Modified sulfide solid electrolyte, manufacturing method thereof, electrode composite material and lithium ion battery
A modified sulfide solid electrolyte with heterocyclic rings improves coating adaptability and battery performance by attaching a compound with carbon and oxygen atoms, addressing manufacturing challenges and enhancing lithium-ion battery production efficiency.
Patent Information
- Application Number
- CN202380030536.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-28
- Publication Date
- 2024-12-06
AI Technical Summary
Existing sulfide solid electrolytes with large specific surface areas face challenges in coating adaptability and viscosity issues, leading to reduced battery performance during the manufacturing process, which complicates the production of lithium-ion batteries.
A modified sulfide solid electrolyte is developed by attaching a compound with two or more heterocyclic rings having carbon and oxygen atoms to the surface of a sulfide solid electrolyte, which improves coating adaptability and maintains excellent battery performance.
The modified sulfide solid electrolyte exhibits enhanced coating suitability and effective battery performance, facilitating efficient manufacturing of lithium-ion batteries with improved density and reduced drying time, effectively addressing the viscosity and coating adaptability issues.
Smart Images

Figure BDA0005060546740000071 
Figure BDA0005060546740000121 
Figure BDA0005060546740000231
Abstract
Description
Technical Field
[0001] The invention relates to a modified sulfide solid electrolyte and a preparation method thereof, an electrode composite material and a lithium ion battery. Background Art
[0002] In recent years, with the rapid spread of information-related devices and communication devices such as personal computers, video cameras and mobile phones, the development of batteries used as their power sources has also attracted attention. Among them, lithium-ion batteries have attracted attention due to their high energy density.
[0003] In the past, an electrolyte containing a flammable organic solvent was used in a battery for such a purpose, and therefore, a safety device for suppressing the temperature rise during a short circuit, a structure for preventing a short circuit, and improvements in materials were required. In contrast, by changing the electrolyte to a solid electrolyte and making the battery fully solid, a flammable organic solvent is not used in the battery, and the safety device is simplified, and the manufacturing cost and productivity are excellent, so a battery in which the electrolyte is replaced by a solid electrolyte layer is developed.
[0004] As a solid electrolyte used in a solid electrolyte layer, a sulfide solid electrolyte is known in the past, and it is first desired to improve the ion conductivity of the sulfide solid electrolyte. For example, in order to improve the ion conductivity, a method for producing a composite solid electrolyte obtained by coating the surface of a sulfide solid electrolyte with a predetermined halogenated hydrocarbon compound as a coating material has been proposed (for example, see Patent Document 1).
[0005] As a surface coating technology, for example, Patent Document 2 discloses a solid electrolyte composition obtained by forming a coating film on the surface of a sulfide solid electrolyte using a compound having a C=O bond or a compound having an S=O bond in order to improve the affinity between an active material used in a negative electrode, a positive electrode, etc. when manufacturing a lithium ion battery and a solid electrolyte. In addition, Patent Document 3 discloses that in a sulfide solid electrolyte containing lithium, phosphorus, and sulfur and also containing an ester compound of a carboxylic acid and an alcohol, the ester compound is bonded or adsorbed to the surface of the conductive sulfide to improve the cycle characteristics of the solid battery, and the solid sulfide electrolyte is obtained by a production method having a step of wet-grinding a slurry containing a lithium ion conductive sulfide, an organic solvent, and an ester compound.
[0006] Furthermore, for example, Patent Document 4 discloses: a method for producing a solid electrolyte comprising mixing an anionic surfactant such as sulfosuccinate salt or benzenesulfonate as a monomer or oligomer, a solvent, and a sulfide solid electrolyte, and then removing the solvent; and a solid electrolyte containing a predetermined amount of the surfactant in terms of specific surface area. Furthermore, the invention discloses that the generation of hydrogen sulfide and the coarsening of the particle size are suppressed by using a surfactant.
[0007] As described above, in recent years, with the goal of practical application of lithium-ion batteries, there have been diverse demands for improving not only the ion conductivity of the sulfide solid electrolyte itself but also other performances. In order to meet such demands, surface coating technology has been applied.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2020-87633
[0011] Patent Document 2: Japanese Patent Application Publication No. 2017-147173
[0012] Patent Document 3: International Publication No. 2020 / 203231
[0013] Patent Document 4: International Publication No. 2021 / 029315 Summary of the invention
[0014] Technical problem to be solved by the invention
[0015] The present invention has been made in view of such actual conditions, and its object is to provide a modified sulfide solid electrolyte and a method for producing the same, which has excellent coating adaptability when applied as a paste and can effectively exhibit excellent battery performance even if the sulfide solid electrolyte has a large specific surface area. In addition, the present invention aims to provide an electrode composite material and a lithium ion battery exhibiting excellent battery performance.
[0016] Solutions for solving the above technical problems
[0017] The modified sulfide solid electrolyte of the present invention is:
[0018] A modified sulfide solid electrolyte, comprising: a sulfide solid electrolyte having a BET specific surface area of 10 m 2 / g or more and containing a lithium atom, a sulfur atom, a phosphorus atom and a halogen atom; and having two or more heterocyclic rings having carbon atoms and oxygen atoms.
[0019] In addition, the method for producing the modified sulfide solid electrolyte of the present invention is:
[0020] A method for preparing a modified sulfide solid electrolyte comprises: mixing a sulfide solid electrolyte, a compound having two or more heterocyclic rings having carbon atoms and oxygen atoms, and an organic solvent, wherein the sulfide solid electrolyte has a BET specific surface area of 10 m 2 / g or more and contains lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms;
[0021] The organic solvent is removed.
[0022] The electrode composite material of the present invention is:
[0023] An electrode composite material comprises the modified sulfide solid electrolyte of the present invention and an electrode active material.
[0024] Furthermore, the lithium ion battery of the present invention is,
[0025] A lithium ion battery comprises at least one of the modified sulfide solid electrolyte of the present invention and the electrode composite material of the present invention.
[0026] Effects of the Invention
[0027] According to the present invention, a modified sulfide solid electrolyte having excellent coating adaptability when applied as a paste and capable of effectively exhibiting excellent battery performance and a method for producing the same can be provided. In addition, according to the present invention, an electrode composite material and a lithium ion battery exhibiting excellent battery performance can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 CV curves of the modified sulfide solid electrolytes of Examples 2, 9, 11, and 13 and the sulfide solid electrolyte of Comparative Example 1. DETAILED DESCRIPTION
[0029] Hereinafter, an embodiment of the present invention (hereinafter sometimes referred to as "the present embodiment") is described. In addition, in this specification, the upper and lower limits of the numerical ranges of "above", "below", and "to" are numerical values that can be combined arbitrarily, and the numerical values of the embodiments can also be used as the upper and lower limits.
[0030] (Discovery made by the inventors to complete the present invention)
[0031] The present inventors have conducted intensive studies to solve the above-mentioned technical problems and, as a result, have found the following matters and have completed the present invention.
[0032] Conventionally, there is a technique for coating a certain compound on the surface of a sulfide solid electrolyte, as in Patent Documents 1 to 4. The problem of the techniques in Patent Documents 1 to 4 is to improve the battery performance such as improving the ion conductivity and improving the affinity between the active material used in the negative electrode, positive electrode, etc. when manufacturing a lithium ion battery and the sulfide solid electrolyte, thereby improving the cycle characteristics.
[0033] However, in the manufacturing process of lithium-ion batteries (also called "all-solid batteries"), a paste mixed with a solid electrolyte, other specified components and a solvent is prepared and applied to form a diaphragm layer and an electrode composite material layer. In order to improve the performance of these layers, it is necessary to increase the density of the solid electrolyte constituting these layers. For the increase in this density, it is effective to use a solid electrolyte with a large specific surface area.
[0034] Thus, there is a requirement to use a solid electrolyte with a large specific surface area as the solid electrolyte, but if the specific surface area of the solid electrolyte is large, there will be manufacturing problems such as increased viscosity of the paste and significantly reduced coating adaptability. On the other hand, although the coating adaptability of the paste can be improved by reducing the viscosity of the paste by using a large amount of solvent, there will be problems such as a longer drying time and a decrease in the density of the solid electrolyte constituting the layer, which leads to reduced battery performance. Therefore, the coating adaptability of the paste is in a contradictory relationship with obtaining higher battery performance. In addition, a solid electrolyte with a large specific surface area of 10m 2 When a sulfide solid electrolyte having a viscosity of more than 100 μg is prepared as a paste, the viscosity becomes high, which not only significantly reduces the coating suitability, but also requires a large amount of solvent to reduce the viscosity of the paste, thereby prolonging the drying time and significantly reducing the battery performance due to the reduction in density.
[0035] As described in Patent Documents 1 to 4, a lot of research has been conducted on technical issues such as improving ion conductivity and battery performance. However, the present inventors have noticed that, with the rapid progress in the practical application of lithium-ion batteries, no research has been conducted on methods for improving performance in the manufacturing process such as the coating adaptability of the paste with a view to mass production.
[0036] The present inventors have continued to conduct intensive research based on the techniques disclosed in Patent Documents 1 to 4 for coating a certain compound on the surface of a sulfide solid electrolyte and have found that even a sulfide solid electrolyte with a large specific surface area of 10 m 2A sulfide solid electrolyte with a specific surface area of 10 m / s or more can be made into a sulfide solid electrolyte with excellent coating adaptability when applied as a paste and can effectively demonstrate excellent battery performance by attaching a compound having two or more heterocyclic rings having carbon atoms and oxygen atoms to the surface. By attaching a compound having two or more heterocyclic rings having carbon atoms and oxygen atoms to the surface of the sulfide solid electrolyte, even if the specific surface area is large and is 10 m / s, the sulfide solid electrolyte can be made into a sulfide solid electrolyte with excellent coating adaptability when applied as a paste and can effectively demonstrate excellent battery performance. 2 / g or more, even a sulfide solid electrolyte can obtain an effect of excellent coating suitability when applied as a paste, which is a surprising phenomenon that has never been recognized so far.
[0037] In this specification, "solid electrolyte" refers to an electrolyte that remains solid at 25° C. in a nitrogen atmosphere. The "sulfide solid electrolyte" obtained by the production method of this embodiment is a solid electrolyte containing lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms, and having ion conductivity caused by lithium atoms.
[0038] The "sulfide solid electrolyte" includes both crystalline sulfide solid electrolytes and amorphous sulfide solid electrolytes having a crystal structure. In this specification, the crystalline sulfide solid electrolyte refers to a solid electrolyte in which a peak derived from a solid electrolyte is observed in an X-ray diffraction pattern in a powder X-ray diffraction (XRD) measurement, and is a material that is independent of whether or not there is a peak derived from a raw material of the solid electrolyte. That is, the crystalline sulfide solid electrolyte includes a crystal structure derived from a solid electrolyte, and a part of it may be a crystal structure derived from the solid electrolyte, or all of it may be a crystal structure derived from the solid electrolyte. In addition, as long as the crystalline sulfide solid electrolyte has the above-mentioned X-ray diffraction pattern, it may also include an amorphous sulfide solid electrolyte (also referred to as a "glass component") in a part thereof. Therefore, the crystalline sulfide solid electrolyte includes so-called glass ceramics obtained by heating an amorphous solid electrolyte (glass component) to a crystallization temperature or above.
[0039] In addition, in this specification, an amorphous sulfide solid electrolyte (glass component) means that in powder X-ray diffraction (XRD) measurement, the X-ray diffraction pattern is a halo pattern in which substantially no peaks other than peaks derived from the material are observed, regardless of the presence or absence of peaks derived from the raw materials of the solid electrolyte.
[0040] In the present embodiment, the above distinction between crystallinity and amorphousness is also applicable to both the sulfide solid electrolyte and the modified sulfide solid electrolyte.
[0041] (Various Aspects of the Present Embodiment)
[0042] The modified sulfide solid electrolyte of the first embodiment of the present embodiment is,
[0043] A modified sulfide solid electrolyte, comprising: a sulfide solid electrolyte having a BET specific surface area of 10 m 2 / g or more and containing a lithium atom, a sulfur atom, a phosphorus atom and a halogen atom; and having two or more heterocyclic rings having carbon atoms and oxygen atoms.
[0044] As the sulfide solid electrolyte containing lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms, a sulfide solid electrolyte obtained by a conventional method, for example, using lithium sulfide, phosphorus pentasulfide, lithium halide, monomeric halogen, etc. as raw materials can be typically exemplified. That is, the modified sulfide solid electrolyte of the present embodiment includes a sulfide solid electrolyte having a BET specific surface area of 10 m2 obtained by a conventional method. 2 / g or more sulfide solid electrolyte having a large specific surface area, and a compound having two or more heterocyclic rings having carbon atoms and oxygen atoms (hereinafter sometimes referred to as "heteropolycyclic compound").
[0045] In the past, the BET specific surface area was relatively large, only 10m 2 In a sulfide solid electrolyte having a content of more than 100 g, the coating performance of the paste containing the required content to ensure the density of the solid electrolyte in the layer in order to exhibit the specified battery performance is significantly reduced, and it is extremely difficult to effectively form the positive electrode, the negative electrode, and the electrolyte layer. The sulfide solid electrolyte of this embodiment has a significantly improved coating adaptability by containing a conventional sulfide solid electrolyte and a heteropolycyclic compound, that is, it should be called a "modified sulfide solid electrolyte" because it is "modified".
[0046] The modified sulfide solid electrolyte of this embodiment needs to use a heteropolycyclic compound having two or more heterocyclic rings among heterocyclic compounds. The use of the heteropolycyclic compound exhibits the following effects: excellent coating adaptability when applied as a paste, and excellent battery performance can be effectively exhibited.
[0047] In the modified sulfide solid electrolyte of the present embodiment, it is not yet determined how the heteropolycyclic compound is contained, but it is presumed that the heteropolycyclic compound is attached to the surface of the sulfide solid electrolyte while maintaining its structure. This is because when the modified sulfide solid electrolyte of the present embodiment is analyzed by FT-IR analysis (ATR method), in the infrared absorption spectrum, when an epoxy compound is used as the heteropolycyclic compound, the 2800 to 3000 cm-1 wavelength that can be observed in the epoxy compound is -1 This is because, since the peak due to the presence of the epoxy compound is clearly detected, it is considered that it exists in a form that is easily detected.
[0048] In addition, the examples confirmed that the oil absorption is lower than that of the sulfide solid electrolyte not containing the heteropolycyclic compound. It is reasonable to assume that the reduction in oil absorption is caused by the heteropolycyclic compound adhering to the surface of the sulfide solid electrolyte and blocking at least a part of the pores of the sulfide solid electrolyte. It is known that in general, in order to improve coating adaptability, the oil absorption is also related to the specific surface area. It can be inferred that by making the heteropolycyclic compound adhere to the surface of the sulfide solid electrolyte, the oil absorption is reduced and the coating adaptability is improved.
[0049] Regarding the attachment of the heteropolycyclic compound to the surface of the sulfide solid electrolyte, it is not clear in what form, that is, whether it is physical attachment or chemical attachment. However, since heteroatoms such as oxygen atoms have the property of easily bonding with lithium atoms, halogen atoms, etc., in the heteropolycyclic compound, the oxygen atoms contained in at least two epoxy groups are bonded with lithium atoms, halogen atoms, etc. constituting the sulfide solid electrolyte and are attached to the surface, that is, there is a high possibility of chemical attachment.
[0050] In the modified sulfide solid electrolyte of the present embodiment, regardless of the above-mentioned attachment, as long as the heteropolycyclic compound is attached to the surface, the oil absorption is likely to be reduced, resulting in improved coating suitability and improved battery performance.
[0051] The modified sulfide solid electrolyte of the second embodiment of the present invention is, in the above-mentioned first embodiment,
[0052] The compound having two or more heterocyclic rings having carbon atoms and oxygen atoms is a compound containing two or more groups having oxirane rings.
[0053] As the heteropolycyclic compound used in the modified sulfide solid electrolyte of the present embodiment, any compound having two or more heterocyclic rings having at least carbon atoms and oxygen atoms can be used without particular limitation. The details will be described later. As heterocyclic rings having carbon atoms and oxygen atoms, heterocyclic rings such as oxirane rings, oxetane rings, and tetrahydrofuran rings can be representatively and preferably exemplified. Among these, oxirane rings are particularly preferred. By having a group having an oxirane ring, the oil absorption is reduced, and excellent coating adaptability is easily obtained, and excellent battery performance can be obtained more effectively. As a group having an oxirane ring, the details will be described later. An epoxy group or a glycidyl group or a glycidyl ether group as a group containing an epoxy group can be preferably exemplified.
[0054] The modified sulfide solid electrolyte of the third aspect of the present embodiment is, in the first or second aspect,
[0055] The compound having two or more heterocyclic rings having carbon atoms and oxygen atoms is an epoxy compound represented by the following general formula (1), and the epoxy compound has at least two groups selected from epoxy groups, glycidyl groups and glycidyl ether groups.
[0056]
Chemistry 1
[0057]
[0058] (In general formula (1), X 1 is a single bond or an aliphatic group, an alicyclic group, an aromatic group, an organic group having a siloxane structure, or an organic group consisting of a combination of these, l1, m1, and n1 are integers of 0 to 16, and l1+m1+n1≥2 is satisfied. 1 When the organic group has the alicyclic group, the epoxy group may be a group condensed with the alicyclic ring in the alicyclic group.
[0059] As described above, in the modified sulfide solid electrolyte of the present embodiment, any heteropolycyclic compound can be used without particular limitation, that is, excellent coating suitability can be obtained. However, by using an epoxy compound represented by the above general formula (1), which has at least two or more groups selected from epoxy groups, glycidyl groups and glycidyl ether groups as groups having an oxirane ring as a heterocyclic ring, the oil absorption is reduced, and excellent coating suitability is easily obtained, and excellent battery performance can be obtained more effectively.
[0060] The modified sulfide solid electrolyte of a fourth aspect of the present embodiment is, in the above-mentioned third aspect,
[0061] As X in the general formula (1) 1 The group composed of these combinations is a group formed by at least two groups selected from the aliphatic group, the alicyclic group, the aromatic group and the organic group having a siloxane structure bonded via a single bond or a bonding group selected from -O-, -SO2-, -CO-, -C(=O)O-, -N- and -S-.
[0062] In the above general formula (1), X is defined as 1 The organic group may be composed of a single bond or a combination of an aliphatic group, an alicyclic group, an aromatic group, and an organic group having a siloxane structure, but when these organic groups are combined, in addition to a single bond, an organic group bonded via a bonding group such as -O- is also included. The fourth scheme is a scheme that clarifies this point.
