Metal silicide contact formation

By depositing and annealing the tungsten or molybdenum metal layers in 3D-DRAM structures, the problem of metal layer uniformity and annealing in complex geometries is solved, and the formation of a uniform metal silicide layer is achieved, reducing contact resistance and improving equipment reliability is improved and productivity.

CN119096326APending Publication Date: 2024-12-06LAM RES CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036990.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In 3D-DRAM structures, forming a uniform and selective metal layer is difficult, especially in complex geometric shapes and high aspect ratio structures, it is difficult for the prior art to anneale metal silicide contacts without destroying vacuum environments. Causes uneven contact resistance and equipment failure.

Method used

By depositing a tungsten or molybdenum metal layer on the surface of the crystalline silicon and performing in-situ annealing without covering the layer, the metal silicide layer is formed using a high flow rate ratio of metal halide precursor and reducing agent flow rate ratio, and the reaction rate is controlled to Reduce the formation of wormholes and defects.

Benefits of technology

The uniform and selective formation of the metal silicide layer in the 3D-DRAM structure is achieved, which reduces contact resistance, improves equipment reliability and production efficiency, and avoids multiple process steps and cost increase.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096326A_ABST
    Figure CN119096326A_ABST
Patent Text Reader

Abstract

A process for forming a metal silicide contact is provided that includes providing a substrate having a bottom crystalline silicon and a dielectric sidewall. A metal layer may then be selectively formed on the bottom crystalline silicon by metal layer deposition using a metal halide precursor and a reducing agent. The ratio of reductant flow rate to metal halide precursor flow rate is at least 10: 1 or 10: 1 to 10,000: 1. After depositing the metal layer, the substrate is annealed to convert the metal layer into a metal silicide layer without contaminating the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Incorporation by Reference

[0001] The PCT application form is filed concurrently with this specification as a part of this application. Each application identified in the concurrently filed PCT application form to which this application claims the benefit or priority is incorporated herein by reference in its entirety and for all purposes. Background Art

[0002] Metal silicides can be formed during the fabrication of a variety of semiconductor devices. For example, dynamic random access memory (DRAM) can include metal silicide contacts on crystalline silicon. Forming silicides for complex structures such as 3D-DRAM structures can be challenging.

[0003] The background description provided here is for the purpose of generally presenting the background of the present disclosure. The work of the currently designated inventors within the scope described in this background section and aspects of the specification that were not determined to be prior art at the time of filing the application are neither explicitly nor implicitly admitted to be prior art against the present disclosure. Summary of the invention

[0004] Provided herein is a method for forming a metal silicide contact in a feature comprising a bottom crystalline silicon surface and an oxide or nitride sidewall surface. The method may involve depositing tungsten (W) or molybdenum (Mo) on the bottom crystalline silicon without depositing W or Mo on the sidewall surface. Subsequently, the W or Mo film may be annealed to form a tungsten silicide (WSi x ) or molybdenum silicide (MoSi x ). Annealing can be performed in situ without breaking vacuum. In some embodiments, annealing is performed without a capping layer.

[0005] One aspect of the present disclosure relates to a method comprising providing a feature having a feature bottom and a feature sidewall. The feature bottom comprises a crystalline silicon surface and the feature sidewall comprises an oxide or nitride surface. The method further comprises exposing the feature to a metal halide precursor flow comprising a metal halide precursor and a reducing agent flow comprising a reducing agent, thereby selectively forming a metal layer on the crystalline silicon surface. The metal halide precursor flow and the reducing agent flow have a flow rate ratio of at least 10:1. The method further comprises annealing the metal layer to form a metal silicide layer from the metal layer.

[0006] In some embodiments, the method further comprises cleaning the feature bottom and feature sidewalls prior to exposing the feature to the metal halide precursor flow.

[0007] In some embodiments, the metal halide precursor comprises a metal chloride or a metal fluoride.

[0008] In some such embodiments, the metal halide precursor comprises tungsten hexafluoride, tungsten pentachloride, molybdenum hexafluoride, or molybdenum pentachloride.

[0009] In some embodiments, the metal layer comprises tungsten or molybdenum.

[0010] In some embodiments, the reducing agent comprises hydrogen, silane, or a combination thereof.

[0011] In some embodiments, the flow rate ratio ranges from about 10:1 to about 10,000:1.

[0012] In some embodiments, the metal layer has a thickness ranging from about 2 nm to about 20 nm.

[0013] In some embodiments, the crystalline silicon on the crystalline silicon surface is a doped or undoped single crystal silicon crystal or a doped or undoped polycrystalline silicon.

