and shaped ceramic abrasive particles that exhibit such variations are included within the definition of shaped ceramic abrasive particles as used herein.
[0067] 2A-2C illustrate different shaped abrasive particles that can be used to form abrasive articles. Figure 2A-1 and Figure 2A-2 A triangular shaped abrasive particle 200 is shown having a side length 210 and a thickness 215. The particle 200 was made using a mold having an aspect ratio of 4:1 (side length 210 is four times as long as thickness 215). Figure 2B-1 and Figure 2B-2 A triangular shaped abrasive particle 220 is shown having a side length 230 and a thickness 235. The particle 220 was made using a mold having an aspect ratio of 3:1 (side length 230 is three times the thickness 235). However, it is noted that the final aspect ratio of the fired particle changes due to the manufacturing process, as shown in Table 1 below.
[0068] Figure 2C-1 and Figure 2C-2 A particle 250 is shown having three sides, each side having a concave curvature. Figure 2C-2 As shown, the concave curvature of each side 255 may cause some shrinkage to produce curvature 262 along the edge as a result of the particle drying process. - Particle 250 is manufactured using a mold with an aspect ratio of 7:2 (where side length 255 is 3.5 times the length of thickness 260).
[0069] Table 1 below shows some exemplary parameter ranges for particles 200, 220, and 250. As noted, final particle EQ5:1 is not shown in FIGS. 2A-2C , but the included ranges are examples of particles of equilateral triangle shape similar to particles 200 and 220, but from a mold having an aspect ratio of 5:1.
[0070] Table 1
[0071]
[0072] As shown in Table 1, in embodiments herein, the aspect ratio of the fired particles may be in the range of 3: 1 to 7: 1, or in some embodiments, in the range of 3: 1 to 6: 1. In some further embodiments, the aspect ratio of the particles described in the embodiments herein may be in the range of 3.5: 1 to 5.5: 1. Figure 3 Methods of forming abrasive articles according to embodiments herein are shown.
[0073] Shaped ceramic abrasive particles can be used, for example, to construct abrasive articles, including, for example, coated abrasive articles (e.g., conventional make- and size-coated abrasive articles, slurry-coated abrasive articles, and structured abrasive articles). Generally, abrasive articles comprise a plurality of abrasive particles retained in a binder. Figure 3 A method of manufacturing a coated abrasive article according to embodiments described herein is shown. Method 300 can be used, for example, to prepare any of the coated abrasive articles discussed herein. However, it can also be used to prepare other suitable coated abrasive articles.
[0074] In frame 310, a backing is provided. In some embodiments, the backing can be pre-treated before the coating process. For example, the pre-treatment can help increase adhesion, reduce abrasive weight loss, or reduce static electricity. In other embodiments, the backing provided can also be untreated. The backing can also have other features, such as perforations, laminated layers, etc. The backing can be flexible or rigid and can be made of any suitable woven or nonwoven material.
[0075] In block 320, a make coat is provided. The make coat is typically provided in an uncured form so that the deposited abrasive particles can be embedded. The make coat can be deposited on the backing in any number of suitable ways, including, for example, spraying, rolling, knife coating, and the like.
[0076] In frame 330, abrasive grains are embedded in the make coat. As described herein, for comparative purposes, abrasive grains 200, 220, and 250 are all used to prepare abrasive articles described herein in the embodiments. However, it is clearly contemplated that other shapes may be used. Abrasive articles are embedded with a coating weight 336, which refers to the average number of grains on the abrasive article, typically expressed as grains per square inch.
[0077] The inventors surprisingly noted that abrasive belts made with abrasive grains 250 at a coating weight exceeding 400 grains per square inch exhibited good abrasive behavior over a wide range of pressures. Generally, high coating weights would be expected to perform well in high pressure applications, but not at medium or low pressures. However, abrasive belts made with abrasive grains 250 at a high coating weight had better than expected cut rates over a wide range of applied pressures.
[0078] Additionally, note that the high coating weight tape made with abrasive grains 250 exhibits high peak counts (correct orientation), high cut rates, and low abrasive weight loss. It is difficult to balance all three of these parameters.
[0079] It was also surprisingly discovered that the same particles also exhibited higher cut rates and lower abrasive weight loss than expected when used at low coating weights. Generally, lower coating weight applications would be expected not to perform well at high pressures because the particles would break up quickly.
[0080] The first set of abrasive particles can be deposited and oriented on the backing using any suitable method, such as using electrostatic alignment, which will orient the particles in the XY directions, but not in the Z direction. Alternatively, in embodiments where the abrasive particles include a magnetically responsive element or coating, the first set of abrasive particles can be deposited and oriented using magnetic alignment, such that the particles will be oriented in a desired orientation when exposed to a magnetic field.
[0081] Orientation may include orienting the abrasive particles so that corresponding faces of adjacent particles are parallel to each other, as indicated in box 332, and so that sharp tips or edges face away from the backing, as indicated in box 334. Alignment of the abrasive particles may be accomplished using electrostatic coatings or magnetic coatings, as described in the following applications: PCT Patent Application Publication Nos. WO2018 / 080703 (Nelson et al.), WO2018 / 080756 (Eckel et al.), WO2018 / 080704 (Eckel et al.), WO2018 / 080705 (Adefris et al.), WO2018 / 080765 (Nelson et al.), WO2018 / 080784 (Eckel et al.), WO2018 / 136271 (Eckel et al.), WO2018 / 134732 (Nienaber et al.), WO2018 / 080755 (Martris et al.), inez et al.), WO2018 / 080799 (Nienaber et al.), WO2018 / 136269 (Nienaber et al.), WO2018 / 136268 (Jesme et al.), WO2019 / 207415 (Nienaber et al.), WO2019 / 207417 (Eckel et al.), WO2019 / 207416 (Nienaber et al.), and U.S. Provisional Application No. 62 / 914,778 filed on October 14, 2019, U.S. Provisional Application No. 62 / 875,700 filed on July 18, 2019, and U.S. Provisional Application No. 62 / 924,956 filed on October 23, 2019.
[0082] Making the particles magnetically responsive may include coating non-magnetically responsive particles with a magnetically responsive coating. However, in other embodiments, the particles are formed of a magnetically responsive material, for example, as described in co-owned provisional patent US62 / 914778 filed on October 14, 2019. At least one magnetic material may be contained within or coated onto the shaped abrasive particles. Examples of magnetic materials include iron; cobalt; nickel; various alloys of nickel and iron sold as various grades of Permalloy; sold as Fernico, Kovar, Fernico I, or Fernico II. II); various alloys of iron, aluminum, nickel, cobalt, and sometimes copper and / or titanium sold as various grades of aluminum nickel cobalt (Alnico); alloys of iron, silicon, and aluminum (about 85:9:6 by weight) sold as FeAlSi; Heusler alloys (e.g., Cu2MnSn); manganese bismuth (also known as bismuth manganese (Bismanol)); rare earth magnetite , such as alloys of gadolinium, dysprosium, holmium, europium oxide, neodymium, iron and boron (e.g., Nd2Fe14B) and samarium and cobalt (e.g., SmCo5); MnSb; MnOFe2O3; Y3Fe5O12; CrO2; MnAs; ferrites, such as ferrite, magnetite; zinc ferrite; nickel ferrite; cobalt ferrite, magnesium ferrite, barium ferrite and strontium ferrite; yttrium iron garnet; and combinations of the foregoing. In some embodiments, the magnetizable material is an alloy containing 8 to 12 weight percent aluminum, 15 to 26 weight percent nickel, 5 to 24 weight percent cobalt, up to 6 weight percent copper, up to 1 weight percent titanium, with the balance of the material totaling 100 weight percent being iron. In some other embodiments, a magnetizable coating can be deposited on the abrasive particles 100 using vapor deposition techniques such as, for example, physical vapor deposition (PVD), including magnetron sputtering. The inclusion of these magnetizable materials can make the shaped abrasive particles responsive to a magnetic field. Any of the shaped abrasive particles can include the same material or include different materials.