[0063] The modified sulfide solid electrolyte of a fifth aspect of the present embodiment is, in the first to fourth aspects described above,
[0064] In the infrared absorption spectrum based on FT-IR analysis (ATR method), the -1 As described above, since this peak is not a peak detectable from the sulfide solid electrolyte, it is considered to be a peak derived from the heteropolycyclic compound contained in the modified sulfide solid electrolyte.
[0065] Thus, when the heteropolycyclic compound is present as a peak in the infrared absorption spectrum by FT-IR analysis (ATR method), the oil absorption is reduced, excellent coating suitability is easily obtained, and excellent battery performance can be obtained more effectively.
[0066] The modified sulfide solid electrolyte of a sixth aspect of the present embodiment is, in the fifth aspect,
[0067] In the infrared absorption spectrum based on FT-IR analysis (ATR method), the -1 The detected peak is a peak derived from the CH stretching vibration of the alkyl chain in the heteropolycyclic compound.
[0068] As described above, this peak is a peak that cannot be detected in a sulfide solid electrolyte based on a conventional method, and is a peak that appears by including a heteropolycyclic compound. Therefore, it is considered that the heteropolycyclic compound exists in a state where its structure is maintained. Moreover, by existing in such a form, the oil absorption is reduced, it is easy to obtain excellent coating adaptability, and excellent battery performance can be obtained more effectively.
[0069] The modified sulfide solid electrolyte of a seventh aspect of the present embodiment is, in the above-mentioned sixth aspect,
[0070] exist 1 In the H-NMR spectrum, there is a peak at 0.0 to 5.0 ppm derived from the alkyl chain.
[0071] It is considered that the modified sulfide solid electrolyte of the present embodiment has this peak, and the heteropolycyclic compound exists in the modified sulfide solid electrolyte in a state where its structure is maintained. By existing in such a form, the oil absorption is reduced, and excellent coating adaptability is easily obtained, and excellent battery performance can be obtained more effectively.
[0072] The modified sulfide solid electrolyte according to an eighth aspect of the present embodiment is, in the first to seventh aspects,
[0073] The content of the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms is 0.03 parts by mass or more and 25 parts by mass or less based on 100 parts by mass of the sulfide solid electrolyte.
[0074] If the content of the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms (heteropolycyclic compound) is within the above range, the heteropolycyclic compound is appropriately dispersed and attached to the surface of the sulfide solid electrolyte to reduce the oil absorption, and the lithium ion conductivity can be appropriately maintained, so the coating adaptability is easily improved, and excellent battery performance is easily and effectively manifested. Regarding the "content of the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms", if the amount of the heteropolycyclic compound used when manufacturing the modified sulfide solid electrolyte is known, the amount used directly becomes the content.
[0075] A ninth modified sulfide solid electrolyte according to the present embodiment is, in the first to eighth embodiments,
[0076] The number average molecular weight of the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms is 10,000 or less,
[0077] A tenth modified sulfide solid electrolyte according to the present embodiment is, in the first to ninth embodiments,
[0078] The content of the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms and having a number average molecular weight of 10,000 or less among the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms is 90% by mass or more,
[0079] The modified sulfide solid electrolyte according to an eleventh aspect of the present embodiment is, in the above-mentioned first to tenth aspects,
[0080] The content of the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms and having a number average molecular weight exceeding 10,000 among the compounds having two or more heterocyclic rings having carbon atoms and oxygen atoms is 10% by mass or less.
[0081] The heteropolycyclic compound used in the modified sulfide solid electrolyte of the present embodiment is a compound with a relatively small number average molecular weight, so that the oil absorption is reduced, excellent coating adaptability is easily obtained, and excellent battery performance can be obtained more effectively. Therefore, it is preferred that the number average molecular weight of the compound is relatively large, that is, the number average molecular weight exceeds 10000.
[0082] The method for producing a modified sulfide solid electrolyte according to the twelfth aspect of the present embodiment is:
[0083] A method for preparing a modified sulfide solid electrolyte comprises: mixing a sulfide solid electrolyte, a compound having two or more heterocyclic rings having carbon atoms and oxygen atoms, and an organic solvent, wherein the sulfide solid electrolyte has a BET specific surface area of 10 m 2 / g or more and contains lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms;
[0084] The organic solvent is removed.
[0085] As described above, the modified sulfide solid electrolyte of the present embodiment is not particularly limited in its production method as long as it is a modified sulfide solid electrolyte containing a heteropolycyclic compound. According to the method for producing a modified sulfide solid electrolyte of the ninth embodiment of the present embodiment, the heteropolycyclic compound can become a compound that exists by adhering to the surface of the sulfide solid electrolyte, and therefore has excellent coating adaptability, and can effectively demonstrate excellent battery performance, and it becomes possible to more efficiently produce such a modified sulfide solid electrolyte of the present embodiment.
[0086] By mixing the sulfide solid electrolyte, the heteropolycyclic compound and the organic solvent, a solution or slurry mixture can be obtained. However, if the mixture is kept in this state, the modified sulfide solid electrolyte cannot be used. Therefore, the organic solvent is removed from the solution or slurry.
[0087] The method for producing a modified sulfide solid electrolyte according to a thirteenth aspect of the present embodiment is that the organic solvent used in the production method of the twelfth aspect is,
[0088] At least one solvent selected from aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, aromatic hydrocarbon solvents, ether solvents, ester solvents, and nitrile solvents.
[0089] By using the above solvent as the organic solvent, adhesion of the heteropolycyclic compound to the surface of the sulfide solid electrolyte can be promoted, and coating suitability can be easily improved.
[0090] An electrode composite material according to a fourteenth aspect of the present embodiment includes the modified sulfide solid electrolyte or the like according to any one of the first to eleventh aspects described above and an electrode active material.
[0091] Furthermore, a lithium ion battery according to a fifteenth aspect of the present embodiment includes at least one of the modified sulfide solid electrolyte or the like according to any one of the first to eleventh aspects and the electrode active material according to the fourteenth aspect.
[0092] As described above, the modified sulfide solid electrolyte of the present embodiment has excellent coating adaptability when applied as a paste, and can effectively demonstrate excellent battery performance. Therefore, the electrode composite material including the modified sulfide solid electrolyte of the present embodiment also has excellent coating adaptability, so that lithium ion batteries can be efficiently manufactured, and the obtained lithium ion batteries have excellent battery performance.
[0093] 〔Modified sulfide solid electrolyte〕
[0094] The modified sulfide solid electrolyte of this embodiment includes: a sulfide solid electrolyte having a BET specific surface area of 10 m 2 / g or more and containing a lithium atom, a sulfur atom, a phosphorus atom and a halogen atom; and having two or more heterocyclic rings having carbon atoms and oxygen atoms.
[0095] Hereinafter, the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms (heteropolycyclic compound) contained in the modified sulfide solid electrolyte of the present embodiment will be described.
[0096] (Heteropolycyclic compounds)
[0097] The modified sulfide solid electrolyte of the present embodiment includes a compound having two or more heterocyclic rings having carbon atoms and oxygen atoms (heteropolycyclic compound). As the heteropolycyclic compound, any heteropolycyclic compound having two or more heterocyclic rings having carbon atoms and oxygen atoms can be used without particular limitation, and the coating adaptability when applied as a paste can be excellent, and the effect of being able to effectively demonstrate excellent battery performance can be obtained.
[0098] As the heterocyclic ring having carbon atoms and oxygen atoms, any heterocyclic ring consisting of 2 or more carbon atoms and 1 or more oxygen atoms can be used without particular limitation, and the number of atoms constituting the heterocyclic ring is preferably 3 or more, and the upper limit is not particularly limited, but is preferably 24 or less, more preferably 20 or less, further preferably 16 or less, and further preferably 12 or less. When the number of atoms constituting the heterocyclic ring is within the above range, the oil absorption is reduced, excellent coating adaptability is easily obtained, and excellent battery performance can be more effectively obtained.
[0099] For example, a ring having three atoms constituting a heterocyclic ring is also called a three-membered ring, and examples thereof include saturated heterocyclic rings such as an oxirane ring and a dioxirane ring. In addition, an oxaziridine ring containing an oxygen atom and a nitrogen atom also contains an oxygen atom, and therefore a compound having an oxaziridine ring as a heterocyclic ring can also be used.
[0100] Among the compounds having an oxirane ring as a heterocyclic ring, a compound having two or more oxirane rings (hereinafter also referred to as a "polyfunctional epoxy compound") is a particularly preferred compound among the heteropolycyclic compounds used in the modified sulfide solid electrolyte of the present embodiment. The polyfunctional epoxy compound will be described in detail below.
[0101] As the heterocyclic ring composed of 4 or more atoms, representative and preferred examples include: four-membered rings such as saturated heterocyclic rings such as oxetane ring and dioxetane ring, and unsaturated heterocyclic rings such as oxetene ring; five-membered rings such as saturated heterocyclic rings such as tetrahydrofuran ring, dioxolane ring, oxazolidine ring, oxathiolane ring, and unsaturated heterocyclic rings such as furan ring, oxazole ring, and oxadiazole ring; six-membered rings such as saturated heterocyclic rings such as tetrahydropyran ring, dioxane ring, and morpholine ring, and unsaturated heterocyclic rings such as pyran ring, dioxin ring, and oxazine ring; and the like.
[0102] In addition, as a heterocycle having carbon atoms and oxygen atoms, as long as it has a heterocycle containing an oxygen atom, it is not limited to the monocyclic heterocycle as described above, and it may also be a polycyclic heterocycle obtained by condensing two or more alicyclic rings, for example, representative heterocycles include a cyclohexyl oxide ring obtained by condensing cyclohexane and ethylene oxide, an oxaspirodecane ring obtained by condensing cyclohexane and tetrahydrofuran, and a benzofuran ring obtained by condensing benzene and furan.
[0103] Taking into account the reduction in oil absorption, the ease of obtaining excellent coating adaptability, the ability to more effectively obtain excellent battery performance, as well as the ease of availability and price, among the above-mentioned compounds having a heterocyclic ring, compounds having two or more monocyclic heterocyclic rings are preferred, and the heterocyclic ring is preferably a saturated heterocyclic ring, and the number of atoms constituting the heterocyclic ring is preferably 3 or more, and the upper limit is preferably 12 or less, more preferably 8 or less, further preferably 6 or less, and further preferably 5 or less.
[0104] (Multifunctional Epoxy Compound)
[0105] As one of the preferred compounds among the heteropolycyclic compounds used in the present embodiment, a compound having two or more oxirane rings as a heterocyclic ring (polyfunctional epoxy compound) will be described.
[0106] The group having an oxirane ring possessed by the multifunctional epoxy compound is preferably contained in the form of an epoxy group, or a glycidyl group or a glycidyl ether group containing an epoxy group. That is, as the multifunctional epoxy compound, an epoxy compound having at least two or more groups selected from an epoxy group, a glycidyl group, and a glycidyl ether group is preferred. This is because the oil absorption is reduced, excellent coating adaptability is easily obtained, and excellent battery performance can be obtained more effectively.
[0107] Preferred examples of such a polyfunctional epoxy compound include epoxy compounds represented by the following general formula (1) and having at least two groups selected from an epoxy group, a glycidyl group and a glycidyl ether group.
[0108]
Chemistry 2
[0109]
[0110] In the general formula (1), X 1 is a single bond or an aliphatic group, an alicyclic group, an aromatic group, an organic group having a siloxane structure, or an organic group consisting of a combination of these, l1, m1, and n1 are integers of 0 to 16, and l1+m1+n1≥2 is satisfied. 1 When the organic group has the alicyclic group, the epoxy group may be a group condensed with the alicyclic ring in the alicyclic group.
[0111] (single bond)
[0112] In X 1 When X is a single bond, the polyfunctional epoxy compound preferably includes butadiene diepoxide formed by two epoxy groups bonded together, hexadiene diepoxide formed by two glycidyl groups bonded together, and the like. In addition, hexadiene diepoxide formed by two glycidyl groups bonded together can be regarded as X in the general formula (1). 1 The epoxy compound wherein m1 is a single bond, m1 is 2, l1 and n1 are 0 can also be regarded as a compound in which two epoxy groups are bonded to both ends of the ethylene group, and X in the above general formula (1) 1 An epoxy compound wherein l1 is 2, m1 and n1 are 0.
[0113] In addition, in X 1 When it is a single bond, the polyfunctional epoxy compound preferably includes diglycidyl ether formed by bonding a glycidyl group to a glycidyl ether group. Diglycidyl ether is a compound in which X 1 It is an epoxy compound with a single bond, m1=1, and n1=1.
[0114] (Aliphatic group)
[0115] Regarding X in general formula (1) 1 As an aliphatic group, a group having a chemical bond formed by removing a number of hydrogen atoms (l1+m1+n1) corresponding to the number of groups selected from epoxy, glycidyl and glycidyl ether groups from alkanes, alkenes and alkynes can be preferably exemplified. For example, a group having a chemical bond formed by removing two hydrogen atoms from an alkane (a divalent aliphatic group) is an alkanediyl (alkylene) group, and a group having a chemical bond formed by removing three hydrogen atoms (a trivalent aliphatic group) is an alkanetriyl group.
[0116] Thus, in this embodiment, the name of the group can be based on X 1 The number of chemical bonds (i.e., 1The number of groups selected from the epoxy group, glycidyl group and glycidyl ether group to be bonded is changed by the number (l1+m1+n1) corresponding to the number of groups. Therefore, in this specification, the basic structure (for example, the above-mentioned alkane, alkene, and alkyne corresponding to it) that forms the basis of the aliphatic group and other groups is described below.
[0117] As the basic structure of the aliphatic group, as described above, preferably, alkanes, alkenes, and alkynes can be exemplified. The oil absorption is reduced, excellent coating adaptability is easily obtained, and excellent battery performance can be obtained more effectively. In addition, considering the ease of acquisition, alkanes and alkenes are more preferred, and alkanes are further preferred.
[0118] The carbon number of these aliphatic groups is preferably 1 or more, more preferably 2 or more, and the upper limit is 24 or less, preferably 16 or less, more preferably 10 or less, further preferably 8 or less, and further preferably 6 or less. When the carbon number of the aliphatic group is within the above range, the oil absorption is reduced, excellent coating suitability is easily obtained, and excellent battery performance can be obtained more effectively.
[0119] In the general formula (1), the aliphatic group as X 1 In the case of a polyfunctional epoxy compound, representative preferred examples include ethylene glycol diglycidyl ether in which the aliphatic group is ethylene and has two glycidyl ether groups (n1 is 2), butanediol diglycidyl ether in which the aliphatic group is butylene and has two glycidyl ether groups (n1 is 2), hexanediol diglycidyl ether in which the aliphatic group is hexylene and has two glycidyl ether groups (n1 is 2), and octadiene diepoxide in which the aliphatic group is ethylene and has two glycidyl groups (m1 is 2).
[0120] In the present specification, for example, when described as the above-mentioned "butanediol diglycidyl ether", butane (an alkane having 4 carbon atoms) includes both linear and branched butanes, and includes all butanes in which the position of the carbon atom to which the diglycidyl ether group is attached (the position of the diol) is an adoptable position.
[0121] More specifically, "butanediol diglycidyl ether" includes, in addition to 1,4-butanediol diglycidyl ether (the multifunctional epoxy compound used in the examples) in which one glycidyl ether group is connected to the carbon at the 1-position and the 4-position of butanediol, compounds in which a glycidyl ether group is connected to other carbons, such as 1,2-butanediol diglycidyl ether in which one glycidyl ether is connected to the carbon at the 1-position and the 2-position of butanediol, and 1,3-butanediol diglycidyl ether in which one glycidyl ether is connected to the carbon at the 1-position and the 3-position of butanediol. In addition, it also includes 2-methyl-1,3-propanediol diglycidyl ether in which the butane of 1,3-butanediol is branched into 2-methylpropane, and 2-methyl-1,3-propanediol diglycidyl ether in which one glycidyl ether is connected to the carbon at the 1-position and the 3-position of 2-methyl-1,3-propanediol.
[0122] These aliphatic groups may be linear or branched.
[0123] Furthermore, at least a part of the hydrogen atoms may be substituted with a halogen atom, a hydroxyl group, an amino group, etc. In this case, the halogen atom is preferably a fluorine atom.
[0124] In the general formula (1), X is a branched aliphatic group. 1 In the case of a polyfunctional epoxy compound, representative preferred examples include neopentyl glycol diglycidyl ether in which the aliphatic group is a neopentylene group and has two glycidyl groups (n1 is 2), trimethylolpropane triglycidyl ether in which the aliphatic group is a group obtained by removing three hydrogen atoms from 2,2-dimethylbutane, a branched alkane as a basic structure, and has three glycidyl groups (n1 is 3), and pentaerythritol trimethylolpropane triglycidyl ether in which the aliphatic group is a group obtained by removing four hydrogen atoms from pentaerythritol as a basic structure and has four glycidyl groups (m1 is 4) (which may also be referred to as a compound in which the aliphatic group is a group obtained by removing four hydrogen atoms from 2,2-dimethylbutane as a basic structure and has four glycidyl groups (n1 is 4)).
[0125] In the general formula (1), X is an aliphatic group in which at least a part of hydrogen atoms is substituted. 1 In the case of a polyfunctional epoxy compound, a representative and preferred example is 2,2'-(2,2,3,3,4,4,5,5-octafluorohexane-1,6-diyl)dioxirane having two epoxy groups (l1 is 2) in which the aliphatic group is a group obtained by removing two hydrogen atoms from 2,2,3,3,4,4,5,5-octafluorohexane as a basic structure in which eight hydrogen atoms of hexane are replaced by fluorine atoms (2,2,3,3,4,4,5,5-octafluorohexane-1,6-diyl).
[0126] The above-mentioned 2,2'-(2,2,3,3,4,4,5,5-octafluorohexane-1,6-diyl)dioxirane is a compound used in the examples, and therefore the position substituted by the fluorine atom is clearly described. However, in this specification, regarding the compound whose position is clearly described, when described in the examples, it refers to itself, but other than the cases described in the examples, as in the case where the compound is described without specifying the above-mentioned position, as hexane (alkane having 6 carbon atoms), it includes any of linear and branched forms, and includes all hexanes in which the position of the carbon atom substituted by fluorine and the position of the carbon atom to which the oxirane ring (epoxy group) is a position that can be adopted.
[0127] (Alicyclic Group)
[0128] Regarding X in general formula (1) 1 As the basic structure of the alicyclic group, cycloalkanes and cycloolefins can be preferably exemplified. The oil absorption is reduced, excellent coating adaptability is easily obtained, and excellent battery performance can be obtained more effectively. In addition, considering the ease of acquisition, cycloalkanes are more preferred.