[0014] In some embodiments, annealing of the metal layer is performed between about 500°C and about 800°C.

[0015] In some embodiments, annealing of the metal layer is performed at a pressure range between approximately 1 Torr-100 Torr.

[0016] In some embodiments, the flow of a metal halide precursor and the flow of a reducing agent are alternated to form a metal layer by atomic layer deposition (ALD).

[0017] In some embodiments, a metal halide precursor flow and a reducing agent flow are co-flowed to form a metal layer by chemical vapor deposition (CVD).

[0018] In some embodiments, the metal halide precursor flow is pulsed and the reducing agent flow is continuously flowed to form the metal layer by pulsed CVD.

[0019] In some embodiments, the metal silicide layer forms an ohmic contact with the crystalline silicon surface.

[0020] In some embodiments, the metal silicide layer includes tungsten silicide or molybdenum silicide.

[0021] Another aspect of the present disclosure relates to a method comprising providing a feature having a feature bottom and a feature sidewall. The feature bottom comprises a crystalline silicon surface, and the feature sidewall comprises an oxide or nitride surface. The method further comprises exposing the feature to a first metal halide precursor flow and a first reducing agent flow, the first metal halide precursor flow comprising a first metal halide precursor, and the first reducing agent flow comprising a first reducing agent, thereby selectively forming a first metal layer on the crystalline silicon surface. The first metal halide precursor flow and the first reducing agent flow have a flow rate ratio of at least 10:1. The method further comprises providing a second metal halide precursor flow and a second reducing agent flow to the first metal layer, the second metal halide precursor flow comprising a second metal halide precursor, and the second reducing agent flow comprising a second reducing agent, thereby forming a second metal layer. The second metal halide precursor flow and the second reducing agent flow have a flow rate ratio of at least 10:1. The method further comprises annealing the second metal layer to form a metal silicide layer.

[0022] In some embodiments, the first metal halide precursor and the second metal halide precursor are selected from tungsten hexafluoride, tungsten pentachloride, molybdenum hexafluoride, and molybdenum pentachloride, respectively.

[0023] In some embodiments, the first reducing agent and the second reducing agent are each selected from hydrogen, silane, or a combination thereof.

[0024] In some embodiments, the metal silicide layer includes tungsten silicide or molybdenum silicide.

[0025] In some embodiments, the first and second metal halide precursors and the first and second reducing agents are supplied by chemical vapor deposition or atomic layer deposition.

[0026] These and other aspects of the disclosure are discussed further below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1A is a schematic diagram showing a cross-sectional representation of a recessed lateral contact in a 3D dynamic random access memory (3D-DRAM) before a metal silicide layer is formed, according to various embodiments. Figure 1B is a schematic diagram showing a cross-sectional view of a lateral contact in a 3D-DRAM structure after forming a metal silicide layer and a barrier metal / bottom electrode according to various embodiments.

[0028] Figure 2 is a schematic diagram showing a cross-sectional drawing of features in a vertical structure according to various embodiments.

[0029] Figure 3 is a process flow diagram showing certain operations in a method according to various embodiments.

[0030] Figure 4A is a schematic diagram showing providing tungsten hexafluoride (WF6) and hydrogen (H2) to a silicon (Si) surface according to various embodiments.

[0031] Figure 4B FIG. 5 is a schematic diagram showing a cross-sectional view of forming a tungsten (W) layer on Si using WF6 / H2 according to various embodiments.

[0032] Figure 5 is a schematic diagram showing a cross-sectional view of forming a W metal layer using WF6 / H2 according to various embodiments.

[0033] Fig. 6A and 6B Schematic diagram showing a cross-sectional view of forming a W metal layer using WF6 / SiH4 and WF6 / H2 according to various embodiments.

[0034] Fig. 7A and Figure 7B is a schematic diagram showing a cross-sectional view of forming a W metal layer using WF6 / H2 and WCl5 / H2 according to various embodiments.

[0035] Fig. 8A is an example of a flow sequence that may be used in a pulsed chemical vapor deposition (CVD) process to form a metal layer.

[0036] Figure 8B is an example of a flow sequence that can be used for a co-flow CVD process to form a metal layer.

[0037] Figure 8C is another example of a flow sequence that can be used for a co-flow CVD process to form a metal layer.

[0038] Fig.8D is an example of a flow sequence that may be used in an atomic layer deposition (ALD) process to form a metal layer.

[0039] Fig. 9 An example of an apparatus that can be used to perform the methods described herein is shown.