[0083] The magnetic coating can be a continuous coating, for example, the continuous coating coats the entire abrasive grain, or at least coats an entire surface of the abrasive grain. In another embodiment, a continuous coating refers to a coating in which there is no uncoated portion on the coated surface. In one embodiment, the coating is an integral coating formed by a single layer of magnetic material, rather than as discrete magnetic particles. In one embodiment, a magnetic coating is provided on the abrasive grain while the abrasive grain is still in the mold cavity, so that the magnetic coating directly contacts the surface of the abrasive grain precursor. In one embodiment, the thickness of the magnetic coating is at most equal to or preferably less than the thickness of the abrasive grain. In one embodiment, the magnetic coating does not exceed about 20% by weight of the final grain, or does not exceed about 10% by weight of the final grain, or does not exceed 5% by weight of the final grain.
[0084] Two steps are generally required to magnetically align abrasive particles relative to each other. First, the magnetizable abrasive particles described herein are provided on a substrate having a major surface. Second, a magnetic field is applied to the magnetizable abrasive particles so that most of the magnetizable abrasive particles are oriented to be approximately perpendicular to the major surface. Without applying a magnetic field, the resulting magnetizable abrasive particles may not have a magnetic moment, and the constituent abrasive particles or magnetizable abrasive particles may be randomly oriented. However, when a sufficient magnetic field is applied, the magnetizable abrasive particles will tend to align with the magnetic field. In an advantageous embodiment, the ceramic particles have a major axis (e.g., an aspect ratio of 2) and the major axis is aligned parallel to the magnetic field. Preferably, most or even all of the magnetizable abrasive particles will have magnetic moments that are aligned approximately parallel to each other. As described above, the abrasive particles described herein may have more than one magnetic moment and will be aligned with the net magnetic moment.
[0085] The magnetic field may be provided by any external magnet (e.g., a permanent magnet or an electromagnet) or group of magnets. In some embodiments, the magnetic field is typically in the range of 0.5 to 1.5 kOe. Preferably, the magnetic field is substantially uniform over the scale of a single magnetizable abrasive particle.
[0086] For the production of abrasive articles, a magnetic field may optionally be used to position and / or orient the magnetizable abrasive particles prior to curing a binder (e.g., glassy or organic) precursor to produce the abrasive article. The magnetic field may be substantially uniform across the magnetizable abrasive particles before the particles are fixed in place in the binder or continuous throughout the binder, or the magnetic field may be non-uniform, or even effectively separated into discrete portions. Typically, the orientation of the magnetic field is configured to achieve alignment of the magnetizable abrasive particles according to a predetermined orientation, such as causing the abrasive particles to be parallel to each other and have cut faces facing in a downweb direction.
[0087] Examples of magnetic field configurations and apparatus for generating magnetic fields are described in U.S. Pat. No. 8,262,758 (Gao) and U.S. Pat. Nos. 2,370,636 (Carlton), 2,857,879 (Johnson), 3,625,666 (James), 4,008,055 (Phaal), 5,181,939 (Neff) and UK Patent No. 1 477 767 (Edenville Engineering Works Limited).
[0088] As shown in boxes 332 and 335, orientation can also be achieved using patterned drop coating. In some embodiments, patterned drop coating can be achieved using an alignment tool by a method similar to that described in PCT Patent Application Publication Nos. 2016 / 205133 (Wilson et al.), 2016 / 205267 (Wilson et al.), 2017 / 007703 (Wilson et al.), 2017 / 007714 (Liu et al.). The method generally involves the following steps: filling each cavity in the production tool with one or more triangular abrasive particles (usually one or two); aligning the filled production tool and the backing coated with the make layer precursor to transfer the triangular abrasive particles to the make layer precursor; transferring the abrasive particles from the cavity to the backing coated with the make layer precursor; and removing the production tool from the aligned position. The make coat precursor is then at least partially cured (typically to a degree sufficient to securely adhere the triangular abrasive grains to the backing), a size coat precursor is then applied to the make coat precursor and the abrasive grains, and the size coat precursor is at least partially cured to provide a coated abrasive belt. The process can be batch or continuous and can be performed manually or automatically, for example, using robotic equipment. It is not necessary to perform all steps or to perform them continuously, but the steps can be performed in the order listed or additional steps can be performed between each step. The triangular abrasive grains can be placed in a desired Z-axis rotational orientation, which is formed by first placing the triangular abrasive grains in an appropriately formed cavity in a dispensing surface of a production tool, which is arranged to have a complementary rectangular grid pattern, or other suitable pattern based on the shape of the abrasive grains.
[0089] Transfer coating using a tool with a patterned cavity can be similar to the transfer coating described in U.S. Patent Application Publication No. 2016 / 0311081A1 (Culler et al.). In some embodiments, abrasive particles can be applied to the make layer through a patterned mesh or screen.
[0090] The abrasive particles may also have other features 338 .
[0091] Examples of suitable abrasive grains include: fused alumina; heat treated alumina; white fused alumina; ceramic alumina materials, such as those commercially available from 3M Company, St. Paul, MN, under the trade name 3M CERAMIC ABRASIVE GRAIN; brown alumina; blue alumina; silicon carbide (including green silicon carbide); titanium diboride; boron carbide; tungsten carbide; garnet; titanium carbide; diamond; cubic boron nitride; garnet; fused alumina-zirconia; iron oxide; chromium oxide; zirconium oxide; titanium dioxide; tin oxide; quartz; feldspar; flint; corundum; sol-gel abrasive grains; and combinations thereof. Among these materials, molded sol-gel alpha alumina abrasive grains are preferred in many embodiments. Abrasive materials that cannot be processed by sol-gel methods can be molded with a temporary or permanent binder to form shaped precursor particles, which are then sintered to form abrasive particles, for example, as disclosed in U.S. Patent Application Publication No. 2016 / 0068729A1 (Erickson et al.).
[0092] Examples of sol-gel prepared abrasive particles and methods of preparing the same can be found in U.S. Pat. Nos. 4,314,827 (Leitheiser et al.), 4,623,364 (Cottringer et al.), 4,744,802 (Schwabel), 4,770,671 (Monroe et al.), and 4,881,951 (Monroe et al.). It is also contemplated that the abrasive particles may include abrasive agglomerates, such as, for example, those described in U.S. Pat. Nos. 4,652,275 (Bloecher et al.) or 4,799,939 (Bloecher et al.). In some embodiments, the first and / or abrasive particles may be surface treated with a coupling agent (e.g., an organosilane coupling agent) or otherwise physically treated (e.g., iron oxide or titanium oxide) to enhance adhesion of the abrasive particles to a binder (e.g., a primer layer and / or a size layer). The abrasive grains may be treated before they are combined with the corresponding binder precursor, or they may be surface treated in situ by including a coupling agent into the binder.
[0093] Preferably, the abrasive particles are ceramic abrasive particles, such as, for example, polycrystalline alpha alumina particles prepared by a sol-gel process. Abrasive particles composed of microcrystals of alpha alumina, magnesium aluminum spinel, and rare earth hexaaluminates can be prepared using sol-gel precursor alpha alumina particles according to the methods described in the following patents: for example, U.S. Patent No. 5,213,591 (Celikkaya et al.) and U.S. Patent Application Publication Nos. 2009 / 0165394A1 (Culler et al.) and 2009 / 0169816A1 (Erickson et al.).