[0129] In this embodiment, as the basic structure of the alicyclic group, a basic structure including multiple alicyclic rings can also be exemplified, for example, a bonded multi-alicyclic structure such as a bicyclohexyl group; a structure obtained by condensing two or more alicyclic rings such as hexahydronaphthalene, octahydronaphthalene, and decahydronaphthalene; a cross-linked ring structure such as norbornane, norbornene, adamantane, tricyclodecane, and pinene. In addition to these, as the basic structure having a double bond in the alicyclic ring, basic structures such as pentalylene and azulene can also be exemplified.
[0130] Furthermore, a structure in which any of the above-mentioned single alicyclic basic structure, multiple alicyclic basic structures, and aromatic ring basic structures described later are bonded or condensed can also be exemplified as a basic structure that can be preferably exemplified.
[0131] In the general formula (1), the alicyclic group as X 1 In the case of a polyfunctional epoxy compound, a representative preferred example is cyclohexanedimethanol diglycidyl ether (in the examples, 1,4-cyclohexanedimethanol diglycidyl ether is used) in which the alicyclic group is dimethylcyclohexylene and has two glycidyl ether groups (n1 is 2).
[0132] In the present embodiment, the basic structure of the alicyclic group may be a structure having a heterocyclic ring in which carbon atoms in the basic structures exemplified above are substituted with hetero atoms such as nitrogen atoms, oxygen atoms, sulfur atoms, and phosphorus atoms.
[0133] In addition, it can also be a structure in which at least a part of the hydrogen atoms in the above-exemplified basic structure is replaced by a halogen atom such as a fluorine atom, a hydroxyl group, an amino group, or the above-mentioned aliphatic group. In this case, the aliphatic group is preferably an alkyl group or an alkenyl group, and the carbon number is preferably 1 or more, and the upper limit is preferably 12 or less, more preferably 8 or less, further preferably 6 or less, and further preferably 4 or less.
[0134] In X 1 In the case of an alicyclic group, an epoxy group (ethylene oxide ring) may be present in a condensed state with an alicyclic ring in the alicyclic group.
[0135] As the basic structure of such an alicyclic group that can be fused with an epoxy group (ethylene oxide ring), cyclopentane, cyclohexane, cyclooctane, etc. can be representatively and preferably exemplified. From the viewpoint of easy availability, cyclohexane is preferred. For example, when the basic structure of the alicyclic group is cyclohexane, if it is fused with an epoxy group, cyclohexyl oxide is formed, and thus as a multifunctional epoxy compound, it becomes a compound having cyclohexyl oxide in a part thereof. As such a multifunctional epoxy compound, for example, 1,3-bis[2-(7-oxabicyclo[4.1.0]heptane-3-yl)ethyl]-1,1,3,3-tetramethyldisiloxane (in the above general formula (1), X 1 The basic structure is 1,3-ethylcyclohexyl-1,1,3,3-tetramethyldisiloxane (a compound obtained by replacing the hydrogen atom connected to the silicon atom in tetramethyldisiloxane with a propyl group), l1 is 2, and the epoxy group is condensed with cyclohexane to exist in the form of epoxycyclohexane).
[0136] As a polyfunctional epoxy compound containing an alicyclic ring fused with an epoxy group, for example, a compound in which an alicyclic ring fused with an epoxy group such as cyclohexene oxide is bonded to other groups such as an aliphatic group, an alicyclic group, an aromatic group, etc. via / or not via a chemical bond described later, and an epoxy group, a glycidyl group, or a glycidyl ether group is bonded to the other group. In this case, the epoxy group bonded to the other group may be fused with the alicyclic ring.
[0137] Furthermore, for example, in a basic structure having a crosslinked ring structure, an epoxy compound in which two or more epoxy groups are condensed with an alicyclic ring, for example, a bifunctional epoxy compound such as 4,5:8,9-diepoxytricyclo[5.2.1.02,6]decane may be used.
[0138] The carbon number of the alicyclic group is 3 or more, preferably 4 or more, more preferably 6 or more, and the upper limit is preferably 24 or less, more preferably 20 or less, further preferably 16 or less, and further preferably 12 or less.
[0139] (Aromatic Group)
[0140] Regarding X in general formula (1) 1 As the basic structure of the aromatic group, preferably exemplified are: monocyclic aromatic compounds such as benzene, toluene, and styrene; polycyclic aromatic compounds such as biphenyl, diphenylmethane (benzylbenzene), diphenylethane (bibenzyl), methylenetriphenol, and triphenylcyclohexane formed by bonding multiple aromatic rings; naphthalene, phenanthrene, anthracene, pyrene, triphenylene, tetracene, pentacene, etc., obtained by condensing multiple aromatic rings, or polycyclic aromatic compounds such as indene, indacene, acenaphthene, dihydronaphthalene, tetrahydronaphthalene, biphenylene, fluorene, and fluoranthene, obtained by condensing aromatic rings with alicyclic rings; etc.
[0141] Furthermore, structures obtained by bonding or condensing any of these aromatic ring basic structures, the above-mentioned single alicyclic basic structures, and multiple alicyclic basic structures, such as diphenylfluorene (9,9-diphenyl-9H-fluorene) in which two benzenes are single-bonded at the 9-position of fluorene, can also be representatively and preferably exemplified as basic structures.
[0142] In the general formula (1), an aromatic group is present as X 1 In the case of a polyfunctional epoxy compound, representative and preferred examples include diglycidylresorcinol ether (a compound having 1,3-phenylene) and 1,4-diglycidyloxybenzene (a compound having 1,4-phenylene) in which the aromatic group is a phenylene group and has two glycidyl ether groups (n1 is 2), and tris(4-hydroxyphenyl)methane triglycidyl ether in which the aromatic group is a group obtained by removing three hydrogen atoms from methylenetriphenol, a bonded polycyclic aromatic compound as a basic structure, and has three glycidyl groups (m1 is 3).
[0143] In addition, a representative and preferred example is 9,9-bis(4-glycidyloxyphenyl)fluorene, in which the aromatic group is a group obtained by removing two hydrogen atoms from 9,9-bis(4-hydroxyphenyl)fluorene, a condensed polycyclic aromatic compound as a basic structure, and has two glycidyl groups (m1 is 2).
[0144] As a preferred example of the basic structure of the aromatic group, a bisphenol compound can also be mentioned. As the main bisphenol compound, preferably, bisphenol compounds such as bisphenol A (2,2-bis(4-hydroxyphenyl)propane), bisphenol AP (1,1-bis(4-hydroxyphenyl)-1-phenylethane), bisphenol B (2,2-bis(4-hydroxyphenyl)butane), bisphenol BP (bis(4-hydroxyphenyl)diphenylmethane), bisphenol M (1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene), bisphenol PH (5,5'-(1-methylethylidene)-bis[1,1'-(bisphenyl)-2-ol]propane), bisphenol Z (1,1-bis(4-hydroxyphenyl)cyclohexane), and compounds containing these bisphenol compounds can be mentioned.
[0145] Examples of the bisphenol compound that are preferred in addition to the above compounds include compounds such as bisphenol AF (2,2-bis(4-hydroxyphenyl)hexafluoropropane) in which a part of the bisphenol is substituted with a halogen atom such as a fluorine atom, and bisphenol S (bis(4-hydroxyphenyl)sulfone) containing an oxygen atom and a sulfur atom in the molecule.
[0146] In the general formula (1), an aromatic group is present as X 1 In the case of a polyfunctional epoxy compound, among the polyfunctional epoxy compounds whose basic structure as the aromatic group is a bisphenol compound, representative preferred examples include bisphenol A diglycidyl ether having two glycidyl groups (m1 is 2) in which the aromatic group is a group obtained by removing a hydrogen atom from a hydroxyl group of bisphenol A as a basic structure, and bisphenol A propoxylated diglycidyl ether having two glycidyl ether groups (n1 is 2) in which the aromatic group is a group obtained by removing a hydrogen atom from a propyl group of 2,2-bis((4-propoxyphenyl)propane) in which the hydrogen atom of the hydroxyl group of bisphenol A as a basic structure is substituted with a propyl group, and the like.
[0147] In the present embodiment, the basic structure of the aromatic group may be a structure having a heterocyclic ring in which carbon atoms in the above-exemplified basic structures are substituted with hetero atoms such as nitrogen atoms, oxygen atoms, sulfur atoms, and phosphorus atoms.
[0148] It can also be a structure in which at least a part of the hydrogen atoms in the above-exemplified basic structure is replaced by a halogen atom such as a fluorine atom, a hydroxyl group, an amino group, or the above-mentioned aliphatic group. In this case, the aliphatic group is preferably an alkyl group or an alkenyl group, and the carbon number is preferably 1 or more, and the upper limit is preferably 12 or less, more preferably 8 or less, further preferably 6 or less, and further preferably 4 or less.
[0149] In the basic structure of the aromatic group, amino and hydroxyl groups are preferred among these substituents. When the aromatic group is substituted with an amino group, aniline, dimethylaniline, etc. can be preferably exemplified, and when the aromatic group is substituted with a hydroxyl group, phenol, diphenol, etc. can be preferably exemplified. In addition, hydroxyaniline (aminophenol) substituted with an amino group and a hydroxyl group can also be preferably exemplified.
[0150] In the general formula (1), an aromatic group is present as X 1In the case of a polyfunctional epoxy compound, the polyfunctional epoxy compound in which the basic structure as the aromatic group is substituted with an amino group, a hydroxyl group, etc., can be representatively preferably exemplified as a group in which the aromatic group is a group obtained by removing hydrogen atoms from an amino group and a hydroxyl group of hydroxyaniline (a compound in which 2 hydrogen atoms of benzene are substituted with an amino group and a hydroxyl group) as a basic structure and having two glycidyl groups (m1 is 3) N,N-diglycidyl-4-glycidyloxyaniline, and an aromatic group is a group obtained by removing hydrogen atoms from an amino group of 4,4'-methylenebis(N,N-dimethylaniline) (a compound in which 2 hydrogen atoms of diphenylmethane are substituted with an amino group) as a basic structure and having four glycidyl groups (m1 is 4).
[0151] Furthermore, if the diglycidylresorcinol ether and 1,4-diglycidyloxybenzene cited as the above specific examples are regarded as compounds having two glycidyl groups (m1 is 2) in which the aromatic group is a group obtained by removing a hydrogen atom from a hydroxyl group of a compound (refined diol) in which two hydrogen atoms of benzene are replaced by hydroxyl groups, then it can also be considered that the compounds having an aromatic group as X in the general formula (1) are 1 In the polyfunctional epoxy compounds, the basic structure of the aromatic group is substituted by amino group, hydroxyl group, etc.
[0152] The number of carbon atoms in the aromatic group is 6 or more, preferably 4 or more, more preferably 6 or more, and the upper limit is preferably 36 or less, more preferably 32 or less, and further preferably 28 or less.
[0153] (Organic group having a siloxane structure)
[0154] Regarding X in general formula (1) 1 As the basic structure of the organic group having a siloxane structure, any one having at least a -Si-O- bond can be used without particular limitation, and preferably includes: alkoxysilanes having one silicon atom, such as dimethylmethoxysilane, dimethoxymethylsilane, trimethoxysilane, trimethoxymethylsilane, and tetramethoxysilane; disiloxane compounds having two silicon atoms, such as tetramethyldisiloxane, hexamethyldisiloxane, and divinyltetramethyldisiloxane; and the like chain siloxane compounds.
[0155] Furthermore, cyclic siloxane compounds such as hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane and decamethylcyclopentasiloxane, and cage-type siloxane compounds such as silsesquioxane are also preferably mentioned.
[0156] Regarding the above-mentioned chain siloxane compounds and cyclic siloxane compounds, the compounds in which the groups bonded to the silicon atom and the alkyl groups in the alkoxy groups are methyl groups are exemplified, and of course, compounds bonded to groups other than methyl groups, i.e., ethyl groups, propyl groups, etc., the above-mentioned aliphatic groups, alicyclic groups, and aromatic groups can also be included. In this case, the aliphatic group is preferably an alkyl group or an alkenyl group, and the carbon number is preferably 1 or more, and the upper limit is preferably 12 or less, more preferably 8 or less, further preferably 6 or less, and further preferably 4 or less.
[0157] Regarding the above-mentioned chain siloxane compound, as a compound containing a group other than a methyl group, from the perspective of easy availability, for example, the following compounds can be preferably cited as chain siloxane compounds forming a basic structure: a polyfunctional epoxy compound having a basic structure such as siloxane compounds such as 1,3-dipropyl-1,1,3,3-tetramethyldisiloxane in which one methyl group bonded to two silicon atoms is respectively a propyl group, or 1,3-dicyclohexylethyl-1,1,3,3-tetramethyldipropyldisiloxane in which one methyl group bonded to two silicon atoms is respectively a cyclohexylethyl group in hexamethyldisiloxane.
[0158] In the general formula (1), an organic group having a siloxane structure is provided as X 1 In the case of a polyfunctional epoxy compound, a representative and preferred example of an organic group having a siloxane structure is 1,3-bis(3-glycidyloxypropyl)tetramethyldisiloxane having two glycidyl ether groups (n1 is 3) and is obtained by removing two hydrogen atoms from the propyl group of 1,3-dipropyl-1,1,3,3-tetramethyldisiloxane as a basic structure.
[0159] In addition, 1,3-bis[2-(7-oxabicyclo[4.1.0]heptane-3-yl)ethyl]-1,1,3,3-tetramethyldisiloxane described as a compound having cyclohexene oxide in which an alicyclic group and an epoxy group are condensed can also be preferably exemplified as a representative example of an organic group having a siloxane structure as X of the general formula (1): 1 of multifunctional epoxy compounds.
[0160] In addition, regarding the above-mentioned cyclic siloxane compound, from the perspective of easy availability, the following compounds can be preferably cited as the cyclic siloxane compound forming the basic structure: a polyfunctional epoxy compound having as its basic structure 2,4,6,8-tetramethyl-2,4,6,8-tetrapropylcyclotetrasiloxane in which one methyl group bonded to four silicon atoms in octamethylcyclotetrasiloxane is respectively converted into a propyl group.
[0161] In the general formula (1), an organic group as X 1In the case where the organic group has a siloxane structure whose basic structure is a cyclic siloxane compound, a representative and preferred example of an organic group having a siloxane structure is 1,3-bis(3-glycidyloxypropyl)tetramethyldisiloxane which is a group obtained by removing four hydrogen atoms from the propyl group of 2,4,6,8-tetramethyl-2,4,6,8-tetrapropylcyclotetrasiloxane as a basic structure and has four glycidyl ether groups (n1 is 4).
[0162] In the general formula (1), an organic group as X 1 In the case of a polyfunctional epoxy compound, in which the organic group has a siloxane structure whose basic structure is a cage-type siloxane compound, a representative and preferred example of an organic group having a siloxane structure is a compound having 8 silicon atoms of a silsesquioxane (PSS-octamethyl substitution) as a basic structure and to which each of the 8 propyldimethylsiloxy groups is bonded (a compound which may also be referred to as "PSS-octa[propyldimethylsiloxy] substitution" compound) and to which each of the 8 propyl groups is bonded, namely, PSS-octa[(3-glycidyloxypropyl)dimethylsiloxy] substitution having 8 glycidyl ether groups (n1 is 8).
[0163] The number of silicon atoms in the basic structure having a siloxane structure is preferably 1 or more, more preferably 2 or more, and the upper limit is preferably 12 or less, more preferably 8 or less, further preferably 6 or less, and further preferably 4 or less.
[0164] (Bonding Group)
[0165] In this embodiment, X 1 The group consisting of the combination of these may be a group formed by at least two groups selected from the above-mentioned aliphatic group, the above-mentioned alicyclic group, the above-mentioned aromatic group and the above-mentioned organic group having a siloxane structure bonded via a single bond or a bonding group selected from -O-, -SO2-, -CO-, -C(=O)O-, -N- and -S-. In addition, in this specification, X 1 The aliphatic group, alicyclic group, aromatic group and organic group having a siloxane structure are described as being replaced by a basic structure containing these groups, and therefore the above basic structure can also be regarded as being bonded via a single bond, -O- or other bonding group.
[0166] In X 1In the case of a group formed by single-bonding at least two groups selected from an aliphatic group, an alicyclic group, an aromatic group, and an organic group having a siloxane structure, the following cases are preferably exemplified: a case where one of the above-mentioned groups is substituted by another group, or a case where two benzenes as other basic structures are single-bonded to the 9-position of a basic structure of fluorene such as the above-mentioned diphenylfluorene (9,9-diphenyl-9H-fluorene), etc.
[0167] In addition, as X 1 In the case of a group formed by a single bond, preferably exemplified are: as a basic structure containing aniline, 4,4-methylenedianiline (p-toluidine) formed by a single bond between aniline and 4-methylaniline, 4,4'-methylenebis(N,N-dimethylaniline) formed by a single bond between dimethylaniline and 4,N,N-trimethylaniline, and the like.
[0168] As X 1 In the case of having -O- as a bonding group, for example, when a plurality of aliphatic groups are bonded via -O-, more specifically, for example, representative examples thereof preferably include oxyethylene, oxypropylene, etc. 1 O-(R 1 The basic structure of the repeating unit is a divalent aliphatic group, preferably an alkylene group.
[0169] In the basic structure with -R 1 In the case of O-, -R 1 O- may have 1 or more than 2. When having more than 2, the average repetition number (n) is preferably more than 2, more preferably more than 4, and further preferably more than 5, and the upper limit is preferably less than 200, more preferably less than 180, and further preferably less than 170.
[0170] In addition, the number average molecular weight of the multifunctional epoxy compound in this case can be adjusted by making -R 1 R in O 1 It varies depending on the reason and cannot be generalized, but it is preferably 200 or more, more preferably 300 or more, and further preferably 350 or more. The upper limit is preferably 10000 or less, more preferably 8000 or less, further preferably 7000 or less, and further preferably 6500 or less.
[0171] As X 1 In the case of a polyfunctional epoxy compound having -O- as a bonding group, representative examples thereof include: 1 O- is oxypropylene (R 1 as a propylene group) and having one glycidyl group and a glycidyl ether group (m1 is 1, n1 is 1), as -R1 O- is oxyethylene (R 1 In addition, the average repeating number (n) of these polyethylene glycol diglycidyl ethers and polypropylene glycol diglycidyl ethers can be appropriately selected from the above range.
[0172] As X 1 As the basic structure having -O- as a bonding group, compounds in which an aliphatic group such as diethylene glycol and diglycerol is bonded via -O- are also preferably exemplified.
[0173] In addition, as X 1 The basic structure in the case of having -O- as a bonding group may preferably include compounds in which alicyclic rings such as dicyclohexyl ether are bonded via -O-; compounds in which aromatic rings such as dihydroxydiphenyl ether and phenylbiphenyl ether are bonded via -O-; and the like.