[0040] Fig. 10A An example of an apparatus that can be used to perform the methods described herein is shown.

[0041] Fig. 10B An example of an apparatus that can be used to perform the methods described herein is shown. DETAILED DESCRIPTION

[0042] A method for forming a metal silicide contact using crystalline silicon is provided. The method involves forming a metal layer comprising tungsten (W) or molybdenum (Mo), followed by annealing to convert the metal layer into a metal silicide layer. The metal layer can be formed in a pulsed chemical vapor deposition (CVD), co-current CVD, or atomic layer deposition (ALD) process. In some embodiments, the annealing is performed without first forming a capping layer.

[0043] Forming electrical contacts in semiconductor device manufacturing can involve forming a metal layer in a recessed feature with tungsten, molybdenum or other conductive materials. The feature may contain holes, trenches and vias. The metal layer in the feature can be annealed to form a metal silicide. The metal silicide can form an ohmic contact with semiconductor silicon, thereby reducing contact resistance. For example, W provides a low resistance and low stress layer and has a thermal expansion coefficient close to that of silicon. In addition, tungsten has high resistance to electromigration.

[0044] When forming a metal layer such as tungsten from a halide precursor, uncontrolled metal growth may result in a non-uniform interface between the metal and silicon, depending on the nature and reaction of competing precursors and other reactants. These defects may be the cause of non-uniform contact resistance in the contacts or failure of semiconductor devices. These defects may be critical for devices with smaller technology nodes and more complex pattern structures, where uniform metal growth is a major challenge.

[0045] Uniform metal growth can be a particular challenge in 3D dynamic random access memory (3D DRAM) structures, which may contain hundreds of lateral features stacked in a vertical direction. 3D DRAMs have an increased number of contacts but a reduced contact area compared to existing semiconductor devices. Deposition in 3D DRAM structures by methods such as sputtering metal targets in physical vapor deposition (PVD) methods is particularly challenging because most structures are out of line of sight of the deposited material. Plasma-based methods such as plasma-enhanced CVD (PECVD) also have poor step coverage in complex geometries. Uniform metal growth can also be challenging in vertical structures, such as in vertical DRAMs or logic structures containing multiple vertical features. In particular, deposition in tall structures or high aspect ratio structures formed in many stacked layers can be challenging.

[0046] In some embodiments, the methods described herein include deposition of a metal layer using a metal halide precursor. In some embodiments, the methods described herein include deposition of a thin tungsten layer using a tungsten halide precursor. The tungsten halide precursor is composed of the formula WX Z Wherein X is halogen (fluorine (F), chlorine (Cl), bromine (Br) or iodine (I)) and z is 2, 3, 4, 5 or 6. WX ZExamples of precursors include tungsten hexafluoride (WF6), tungsten hexachloride (WCl6), and tungsten pentachloride (WCl5). In some embodiments, the desired thickness of the W layer can be in the range of about 3 nm to 5 nm.

[0047] In some embodiments, the processes described herein include depositing a thin molybdenum layer using a molybdenum halide precursor. The molybdenum halide precursor is composed of the molecular formula MoX Z Wherein X is halogen (fluorine (F), chlorine (Cl), bromine (Br) or iodine (I)) and z is 2, 3, 4, 5 or 6. MoX Z Examples of precursors include molybdenum hexafluoride (MoF6). The molybdenum chloride precursor has the molecular formula MoCl x Given, wherein x is 2, 3, 4, 5 or 6, and comprises molybdenum dichloride (MoCl2), molybdenum trichloride (MoCl3), molybdenum tetrachloride (MoCl4), molybdenum pentachloride (MoCl5) and molybdenum hexachloride (MoCl6). In some embodiments, the desired thickness of the Mo layer can be in the range of about 3 to 5 nm.

[0048] Using an oxygen-free precursor to deposit the initial W or Mo layer prevents oxidation of the feature surface. It also prevents oxygen from incorporating into the initial W or Mo layer. Oxidation increases contact resistance. The lack of oxidation and oxygen incorporation ensures that contact resistance is kept low.

[0049] Examples of reducing agents include hydrogen (H2), silane (SiH4), diborane (B2H6), germane (GeH4), ammonia (NH3) and hydrazine (N2H4). In some embodiments, one or more reducing agents having a predetermined mixing ratio can be pulsed with a tungsten halide precursor or a molybdenum halide precursor to form tungsten or molybdenum metal.