[0094] Shaped abrasive particles based on alpha alumina can be prepared according to a well-known multi-step process. Briefly, the method includes the steps of making a seeded or unseeded sol-gel alpha alumina precursor dispersion that can be converted to alpha alumina; filling one or more mold cavities with shaped abrasive particles of the desired shape with the sol-gel, drying the sol-gel to form precursor triangular abrasive particles; removing the precursor abrasive particles from the mold cavity; calcining the precursor abrasive particles to form calcined precursor abrasive particles, and then sintering the calcined precursor abrasive particles to form a first group of abrasive particles and / or a second group of abrasive particles. The process will now be described in more detail.
[0095] Further details regarding methods of making sol-gel prepared abrasive particles can be found, for example, in U.S. Pat. Nos. 4,314,827 (Leitheiser); 5,152,917 (Pieper et al.); 5,435,816 (Spurgeon et al.); 5,672,097 (Hoopman et al.); 5,946,991 (Hoopman et al.); 5,975,987 (Hoopman et al.); and 6,129,540 (Hoopman et al.); and in U.S. Published Patent Application No. 2009 / 0165394 Al (Culler et al.).
[0096] Examples of slurry-made alpha alumina abrasive particles can be found in WO 2014 / 070468, published on May 8, 2014. Slurry-made particles can be formed from a powder precursor, such as alumina powder. Slurry processing can be advantageous for larger particles that are difficult to make using sol-gel techniques.
[0097] The abrasive grains may undergo a sintering process such as, for example, that described in U.S. Patent 10,400,146, issued September 3, 2019. However, other processing techniques are expressly contemplated.
[0098] Ultrafine grain shape grains may be formed using the techniques described in USPAP 2019 / 0233693 published on August 1, 2019, WO2018023177 published on December 20, 2018, or WO 2018 / 207145 published on November 15, 2018.
[0099] Softer shaped grain particles with a Mohs hardness between 2.0 and 5.0 can be prepared according to the method described in WO 2019 / 215539 published on November 14, 2019, which can be used for scratch-free applications.
[0100] In some preferred embodiments, the abrasive particles are precisely shaped, and an individual abrasive particle will have a shape that is substantially the shape of a portion of the cavity of a mold or production tool in which the particle precursor is dried prior to optional calcining and sintering.
[0101] Abrasive particles used in the present disclosure can generally be prepared using a tool (ie, a mold) and cut using precision machining, thereby providing greater feature definition than other fabrication alternatives such as, for example, stamping or punching.
[0102] The shaped abrasive particles may have at least one sidewall, which may be an inclined sidewall. In some embodiments, there may be more than one (e.g., two or three) inclined sidewalls, and the inclination or angle of each inclined sidewall may be the same or different. In other embodiments, for particles where the first and second faces taper to a thin edge or point where they meet without a sidewall, the sidewall may be minimized. The inclined sidewall may also be defined by a radius R (e.g., as in U.S. Patent Application No. 2010 / 0151196). Figure 5B ). The radius R of each of the side walls may vary.
[0103] Specific examples of shaped particles having ridges include roof-shaped particles, such as those described in WO 2011 / 068714. Figure 4 A to Figure 4 The particles shown in C. Preferred roof-shaped particles include particles having a hip roof or a hip roof shape (a type of roof in which any side wall facets present slope downward from a ridgeline to a first side). A hip roof generally does not include vertical side walls or facets.
[0104] Methods for making shaped abrasive particles having at least one sloped sidewall are described, for example, in US Patent Application Publication No. 2009 / 0165394.
[0105] The shaped abrasive particles may also include a plurality of ridges on their surface. A plurality of grooves (or ridges) may be formed by a plurality of ridges (or grooves) in the bottom surface of the mold cavity, which have been found to make it easier to remove the shaped abrasive particle precursors from the mold.
[0106] A plurality of grooves (or ridges) are not specifically limited, and may for example include parallel lines, which may extend completely or incompletely through the side. Preferably, the parallel lines intersect with the periphery at a 90 ° angle along the first edge. The cross-sectional geometry of a groove or ridge may be a truncated triangle, a triangle or other geometric shapes, as further discussed below. In various embodiments of the present invention, the depth of a plurality of grooves may be between approximately 1 micron and approximately 400 microns.
[0107] According to another embodiment, a plurality of grooves include a cross-hatch pattern of intersecting parallel lines, which may extend through the face completely or incompletely. In various embodiments, the cross-hatch pattern may adopt various cross-sectional geometries of intersecting parallel lines or non-parallel lines, percentage spacing between various lines, arcuate cross lines or grooves. In other embodiments, the number of ridges (or grooves) in the bottom surface of each die cavity may be between 1 and approximately 100, or between 2 to approximately 50, or between approximately 4 to approximately 25, thereby forming a corresponding number of grooves (or ridges) in the shaped abrasive particles.
[0108] Methods for making shaped abrasive particles having grooves on at least one side are described, for example, in US Patent Application Publication No. 2010 / 0146867.
[0109] The shaped abrasive particles may also have one or more recesses on one of the faces of the abrasive particles, as described in PCT application serial number IB2019 / 060861 filed on December 16, 2019.
[0110] The shaped abrasive particles can have openings (preferably openings extending or passing through the first side and the second side). Methods for making shaped abrasive particles having openings are described, for example, in US Patent Application Publication Nos. 2010 / 0151201 and 2009 / 0165394.
[0111] The shaped abrasive particles may also have at least one concave (or concave) face or facet; at least one face or facet that is outwardly shaped (or convex). Methods for preparing dish-shaped abrasive particles are described, for example, in U.S. Patent Application Publication Nos. 2010 / 0151195 and 2009 / 0165394. In addition, the shaped abrasive particles may also have a multi-faceted surface, as described in U.S. Patent No. 10,150,900, published on December 11, 2018.
[0112] The shaped abrasive particles can also have at least one fractured surface.Methods for making shaped abrasive particles having at least one fractured surface are described, for example, in US Patent Application Publication Nos. 2009 / 0169816 and 2009 / 0165394.
[0113] The shaped abrasive particles may also have cavities.The shaped abrasive particles may also include pores, such as described in US Pat. No. 8,142,532, issued Mar. 27, 2012, which is incorporated herein by reference.
[0114] The shaped abrasive particles may also have a low roundness coefficient. Methods for making shaped abrasive particles having a low roundness coefficient are described, for example, in US Patent Application Publication No. 2010 / 0319269.
[0115] The shaped abrasive particles may have a second vertex on the second side, as described in U.S. 9,447,311 published on September 16, 2016. Methods for preparing abrasive particles in which the second side is a vertex (e.g., a double-wedge abrasive particle) or a ridgeline (e.g., a roof-shaped particle) are described, for example, in U.S. Provisional Application 2012 / 022733 published on September 13, 2012.
[0116] The shaped abrasive particles can be formed to have sharp tips, such as those described in U.S. Provisional Application 2019 / 0233693, published on August 1, 2019, or U.S. Provisional Application Serial No. 62 / 877,443, filed on July 23, 2019.
[0117] The shaped abrasive particles may also be formed to include rake angles, such as those described in WO 2019 / 207423, published on October 31, 2019, or those described in WO 2019 / 207417, published on October 31, 2019, or those described in PCT application serial number IB 2019 / 059112, filed on October 24, 2019.
[0118] The shaped abrasive particles can also be formed to have precisely shaped portions and non-shaped portions, such as crushed portions, as described in U.S. Provisional Patent Application No. 62 / 833,865, filed on April 15, 2019.
[0119] The shaped abrasive particles may also have a combination of one or more of the shape features discussed herein, including sloped sidewalls, grooves, recesses, facets, fractured surfaces, cavities, more than one vertex, sharp edges, non-shaped portions, notches, tilt angles, and / or a low roundness factor.
[0120] The shaped abrasive particles may have an elongated shape, such as the shapes described in U.S. Provisional Application 2019 / 0106362, published on April 11, 2019, or the shapes described in WO 2019 / 069157, published on April 11, 2019. The elongated shape may be triangular prism-shaped, rod-shaped, or otherwise include one or more vertices along the perimeter.