[0174] As X 1 The polyfunctional epoxy compound having -O- as a bonding group can be representatively preferably exemplified by a group X1 having -O- as a bonding group, which is -CH2CH2-O-CH2CH2- (a group having a basic structure of diethylene glycol with two hydrogen atoms removed) formed by two ethylene groups bonded via -O-, and diethylene glycol diglycidyl ether having two glycidyl groups (n1 is 2), and the like.
[0175] As X 1 In the case of having -C(=O)O- as a bonding group, for example, preferably, there can be mentioned a compound in which two alicyclic rings are bonded via -C(=O)O-, such as cyclohexylmethyl cyclohexanecarboxylate.
[0176] (About l1, m1 and n1)
[0177] l1, m1 and n1 are respectively integers greater than or equal to 0 and less than or equal to 16, satisfying l1+m1+n1≥2.
[0178] There is no particular limitation as long as the total of l1, m1 and n1 (l1+m1+n1) is 2 or more, but when it is 1 or more, it is preferably 2 or more, and the upper limit is preferably 10 or less, more preferably 8 or less, and further preferably 4 or less.
[0179] Furthermore, l1+m1+n1 is not particularly limited as long as it is 2 or more, but is preferably 2 or more, and the upper limit is preferably 10 or less, more preferably 8 or less, and further preferably 4 or less.
[0180] If l1, m1 and n1 satisfy the above range, the oil absorption is reduced, excellent coating adaptability is easily obtained, and excellent battery performance is more effectively obtained. In addition, considering the ease of acquisition, it is preferred that any one of l1, m1 and n1 is 2 or more, and the other two are 0. That is, from the viewpoint of the ease of acquisition, the polyfunctional epoxy compound used in this embodiment preferably has two or more epoxy groups, glycidyl groups, and glycidyl ether groups.
[0181] In addition, considering the ease of availability, it is also preferred that any one of l1, m1 and n1 is 1, and any one of the other two is 1 or more. In this case, from the same viewpoint, a polyfunctional epoxy compound having one glycidyl ether group and one or more glycidyl groups is preferred, and a polyfunctional epoxy compound having one glycidyl ether group and two glycidyl groups is more preferred.
[0182] (Other heteropolycyclic compounds)
[0183] As the heteropolycyclic compound used in the present embodiment, as a compound other than the above-mentioned polyfunctional epoxy compound, a compound having a heterocyclic ring other than an oxirane ring in a heterocyclic ring composed of 3 atoms, and a compound having a heterocyclic ring composed of 4 or more atoms can be exemplified. As a heteropolycyclic compound other than such a polyfunctional epoxy compound, a compound represented by the following general formula (2) can be preferably exemplified.
[0184]
Chemistry 3
[0185]
[0186] In the general formula (2), X 2 is a single bond or an aliphatic group, an alicyclic group, an aromatic group, an organic group having a siloxane structure, or an organic group consisting of a combination of these, R 2a , R 2b and R 2c Each independently represents an aliphatic group having 1 or more carbon atoms. 2a , R 2b and R 2c The heterocyclic ring may contain a bonding group selected from -O-, -SO2-, -CO-, -C(=O)O-, -N- and -S-.
[0187] l2, m2 and n2 are integers of 0 to 16, respectively, and l2+m2+n2≥2. 2 When the organic group has the alicyclic group, the heterocyclic group may be a group condensed with the alicyclic ring in the alicyclic group.
[0188] In the above general formula (2), X2 A single bond or an aliphatic group, an alicyclic group, an aromatic group, an organic group having a siloxane structure, or an organic group composed of a combination of these and X as the above general formula (1) 1 The same as described above is the single bond or aliphatic group, alicyclic group, aromatic group, organic group having a siloxane structure or an organic group composed of a combination of these.
[0189] In addition, l2, m2 and n2 are the same as those described as l1, m1 and n1, respectively, in the above general formula (1).
[0190] In the above general formula (2), R 2a , R 2b and R 2c The aliphatic group forms an alicyclic structure together with the oxygen atom. 2a , R 2b and R 2c The aliphatic group may be a divalent aliphatic group such as an alkylene group, an alkenylene group, and an alkynylene group. In the present embodiment, any of these may be used, and if the availability is considered, an alkylene group and an alkenylene group are preferred, and an alkylene group is more preferred.
[0191] In addition, from the same point of view, as R 2a , R 2b and R 2c The carbon number of the aliphatic group is preferably 2 or more, more preferably 3 or more, and the upper limit is preferably 12 or less, more preferably 8 or less, and further preferably 6 or less.
[0192] The compound represented by the general formula (2) is a heteropolycyclic compound other than the above-mentioned polyfunctional epoxy compound. 2a , R 2b and R 2c is an aliphatic group having 2 carbon atoms, and 22 、m 22 and n 22 When each of R is 1, the aliphatic group having 2 carbon atoms is a group other than an alkylene group, that is, an alkenylene group or an alkynylene group. 2a , R 2b and R 2c is an aliphatic group having 2 carbon atoms, and 22 、m 22 and n 22 1 respectively, and in the case where the heterocyclic ring contains a bonding group described later, the aliphatic group having 2 carbon atoms may also be an alkylene group (i.e., ethylene group). For example, as the case where the aliphatic group having 2 carbon atoms may be an alkylene group (i.e., ethylene group), R 2a , R 2b and R 2cAn oxathietane ring which is an ethylene group and has -S- as a bonding group.
[0193] R as a heterocyclic ring 2a When the heteropolycyclic compound is an alkylene group, a representative example of a preferred embodiment is X 2 A group obtained by removing two hydrogen atoms from butanediol as a basic structure and having two tetrahydrofuran rings (R 2a bis(tetrahydrofuranyloxy)butane (particularly 1,4-bis(2-tetrahydrofuranyloxy)butane) wherein l2 is 2 and l2 is 1,4-bis(2-tetrahydrofuranyloxy)butane.
[0194] Contains R 2a , R 2b and R 2c The heterocyclic ring may contain a bonding group selected from -O-, -SO2-, -CO-, -C(=O)O-, -N- and -S-.
[0195] For example, when the heterocyclic ring is a dioxirane ring, R 2a , R 2b and R 2c The aliphatic group is a methylene group having 1 carbon number, and the methylene group is connected to the oxygen atom possessed by the heterocyclic ring through -O-. In addition, for example, when the heterocyclic ring is 1,3-dioxolane, R 2a , R 2b and R 2c The aliphatic group is methylene and ethylene, and these groups are connected to the oxygen atom possessed by the heterocyclic ring through -O-. In addition, for example, when the heterocyclic ring is an oxazolidine ring, R 2a , R 2b and R 2c The aliphatic group is methylene and ethylene, and these groups are linked to the oxygen atom of the heterocyclic ring through -N-. Although several examples of the heterocyclic ring containing a bonding group have been described, the present embodiment is not limited to these examples.
[0196] When the heterocyclic ring has a bonding group, the number of carbon atoms in R 2a , R 2b and R 2c The carbon number of the aliphatic group may be within the range.
[0197] The aliphatic group may be a group in which at least a part of hydrogen atoms are substituted by a halogen atom, a hydroxyl group, an amino group or the like, or a group in which at least a part of hydrogen atoms are substituted by a monovalent aliphatic group.
[0198] In addition, the heterocyclic ring in the general formula (2) may be a heterocyclic ring in which an alicyclic ring and an aromatic ring are bonded or fused. Here, the bonded heterocyclic ring is a heterocyclic ring in which another alicyclic ring or an aromatic ring is bonded to at least one carbon atom of the heterocyclic ring in the general formula (2), and the fused heterocyclic ring is a heterocyclic ring in which another alicyclic ring or an aromatic ring is fused to at least one carbon atom of the heterocyclic ring in the general formula (2). Among the heterocyclic rings in the general formula (2), the bonded or fused heterocyclic ring may be a heterocyclic ring in the above general formula (1). 1 The heterocyclic ring is a ring obtained by bonding or condensing any one of the alicyclic group in the above description, the condensed ring in the aromatic group, that is, the basic structure of the single alicyclic ring, the basic structure of multiple alicyclic rings, and the basic structure of the aromatic ring described above.
[0199] In the case where the heterocyclic ring is a heterocyclic ring obtained by bonding or condensing an alicyclic ring and an aromatic ring, the number of carbon atoms in the heterocyclic ring or the aromatic ring is such that the number of carbon atoms in R 2a , R 2b and R 2c The carbon number of the aliphatic group may be within the range.
[0200] (Properties of the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms)
[0201] Regarding the properties of the heteropolycyclic compound used in the present embodiment described above, the upper limit of the number average molecular weight is preferably 10,000 or less, more preferably 8,000 or less, further preferably 7,000 or less, and further preferably 6,500 or less, that is, the above-mentioned polyfunctional epoxy compound is a compound represented by the general formula (1) and X 1 With -R 1 The upper limit is preferably 80 or more when the basic structure of O- is used as a bonding group.
[0202] The heteropolycyclic compound used in the present embodiment is preferably a compound having a smaller number average molecular weight as shown in the above numerical range, and the content of heteropolycyclic compounds having a number average molecular weight of less than 10,000 in the total amount of heteropolycyclic compounds is preferably 90% by mass or more, more preferably 95% by mass or more, further preferably 99% by mass or more, and further preferably 100% by mass, that is, the total amount is preferably heteropolycyclic compounds having a number average molecular weight of less than 10,000.
[0203] The content of heteropolycyclic compounds having a number average molecular weight exceeding 10,000 in the total amount of heteropolycyclic compounds is preferably 10% by mass or less, more preferably 5% by mass or less, further preferably 1% by mass or less, and further preferably 0% by mass, that is, preferably not contained.
[0204] The content of the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms (heteropolycyclic compound) contained in the modified sulfide solid electrolyte can vary depending on the type of heteropolycyclic compound used, and therefore cannot be generalized, but is preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass, further preferably 0.1 parts by mass or more, and further preferably 0.5 parts by mass, relative to 100 parts by mass of the sulfide solid electrolyte, and the upper limit is preferably 25 parts by mass or less, and more preferably 20 parts by mass or less. Within the above range, the coating adaptability when applied as a paste can be efficiently improved, and excellent battery performance can be obtained more efficiently.
[0205] (Infrared absorption spectrum based on FT-IR analysis)
[0206] The modified sulfide solid electrolyte of the present embodiment preferably has a wavelength of 2800 to 3000 cm in the infrared absorption spectrum by FT-IR analysis (ATR method). -1 Has a peak.
[0207] Since this peak is not a peak that can be detected from the sulfide solid electrolyte, it is considered to be a peak derived from the heteropolycyclic compound contained in the modified sulfide solid electrolyte. If the heteropolycyclic compound exists in a manner confirmed as a peak in the infrared absorption spectrum based on FT-IR analysis (ATR method), the oil absorption is reduced, it is easy to obtain excellent coating adaptability, and excellent battery performance can be obtained more effectively.
[0208] In this specification, FT-IR analysis is analysis using a Fourier transform infrared spectrophotometer and refers to measurement using a total reflectance measurement method (ATR method), and infrared absorption spectrum is a spectrum measured using an FT-IR device under the following conditions.
[0209] Measurement method: Total reflection measurement method (ATR method)
[0210] Measurement wave number range: 650~4000cm -1
[0211] Light source: Silicon carbide lamp (SiC)
[0212] Detector: DTGS detector
[0213] Resolution: 4cm -1
[0214] Measuring time: 1 second / time
[0215] Total times: 256 times
[0216] It is known that in the infrared absorption spectrum, 2800-3000cm -1The peak at is a peak derived from CH stretching vibration. It is believed that this peak is a peak derived from a heteropolycyclic compound, more specifically, a peak derived from a CH bond possessed by the heteropolycyclic compound. In addition, when the heteropolycyclic compound has an alkyl chain, this peak is a peak derived from a CH bond (CH stretching vibration) of the alkyl chain in the heteropolycyclic compound.
[0217] The modified sulfide solid electrolyte of the present embodiment can clearly detect this peak, so it is believed that the heteropolycyclic compound is contained in a form that is easily detected, that is, it exists in a form attached to the surface of the sulfide solid electrolyte. Moreover, it is believed that by existing in this way, the oil absorption of the sulfide solid electrolyte can be reduced, it is easy to obtain excellent coating suitability, and excellent battery performance can be more effectively obtained.
[0218] The modified sulfide solid electrolyte of this embodiment is preferably 1 In the H-NMR spectrum, there is a peak at 0.0 to 5.0 ppm derived from the alkyl chain of the heteropolycyclic compound.
[0219] In this manual, 1 The peaks of the H-NMR spectrum are peaks measured using a nuclear magnetic resonance apparatus (NMR apparatus) under the following conditions.
[0220] Observation core: 1 H
[0221] Resonance frequency: 500MHz
[0222] Probe: 5mmφTCI CryoProbe
[0223] Measurement temperature: 25℃
[0224] Total times: 16 times
[0225] The modified sulfide solid electrolyte of this embodiment has a wavelength of 2800 to 3000 cm in the infrared absorption spectrum. -1 The peak of the heteropolycyclic compound is detected, and it is considered that the heteropolycyclic compound exists in a form in which the peak can be clearly detected, that is, in a form attached to the surface of the sulfide solid electrolyte. 1 The presence of the peak derived from the alkyl chain in the H-NMR spectrum is similar to the infrared absorption spectrum. It is believed that the oil absorption of the sulfide solid electrolyte can be reduced, excellent coating suitability can be easily obtained, and excellent battery performance can be more effectively obtained.
[0226] In addition, as shown in the examples described later, when a modified sulfide solid electrolyte obtained by mixing a sulfide solid electrolyte and a heteropolycyclic compound in an organic solvent is added to a solvent such as toluene to form a slurry and allowed to stand, the supernatant is analyzed by gas chromatography mass spectrometry (GC / MS method). No heteropolycyclic compound is detected. On the other hand, when the precipitated powder is dried to remove the solvent and then dissolved in deuterated methanol, 1 In H-NMR measurement, the chemical shift of the group (alkyl group etc.) derived from the heteropolycyclic compound is detected.
[0227] This phenomenon is considered to indicate that, in the modified sulfide solid electrolyte, the heteropolycyclic compound is firmly attached to the surface of the sulfide solid electrolyte, and this attachment results in a modified sulfide solid electrolyte having reduced oil absorption and excellent coating suitability.
[0228] When the heteropolycyclic compound is attached to the surface of the sulfide solid electrolyte, it may be attached to cover the entire surface of the sulfide solid electrolyte or may be attached to a part of the surface. Either method is acceptable.
[0229] (Manufacturing of sulfide solid electrolyte)
[0230] Next, the sulfide solid electrolyte forming the modified sulfide solid electrolyte of the present embodiment is described. The sulfide solid electrolyte that can be used in the present embodiment contains lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms, and has a BET specific surface area of 10 m 2 / g or more, it can be used without particular limitation, and a commercially available product can be used as it is or can be produced and used.
[0231] In the case of manufacturing and using a sulfide solid electrolyte that can be used in the present embodiment, a manufacturing method thereof will be described. The sulfide solid electrolyte that can be used in the present embodiment can be manufactured by, for example, the following manufacturing method: the manufacturing method includes mixing two or more raw materials selected from a compound containing at least one atom of a lithium atom, a sulfur atom, a phosphorus atom, and a halogen atom.
[0232] (raw material)
[0233] As the raw material, two or more compounds selected from compounds containing at least one atom of a lithium atom, a sulfur atom, a phosphorus atom, and a halogen atom can be used.
[0234] The compound that can be used as a raw material is a compound containing at least one of a lithium atom, a phosphorus atom, a sulfur atom and a halogen atom. More specifically, representative examples include: lithium sulfide; lithium halides such as lithium fluoride, lithium chloride, lithium bromide, and lithium iodide; alkali metal halides such as sodium iodide, sodium fluoride, sodium chloride, and sodium bromide; phosphorus sulfides such as phosphorus trisulfide (P2S3) and phosphorus pentasulfide (P2S5); various phosphorus fluorides (PF3, PF5), various phosphorus chlorides (PCl3, PCl5, P2Cl4), various phosphorus bromides (PBr3, PB r5), various phosphorus iodides (PI3, P2I4) and other phosphorus halides; thiophosphoryl fluoride (PSF3), thiophosphoryl chloride (PSCl3), thiophosphoryl bromide (PSBr3), thiophosphoryl iodide (PSI3), thiophosphoryl fluoride dichloride (PSCl2F), thiophosphoryl fluoride dibromide (PSBr2F) and other thiophosphoryl halides; and other raw materials composed of at least two atoms selected from the above four atoms; halogen monomers such as fluorine (F2), chlorine (Cl2), bromine (Br2), iodine (I2), preferably bromine (Br2) and iodine (I2).
[0235] Compounds other than the above that can be used as raw materials include, for example, compounds containing at least one atom selected from the above four atoms and atoms other than the four atoms. More specifically, examples include: lithium compounds such as lithium oxide, lithium hydroxide, and lithium carbonate; alkali metal sulfides such as sodium sulfide, potassium sulfide, rubidium sulfide, and cesium sulfide; metal sulfides such as silicon sulfide, germanium sulfide, boron sulfide, gallium sulfide, tin sulfide (SnS, SnS2), aluminum sulfide, and zinc sulfide; phosphoric acid compounds such as sodium phosphate and lithium phosphate; metal halides such as aluminum halides, silicon halides, germanium halides, arsenic halides, selenium halides, tin halides, antimony halides, tellurium halides, and bismuth halides; halogenated phosphorus oxides such as phosphorus oxychloride (POCl3) and phosphorus oxybromide (POBr3); and the like.
[0236] In this embodiment, from the viewpoint of more easily obtaining a sulfide solid electrolyte with high ionic conductivity, chlorine atoms, bromine atoms, and iodine atoms are preferred among the halogen atoms, and bromine atoms and iodine atoms are more preferred. In addition, these atoms can be used alone or in combination. That is, taking lithium halide as an example, lithium bromide can be used alone, lithium iodide can be used alone, or lithium bromide and lithium iodide can be used in combination.
[0237] In addition, from the same point of view, as compounds that can be used as raw materials, among the above, lithium sulfide is preferred; phosphorus sulfides such as phosphorus trisulfide (P2S3) and phosphorus pentasulfide (P2S5); halogen monomers such as fluorine (F2), chlorine (Cl2), bromine (Br2), and iodine (I2); lithium halides such as lithium fluoride, lithium chloride, lithium bromide, and lithium iodide. Among phosphorus sulfides, phosphorus pentasulfide is preferred; among halogen monomers, chlorine (Cl2), bromine (Br2), and iodine (I2) are preferred; and among lithium halides, lithium chloride, lithium bromide, and lithium iodide are preferred.