[0121] The shaped abrasive particles may have a variable cross-sectional area along the length of the particle, such as those described in U.S. Provisional Application 2019 / 0249051. For example, the shaped abrasive particles may be dog-bone shaped, or otherwise have a cross-sectional area that varies from a first end to a second end.
[0122] The shaped abrasive particles may have a tetrahedral shape, such as those described in WO 2018 / 207145, published on November 15, 2018, or those described in U.S. Patent No. 9,573,250, issued on February 21, 2017.
[0123] The shaped abrasive particles may also have concave or convex portions, or may be defined as having one or more acute internal angles, such as those described in U.S. Patent No. 10,301,518, issued May 28, 2019.
[0124] The shaped abrasive particles may also include shape-to-shape particles, such as plate-to-plate shaped particles as described in 8,728,185, published May 20, 2014.
[0125] The shaped abrasive particles may also include shaped abrasive particles having irregular polygonal shapes, as described in U.S. Provisional Patent Application 62 / 924,956, filed on October 23, 2019.
[0126] The shaped abrasive particles can also be shaped as free-standing abrasive particles so that the cutting portion is more likely to be embedded in the make coat, for example, in an orientation away from the backing, such as those described in PCT application serial number IB 2019 / 060457 filed on December 4, 2019.
[0127] The first and / or second set of abrasive particles are typically selected to have a length in the range of 1 micron to 15,000 microns, more typically 10 microns to about 10,000 microns, and still more typically 150 microns to 2,600 microns, although other lengths may be used.
[0128] The first group of abrasive grains is selected to have the length of side (measured from tip to tip as described below about Fig. 5) in the range of 0.1 micron to 3500 micron, more generally 50 microns to 3000 microns and more generally 100 microns to 2600 microns conventionally, but other lengths may also be used.In some embodiments discussed herein, the length of side of abrasive grain is at least 1275 microns and less than 1525 microns.In other embodiments of this paper, the length of side of abrasive grain is at least 575 microns and less than 750 microns.In other embodiments of this paper, the length of side of abrasive grain is at least 450 microns and less than 575 microns.In some embodiments, abrasive grain can have at least 2,3,4,5,6,7 or larger aspect ratio (ratio of length to thickness).
[0129] The surface coating of the abrasive particles can be used to improve the adhesion between the abrasive particles and the binder in the abrasive article, or can be used to assist in the electrostatic deposition of the abrasive particles. In one embodiment, the surface coating described in U.S. Pat. No. 5,352,254 (Celikkaya) can be used in an amount of 0.1% to 2% of the surface coating relative to the weight of the abrasive particles. Such surface coatings are described in U.S. Pat. Nos. 5,213,591 (Celikkaya et al.); 5,011,508 (Wald et al.), 1,910,444 (Nicholson), 3,041,156 (Rowse et al.), 5,009,675 (Kunz et al.), 5,085,671 (Martin et al.), 4,997,461 (Markhoff-Matheny et al.), and 5,042,991 (Kunz et al.). In addition, the surface coating can prevent the abrasive particles from blocking. "Capping" is a term that describes the phenomenon whereby metal particles from the workpiece being abraded become welded to the tops of the abrasive particles.Surface coatings that perform the above functions are known to those skilled in the art.
[0130] Once the first abrasive particles and the second abrasive particles are embedded in the primer layer precursor, they are at least partially cured so as to maintain the orientation of the mineral during the application of the double-layer precursor. Typically, this involves B-staging the primer layer precursor, but further curing may be used as required. B-staging may be achieved, for example, using heating and / or light and / or using a curing agent, depending on the properties of the selected primer layer precursor. The primer layer precursor may include, for example, glue, phenolic resin, aminoplast resin, urea-formaldehyde resin, melamine-formaldehyde resin, urethane resin, multifunctional (meth) acrylates that can be polymerized in a free radical manner (e.g., aminoplast resins with side chain α,β-unsaturated groups, acrylated urethanes, acrylated epoxy resins, acrylated isocyanurates), epoxy resins (including bis-maleimide and fluorene-modified epoxy resins), isocyanurate resins, and mixtures thereof.
[0131] The basis weight of the make layer will necessarily vary depending on the intended use, the type of abrasive grains, and the nature of the coated abrasive belt being manufactured, but the basis weight will typically range from 1 gsm or 20 gsm to 200 gsm, 300 gsm, or even 400 gsm or more. The size layer precursor may be applied by any known coating method for applying a size layer precursor.
[0132] In frame 340, a size coating is applied to the embedded particles. A size coating precursor is applied to the at least partially cured primer layer precursor and abrasive particles. A size coating can be formed by applying a curable size coating precursor to the backing main surface. The size coating precursor can include, for example, glue, phenolic resin, amino plastic resin, urea-formaldehyde resin, melamine-formaldehyde resin, carbamate resin, multifunctional (meth) acrylates (e.g., amino plastic resins with hanging α, β-unsaturated groups, acrylated carbamates, acrylated epoxy resins, acrylated isocyanurates) that can be polymerized in a free radical manner, epoxy resins (including bis-maleimide and fluorene-modified epoxy resins), isocyanurate resins, and mixtures thereof. If a phenolic resin is used to form a primer layer, it is preferably also used to form a size coating. The size layer precursor can be applied by any known coating method for applying a size layer to a backing, including roller coating, extrusion die coating, curtain coating, knife coating, gravure coating, spray coating, etc. If desired, a presize layer precursor or a make layer precursor according to the present invention can also be used as a size layer precursor.
[0133] The basis weight of the size layer will also necessarily vary depending on the intended use, the type of abrasive grains, and the properties of the coated abrasive belt being manufactured, but the basis weight is typically in the range of 1 gsm or 50 gsm to 300 gsm, 400 gsm, or even 800 gsm or more. The size layer precursor can be applied by any known coating method for coating a size layer precursor (e.g., size coat) onto a backing, including, for example, roll coating, extrusion die coating, curtain coating, and spray coating.
[0134] Once applied, the size layer precursor and the usually partially cured base layer precursor are fully cured to provide a usable coated abrasive article. Generally speaking, the curing step involves thermal energy, but other forms of energy, such as radiation curing, may also be used. Available forms of thermal energy include, for example, thermal radiation and infrared radiation. Exemplary thermal energy sources include ovens (e.g., hanging ovens), heated rollers, hot air blowers, infrared lamps, and combinations thereof.
[0135] In addition to other components, the binder precursor (if present) in the make layer precursor and / or presize layer precursor of the coated abrasive tape according to the present disclosure may optionally contain a catalyst (e.g., a thermally activated catalyst or a photocatalyst), a free radical initiator (e.g., a thermal initiator or a photoinitiator), a curing agent to promote curing. Such catalysts (e.g., thermally activated catalysts or photocatalysts), free radical initiators (e.g., thermal initiators or photoinitiators) and / or curing agents may be any type known for use in coated abrasive tapes, including, for example, those described herein.
[0136] In addition to other components, the primer layer precursor and the size layer precursor may also contain optional additives, for example, to modify performance and / or appearance. Exemplary additives include grinding aids, fillers, plasticizers, wetting agents, surfactants, pigments, coupling agents, fibers, lubricants, thixotropic materials, antistatic agents, suspending agents and / or dyes.
[0137] Exemplary grinding aids can be organic or inorganic, including waxes, halogenated organic compounds, for example chlorinated waxes, such as tetrachloronaphthalene, pentachloronaphthalene, and polyvinyl chloride; halide salts, such as sodium chloride, potassium cryolite, sodium cryolite, ammonium cryolite, potassium tetrafluoroborate, sodium tetrafluoroborate, silicon fluoride, potassium chloride, magnesium chloride; and metals and their alloys, such as tin, lead, bismuth, cobalt, antimony, cadmium, iron, and titanium. Other examples of grinding aids include sulfur, organic sulfur compounds, graphite, and metal sulfides. Combinations of different grinding aids can be used.
[0138] Exemplary antistatic agents include conductive materials such as vanadium pentoxide (eg, dispersed in sulfonated polyester), wetting agents, carbon black and / or graphite in a binder.
[0139] Examples of fillers that can be used in the present disclosure include silicas such as quartz, glass beads, glass bubbles, and glass fibers; silicates such as talc, clay, (montmorillonite) feldspar, mica, calcium carbonate, calcium silicate, calcium metasilicate, sodium aluminosilicate, sodium silicate; metal sulfates such as calcium sulfate, barium sulfate, sodium sulfate, sodium aluminum sulfate, aluminum sulfate; gypsum; vermiculite; wood flour; aluminum trihydrate; carbon black; alumina; titanium dioxide; cryolite; cryolite; and metal sulfites (such as calcium sulfite).
[0140] In addition, in some embodiments, in frame 350, top glue coating is applied on the re-sizing coating.Top glue coating can include filler, grinding aid, lubricant, adhesive or other suitable materials.When present, top glue generally includes grinding aid and / or anti-filling material.Optional top glue layer can help to prevent or reduce the accumulation of grinding debris (material ground from workpiece) between abrasive particles, and this accumulation can significantly reduce the cutting ability of coated abrasive belt.Available top glue layer generally includes grinding aid (for example, potassium tetrafluoroborate), fatty acid metal salt (for example, zinc stearate or calcium stearate), salt of phosphate ester (for example, potassium behenyl phosphate), phosphate ester, urea-formaldehyde resin, mineral oil, cross-linked silane, cross-linked organosilicon and / or fluorinated compound.Useful top glue material is further described in for example U.S. Patent No. 5,556,437 (Lee et al.) and U.S. Patent No. 5,508,850 (Helmin). Typically, the amount of grinding aid included in the coated abrasive product is from about 50 gsm to about 700 gsm, more typically from about 80 gsm to about 500 gsm. The supersize may contain a binder, such as, for example, those used to make a size coat or make coat, but it need not have any binder.
[0141] Further details regarding the construction of coated abrasive articles comprising an abrasive layer secured to a backing, wherein the abrasive layer comprises abrasive grains and a make coat, a size coat, and an optional top coat are well known and can be found, for example, in U.S. Pat. Nos. 4,734,104 (Broberg); 4,737,163 (Larkey); 5,203,884 (Buchanan et al.); 5,152,917 (Pieper et al.); 5,378,251 (Culler et al.); 5,417,726 (Stout et al.); 5,436,063 (Fol. 5,496,386 (Broberg et al.); 5,609,706 (Benedict et al.); 5,520,711 (Helmin); 5,954,844 (Law et al.); 5,961,674 (Gagliardi et al.); 4,751,138 (Bange et al.); 5,766,277 (DeVoe et al.); 6,077,601 (DeVoe et al.); 6,228,133 (Thurber et al.); and 5,975,988 (Christianson).
[0142] Figure 4 A cross-sectional view of an exemplary abrasive article according to an embodiment of the present invention is shown. For example, the abrasive article 400 can be a grinding belt. The coated abrasive article 400 has a backing (substrate) 400. Abrasive particles 430 are connected to the backing 410 by a primer coating 412. The abrasive particles 430 are shown as equilateral triangles, but this is only exemplary. It is clearly envisioned that the abrasive particles 430 can be any suitable shape. The abrasive particles 430 can be covered by a size coating 440.
[0143] Coated abrasive articles generally include a backing, abrasive particles, and at least one binder that fixes the abrasive particles to the backing. The backing can be any suitable material, including cloth, polymer film, fiber, nonwoven web, paper, combinations thereof, and processed forms thereof. Suitable binders include inorganic binders or organic binders (including heat-curable resins and radiation-curable resins). The abrasive particles can be present in one layer or in two layers of the coated abrasive article.
[0144] The binder material may also contain a filler material or a grinding aid, usually in the form of a particulate material. Typically, the particulate material is an inorganic material. Examples of fillers that can be used in the present disclosure include: metal carbonates (e.g., calcium carbonate (e.g., chalk, calcite, marl, travertine, marble and limestone), calcium magnesium carbonate, sodium carbonate, magnesium carbonate), silica (e.g., quartz, glass beads, glass bubbles and glass fibers) silicates (e.g., talc, clay, (montmorillonite) feldspar, mica, calcium silicate, calcium metasilicate, sodium aluminate, sodium silicate) metal sulfates (e.g., calcium sulfate, barium sulfate, sodium sulfate, sodium aluminum sulfate, aluminum sulfate), gypsum, vermiculite, wood flour, aluminum trihydrate, carbon black, metal oxides (e.g., calcium oxide (lime), aluminum oxide, titanium dioxide) and metal sulfites (e.g., calcium sulfite).
[0145] Generally speaking, the addition of grinding aids can increase the useful life of abrasive articles. A grinding aid is a material that significantly affects the chemical and physical processes of grinding, resulting in improved performance. While not wanting to be limited by theory, it is believed that grinding aids can (a) reduce friction between the abrasive particles and the workpiece being ground; (b) prevent abrasive particles from "blocking" (i.e., preventing metal particles from being welded to the top of the abrasive particles), or at least reduce the tendency of abrasive particles to block; (c) reduce the interface temperature between the abrasive particles and the workpiece; or (d) reduce grinding forces.
[0146] Grinding aids are particularly useful in coated abrasive articles and bonded abrasive articles. In coated abrasive articles, grinding aids are typically used in a top size coat, which is applied to the surface of the abrasive particles. However, grinding aids are sometimes added to the size coat. Typically, the amount of grinding aid incorporated into a coated abrasive article is about 50 g / m 2 Up to 300g / m 2 (Desirably, about 80 g / m 2 Up to 160g / m 2 ). In vitrified bonded abrasive articles, grinding aids are typically impregnated into the pores of the article.
[0147] The abrasive particles can be uniformly distributed within the abrasive article or concentrated in selected areas or portions of the abrasive article. For example, in a coated abrasive, there can be two layers of abrasive particles. The first layer includes abrasive particles that are not shaped ceramic abrasive particles prepared according to the present disclosure, while the second (outermost) layer includes abrasive particles that are shaped ceramic abrasive particles prepared according to the present disclosure. Similarly, in a bonded abrasive, the grinding wheel can have two different parts. The outermost portion can include abrasive particles prepared according to the present disclosure, while the innermost layer does not include abrasive particles prepared according to the present disclosure. Alternatively, the shaped ceramic abrasive particles prepared according to the present disclosure can be uniformly distributed throughout the bonded abrasive article.
[0148] Further details regarding coated abrasive articles can be found, for example, in U.S. Pat. No. 4,734,104 (Broberg), U.S. Pat. No. 4,737,163 (Larkey), U.S. Pat. No. 5,203,884 (Buchanan et al.), U.S. Pat. No. 5,152,917 (Pieper et al.), U.S. Pat. No. 5,378,251 (Culler et al.), U.S. Pat. No. 5,417,726 (Stout et al.), U.S. Pat. No. 5,436,063 (Follett et al.), U.S. Pat. No. 5,496,386 (Broberg et al.), U.S. Pat. No. 5,609,706 (Benedict et al.), U.S. Pat. No. 5,520,711 (Helmin), U.S. Pat. No. 5,954,844 (Law et al.), U.S. Pat. No. 5,961,674 (Gagliardi et al.), and U.S. Pat. No. 5,975,988 (Christianson). Further details regarding bonded abrasive articles can be found, for example, in U.S. Pat. No. 4,543,107 (Rue), U.S. Pat. No. 4,741,743 (Narayanan et al.), U.S. Pat. No. 4,800,685 (Haynes et al.), U.S. Pat. No. 4,898,597 (Hay et al.), U.S. Pat. No. 4,997,461 (Markhoff-Matheny et al.), U.S. Pat. No. 5,037,453 (Narayanan et al.), U.S. Pat. No. 5,110,332 (Narayanan et al.), and U.S. Pat. No. 5,863,308 (Qi et al.). More details about vitreous bonded abrasives can be found, for example, in U.S. Pat. No. 4,543,107 (Rue), U.S. Pat. No. 4,898,597 (Hay et al.), U.S. Pat. No. 4,997,461 (Markhoff-Matheny et al.), U.S. Pat. No. 5,094,672 (Giles Jr. et al.), U.S. Pat. No. 5,118,326 (Sheldon et al.), U.S. Pat. No. 5,131,926 (Sheldon et al.), U.S. Pat. No. 5,203,886 (Sheldon et al.), U.S. Pat. No. 5,282,875 (Wood et al.), U.S. Pat. No. 5,738,696 (Wu et al.), and U.S. Pat. No. 5,863,308 (Qi). More details about nonwoven abrasive articles can be found, for example, in U.S. Pat. No. 2,958,593 (Hoover et al.).