[0238] As combinations of compounds that can be used as raw materials, for example, combinations of lithium sulfide, phosphorus pentasulfide and lithium halides, and combinations of lithium sulfide, phosphorus pentasulfide and halogen monomers can be preferably mentioned. Lithium bromide, lithium iodide and lithium chloride are preferred as lithium halides, and chlorine, bromine and iodine are preferred as halogen monomers.
[0239] In the present embodiment, when lithium sulfide is used as the compound containing lithium atoms, the lithium sulfide is preferably in the form of particles.
[0240] The average particle size of lithium sulfide particles (D 50 ) is preferably 10 μm to 2000 μm, more preferably 30 μm to 1500 μm, and even more preferably 50 μm to 1000 μm. In this specification, the average particle size (D 50 ) is the particle size when the particle size distribution cumulative curve is drawn from the smallest particle to 50% of the total, and the volume distribution is, for example, the average particle size that can be measured using a laser diffraction / scattering particle size distribution measuring device. In addition, among the substances exemplified as the above-mentioned raw materials, the solid raw material preferably has an average particle size of the same degree as the above-mentioned lithium sulfide particles, that is, the average particle size is preferably within the same range as the average particle size of the above-mentioned lithium sulfide particles.
[0241] When lithium sulfide, phosphorus pentasulfide and lithium halide are used as raw materials, from the viewpoint of obtaining higher chemical stability and the viewpoint of increasing the PS4 fraction and obtaining high ion conductivity, the ratio of lithium sulfide to the total of lithium sulfide and phosphorus pentasulfide is preferably 60 mol% or more, more preferably 65 mol% or more, further preferably 68 mol% or more, and the upper limit is preferably 80 mol% or less, more preferably 78 mol% or less, further preferably 76 mol% or less.
[0242] When lithium sulfide, phosphorus pentasulfide, lithium halide, and other raw materials used as needed are used, the content of lithium sulfide and phosphorus pentasulfide relative to the total of these is preferably 60 mol% or more, more preferably 65 mol% or more, and further preferably 70 mol% or more, and the upper limit is preferably 100 mol% or less, more preferably 90 mol% or less, and further preferably 80 mol% or less.
[0243] In addition, when lithium bromide and lithium iodide are used in combination as lithium halides, from the viewpoint of increasing the PS4 fraction and obtaining high ion conductivity, the ratio of lithium bromide to the total of lithium bromide and lithium iodide is preferably 1 mol% or more, more preferably 20 mol% or more, further preferably 40 mol% or more, further preferably 50 mol% or more, and the upper limit is preferably 99 mol% or less, more preferably 90 mol% or less, further preferably 80 mol% or less, further preferably 70 mol% or less.
[0244] When a halogen monomer is used as a raw material and lithium sulfide and phosphorus pentasulfide are used, the ratio of the mole number of lithium sulfide obtained by removing the same mole number of lithium sulfide as the mole number of the halogen monomer to the total mole number of lithium sulfide and phosphorus pentasulfide obtained by removing the same mole number of lithium sulfide as the mole number of the halogen monomer is preferably in the range of 60 to 90%, more preferably in the range of 65 to 85%, further preferably in the range of 68 to 82%, further preferably in the range of 72 to 78%, and particularly preferably in the range of 73 to 77%. This is because, if these ratios are used, higher ion conductivity can be obtained. In addition, from the same viewpoint, when lithium sulfide, phosphorus pentasulfide and a halogen monomer are used, the content of the halogen monomer relative to the total amount of lithium sulfide, phosphorus pentasulfide and the halogen monomer is preferably 1 to 50 mol%, more preferably 2 to 40 mol%, further preferably 3 to 25 mol%, and further preferably 3 to 15 mol%.
[0245] When lithium sulfide, phosphorus pentasulfide, a halogen monomer and a lithium halide are used, the content of the halogen monomer relative to the total amount of these (α mol%) and the content of the lithium halide relative to the total amount of these (β mol%) preferably satisfy the following formula (1), more preferably satisfy the following formula (2), further preferably satisfy the following formula (3), and further preferably satisfy the following formula (4).
[0246] 2≤2α+β≤100…(1)
[0247] 4≤2α+β≤80…(2)
[0248] 6≤2α+β≤50…(3)
[0249] 6≤2α+β≤30…(4)
[0250] (mix)
[0251] The mixing of two or more raw materials selected from compounds containing at least one of lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms can be performed by mixing the raw materials using, for example, a mixer, a stirrer, a pulverizer or the like.
[0252] This is because the raw materials can be mixed even when a stirrer is used, and when a pulverizer is used, the raw materials are pulverized and mixed at the same time. That is, it can be said that the sulfide solid electrolyte used in the present embodiment can be mixed by stirring, mixing, pulverizing, or any combination of two or more raw materials selected from compounds containing at least one of lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms.
[0253] As agitators and mixers, for example, a mechanical stirring mixer having stirring blades in a reaction tank and capable of stirring (also referred to as mixing brought by stirring, stirring and mixing) can be exemplified. As mechanical stirring mixers, high-speed stirring mixers, double-arm mixers, etc. can be exemplified. In addition, as high-speed stirring mixers, vertical axis rotating mixers, horizontal axis rotating mixers, etc. can be exemplified, and any type of mixer can also be used.
[0254] The shape of the stirring blade used in the mechanical stirring mixer may be a blade type, an arm type, an anchor type, a paddle type, a stirring paddle type, a belt type, a multi-stage blade type, a double-arm type, a bucket type, a double-shaft blade type, a flat blade type, a C-blade type, etc. From the viewpoint of more efficiently promoting the reaction of the raw materials, a bucket type, a flat blade type, a C-blade type, an anchor type, a paddle type, a stirring paddle type is preferred, and an anchor type, a paddle type, a stirring paddle type is more preferred.
[0255] When a mechanical stirring mixer is used, the rotation speed of the stirring blade can be appropriately adjusted according to the capacity, temperature, shape of the stirring blade, etc. of the fluid in the reaction tank, without any particular limitation, and is usually set to about 5 rpm to about 400 rpm. From the viewpoint of more efficiently promoting the reaction of the raw materials, it is preferably 10 rpm to 300 rpm, more preferably 15 rpm to 250 rpm, and further preferably 20 rpm to 200 rpm.
[0256] The temperature conditions for mixing using a mixer are not particularly limited, and are, for example, usually -30 to 120° C., preferably -10 to 100° C., more preferably 0 to 80° C., and further preferably 10 to 60° C. The mixing time is usually 0.1 to 500 hours, and from the viewpoint of making the dispersion state of the raw materials more uniform and promoting the reaction, is preferably 1 to 450 hours, more preferably 10 to 425 hours, further preferably 20 to 400 hours, and further preferably 40 to 375 hours.
[0257] The method of mixing with pulverization using a pulverizer is a method conventionally adopted as a solid phase method (mechanical grinding method). As the pulverizer, for example, a media type pulverizer using pulverizing media can be used.
[0258] The media pulverizer is roughly divided into a container-driven pulverizer and a media-stirring pulverizer. As the container-driven pulverizer, a stirring tank, a crushing tank, or a ball mill or a bead mill in which these are combined can be cited. In addition, as the media-stirring pulverizer, there can be cited: impact pulverizers such as a cutter mill, a hammer mill, and a pin mill; tower-type pulverizers such as a tower mill; stirring tank-type pulverizers such as a grinder, a wet sand mill (aquamizer), and a sand mill; flow-through trough-type pulverizers such as a viscose mill and a coarse crusher; flow-through tube-type pulverizers; annular pulverizers such as a combined ball mill; a continuous dynamic pulverizer; various pulverizers such as a single-shaft or multi-shaft kneading machine. Among them, if the ease of adjusting the particle size of the obtained sulfide is considered, the ball mill and bead mill exemplified as the container-driven pulverizer are preferred, and a planetary pulverizer is preferred.
[0259] These pulverizers can be appropriately selected according to the desired scale, etc. For a relatively small scale, a container-driven pulverizer such as a ball mill or a bead mill can be used. In the case of large-scale or mass production, other types of pulverizers can also be used.
[0260] Furthermore, as described later, when the mixture is in a liquid state accompanied with a liquid such as a solvent or in a slurry state during mixing, a wet pulverizer capable of wet pulverization is preferred.
[0261] As wet pulverizers, wet bead mills, wet ball mills, wet vibration mills, etc. can be representatively cited. From the perspective of being able to freely adjust the conditions of the pulverization operation and being easy to handle materials with smaller particle sizes, wet bead mills using beads as pulverization media are preferred. In addition, dry pulverizers such as dry bead mills, dry ball mills, dry vibration mills, and dry non-media pulverizers such as jet mills can also be used.
[0262] In addition, when the object to be mixed is in a liquid state or a slurry state, a flow-through pulverizer can be used, which can be circulated as needed. Specifically, a pulverizer that circulates between a pulverizer (pulverizing mixer) for pulverizing slurry and a temperature-maintaining tank (reaction container) can be cited.
[0263] The size of the beads or balls used in the above-mentioned ball mill or bead mill can be appropriately selected according to the desired particle size, processing volume, etc. For example, the diameter of the beads is usually 0.05 mmφ or more, preferably 0.1 mmφ or more, more preferably 0.3 mmφ or more, and the upper limit is usually 5.0 mmφ or less, preferably 3.0 mmφ or less, and more preferably 2.0 mmφ or less. In addition, the diameter of the balls is usually 2.0 mmφ or more, preferably 2.5 mmφ or more, and more preferably 3.0 mmφ or more, and the upper limit is usually 20.0 mmφ or less, preferably 15.0 mmφ or less, and more preferably 10.0 mmφ or less.
[0264] In addition, examples of the material include metals such as stainless steel, chrome steel, and tungsten carbide; ceramics such as zirconium oxide and silicon nitride; and minerals such as agate.
[0265] When a ball mill or a bead mill is used, the rotation speed cannot be generally specified because it varies according to the scale of treatment, but is usually 10 rpm or more, preferably 20 rpm or more, and more preferably 50 rpm or more, and the upper limit is usually 1,000 rpm or less, preferably 900 rpm or less, more preferably 800 rpm or less, and further preferably 700 rpm or less.
[0266] The pulverization time in this case cannot be generally stated because it varies depending on the scale of treatment, but is usually 0.5 hours or more, preferably 1 hour or more, more preferably 5 hours or more, and further preferably 10 hours or more, and the upper limit is usually 100 hours or less, preferably 72 hours or less, more preferably 48 hours or less, and further preferably 36 hours or less.
[0267] By selecting the size and material of the medium (beads, balls) used, the rotation speed and time of the rotor, etc., mixing, stirring, pulverization, or any combination of these can be performed, and the particle size of the obtained sulfide can be adjusted.
[0268] (Solvent)
[0269] When the above-mentioned mixing is performed, a solvent may be added to the above-mentioned raw materials for mixing. As the solvent, various solvents called organic solvents and the like can be widely used.
[0270] As the solvent, a wide range of solvents conventionally used in the production of solid electrolytes can be adopted, and examples thereof include hydrocarbon solvents such as aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, and aromatic hydrocarbon solvents.
[0271] Examples of aliphatic hydrocarbons include hexane, pentane, 2-ethylhexane, heptane, octane, decane, undecane, dodecane and tridecane. Examples of alicyclic hydrocarbons include cyclohexane and methylcyclohexane. Examples of aromatic hydrocarbon solvents include benzene, toluene, xylene, mesitylene, ethylbenzene, tert-butylbenzene, trifluoromethylbenzene and nitrobenzene.
[0272] In addition to the above-mentioned hydrocarbon solvents, solvents containing atoms other than carbon atoms and hydrogen atoms, such as nitrogen atoms, oxygen atoms, sulfur atoms, halogen atoms and other heteroatoms, can also be exemplified. Such solvents have the property of easily forming complexes with compounds containing lithium atoms, phosphorus atoms, sulfur atoms and halogen atoms used as raw materials (hereinafter, such solvents are also referred to as "complexing agents"), and because they have the property of making halogen atoms easily remain in the structure of the sulfide solid electrolyte, they are useful in obtaining higher ion conductivity. As such complexing agents, in addition to ether solvents and ester solvents containing oxygen atoms as heteroatoms, alcohol solvents, aldehyde solvents and ketone solvents can also be preferably exemplified.
[0273] As the ether solvent, for example, preferably there can be mentioned aliphatic ethers such as dimethyl ether, diethyl ether, tert-butyl methyl ether, dimethoxymethane, dimethoxyethane, diethylene glycol dimethyl ether (diglyme), triethylene glycol dimethyl ether (triglyme) or diethylene glycol, triethylene glycol; alicyclic ethers such as ethylene oxide, propylene oxide, tetrahydrofuran, tetrahydropyran, dimethoxytetrahydrofuran, cyclopentyl methyl ether, dioxane; heterocyclic ethers such as furan, benzofuran, benzopyran; aromatic ethers such as methyl phenyl ether (anisole), ethyl phenyl ether, dibenzyl ether, diphenyl ether.
[0274] As the ester solvent, for example, preferably exemplified are methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate; aliphatic esters such as methyl propionate, ethyl propionate, dimethyl oxalate, diethyl oxalate, dimethyl malonate, diethyl malonate, dimethyl succinate, diethyl succinate; alicyclic esters such as methyl cyclohexanecarboxylate, ethyl cyclohexanecarboxylate, dimethyl cyclohexanedicarboxylate; heterocyclic esters such as methyl pyridinecarboxylate, methyl pyrimidinecarboxylate, acetyl lactone, propiolactone, butyrolactone, valerolactone; aromatic esters such as methyl benzoate, ethyl benzoate, dimethyl phthalate, diethyl phthalate, butyl benzyl phthalate, dicyclohexyl phthalate, trimethyl trimellitate, triethyl trimellitate.
[0275] In addition, preferably, there can be mentioned alcohol solvents such as ethanol and butanol; aldehyde solvents such as formaldehyde, acetaldehyde and dimethylformamide; ketone solvents such as acetone and methyl ethyl ketone.
[0276] Examples of the solvent containing a nitrogen atom as a hetero atom include solvents having a group containing a nitrogen atom such as an amino group, an amide group, a nitro group or a nitrile group.
[0277] For example, as the solvent having an amino group, preferably exemplified are aliphatic amines such as ethylenediamine, diaminopropane, dimethylethylenediamine, diethylethylenediamine, dimethyldiaminopropane, tetramethyldiaminomethane, tetramethylethylenediamine (TMEDA), and tetramethyldiaminopropane (TMPDA); alicyclic amines such as cyclopropanediamine, cyclohexanediamine, and bisaminomethylcyclohexane; heterocyclic amines such as isophoronediamine, piperazine, dipiperidylpropane, and dimethylpiperazine; and aromatic amines such as phenylenediamine, toluenediamine, naphthalenediamine, methylphenylenediamine, dimethylnaphthalenediamine, dimethylphenylenediamine, tetramethylphenylenediamine, and tetramethylnaphthalenediamine.
[0278] Also preferably, there can be mentioned nitrile solvents such as acetonitrile and acrylonitrile; and solvents containing nitrogen atoms such as dimethylformamide, nitrobenzene and dimethylacetamide.
[0279] As the solvent containing a halogen atom as a hetero atom, preferably, chloroform, carbon tetrachloride, dichloromethane, chlorobenzene, trifluoromethylbenzene, chlorobenzene, chlorotoluene, bromobenzene and the like are exemplified.
[0280] Furthermore, as the solvent containing a sulfur atom, dimethyl sulfoxide, carbon disulfide, etc. can be preferably exemplified.
[0281] When using a solvent, the usage amount of the solvent is preferably more than 100 mL relative to the total amount 1kg of the raw material, more preferably more than 200 mL, further preferably more than 250 mL, more preferably more than 300 mL, and as the upper limit is preferably below 3000 mL, more preferably below 2500 mL, further preferably below 2000 mL, and further preferably below 1550 mL. If the usage amount of the solvent is within the above range, the raw material reaction can be efficiently made.
[0282] (dry)
[0283] In the case of using a solvent for mixing, the fluid (usually a slurry) obtained by mixing may be dried after mixing. In the case of using a complexing agent as a solvent, the sulfide solid electrolyte can be obtained by removing the complexing agent from the complex containing the complexing agent, and in the case of using a complexing agent and a solvent in combination, by removing the complexing agent from the complex containing the complexing agent and removing the solvent, and in the case of using a solvent other than a complexing agent, by removing the solvent. The obtained sulfide solid electrolyte exhibits ionic conductivity caused by lithium atoms.
[0284] The fluid obtained by mixing can be dried at a temperature corresponding to the type of solvent, for example, at a temperature equal to or higher than the boiling point of the complexing agent.
[0285] Furthermore, the complexing agent and the solvent used as required can be dried by volatilizing them by using a vacuum pump or the like under reduced pressure (vacuum drying) at usually 5 to 100°C, preferably 10 to 85°C, more preferably 15 to 70°C, and still more preferably around room temperature (23°C) (e.g. around room temperature ±5°C).
[0286] The fluid may also be dried by filtration using a glass filter, solid-liquid separation by decantation, or solid-liquid separation using a centrifuge. When a solvent other than a complexing agent is used, a sulfide solid electrolyte can be obtained by solid-liquid separation. In addition, when a complexing agent is used as a solvent, after solid-liquid separation, drying under the above-mentioned temperature conditions is performed to remove the complexing agent introduced into the complex.
[0287] Specifically, as a solid-liquid separation, the fluid is transferred to a container, and after the sulfide (or the complex (a substance that can be called a precursor of a sulfide solid electrolyte)) is precipitated, it is easier to remove the complexing agent and solvent that become the supernatant by decantation or by filtering using, for example, a glass filter with a pore size of about 10 to 200 μm, preferably 20 to 150 μm.
[0288] Drying may be performed after mixing and before the hydrogen treatment described below, or after the hydrogen treatment.
[0289] The sulfide solid electrolyte obtained by the above mixing, or the sulfide solid electrolyte obtained by removing the solvent by the above drying when a solvent is used, expresses ion conductivity due to lithium atoms.
[0290] The sulfide solid electrolyte obtained by the above mixing basically becomes an amorphous sulfide solid electrolyte (glass component) unless the mixture is pulverized to a degree of crystallization using a pulverizer, for example.
[0291] The sulfide solid electrolyte obtained by the above mixing may be an amorphous sulfide solid electrolyte (glass component) or a crystalline sulfide solid electrolyte, and can be appropriately selected as desired. When a crystalline sulfide solid electrolyte is produced, the amorphous sulfide solid electrolyte obtained by the above mixing is heated to produce a crystalline sulfide solid electrolyte.
[0292] As a sulfide solid electrolyte, in order to adjust the particle size of the powder of the crystalline sulfide solid electrolyte, after subjecting it to a treatment such as pulverization described below, a crystalline sulfide solid electrolyte having an amorphous component (glass component) formed on its surface may be included. Therefore, the sulfide solid electrolyte containing an amorphous component also includes an amorphous sulfide solid electrolyte or a crystalline sulfide solid electrolyte having an amorphous component formed on its surface.
[0293] (heating)
[0294] When a crystalline sulfide solid electrolyte is produced, heating may be further included. When an amorphous sulfide solid electrolyte (glass component) is obtained by the above mixing, a crystalline sulfide solid electrolyte can be obtained by heating, and when a crystalline sulfide solid electrolyte is obtained, a crystalline sulfide solid electrolyte with improved crystallinity can be obtained.
[0295] In addition, when a complexing agent is used as a solvent during mixing, although a complex containing the complexing agent is formed, the complexing agent can be removed from the complex by heating without the above-mentioned drying to obtain a sulfide solid electrolyte. Depending on the heating conditions, an amorphous substance can be made, and a crystalline substance can be made.
[0296] Regarding the heating temperature, for example, in the case of obtaining an amorphous sulfide solid electrolyte, the heating temperature may be determined according to the structure of the crystalline sulfide solid electrolyte obtained by heating the amorphous sulfide solid electrolyte. Specifically, the amorphous sulfide solid electrolyte is subjected to differential thermal analysis (DTA) using a differential thermal analyzer (DTA apparatus) under a temperature increase condition of 10°C / min, and the temperature of the peak top of the exothermic peak observed on the lowest temperature side is preferably set to a range of 5°C or less, more preferably 10°C or less, and further preferably 20°C or less, with the lower limit not particularly limited, but may be set to a temperature of the peak top of the exothermic peak observed on the lowest temperature side of about -40°C or more. By setting the temperature in such a range, an amorphous sulfide solid electrolyte can be obtained more efficiently and reliably. The heating temperature for obtaining an amorphous sulfide solid electrolyte varies depending on the structure of the obtained crystalline sulfide solid electrolyte and cannot be generally specified, but is usually preferably 135°C or lower, more preferably 130°C or lower, and further preferably 125°C or lower. The lower limit is not particularly limited, but is preferably 90°C or higher, more preferably 100°C or higher, and further preferably 105°C or higher.
[0297] In addition, when heating an amorphous sulfide solid electrolyte to obtain a crystalline sulfide solid electrolyte, the heating temperature may be determined according to the structure of the crystalline sulfide solid electrolyte, and is preferably higher than the above-mentioned heating temperature for obtaining an amorphous sulfide solid electrolyte. Specifically, the amorphous sulfide solid electrolyte is subjected to differential thermal analysis (DTA) using a differential thermal analyzer (DTA device) under a temperature increase condition of 10°C / min, and the temperature of the peak top of the exothermic peak observed on the lowest temperature side is preferably set to 5°C or more, more preferably 10°C or more, and further preferably 20°C or more. The upper limit is not particularly limited, but may be about 40°C or less. By setting the temperature in such a range, a crystalline sulfide solid electrolyte can be obtained more efficiently and reliably. The heating temperature for obtaining a crystalline sulfide solid electrolyte varies depending on the composition and structure of the obtained crystalline sulfide solid electrolyte and cannot be generally specified, but is usually preferably 130° C. or higher, more preferably 135° C. or higher, and further preferably 140° C. or higher. The upper limit is not particularly limited, but is preferably 600° C. or lower, more preferably 550° C. or lower, and further preferably 500° C. or lower.
[0298] The heating time is not particularly limited as long as it is a time for obtaining the desired amorphous sulfide solid electrolyte or crystalline sulfide solid electrolyte, and is, for example, preferably 1 minute or more, more preferably 10 minutes or more, further preferably 30 minutes or more, and further preferably 1 hour or more. In addition, the upper limit of the heating time is not particularly limited, but is preferably 24 hours or less, more preferably 10 hours or less, further preferably 5 hours or less, and further preferably 3 hours or less.
[0299] In addition, heating is preferably performed in an inert gas atmosphere (e.g., a nitrogen atmosphere, an argon atmosphere) or in a reduced pressure atmosphere (particularly in a vacuum). For example, an inert gas atmosphere containing a certain concentration of hydrogen may also be used. This is because it is possible to prevent degradation (e.g., oxidation) of the crystalline sulfide solid electrolyte.
[0300] The heating method is not particularly limited, and examples thereof include methods using a hot plate, a vacuum heating device, an argon atmosphere furnace, a firing furnace, etc. In addition, in industry, a horizontal dryer or a horizontal vibrating fluidized dryer having a heating unit and a feeding mechanism can also be used, and the method can be selected according to the amount of heating treatment.
[0301] (Sulfide solid electrolyte)
[0302] As described above, the sulfide solid electrolyte used in the present embodiment may be a commercially available product or a manufactured sulfide solid electrolyte.
[0303] The sulfide solid electrolyte obtained by the above method is an amorphous (glass component) or crystalline sulfide solid electrolyte containing lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms, and is preferably used as the sulfide solid electrolyte in the present embodiment.
[0304] (BET specific surface area)
[0305] Regarding the specific surface area of the sulfide solid electrolyte used in this embodiment, the BET specific surface area is 10 m 2 / g or more. Although the modified sulfide solid electrolyte of this embodiment has a large specific surface area as described above, it has excellent coating adaptability when applied as a paste and can effectively demonstrate excellent battery performance. The higher the BET specific surface area of the sulfide solid electrolyte, the more the advantage of this effect can be further demonstrated. From this point of view, the BET specific surface area is preferably 12m 2 / g or more, more preferably 15m 2 / g or more, more preferably 20m 2 From the same point of view, there is no particular upper limit, but it is actually 100 m 2 / g or less, preferably 75m 2 / g or less, more preferably 50m 2 / g or less.
[0306] In this specification, the BET specific surface area is a specific surface area measured using krypton gas as an adsorbent in accordance with JIS Z 8830:2013 (method for measuring specific surface area of powders (solids) by gas adsorption).
[0307] (Amorphous sulfide solid electrolyte)
[0308] As the amorphous sulfide solid electrolyte obtained by the above method, it contains lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms. As representative amorphous sulfide solid electrolytes, for example, solid electrolytes composed of lithium sulfide, phosphorus sulfide and lithium halide, such as Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, Li2S-P2S5-LiI-LiBr, etc. can be preferably exemplified; and solid electrolytes such as Li2S-P2S5-Li2O-LiI, Li2S-SiS2-P2S5-LiI, etc., which contain other atoms such as oxygen atoms and silicon atoms. From the viewpoint of obtaining higher ionic conductivity, solid electrolytes composed of lithium sulfide, phosphorus sulfide and lithium halide, such as Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, Li2S-P2S5-LiI-LiBr, etc. can be preferably exemplified.
[0309] The types of atoms constituting the amorphous sulfide solid electrolyte can be confirmed by, for example, an ICP emission spectrometer.
[0310] The shape of the amorphous sulfide solid electrolyte is not particularly limited, and may be, for example, a particle shape. The average particle size (D 50 ) For example, the range of 0.01 μm to 500 μm and 0.1 to 200 μm can be exemplified.
[0311] (Crystalline sulfide solid electrolyte)
[0312] The crystalline sulfide solid electrolyte obtained by the above method can be a so-called glass ceramic obtained by heating an amorphous solid electrolyte to a temperature above the crystallization temperature. As its crystal structure, Li3PS4 crystal structure, Li4P2S6 crystal structure, Li7PS6 crystal structure, Li7P3S 11 A crystal structure, a crystal structure having peaks near 2θ=20.2° and 23.6° (for example, Japanese Patent Application Laid-Open No. 2013-16423), and the like.
[0313] In addition, Li 4-x Ge 1-x P x The S4 type sulfide crystalline lithium superion conductor region II (thio-LISICONRegion II) type crystal structure (see Kanno et al., Journal of The Electrochemical Society, 148 (7) A742-746 (2001)), and Li 4-x Ge 1-x P x S4 type thio-LISICON Region II type crystal structure (see Solid State Ionics, 177 (2006), 2721-2725). From the perspective of obtaining higher ionic conductivity, the crystal structure of the crystalline sulfide solid electrolyte obtained by the manufacturing method of this embodiment is preferably a thio-LISICON Region II type crystal structure among the above. Here, "thio-LISICON Region II type crystal structure" means Li 4-x Ge 1-x P x S4-type sulfide crystalline lithium superion conductor region II (thio-LISICON Region II) crystal structure, and Li 4-x Ge 1-x P xAny crystal structure similar to the S4 type thio-LISICON Region II type crystal structure. In addition, the crystalline sulfide solid electrolyte obtained by the manufacturing method of this embodiment can be a crystalline sulfide solid electrolyte having the above-mentioned thio-LISICON Region II type crystal structure, or it can be a crystalline sulfide solid electrolyte having the thio-LISICON Region II type crystal structure as the main crystal. From the viewpoint of obtaining higher ionic conductivity, it is preferred to have the thio-LISICON Region II type crystal structure as the main crystal. In this specification, "having as the main crystal" means that the proportion of the crystal structure as the object in the crystal structure is 80% or more, preferably 90% or more, and more preferably 95% or more. In addition, from the viewpoint of obtaining higher ionic conductivity, the crystalline sulfide solid electrolyte obtained by the manufacturing method of this embodiment preferably does not contain crystalline Li3PS4 (β-Li3PS4).
[0314] In the X-ray diffraction measurement using CuKα rays, the diffraction peaks of the Li3PS4 crystal structure appear, for example, at 2θ=17.5°, 18.3°, 26.1°, 27.3°, and 30.0°; the diffraction peaks of the Li4P2S6 crystal structure appear, for example, at 2θ=16.9°, 27.1°, and 32.5°; the diffraction peaks of the Li7PS6 crystal structure appear, for example, at 2θ=15.3°, 25.2°, 29.6°, and 31.0°; and the diffraction peaks of the Li7P3S 11 The diffraction peaks of the crystal structure appear near 2θ=17.8°, 18.5°, 19.7°, 21.8°, 23.7°, 25.9°, 29.6°, and 30.0°, for example. 4-x Ge 1-x P x The diffraction peaks of the S4-type sulfide crystalline lithium superion conductor region II (thio-LISICON Region II) crystal structure appear near 2θ=20.1°, 23.9°, and 29.5°, which are similar to Li 4-x Ge 1-x P x The diffraction peaks of the S4 type sulfide crystalline lithium superion conductor region II (thio-LISICON Region II) type crystal structure appear, for example, near 2θ=20.2 and 23.6°. In addition, these peak positions can fluctuate within a range of ±0.5°.
[0315] As described above, when obtaining the crystal structure of the sulfide crystalline lithium superionic conductor region II type in the present embodiment, it is preferably free of crystalline Li3PS4 (β-Li3PS4). The sulfide solid electrolyte obtained by the manufacturing method of the present embodiment does not have diffraction peaks at 2θ = 17.5° and 26.1° that can be observed in crystalline Li3PS4, or even if it has them, it only has a level where the detected peaks are extremely small compared to the diffraction peaks of the sulfide crystalline lithium superionic conductor region II type crystal structure.
[0316] The above-mentioned crystal structure represented by the composition formula Li 7-x P 1- y Si y S6 and Li 7+x P 1-y Si y S6 (where x is -0.6 to 0.6 and y is 0.1 to 0.6) is cubic or orthorhombic, preferably cubic, and in X-ray diffraction measurement using CuKα radiation, it mainly has peaks appearing at positions of 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0° and 52.0°. The above-mentioned crystal structure represented by the composition formula Li 7-x-2y PS 6-x-y Cl x (0.8 ≤ x ≤ 1.7, 0 < y ≤ -0.25x + 0.5) is preferably cubic, and in X-ray diffraction measurement using CuKα radiation, it mainly has peaks appearing at positions of 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0° and 52.0°. In addition, the above-mentioned crystal structure represented by the composition formula Li 7-x PS 6-x Ha x (where Ha is Cl or Br, and x is preferably 0.2 to 1.8) is preferably cubic, and in X-ray diffraction measurement using CuKα radiation, it mainly has peaks appearing at positions of 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0° and 52.0°. These crystal structures basically having the structural framework of Li7PS6 are also called argyrodite-type crystal structures.
[0317] In addition, regarding these peak positions, they can fluctuate within a range of ±0.5°.
[0318] As for the shape of the crystalline sulfide solid electrolyte, there is no particular limitation, and for example, particulate form can be cited. The average particle size (D 50) For example, the range of 0.01 μm to 500 μm and 0.1 to 200 μm can be exemplified.
[0319] (Properties of modified sulfide solid electrolyte)
[0320] The BET specific surface area of the modified sulfide solid electrolyte of this embodiment is 10 m 2 / g or more, having a larger specific surface area. The higher the BET specific surface area of the sulfide solid electrolyte, the more advantageous this effect can be shown. From this point of view, the BET specific surface area is preferably 12 m 2 / g or more, more preferably 15m 2 / g or more, more preferably 20m 2 From the same point of view, there is no particular upper limit, but it is actually 100 m 2 / g or less, preferably 75m 2 / g or less, more preferably 50m 2 / g or less.
[0321] Even if the heteropolycyclic compound is attached to the surface, it will not have a significant effect on the BET specific surface area of the sulfide solid electrolyte. The BET specific surface area of the sulfide solid electrolyte used in this embodiment is substantially the same as the BET specific surface area of the modified sulfide solid electrolyte. 2 / g or more sulfide solid electrolyte as the sulfide solid electrolyte, the BET specific surface area of the modified sulfide solid electrolyte will naturally become 10m 2 / g or above.
[0322] Regarding the oil absorption of the modified sulfide solid electrolyte of the present embodiment, although the BET specific surface area is large as described above, it is usually small and less than 0.9 mL / g due to the effect of the heteropolycyclic compound attached to the surface, and is more preferably 0.85 mL / g or less and less than 0.80 mL / g. Although the modified sulfide solid electrolyte of the present embodiment has a large BET specific surface area, due to the small oil absorption, when it is made into a paste, the increase in the viscosity of the paste can be suppressed, and the coating adaptability during coating is excellent, and there is no need to use a solvent or the like to suppress the increase in the viscosity of the paste, so it is easy to obtain excellent battery performance.
[0323] In this specification, regarding the oil absorption, 1 g of the modified sulfide solid electrolyte is used as a sample, 1 drop of butyl butyrate is added to a mortar or the like, and then stirred with a spatula, and this operation is repeated until the sample becomes a paste, and the total amount of butyl butyrate added is defined as the oil absorption (mL / g). Here, "paste" refers to a state of "a substance that can be extended without breaking or becoming broken and slightly adheres to a measuring plate" as specified in "7.2 Measurement" of JIS K5101-13-1:2004 (Testing Methods for Pigments - Part 13: Oil Absorption - Section 1: Refined Linseed Oil Method).
[0324] In addition, the ion conductivity of the modified sulfide solid electrolyte of this embodiment is usually 0.5 mS / cm or more, further 1.0 mS / cm or more, 1.5 mS / cm or more, 2.0 mS / cm or more, and 2.5 mS / cm or more, and has extremely high ion conductivity, and a lithium battery with excellent battery performance can be obtained.
[0325] (use)
[0326] The modified sulfide solid electrolyte of this embodiment has excellent coating adaptability and can be used in the manufacture of batteries even without using solvents, so it can effectively demonstrate excellent battery performance. In addition, it has high ion conductivity and excellent battery performance, so it is preferably used in batteries.
[0327] The modified sulfide solid electrolyte of this embodiment can be used for the positive electrode layer, the negative electrode layer, or the electrolyte layer. In addition, each layer can be produced by a known method.
[0328] In addition, the battery preferably uses a current collector in addition to the positive electrode layer, the electrolyte layer and the negative electrode layer, and the current collector can use a known current collector. For example, a layer obtained by coating a substance that reacts with the solid electrolyte such as Au, Pt, Al, Ti or Cu can be used.
[0329] [Method for producing modified sulfide solid electrolyte]
[0330] The method for producing the modified sulfide solid electrolyte of this embodiment includes:
[0331] A sulfide solid electrolyte, a compound having two or more heterocyclic rings having carbon atoms and oxygen atoms, and an organic solvent are mixed, wherein the sulfide solid electrolyte has a BET specific surface area of 10 m 2 / g or more and contains lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms;
[0332] The organic solvent is removed.
[0333] According to the production method of the present embodiment, the modified sulfide solid electrolyte of the present embodiment described above can be efficiently produced. That is, the modified sulfide solid electrolyte of the present embodiment is preferably produced by the production method of the present embodiment.
[0334] The BET specific surface area used in the production method of this embodiment is 10 m 2 The sulfide solid electrolyte containing lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms in an amount of 100 g or more is the same sulfide solid electrolyte as that described as being usable in the modified sulfide solid electrolyte of the present embodiment. Therefore, as the sulfide solid electrolyte, a commercially available product can be used, and a sulfide solid electrolyte produced by the method of the sulfide solid electrolyte can also be used.
[0335] As the organic solvent used in the production method of the present embodiment, for example, the solvents described as the solvents that can be used in the method for producing the above-mentioned sulfide solid electrolyte can be exemplified. From the viewpoint of promoting the mixing of the sulfide solid electrolyte and the heteropolycyclic compound, efficiently obtaining a modified sulfide solid electrolyte containing the sulfide solid electrolyte and the heteropolycyclic compound, and from the viewpoint of promoting the adhesion of the heteropolycyclic compound to the sulfide solid electrolyte, among the above-mentioned solvents, preferably, an aliphatic hydrocarbon solvent, an alicyclic hydrocarbon solvent, an aromatic hydrocarbon solvent, and the ether solvent, ester solvent, and nitrile solvent exemplified as a complexing agent can be exemplified, and an aromatic hydrocarbon solvent is more preferable.
[0336] In the production method of the present embodiment, as the organic solvent, one kind among these can be used alone or in combination of two or more kinds.
[0337] In the production method of the present embodiment, the method of mixing the sulfide solid electrolyte, the heteropolycyclic compound, and the organic solvent can be performed by the same method as the "mixing" in the method of producing the sulfide solid electrolyte described above.
[0338] The organic solvent can be removed by the same method as the “drying” in the method for producing the above-mentioned sulfide solid electrolyte.
[0339] In addition, in the production method of the present embodiment, the “heating” in the method for producing the above-mentioned sulfide solid electrolyte may be performed.
[0340] 〔Electrode composite materials〕
[0341] The electrode composite material of the present embodiment is an electrode composite material including the modified sulfide solid electrolyte of the present embodiment described above and an electrode active material, or an electrode composite material including the modified sulfide solid electrolyte of the other embodiment described above and an electrode active material.
[0342] (Electrode Active Material)
[0343] As the electrode active material, a positive electrode active material or a negative electrode active material is used, depending on whether the electrode composite material is used for a positive electrode or a negative electrode.