[0149] The present disclosure provides a method of grinding a surface, the method comprising contacting at least one shaped ceramic abrasive particle prepared according to the present disclosure with a surface of a workpiece; and moving at least one of the shaped ceramic abrasive particle or the contact surface to grind at least a portion of the surface with the abrasive particle. The methods of grinding with the shaped ceramic abrasive particles prepared according to the present disclosure range from rough grinding (i.e., high pressure and high cutting) to polishing (e.g., polishing medical implants with coated grinding belts), wherein the latter is generally accomplished with finer grades (e.g., ANSI 220 and finer) of abrasive particles. The shaped ceramic abrasive particles can also be used in precision grinding applications, such as grinding camshafts with vitrified bonded wheels. The size of the abrasive particles used for a particular grinding application will be apparent to those skilled in the art.
[0150] Grinding with shaped ceramic abrasive particles prepared according to the present disclosure can be accomplished dry or wet. For wet grinding, the introduced liquid can be provided in the form of a light mist to a full stream of water. Examples of commonly used liquids include: water, water-soluble oils, organic lubricants, and emulsions. These liquids can be used to reduce the heat associated with grinding and / or act as a lubricant. The liquid can contain trace amounts of additives, such as fungicides, defoamers.
[0151] Shaped ceramic abrasive particles prepared according to the present disclosure can be used, for example, to abrade workpieces such as aluminum metal, carbon steel, mild steel, tool steel, stainless steel, hardened steel, titanium, glass, ceramics, wood, wood-like materials (e.g., plywood and particle board), coatings, painted surfaces, organic coated surfaces, etc. The force applied during abrasion is typically in the range of about 1 kilogram to about 100 kilograms.
[0152] Objects and advantages of this disclosure are further illustrated by the following non-limiting examples, but the particular materials and amounts thereof recited in these examples, as well as other conditions and details, should not be construed to unduly limit this disclosure.
[0153] Example
[0154] Unless otherwise indicated, all parts, percentages, ratios, etc. in the examples and the rest of the specification are by weight.
[0155] Unit abbreviations used in the examples: gsm = grams per square meter, °C = degrees Celsius; cm = centimeter; mm = millimeter; μm = micrometer; FPM = feet per minute and kV = kilovolts.
[0156] Table 2 below reports the materials used in the examples.
[0157] Table 2
[0158]
[0159]
[0160] Table 3
[0161]
[0162] Example 1: Coated abrasive sample
[0163] Preparation of coated abrasive sample of Example 1 (Example 1-A-2)
[0164] The coated abrasive samples were prepared by coating a 12" wide backing PEB with MR1 using a roll coater to deliver a weight of 210 gsm (grams per square meter). Abrasive particles 250 were electrostatically coated into the primer resin at a mineral weight of 546 gsm. The samples were cured at 90°C for 90 minutes and at 102°C for 1 hour. Next, the samples were size coated with SZ2 using a roll coater to a weight of 609 gsm. The samples were cured at 90°C for 60 minutes and at 1 02°C for 1 hour. Next, the sample was topcoated with SSZ2 using a roll coater to a weight of 483 gsm. Finally, the sample was cured at 90°C for 30 minutes, at 102°C for 12 hours, and at 110°C for 1 hour. The tape was then converted to 7.62 cm x 335.28 cm for testing using Grinding Test 1, and to 7.62 cm x 91.44 cm for testing using Grinding Tests 2, 3, 5, 6.
[0165] Preparation of coated abrasive samples of Examples 2 and 3
[0166] Coated abrasive samples were prepared by coating a 4" wide backing PEB with MR1 using a knife coating kit to deliver a weight of 210 gsm. Abrasive particles 250 were electrostatically coated into the primer resin to achieve the specified weight in gsm as shown in Table 3. The samples were cured at 90°C for 90 minutes and at 102°C for 1 hour. Next, the samples were oversize coated with SZ1 or SZ2 using a 3" coating roller to the specified weight in gsm as shown in Table 3. The samples were cured at 90°C for 60 minutes and at 102°C for 1 hour. Next, the samples were topsize coated to the weight in gsm as shown in Table 3. Finally, the samples were cured at 90°C for 30 minutes, at 102°C for 12 hours, and at 110°C for 1 hour. The tape was then converted to 7.62 cm x 91.44 cm for testing.
[0167] Performance Testing
[0168] Grinding test 1
[0169] Grinding Test 1 (GT1) was conducted using a Hammond Back Stand Polishing and Buffing Machine Model #10-ROH-D-VFD, Series #11368, obtained from Hammond RotoFinish, Kalamazoo, MI. A 35.56 cm diameter 90 Durometer contact wheel with a 1 to 1 sawtooth pattern having 0.95 cm x 0.95 grooves was used. The test was conducted using a 7.62 cm x 335.28 cm abrasive belt. The belt was run at 1800 rpm. The workpiece was a 304 stainless steel bar measuring 1.9 cm x 1.9 cm x 60.96 cm, with the surface to be ground measuring 1.9 cm x 1.9 cm. Ten workpieces were used for each test. The weight (in grams) of each workpiece was recorded before each grinding cycle.
[0170] During each grinding cycle, an overhead table equipped with a pneumatic cylinder is used to force each workpiece into the belt. The entire test is conducted at one of three force settings: 5.54 kg (12.2 lb) (low pressure or "LP"), 10.08 kg (22.2 lb) (medium pressure or "MP"), and 13.63 kg (30 lb) (high pressure or "HP"), depending on the desired test pressure. One of the 10 workpieces is plunged into the center of the belt, removed after 8 seconds, placed in room temperature water to cool for at least 10 seconds, dried with a paper towel, and the weight loss (in grams) of the workpiece for the 8-second plunge is recorded. The remaining 9 workpieces are then ground, cooled, and weighed in the same manner until all 10 workpieces are ground. This set of 10 plunges is called a "cycle."
[0171] An additional cycle of 10 plunges was then performed in the same manner. At a certain point, 50% of the area of the grinding surface of the workpiece was oxidized due to overheating, which was visually indicated by a blue discoloration. The cycle of observing discoloration was completed so that all 10 workpieces had been plunged the same number of times. At this point, the test was completed.
[0172] The results of grinding test 1 are shown in Table 4. The total cutting (GT1 total cutting) in grams is calculated by adding the weight loss data of all cycles of all 10 workpieces. Depending on the pressure selected for the test, the result can be referred to as GT1 total cutting LP, GT1 total cutting MP or GT1 total cutting HP. The initial cutting (GT1 initial cutting LP, GT1 initial cutting MP or GT1 initial cutting HP) in grams is calculated by adding the weight loss data of the first 2 cycles of all 10 workpieces. The total weight loss data after the first 3 cycles is deducted from the total weight loss data after the first 15 cycles and the result is divided by twelve to calculate the cutting rate (GT1 cutting rate LP, GT1 cutting rate MP, GT1 cutting rate HP) (in grams) of each cycle.
[0173] Grinding test 2
[0174] Grinding Test 2 (GT2) was conducted on a 10.16 cm × 91.44 cm belt converted from a coated abrasive sample. A 20.3 cm diameter 70 durometer rubber (1:1 facet to groove ratio) serrated contact wheel was used. The belt was run at 2750 rpm. The workpiece was a 304 stainless steel bar measuring 1.9 cm × 1.9 cm × 60.96 cm, on which the surface to be ground measured 1.9 cm × 1.9 cm. The workpiece weight was recorded in grams, and then the workpiece was pressed into the center portion of the belt with a normal force varying from 4.5 kg to 6.8 kg. Each test cycle consisted of 16 seconds of grinding. The workpiece was then cooled by quenching the 1.3 cm grinding end of the workpiece in 15.5 ° C water for 8 seconds, followed by a continuous jet of pressurized air for 10 seconds to dry the workpiece. The workpiece was then weighed to determine the amount of material removed in grams, thereby ending the cycle. The final workpiece weight from the previous cycle was used as the initial workpiece weight for the subsequent cycle. If the final mass of the workpiece after wear weighs less than 275 grams, a new 304 stainless steel bar of dimensions 1.9 cm x 1.9 cm x 60.96 cm is weighed and used for subsequent cycles. The test is terminated after 40 cycles. The initial cut in grams (GT2 initial cut) is defined as the total amount cut after 2 cycles. The cutting rate in grams (GT2 cutting rate) is defined as the total amount cut after 10 cycles minus the total amount cut after 3 cycles, divided by 7. The total cut in grams (GT2 total cut) is defined as the total amount cut after 40 cycles.
[0175] Grinding test 3
[0176] Grinding Test 3 (GT3) was conducted on a 10.16 cm × 91.44 cm belt converted from a coated abrasive sample. A 20.3 cm diameter 70 durometer rubber (1:1 facet to groove ratio) serrated contact wheel was used. The belt was run at 2750 rpm. The workpiece was a 304 stainless steel bar measuring 1.9 cm × 1.9 cm × 60.96 cm, on which the surface to be ground measured 1.9 cm × 1.9 cm. The workpiece weight was recorded in grams, and then the workpiece was pressed into the center portion of the belt with a normal force varying from 6.8 kg to 11.3 kg. Each test cycle consisted of 16 seconds of grinding. The workpiece was then cooled by quenching the 1.3 cm grinding end of the workpiece in 15.5 ° C water for 8 seconds, followed by a continuous jet of pressurized air for 10 seconds to dry the workpiece. The workpiece was then weighed to determine the amount of material removed in grams, thereby ending the cycle. The final workpiece weight from the previous cycle was used as the initial workpiece weight for the subsequent cycle. If the final mass of the workpiece after wear weighs less than 275 grams, a new 304 stainless steel bar of dimensions 1.9 cm x 1.9 cm x 60.96 cm is weighed and used for subsequent cycles. The test is terminated after 40 cycles. The initial cut in grams (GT3 initial cut) is defined as the total amount cut after 2 cycles. The cutting rate in grams (GT3 cutting rate) is defined as the total amount cut after 10 cycles minus the total amount cut after 3 cycles, divided by 7. The total cut in grams (GT3 total cut) is defined as the total amount cut after 40 cycles.
[0177] Grinding test 4
[0178] Grinding Test 4 (GT4) was conducted on a 10.16 cm x 91.44 cm belt converted from a coated abrasive sample. A 20.3 cm diameter 70 durometer rubber (1:1 land to groove ratio) serrated contact wheel was used. The belt was run at 2750 rpm. The workpiece was a 304 stainless steel bar measuring 1.9 cm x 1.9 cm x 60.96 cm, with the surface to be ground measuring 1.9 cm x 1.9 cm. The workpiece weight was recorded in grams, and the workpiece was then pressed into the center portion of the belt. Testing was conducted at one of three force settings: 5.9 kg (13 lb) (low pressure or "LP"), 8.62 kg (19 lb) (medium pressure or "MP"), and 11.34 kg (25 lb) (high pressure or "HP"), depending on the desired test pressure. Each test cycle consisted of 6 seconds of grinding. The workpiece is then cooled by quenching the 1.3 cm grinding end of the workpiece in 15.5°C water for 8 seconds, followed by a continuous jet of pressurized air for 10 seconds to dry the workpiece. The workpiece is then weighed to determine the amount of material removed in grams, thereby ending the cycle. The final workpiece weight from the previous cycle is used as the initial workpiece weight for the subsequent cycle. If the final mass of the workpiece after wear weighs less than 275 grams, a new 304 stainless steel bar with dimensions of 1.9 cm×1.9 cm×60.96 cm is weighed and used for the subsequent cycle. The test ends after 120 cycles. The initial cut in grams (GT4 initial cut) is defined as the total amount cut after 5 cycles. The cutting rate in grams (GT4 cutting rate) is defined as the total amount cut after 40 cycles minus the total amount cut after 8 cycles, divided by thirty-two. The total cut in grams (GT4 total cut) is defined as the total amount cut after 120 cycles. Depending on the pressure selected, the result may be referred to as GT4 initial cut LP, GT4 initial cut MP, GT4 initial cut HP, GT4 cut rate LP, GT4 cut rate MP, GT4 cut rate HP, GT4 total cut LP, GT4 total cut MP or GT4 total cut HP.
[0179] Grinding test 5
[0180] Grinding Test 5 (GT5) was conducted on a 10.16 cm × 91.44 cm belt converted from a coated abrasive sample. A 20.3 cm diameter 70 durometer rubber (1:1 facet to groove ratio) serrated contact wheel was used. The belt was run at 2750 rpm. The workpiece was a 304 stainless steel bar measuring 1.9 cm × 1.9 cm × 60.96 cm, on which the surface to be ground measured 1.9 cm × 1.9 cm. The workpiece weight was recorded in grams, and then the workpiece was pressed into the center portion of the belt with a normal force varying from 3.2 kg to 4.5 kg. Each test cycle consisted of 16 seconds of grinding. The workpiece was then cooled by quenching the 1.3 cm grinding end of the workpiece in 15.5 ° C water for 8 seconds, followed by a continuous jet of pressurized air for 10 seconds to dry the workpiece. The workpiece was then weighed to determine the amount of material removed in grams, thereby ending the cycle. The final workpiece weight from the previous cycle was used as the initial workpiece weight for the subsequent cycle. If the final mass of the workpiece after wear weighs less than 275 grams, a new 304 stainless steel bar of dimensions 1.9 cm x 1.9 cm x 60.96 cm is weighed and used for subsequent cycles. The test is terminated after 30 cycles. The initial cut in grams (GT5 initial cut) is defined as the total amount cut after 2 cycles. The cutting rate in grams (GT5 cutting rate) is defined as the total amount cut after 10 cycles minus the total amount cut after 3 cycles, divided by 7. The total cut in grams (GT5 total cut) is defined as the total amount cut after 30 cycles.