[0344] As the positive electrode active material, any positive electrode active material can be used without particular limitation as long as it can promote the battery chemical reaction through the relationship with the negative electrode active material, and the battery chemical reaction is accompanied by the movement of lithium ions caused by the atom adopted as the atom reflecting ionic conductivity, preferably the lithium atom. As the positive electrode active material that can carry out such insertion and extraction of lithium ions, oxide-based positive electrode active materials, sulfide-based positive electrode active materials, etc. can be cited.
[0345] As oxide-based positive electrode active materials, preferred examples include lithium-containing transition metal composite oxides such as LMO (lithium manganese oxide), LCO (lithium cobalt oxide), NMC (lithium nickel manganese cobalt oxide), NCA (lithium nickel cobalt aluminum oxide), LNCO (lithium nickel cobalt oxide), and olivine-type compounds (LiMeNPO4, Me = Fe, Co, Ni, Mn).
[0346] Examples of the sulfide-based positive electrode active material include titanium sulfide (TiS2), molybdenum sulfide (MoS2), iron sulfide (FeS, FeS2), copper sulfide (CuS), and nickel sulfide (Ni3S2).
[0347] In addition to the above-mentioned positive electrode active materials, niobium selenide (NbSe 3 ) or the like can also be used.
[0348] The positive electrode active material can be used alone or in combination of two or more.
[0349] As the negative electrode active material, any negative electrode active material that can promote the battery chemical reaction accompanied by the movement of lithium ions caused by atoms used as atoms that embody ionic conductivity, preferably metals that can form alloys with lithium atoms, their oxides, alloys of the metals and lithium atoms, etc., preferably lithium atoms, can be used without particular limitation. As such a negative electrode active material that can allow lithium ions to be inserted and removed, a substance that is known as a negative electrode active material in the battery field can be used without limitation.
[0350] Examples of such negative electrode active materials include metallic lithium such as metallic lithium, metallic indium, metallic aluminum, metallic silicon, and metallic tin, or metals capable of forming alloys with metallic lithium, oxides of these metals, and alloys of these metals with metallic lithium.
[0351] The electrode active material used in the present embodiment may have a coating layer coated on its surface.
[0352] As a material for forming the coating layer, an atom that exhibits ionic conductivity in the sulfide solid electrolyte, preferably a nitride, an oxide, or an ion conductor such as a composite of lithium atoms, can be cited. Specifically, lithium nitride (Li3N), a Li4GeO4-based structure such as Li 4-2x Zn x Conductors with LISICON crystal structures such as GeO4, and conductors with Li3PO4 skeleton structures such as Li 4-x Ge 1-x P x Conductors with sulfide-LISICON crystal structures such as S4, La 2 / 3- x Li 3x Conductors with a perovskite crystal structure such as TiO3, conductors with a NASICON crystal structure such as LiTi2(PO4)3, etc.
[0353] In addition, Li y Ti 3-y O4(0 <y<3)、Li4Ti5O 12 Lithium titanate (LTO), lithium metal oxides of metals belonging to Group 5 of the periodic table such as LiNbO3, LiTaO3, and oxide-based conductors such as Li2O-B2O3-P2O5, Li2O-B2O3-ZnO, and Li2O-Al2O3-SiO2-P2O5-TiO2.
[0354] The electrode active material having a coating layer is obtained by, for example, attaching a solution containing various atoms constituting a material forming the coating layer to the surface of the electrode active material and calcining the attached electrode active material preferably at 200° C. to 400° C.
[0355] Here, as the solution containing various atoms, for example, a solution containing alkoxides of various metals such as lithium ethoxide, titanium isopropoxide, niobium isopropoxide, tantalum isopropoxide, etc. can be used. At this time, as the solvent, an alcohol solvent such as ethanol and butanol; an aliphatic hydrocarbon solvent such as hexane, heptane, octane; an aromatic hydrocarbon solvent such as benzene, toluene, xylene, etc. can be used.
[0356] In addition, the above-mentioned attachment may be performed by dipping, spraying, or the like.
[0357] From the viewpoint of improving manufacturing efficiency and battery performance, the firing temperature is preferably 200° C. to 400° C., more preferably 250° C. to 390° C., and the firing time is usually about 1 minute to 10 hours, preferably 10 minutes to 4 hours.
[0358] As the coating rate of the coating layer, based on the surface area of the electrode active material, it is preferably more than 90%, more preferably more than 95%, and further preferably 100%, that is, preferably the entire surface is coated. In addition, as the thickness of the coating layer, it is preferably more than 1nm, more preferably more than 2nm, and as the upper limit, it is preferably below 30nm, more preferably below 25nm.
[0359] The thickness of the coating layer can be measured by cross-sectional observation using a transmission electron microscope (TEM), and the coverage can be calculated from the thickness of the coating layer, elemental analysis values, and BET specific surface area.
[0360] (Other ingredients)
[0361] The electrode composite material of this embodiment may include other components such as a conductive material and a binder in addition to the modified sulfide solid electrolyte and the electrode active material. That is, the method for manufacturing the electrode composite material of this embodiment may use other components such as a conductive material and a binder in addition to the modified sulfide solid electrolyte and the electrode active material. Other components such as a conductive material and a binder may be further added to the modified sulfide solid electrolyte and the electrode active material in the mixing of the modified sulfide solid electrolyte and the electrode active material and mixed for use.
[0362] As conductive materials, from the viewpoint of improving battery performance by improving electron conductivity, examples include artificial graphite, graphite carbon fiber, resin-fired carbon, pyrolysis vapor-grown carbon, coke, mesophase carbon microbeads, furfuryl alcohol resin-fired carbon, polyphenylene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, and carbon materials that are difficult to graphitize.
[0363] By using a binder, the strength of the positive electrode and the negative electrode can be improved.
[0364] There are no particular restrictions on the binder as long as it can impart functions such as adhesion and flexibility. Examples include fluorine-based polymers such as polytetrafluoroethylene and polyvinylidene fluoride, thermoplastic elastomers such as butene rubber and styrene-butadiene rubber, acrylic resins, acrylic polyol resins, polyvinyl acetal resins, polyvinyl butyral resins, silicone resins and other resins.
[0365] The blending ratio (mass ratio) of the electrode active material and the modified sulfide solid electrolyte in the electrode composite material is preferably 99.5:0.5 to 40:60, more preferably 99:1 to 50:50, and even more preferably 98:2 to 60:40 in consideration of improvement in battery performance and manufacturing efficiency.
[0366] When containing a conductive material, the content of the conductive material in the electrode composite material is not particularly limited. If the battery performance is improved and the manufacturing efficiency is taken into consideration, it is preferably 0.5 mass % or more, more preferably 1 mass % or more, and further preferably 1.5 mass % or more. As an upper limit, it is preferably 10 mass % or less, preferably 8 mass % or less, and further preferably 5 mass % or less.
[0367] In addition, when containing a binder, the content of the binder in the electrode composite material is not particularly limited. If the battery performance is improved and the manufacturing efficiency is taken into consideration, it is preferably 1% by mass or more, more preferably 3% by mass or more, and further preferably 5% by mass or more. As an upper limit, it is preferably 20% by mass or less, preferably 15% by mass or less, and further preferably 10% by mass or less.
[0368] 〔Lithium-ion battery〕
[0369] The lithium ion battery of the present embodiment includes at least one selected from the modified sulfide solid electrolyte and the electrode composite material of the present embodiment described above, or includes at least one selected from the modified sulfide solid electrolyte and the electrode composite material of the other embodiment described above.
[0370] The lithium ion battery of the present embodiment is not particularly limited in its structure as long as it includes the modified sulfide solid electrolyte of the present embodiment described above, an electrode composite material containing the modified sulfide solid electrolyte, or any one of the modified sulfide solid electrolyte of another embodiment and an electrode composite material containing the modified sulfide solid electrolyte of another embodiment, and has the structure of a general lithium ion battery.
[0371] As the lithium ion battery of the present embodiment, for example, a lithium ion battery having a positive electrode layer, a negative electrode layer, an electrolyte layer and a current collector is preferred. As the positive electrode layer and the negative electrode layer, the positive electrode layer and the negative electrode layer of the electrode composite material of the present embodiment are preferably used, and as the electrolyte layer, the modified sulfide solid electrolyte of the present embodiment or the modified sulfide solid electrolyte of another embodiment is preferably used.
[0372] As the current collector, any known current collector may be used. For example, a layer obtained by coating a substance that reacts with the above-mentioned solid electrolyte, such as Au, Pt, Al, Ti, or Cu, with Au or the like can be used.
[0373] Example
[0374] Next, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples at all.
[0375] Production Example: Preparation of Sulfide Solid Electrolyte
[0376] In a Schlenk bottle (capacity: 100 mL) with a stirrer, 0.59 g of lithium sulfide, 0.95 g of phosphorus pentasulfide, 0.19 g of lithium bromide, and 0.28 g of lithium iodide were introduced under a nitrogen atmosphere. After the stirrer was rotated, 20 mL of tetramethylethylenediamine (TMEDA) as a complexing agent was added, and stirring was continued for 12 hours. The obtained complex-containing material was dried under vacuum (room temperature: 23° C.) to obtain a powdered complex. Next, the powder of the complex was heated at 120° C. for 2 hours under vacuum to obtain an amorphous sulfide solid electrolyte. Furthermore, the amorphous sulfide solid electrolyte was heated at 140° C. for 2 hours under vacuum to obtain a crystalline sulfide solid electrolyte 1 (the heating temperature (140° C. in this example) used to obtain a crystalline sulfide solid electrolyte is sometimes referred to as the "crystallization temperature").
[0377] The BET specific surface areas of the amorphous sulfide solid electrolyte and the crystalline sulfide solid electrolyte were measured to be 40 m 2 / g.
[0378] Example 1
[0379] Under a nitrogen atmosphere, 3 g of the crystalline sulfide solid electrolyte obtained in the above manufacturing example was weighed and added to a Schlenk bottle (capacity: 100 mL) with a stirrer, and 22 g of toluene was added and stirred to prepare a slurry-like fluid. To the slurry-like fluid, 0.30 g (10 parts by mass relative to 100 parts by mass of the crystalline sulfide solid electrolyte) of ethylene glycol diglycidyl ether as a polyfunctional epoxy compound (polyfunctional epoxy compound 1, in the above general formula (1), X 1 is a single bond, n1 is 2), and after stirring for 10 minutes, toluene is removed by vacuum drying and distillation to obtain a modified sulfide solid electrolyte.
[0380] The oil absorption and ion conductivity of the modified sulfide solid electrolyte obtained were measured based on the following method. The reduction rate of the oil absorption was calculated based on the following method. The measurement results and calculation results are shown in Table 1. In addition, the results of FT-IR analysis (ATR method) based on the following method confirmed that in the infrared absorption spectrum at 2800 to 3000 cm -1 In addition, the following method was used to 1 As a result of H-NMR measurement, a peak at 0.0 to 5.0 ppm derived from an alkyl chain was also confirmed.
[0381] Embodiments 2 to 29
[0382] A modified sulfide solid electrolyte was prepared in the same manner as in Example 1, except that the type of the polyfunctional epoxy compound was changed to the type shown in Table 1.
[0383] The oil absorption and ion conductivity of the modified sulfide solid electrolyte obtained were measured based on the following method. The reduction rate of the oil absorption was calculated based on the following method. The measurement results and calculation results are shown in Table 1. In addition, the results of FT-IR analysis (ATR method) based on the following method confirmed that in the infrared absorption spectrum at 2800 to 3000 cm -1 In addition, the following method was used to 1 As a result of H-NMR measurement, a peak at 0.0 to 5.0 ppm derived from an alkyl chain was also confirmed.
[0384] Comparative Example 1
[0385] The oil absorption and ion conductivity of the sulfide solid electrolyte obtained in the above production example were measured by the following method. The reduction rate of the oil absorption was calculated by the following method. The measurement results and calculation results are shown in Table 1. The oil absorption of the sulfide solid electrolyte was 1.03 mL / g.
[0386] In addition, as a result of FT-IR analysis (ATR method) based on the following method, no infrared absorption spectrum was found between 2800 and 3000 cm -1 In addition, the following method was used to 1 As a result of H-NMR measurement, no peak at 0.0 to 5.0 ppm derived from the alkyl chain could be confirmed.
[0387] (Measurement of specific surface area)
[0388] The specific surface area was measured by the BET method based on krypton (Kr) adsorption using a gas adsorption amount measuring device.
[0389] (Measurement of oil absorption)
[0390] 1 g of the solid electrolyte obtained in the examples and comparative examples was used as a sample. One drop of butyl butyrate was added using a dropper in an agate mortar and then stirred with a spatula. This operation was repeated until the sample became a paste. The total amount of butyl butyrate added was defined as the oil absorption (mL / g).
[0391] (Reduction rate of oil absorption)
[0392] The oil absorption of the sulfide solid electrolyte obtained in the manufacturing example was measured in the same manner as in the above (Measurement of Oil Absorption). The oil absorption A of the sulfide solid electrolyte and the oil absorption B of the sulfide solid electrolyte obtained in the examples and comparative examples based on the above (Measurement of Oil Absorption) were used to calculate by the following formula, and the calculated value was taken as the reduction rate of the oil absorption.
[0393] Oil absorption reduction rate = (oil absorption A - oil absorption B) / oil absorption A × 100 (%)
[0394] (Measurement of ionic conductivity)
[0395] In this example, the measurement of ion conductivity was performed as follows.
[0396] The sulfide solid electrolyte is formed into a 10 mm diameter (cross-sectional area S: 0.785 cm 2 ), round particles with a height (L) of 0.1 to 0.3 cm are used to make a sample. The top and bottom of the sample are taken as electrode terminals, and the AC impedance method is used for measurement at 25°C (frequency range: 1 MHz to 100 Hz, amplitude: 10 mV) to obtain a Cole-Cole plot. Near the right end of the arc observed in the high-frequency side area, the real part Z'(Ω) at the point where -Z"(Ω) is the smallest is taken as the bulk resistance R(Ω) of the electrolyte, and the ionic conductivity σ(S / cm) is calculated according to the following formula.
[0397] R=ρ(L / S)
[0398] σ=1 / ρ
[0399] (FT-IR analysis (ATR method))
[0400] Measuring device: FR-IR spectrometer "VERTEX 70v (model)", manufactured by BRUKER
[0401] Measurement method: Total reflection measurement method (ATR method)
[0402] Measurement wave number range: 650~4000cm -1
[0403] Light source: Silicon carbide lamp (SiC)
[0404] Detector: DTGS detector
[0405] Resolution: 4cm -1
[0406] Measuring time: 1 second / time
[0407] Total times: 256 times
[0408] Measurement conditions: Diamond prism at an incident angle of 45°
[0409] ( 1 H-NMR measurement)
[0410] Nuclear magnetic resonance apparatus (NMR apparatus): AVANCE III HD (manufactured by BRUKER)
[0411] Observation core: 1 H
[0412] Resonance frequency: 500MHz
[0413] Probe: 5mmφTCI CryoProbe
[0414] Measurement temperature: 25℃
[0415] Total times: 16 times
[0416] [Table 1]
[0417]
[0418] The details of the polyfunctional epoxy compounds shown in Table 1 are as follows.
[0419] Heteropolycyclic compound 1: ethylene glycol diglycidyl ether. In the above general formula (1), X 1 is a single bond, and n1 is 2. The structural formula is as follows.
[0420]
Chemistry 4
[0421]
[0422] Heteropolycyclic compound 2: 1,4-butanediol diglycidyl ether. In the above general formula (1), X 1 is ethylene, and n1 is 2. The structural formula is as follows.
[0423]
Chemistry 5
[0424] Table 1
[0425]
[0426] Heteropolycyclic compound 3: 1,6-hexanediol diglycidyl ether. In the above general formula (1), X 1 is butylene, and n1 is 2. The structural formula is as follows.
[0427]
Chemistry 6
[0428]
[0429] Heteropolycyclic compound 4: neopentyl glycol diglycidyl ether. In the above general formula (1), X 1 Neopentylene (X 1 The basic structure is neopentane), n1 is 2. The structural formula is as follows.
[0430]
Chemistry 7
[0431]
[0432] Heteropolycyclic compound 5: diethylene glycol diglycidyl ether. In the above general formula (1), X 1 A group formed by two ethylene groups bonded via -O- (X 1 The basic structure is diethylene glycol), l1 is 2. The structural formula is as follows.
[0433]
Chemistry 8
[0434]
[0435] Heteropolycyclic compound 6: 1,4-cyclohexanedimethanol diglycidyl ether. In the above general formula (1), X 1 1,4-dimethylcyclohexylene (X 1 The basic structure is 1,4-dimethylcyclohexane), n1 is 2. The structural formula is as follows.
[0436]
Chemistry 9
[0437]
[0438] Heteropolycyclic compound 7: diglycidylresorcinol ether, in the above general formula (1), X 1 is 1,3-phenylene (X 1 The basic structure is benzene), n1 is 2. The structural formula is as follows.
[0439]
Chemistry 10
[0440]
[0441] Heteropolycyclic compound 8: 1,4-diglycidyloxybenzene, in the above general formula (1), X 1 1,4-phenylene (X 1 The basic structure is benzene), n1 is 2. The structural formula is as follows.
[0442]
Chemistry 11
[0443]
[0444] Heteropolycyclic compound 9: bisphenol A diglycidyl ether. In the above general formula (1), X 1 It is a group obtained by removing a hydrogen atom from the hydroxyl group of bisphenol A which is a basic structure, and m1 is 2.
[0445] The structural formula is as follows.
[0446]
Chemistry 12
[0447]
[0448] Heteropolycyclic compound 10: 9,9-bis(4-glycidyloxyphenyl)fluorene. In the above general formula (1), X 1 It is a group obtained by removing a hydrogen atom from 9,9-bis(4-hydroxyphenyl)fluorene as a basic structure, and m1 is 2. The structural formula is as follows.
[0449]
Chemistry 13
[0450]
[0451] Heteropolycyclic compound 11: Bisphenol A propoxylated diglycidyl ether. In the above general formula (1), X 1 It is a group obtained by removing a hydrogen atom from a propyl group of a compound (2,2-bis(4-propoxyphenyl)propane) in which a hydrogen atom of a hydroxyl group of bisphenol A, which is a basic structure, is replaced by a propyl group, and n1 is 2. The structural formula is as follows.
[0452]
Chemistry 14
[0453]
[0454] Heteropolycyclic compound 12: 1,3-bis(3-glycidyloxypropyl)tetramethyldisiloxane. In the above general formula (1), X 1 It is a group obtained by removing a hydrogen atom from the propyl group of 1,3-dipropyl-1,1,3,3-tetramethyldisiloxane which is a basic structure, and n1 is 2. The structural formula is as follows.