[0181] Grinding Test 6
[0182] Grinding Test 6 (GT6) was conducted on a 10.16 cm × 91.44 cm belt converted from a coated abrasive sample. A 20.3 cm diameter 70 durometer rubber (1:1 facet to groove ratio) serrated contact wheel was used. The belt was run at 2750 rpm. The workpiece was a 304 stainless steel bar measuring 1.9 cm × 1.9 cm × 60.96 cm, on which the surface to be ground measured 1.9 cm × 1.9 cm. The workpiece weight was recorded in grams, and then the workpiece was pressed into the center portion of the belt with a normal force of 2.3 kg. Each test cycle consisted of 16 seconds of grinding. The workpiece was then cooled by quenching the 1.3 cm grinding end of the workpiece in 15.5 ° C water for 8 seconds, followed by a continuous jet of pressurized air for 10 seconds to dry the workpiece. The workpiece was then weighed to determine the amount of material removed in grams, thereby ending the cycle. The final workpiece weight from the previous cycle was used as the initial workpiece weight for the subsequent cycle. If the final mass of the workpiece after wear weighs less than 275 grams, a new 304 stainless steel bar with dimensions of 1.9 cm x 1.9 cm x 60.96 cm is weighed and used for subsequent cycles. The test is terminated after 30 cycles. The initial cut in grams (GT6 initial cut) is defined as the total amount cut after 2 cycles. The cutting rate in grams (GT6 cutting rate) is defined as the total amount cut after 10 cycles minus the total amount cut after 3 cycles, divided by 7. The total cut in grams (GT6 total cut) is defined as the total amount cut after 30 cycles.
[0183] Table 4 Figure 7 Shown in.
[0184] Table 5 Figure 8 Shown in.
[0185] Table 6 :
[0186]
[0187] Table 7 :
[0188]
[0189] Table 8 :
[0190]
Claims
1. An abrasive product, comprising: Backing; a primer coating applied on the backing; a plurality of shaped abrasive particles embedded in the make coat; wherein the plurality of shaped abrasive particles has a coating weight greater than 300 particles per square inch; and wherein according to Grinding Test 1, the abrasive article exhibits a GT1 Total Cut LP of at least 975 grams, a GT1 Total Cut MP of at least 4250 grams, and a GT1 Total Cut HP of at least 5075 grams when used to abrade a substrate. 2 . The abrasive article of claim 1 , wherein each shaped abrasive particle of the plurality of shaped abrasive particles has a side length of at least 50 μm and less than 3000 μm. 3 . The abrasive article of claim 1 , wherein each shaped abrasive particle of the plurality of shaped abrasive particles has a side length of at least 200 μm and less than 2900 μm.
4. The abrasive article of claim 1, wherein each shaped abrasive particle of the plurality of shaped abrasive particles has a side length of at least 1275 μm and less than 1525 μm.
5. The abrasive article of claim 1, wherein each shaped abrasive particle of the plurality of shaped abrasive particles has a side length of at least 575 μm and less than 750 μm.
6. The abrasive article of claim 1, wherein each shaped abrasive particle of the plurality of shaped abrasive particles has a side length of at least 450 μm and less than 575 μm.
7. The abrasive article of claim 1, wherein each shaped abrasive particle of the plurality of shaped abrasive particles has an aspect ratio of at least 3:1 and less than 7:
1.
8. The abrasive article of claim 1, wherein each shaped abrasive particle of the plurality of shaped abrasive particles has an aspect ratio of at least 3:1 and less than 6:
1.
9. The abrasive article of claim 1, wherein the coating weight is at least 320 grains per square inch.
10. The abrasive article of claim 1, wherein the coating weight is at least 400 grains per square inch.
11. The abrasive article of claim 1, wherein the coating weight is less than 480 particles per square inch.
12. The abrasive article of claim 1, wherein a majority of the shaped abrasive particles are oriented with pointed ends pointing away from the backing.
13. The abrasive article of claim 1, wherein a majority of the shaped abrasive particles are oriented such that a similar surface in a face of each of the majority of the shaped abrasive particles is oriented with respect to a grinding direction.
14. The abrasive article of claim 1, wherein the abrasive article exhibits improved abrasive weight loss.
15. The abrasive article of claim 1, wherein the plurality of shaped abrasive particles are shaped such that each shaped abrasive particle comprises: A first surface is opposite to a second surface, the first surface and the second surface being separated by a substantially constant thickness.
16. The abrasive article of claim 15, wherein the abrasive particles are dish-shaped abrasive particles.
17. The abrasive article of claim 1, wherein the abrasive article comprises an abrasive belt.
18. An abrasive article, comprising: Backing; a primer coating applied on the backing; a plurality of shaped abrasive particles embedded in the make coat; wherein the plurality of shaped abrasive particles has a coating weight greater than 300 particles per square inch; and wherein according to Grinding Test 4, the abrasive article exhibits a GT4 Total Cut LP of at least 390, a GT4 Total Cut MP of at least 800, and a GT4 Total Cut HP of at least 1100 grams when used to abrade a substrate.
19. The abrasive article of claim 18, wherein each shaped abrasive particle of the plurality of shaped abrasive particles has an edge length of at least 50 μm and less than 3000 μm.
20. The abrasive article of claim 18, wherein each shaped abrasive particle of the plurality of shaped abrasive particles has an edge length of at least 200 μm and less than 2900 μm.
21. The abrasive article of claim 18, wherein each shaped abrasive particle of the plurality of shaped abrasive particles has an edge length of at least 1275 μm and less than 1525 μm.
22. The abrasive article of claim 18, wherein each shaped abrasive particle of the plurality of shaped abrasive particles has an edge length of at least 575 μm and less than 750 μm.
23. The abrasive article of claim 18, wherein each shaped abrasive particle of the plurality of shaped abrasive particles has an edge length of at least 450 μm and less than 575 μm.
24. The abrasive article of claim 18, wherein each shaped abrasive particle of the plurality of shaped abrasive particles has an aspect ratio of at least 3:1 and less than 7:
1.
25. The abrasive article of claim 18, wherein each shaped abrasive particle of the plurality of shaped abrasive particles has an aspect ratio of at least 3:1 and less than 6:
1.
26. The abrasive article of claim 18, wherein the coating weight is at least 320 grains per square inch.
27. The abrasive article of claim 18, wherein the coating weight is at least 400 particles per square inch.
28. The abrasive article of claim 18, wherein the coating weight is less than 480 particles per square inch.
29. The abrasive article of claim 18, wherein a majority of the shaped abrasive particles are oriented with pointed ends pointing away from the backing.
30. The abrasive article of claim 18, wherein a majority of the shaped abrasive particles are oriented such that a similar surface in a face of each of the majority of the shaped abrasive particles is oriented with respect to a grinding direction.
31. The abrasive article of claim 18, wherein the abrasive article exhibits improved abrasive weight loss.
32. The abrasive article of claim 18, wherein the plurality of shaped abrasive particles are shaped such that each shaped abrasive particle comprises: A first surface is opposite to a second surface, the first surface and the second surface being separated by a substantially constant thickness.
33. The abrasive article of claim 32, wherein the plurality of shaped abrasive particles are dish-shaped particles.
34. The abrasive article of claim 18, wherein the abrasive article comprises an abrasive belt.
35. A method of making an abrasive article, the method comprising: depositing a resin primer layer on the backing; Embedding a plurality of abrasive particles into the resin make coat, wherein the embedding comprises: depositing the plurality of abrasive grains; orienting the plurality of abrasive particles such that a majority of the abrasive particles are oriented with pointed ends pointing away from a backing; and wherein the plurality of abrasive particles are deposited at a coating weight of at least 300 particles per square inch; and The resin primer layer is cured.
36. The method of claim 35, wherein the plurality of abrasive grains have an aspect ratio between 3:1 and 7:
1.
37. The method of claim 35, wherein the plurality of abrasive particles have an aspect ratio between 3:1 and 6:
1.
38. The method of claim 35, wherein a similar surface of each abrasive in the majority of abrasives is oriented relative to a grinding direction.
39. The method of claim 1 wherein the coating weight is at least 350 particles per square inch.
40. The method of claim 1 wherein the coating weight is at least 400 particles per square inch.
41. The method of claim 1 wherein the coating weight is at least 500 particles per square inch.
42. The method of claim 1, wherein each of the plurality of abrasive particles has a first curved surface, the first curved surface and a second curved surface separated by a thickness.