[0455]
Chemistry 15
[0456]
[0457] Heteropolycyclic compound 13: trimethylolpropane triglycidyl ether. In the above general formula (1), X 1 It is a group obtained by removing a hydrogen atom from 2,2-dimethylbutane as a basic structure, and n1 is 3. The structural formula is as follows.
[0458]
Chemistry 16
[0459]
[0460] Heteropolycyclic compound 14: tris(4-hydroxyphenyl)methane triglycidyl ether. In the above general formula (1), X 1 It is a group obtained by removing a hydrogen atom from the hydroxyl group of methylene triphenol as the basic structure, and m1 is 3. The structural formula is as follows:
[0461]
Chemistry 17
[0462]
[0463] · Heteropolycyclic compound 15: 2,4,6,8 - tetramethyl - 2,4,6,8 - tetra(propyl glycidyl ether) cyclotetrasiloxane. In the above general formula (1), X 1 is a group obtained by removing a hydrogen atom from the propyl group of 2,4,6,8 - tetramethyl - 2,4,6,8 - tetrapropyl cyclotetrasiloxane as the basic structure, and n1 is 4. The structural formula is as follows.
[0464]
Chemical formula 18
[0465]
[0466] · Heteropolycyclic compound 16: 1,3 - butadiene diepoxide. In the above general formula (1), X 1 is a single bond, and l1 is 2. The structural formula is as follows.
[0467]
Chemical formula 19
[0468]
[0469] · Heteropolycyclic compound 17: 1,5 - hexadiene diepoxide. In the above general formula (1), X 1 is an ethylene group, and m1 is 2. The structural formula is as follows.
[0470]
Chemical formula 20
[0471]
[0472] · Heteropolycyclic compound 18: 1,7 - octadiene diepoxide. In the above general formula (1), X 1 is a butylene group, and m1 is 2. The structural formula is as follows.
[0473]
Chemical formula 21
[0474]
[0475] · Heteropolycyclic compound 19: 2,2'-(2,2,3,3,4,4,5,5 - octafluorohexane - 1,6 - diyl) bis(oxirane). In the above general formula (1), X 1 is 2,2,3,3,4,4,5,5 - octafluorohexane - 1,6 - diyl (the basic structure of X 1 is 2,2,3,3,4,4,5,5 - octafluorohexane), and l1 is 2. The structural formula is as follows.
[0476]
Chemical formula 22
[0477]
[0478] Heteropolycyclic compound 20: 1,3-bis[2-(7-oxabicyclo[4.1.0]heptane-3-yl)ethyl]-1,1,3,3-tetramethyldisiloxane. In the above general formula (1), X 1 The basic structure is 1,3-ethylhexyl-1,1,3,3-tetramethyldisiloxane, where l1 is 2 and the epoxy group is condensed with cyclohexane to exist as cyclohexene oxide. The structural formula is as follows.
[0479]
Chemistry 23
[0480]
[0481] Heteropolycyclic compound 21: N,N-diglycidyl-4-glycidyloxyaniline. In the above general formula (1), X 1 The basic structure is 4-hydroxyaniline, and m1 is 3. The structural formula is as follows.
[0482]
Chemistry 24
[0483]
[0484] Heteropolycyclic compound 22: 4,4'-methylenebis(N,N-diglycidylaniline), in the above general formula (1), X 1 The basic structure is 4,4'-methylenebis(N,N-dimethylaniline), and m1 is 4. The structural formula is as follows.
[0485]
Chemistry 25
[0486]
[0487] Heteropolycyclic compound 23: polypropylene glycol diglycidyl ether (number average molecular weight: 380). In the above general formula (1), X 1 -R is formed by multiple aliphatic groups (propylene groups) bonded via -O- 1 O-(R 1 is a group of repeating units represented by a propylene group), m1 is 1, and n1 is 1. The structural formula is as follows (in the structural formula, n is the average repeating number).
[0488]
Chemistry 26
[0489]
[0490] Heteropolycyclic compound 24: polyethylene glycol diglycidyl ether (number average molecular weight: 500). In the above general formula (1), X 1 -R is a group formed by multiple aliphatic groups (ethylene groups) bonded via -O- 1 O-(R 1A group of repeating units represented by (ethylene group), m1 is 1, and n1 is 1. The structural formula is as follows (in the structural formula, n is the average number of repetitions).
[0491]
Chemical Formula 27
[0492]
[0493] · Heteropolycyclic compound 25: Polyethylene glycol diglycidyl ether (number average molecular weight: 2000), in the above general formula (1), X 1 is -R formed by bonding multiple aliphatic groups (ethylene groups) via -O- 1 O-(R 1 is a group of repeating units represented by (ethylene group), m1 is 1, and n1 is 1. The structural formula is as follows (in the structural formula, n is the average number of repetitions).
[0494]
Chemical Formula 28
[0495]
[0496] · Heteropolycyclic compound 26: Polyethylene glycol diglycidyl ether (number average molecular weight: 6000), in the above general formula (1), X 1 is -R formed by bonding multiple aliphatic groups (ethylene groups) via -O- 1 O-(R 1 is a group of repeating units represented by (ethylene group), m1 is 1, and n1 is 1. The structural formula is as follows (in the structural formula, n is the average number of repetitions).
[0497]
Chemical Formula 29
[0498]
[0499] · Heteropolycyclic compound 27: Pentaerythritol glycidyl ether, in the above general formula (1), X 1 has a basic structure of pentaerythritol, m1 is 4 (it can also be said that X 1 is a group obtained by removing 4 hydrogen atoms from 2,2 - dimethylbutane as the basic structure, and n1 is 4). The structural formula is as follows.
[0500]
Chemical Formula 30
[0501]
[0502] · Heteropolycyclic compound 28: 1,4 - bis(2 - tetrahydrofuranyloxy)butane), in the above general formula (2), X 2 is 1,4 - butanediyl dioxy, and R in the heterocycle 2a is butylene group, l2 is 2 (it can also be said that X 2The group is obtained by removing two hydrogen atoms from 1,4-butanediol as the basic structure. 2a is butylene, l2 is 2). The structural formula is as follows.
[0503]
Chemistry 31
[0504]
[0505] Heteropolycyclic compound 29: PSS-octa[(3-glycidyloxypropyl)dimethylsilyloxy] substituted, in the above general formula (1), X 1 A group obtained by removing a hydrogen atom (a total of 8 hydrogen atoms) from a propyl group in a compound (PSS-octa[propyldimethylsiloxy] substitution) in which one propyldimethylsiloxy group is bonded to each of the 8 silicon atoms in a PSS-octamethyl substitution form as a basic structure (a total of 8 groups), n 1 The structural formula is as follows.
[0506]
Chemistry 32
[0507]
[0508] According to the examples, it was confirmed that the oil absorption of the modified sulfide solid electrolyte of the present embodiment was 0.9 mL / g or less and the reduction rate of the oil absorption was 13% or more. Therefore, even if the specific surface area was large and 10 m 2 / g or more, but it is a modified sulfide solid electrolyte with low oil absorption and excellent coating adaptability. In addition, it is also confirmed that the ion conductivity is 0.5mS / cm or more.
[0509] On the other hand, the sulfide solid electrolyte of Comparative Example 1 which was not mixed with the polyfunctional epoxy compound and did not contain the polyfunctional epoxy compound was the sulfide solid electrolyte prepared in the manufacturing example, that is, a conventional sulfide solid electrolyte. It was confirmed that the specific surface area of Comparative Example 1 was 40 m 2 The sulfide solid electrolyte with a specific surface area of 10 m / g or more has a high oil absorption of 1.03 mL / g, which is a sulfide solid electrolyte with poor coating suitability. 2 A sulfide solid electrolyte with a carbonyl content of 0.1 / g or more is preferred because it can exhibit effects of reducing oil absorption and improving coating suitability.
[0510] Embodiment 30
[0511] In order to confirm whether the polyfunctional epoxy compound adheres to the modified sulfide solid electrolyte obtained in the above examples, the following verification was performed.
[0512] First, for the modified sulfide solid electrolyte of the multifunctional epoxy compound 9 (bisphenol A diglycidyl ether) of Example 9 obtained with a content of 9.1% by mass (the amount of the multifunctional epoxy compound 9 used is 10 parts by mass relative to 100 parts by mass of the sulfide solid electrolyte), toluene was added to make it into a slurry (slurry concentration: 12% by mass), and then it was left to stand for 24 hours. The supernatant produced by the precipitation of the sulfide solid electrolyte was collected and analyzed by gas chromatography mass spectrometry (GC / MS method). For the quantitative analysis in this analysis, the feed liquid (1.1% by mass toluene solution of the multifunctional epoxy compound 9) was also analyzed in the same way as the above supernatant, and the peak area of the multifunctional epoxy compound 9 in the feed liquid was set to 1, and compared with the peak area of the multifunctional epoxy compound 9 remaining in the above supernatant (the closer the peak area of the supernatant is to 1, the more the multifunctional epoxy compound is freed from the sulfide solid electrolyte and dissolved in toluene). According to this analysis, since the polyfunctional epoxy compound was not detected in the supernatant, it is considered that all the polyfunctional epoxy compounds were attached to the sulfide solid electrolyte.
[0513] (Gas chromatography mass spectrometry conditions)
[0514] Gas chromatograph: 6890B (manufactured by Agilent)
[0515] Analysis column: HP-5ms (manufactured by Agilent)
[0516] GC oven heating conditions: initial temperature 50°C
[0517] 50℃~300℃, heating at 10℃ / min
[0518] Keep at 300℃ for 5 minutes
[0519] Sample injection volume: 1μL
[0520] Furthermore, the precipitated sulfide solid electrolyte was washed by adding toluene and stirring, then standing for 12 hours and removing the supernatant. This process was repeated three times to wash the precipitated sulfide solid electrolyte. After washing, the sulfide solid electrolyte obtained by drying the toluene was dissolved in deuterated methanol and subjected to the above method. 1 As a result of H-NMR measurement, chemical shifts of groups (alkyl groups, etc.) derived from the polyfunctional epoxy compound were detected.
[0521] (CV measurement (oxidation current))
[0522] In order to evaluate the oxidation current, the following single cell for CV measurement was used.
[0523] A total of 100 mg of the sulfide solid electrolytes obtained in Examples and Comparative Examples and DENKA BLACK granules (particle size: 35 nm, manufactured by DENKA Corporation) (sulfide solid electrolyte:DENKA BLACK (mass ratio) = 85:15) were mixed in a mortar for 10 minutes to obtain a powder for measurement (1).
[0524] 100 mg of electrolyte for the separator layer was added to a battery cell with a diameter of 10 mm and the pressure was 10 MPa / cm2 using a SUS mold. 2 After pressing three times with each rotation of 120°, 10 mg of the measuring powder (1) was added and the pressure was adjusted to 20 MPa / cm 2 The pressing was repeated three times with each rotation of 120°. 2 Punch 3 times with each rotation of 120°.
[0525] The above-mentioned electrolyte for the separator layer was synthesized under the following conditions.
[0526] In a 1L reaction vessel with a stirring blade, 20.5g of Li2S, 33.1g of P2S5, 10.0g of LiI, and 6.5g of LiBr were added under a nitrogen atmosphere. After the stirring blade was rotated, 630g of toluene was introduced and the slurry was stirred for 10 minutes. A bead mill capable of circulating operation ("STAR MILL LMZ015 (trade name)", manufactured by Ashizawa Finetech Co., Ltd., bead material: zirconium oxide, bead diameter: 0.5mmφ, bead usage: 456g) was connected to the reaction vessel and subjected to a 45-hour pulverization treatment (pump flow rate: 650mL / min, bead mill peripheral speed: 12m / s, mill jacket temperature: 45°C).
[0527] The obtained slurry was dried at room temperature (25°C) under vacuum and then heated (80°C) to obtain a white powder of an amorphous solid electrolyte. Furthermore, the obtained white powder was heated at 195°C for 2 hours under vacuum to obtain a white powder of a crystalline solid electrolyte. In the XRD spectrum of the crystalline solid electrolyte, crystallization peaks were detected at 2θ=20.2° and 23.6°, confirming that it had a type II crystal structure in the sulfide crystalline lithium superion conductor region. In addition, the average particle size (D 50 ) is 4.5μm and the ionic conductivity is 5.0mS / cm.
[0528] On the opposite side of the measuring powder (1) of the electrolyte for the separator layer, an InLi foil (layer structure, " / " indicates the interval between layers. In: 10 mmφ×0.1 mm / Li: 9 mmφ×0.08 mm / SUS: 10 mmφ×0.1 mm) was formed and heated to 6 MPa / cm 2 Punching was performed once. The single cell was fixed by four bolts sandwiching an insulator so that there was no short circuit between the powder for measurement (1) and the InLi foil, and the bolts were fixed with a tightening torque of 8 N·m, thereby obtaining a single cell for measurement.
[0529] The obtained single cell for measurement was connected to a measuring instrument ("VMP-300 (model)", manufactured by Biologic), and a CV curve was obtained under the following conditions.
[0530] Measurement temperature: 25℃
[0531] Scan speed: 0.1mV / s
[0532] Potential measurement range: open circuit voltage (+2.1V) → +5.0V → +2.1V
[0533] Number of cycles: 2 times
[0534] The modified sulfide solid electrolyte of Example 2 and the sulfide solid electrolyte of Comparative Example 1 were subjected to CV measurement based on the above method. The CV curve of the first cycle is shown in Figure 1 .according to Figure 1 The CV curves of Example 2 confirm that the oxidation current of the modified sulfide solid electrolyte is lower than that of Comparative Example 1. In addition, for Examples 9, 11, and 13, the oxidation current is also lowered relative to that of Comparative Example 1 ( Figure 1 ). Although not shown in the figure, it was confirmed that the oxidation current of Examples 1 to 29 was lower than that of Comparative Example 1. As described above, it is known that the oxidation reaction occurring at the interface between the electrolyte and the conductive material can be suppressed by coating with the epoxy compound.
[0535] Industrial Applicability
[0536] The modified sulfide solid electrolyte of the present embodiment has excellent coating adaptability when applied as a paste even if it is a sulfide solid electrolyte with a large specific surface area, and can effectively demonstrate excellent battery performance. In addition, the modified sulfide solid electrolyte of the present embodiment has high ion conductivity and is therefore suitable for use in batteries, particularly batteries used in information-related devices or communication devices such as personal computers, video cameras, and mobile phones.
Claims
1. A modified sulfide solid electrolyte, characterized in that: Contains: Sulfide solid electrolyte with a BET surface area of 10m 2 / g or more and containing a lithium atom, a sulfur atom, a phosphorus atom and a halogen atom; and having two or more heterocyclic rings having carbon atoms and oxygen atoms.
2. The modified sulfide solid electrolyte according to claim 1, characterized in that The compound having two or more heterocyclic rings having carbon atoms and oxygen atoms is a compound containing two or more groups having oxirane rings.
3. The modified sulfide solid electrolyte according to claim 1 or 2, characterized in that The compound having two or more heterocyclic rings having carbon atoms and oxygen atoms is an epoxy compound represented by the following general formula (1), wherein the epoxy compound has at least two groups selected from epoxy groups, glycidyl groups and glycidyl ether groups. [Chemistry 1] In the general formula (1), X 1 is a single bond or an aliphatic group, an alicyclic group, an aromatic group, an organic group having a siloxane structure, or an organic group consisting of a combination of these, l1, m1, and n1 are each an integer from 0 to 16, satisfying l1+m1+n1≥2, and in addition, in the case of X 1 When the organic group has the alicyclic group, the epoxy group may be a group condensed with the alicyclic ring in the alicyclic group.
4. The modified sulfide solid electrolyte according to claim 3, characterized in that As X in the general formula (1) 1 The group composed of these combinations is a group formed by at least two groups selected from the aliphatic group, the alicyclic group, the aromatic group and the organic group having a siloxane structure bonded via a single bond or a bonding group selected from -O-, -SO2-, -CO-, -C(=O)O-, -N- and -S-.
5. The modified sulfide solid electrolyte according to any one of claims 1 to 4, characterized in that In the infrared absorption spectrum based on FT-IR analysis, namely ATR method, the -1 Has a peak.
6. The modified sulfide solid electrolyte according to claim 5, characterized in that The peak is a peak derived from CH stretching vibration of an alkyl chain in the epoxy compound.
7. The modified sulfide solid electrolyte according to claim 6, characterized in that exist 1 In the H-NMR spectrum, there is a peak at 0.0 to 5.0 ppm derived from the alkyl chain.
8. The modified sulfide solid electrolyte according to any one of claims 1 to 7, characterized in that The content of the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms is 0.03 parts by mass or more and 25 parts by mass or less based on 100 parts by mass of the sulfide solid electrolyte.
9. The modified sulfide solid electrolyte according to any one of claims 1 to 8, characterized in that The number average molecular weight of the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms is 10,000 or less.
10. The modified sulfide solid electrolyte according to any one of claims 1 to 9, characterized in that Among the compounds having two or more heterocyclic rings having carbon atoms and oxygen atoms, the content of the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms and having a number average molecular weight of 10,000 or less is 90% by mass or more.
11. The modified sulfide solid electrolyte according to any one of claims 1 to 10, characterized in that The content of the compound having two or more heterocyclic rings having carbon atoms and oxygen atoms and having a number average molecular weight exceeding 10,000 among the compounds having two or more heterocyclic rings having carbon atoms and oxygen atoms is 10% by mass or less.
12. A method for producing a modified sulfide solid electrolyte, characterized in that: include: A sulfide solid electrolyte, a compound having two or more heterocyclic rings having carbon atoms and oxygen atoms, and an organic solvent are mixed, wherein the sulfide solid electrolyte has a BET specific surface area of 10 m 2 / g or more and contains lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms; The organic solvent is removed.
13. The method for producing a modified sulfide solid electrolyte according to claim 12, wherein: The organic solvent is at least one solvent selected from aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, aromatic hydrocarbon solvents, ether solvents, ester solvents, and nitrile solvents.
14. An electrode composite material, characterized in that: A modified sulfide solid electrolyte comprising the modified sulfide solid electrolyte according to any one of claims 1 to 11 and an electrode active material.
15. A lithium ion battery, characterized in that: A modified sulfide solid electrolyte according to any one of claims 1 to 11 and an electrode composite material according to claim 14 are included.
Citation Information
Patent Citations
Solid sulfide electrolyte material, solid-state lithium battery, and method for manufacturing solid sulfide electrolyte material
JP2013016423A
Solid electrolyte composition, sheet for all-solid type secondary battery, all-solid type secondary battery, and methods for manufacturing sheet for all-solid type secondary battery and all-solid type secondary battery
JP2017147173A
Method for producing composite solid electrolyte
JP2020087633A
Sulfide solid electrolyte
WO2020203231A1
Method for producing solid electrolyte
WO2021029315A1