[0050] 1(a) and 1(b) show schematic diagrams of cross-sectional features in a 3D DRAM structure according to various embodiments. Recessed feature 102 has sidewalls 106 including sidewall surfaces 116 and a bottom including crystalline silicon 108. Crystalline silicon 108 includes crystalline silicon surface 110. Recessed feature 102 may be, for example, a hole or a trench. Sidewall 106 may be made of one or more layers. Sidewall 106 includes a dielectric layer. Examples of dielectric materials include oxides, such as silicon oxide (SiO2) and aluminum oxide (Al2O3); nitrides, such as silicon nitride (SiN); carbides, such as nitrogen-doped silicon carbide (NDC) and oxygen-doped silicon carbide (ODC); and low-k dielectrics, such as carbon-doped SiO2.

[0051] The crystalline silicon 108 may extend from a first sidewall in the feature to a second sidewall in the feature and may be made of one or more layers. The crystalline silicon 108 of the crystalline silicon surface 110 may be doped or undoped single crystal silicon or doped or undoped polycrystalline silicon. In one embodiment, the crystalline silicon 108 may be doped polycrystalline silicon (doped polysilicon). In some embodiments, the crystalline silicon 108 may form a gate electrode.

[0052] As shown in FIG. 1( b), a metal silicide layer 112 can be selectively formed on the crystalline silicon 108 to form an ohmic contact. The thickness of the metal silicide layer 112 on the crystalline silicon 108 can be in the range of 2nm-10nm. As further described below, the metal silicide layer 112 can be formed by forming a metal layer on the crystalline silicon 108 and then annealing to convert the metal layer into a metal silicide layer 112. In some embodiments, a co-current CVD, pulsed CVD or ALD can be used to form the metal layer. After forming the metal silicide layer 112, a conformal layer 114 can be formed on the metal silicide layer and the sidewall surface 116. In some embodiments, the conformal layer 114 can be a barrier layer or a bottom electrode of a capacitor. For example, titanium nitride (TiN) can be used as a barrier metal.

[0053] The challenge associated with the above-mentioned 3D-DRAM manufacturing process is to form a metal silicide contact at the bottom of each recessed feature. It may be difficult to controllably selectively form a metal layer at the bottom of each recessed feature before annealing the metal layer to form a metal silicide layer. The selective and uniform formation of a metal layer on Si may be affected by the size of the features in which the metal layer is formed. In some embodiments, the recessed feature 102 has a depth "A" of 100nm-300nm and a height "B" of 10nm-30nm, resulting in an aspect ratio (depth to height) of 3-30. These small feature sizes and high aspect ratios pose challenges to forming metal layers. In some embodiments, a 3D-DRAM structure may include a stack containing more than 400 vertically stacked layers (features). The total stack height "C" may be in the range of about 6μm-12μm. This configuration may also increase the additional complexity of achieving a uniform, selective metal layer in each stack. In some embodiments, techniques used for selective deposition in other structures (eg, PVD or PECVD) may not be suitable for uniformly and selectively forming a metal layer in recessed features of a 3D-DRAM structure.

[0054] Figure 2Schematic diagram showing a cross-sectional feature in a vertically oriented feature. For example, such a feature can be used in a DRAM or logic device. The device can include one or more recessed features 202 having a bottom surface 210 and sidewalls 206. The recessed features 202 can extend in a vertical direction relative to the substrate. The method of selectively forming a metal silicide layer 214 from a metal layer is described herein with respect to horizontally oriented recessed features in a 3D-DRAM structure, which can also be used in vertically oriented structures, such as those in DRAM and / or logic devices.

[0055] Figure 3 FIG. 1 is a process flow diagram illustrating a method of forming a metal silicide ohmic contact with bottom crystalline silicon from a metal layer according to some embodiments. The metal layer may be a tungsten (W) film or a molybdenum (Mo) film. Application examples include 3D-NAND, 3D-DRAM, 2D-DRAM, and logic applications.

[0056] Method 300 begins by providing a substrate including features having bottom silicon and oxide or nitride sidewalls, where tungsten or molybdenum is to be deposited, depending on equipment and / or process requirements, in operation 301. The substrate may be provided to a semiconductor processing tool. For example, the substrate may be placed in a deposition chamber.

[0057] After providing a substrate comprising a feature having bottom crystalline silicon and oxide or nitride sidewalls, an optional cleaning operation 302 may be performed. Optional cleaning may be used to remove an oxide layer formed on the surface of the feature. In some embodiments, atomic layer cleaning based on Cl plasma, hydrogen fluoride (HF) vapor cleaning, ammonium fluoride (NH4F) cleaning, or treatment using other reducing agents may be used to reduce Si oxide at the bottom of the feature. In some embodiments, hydrogen fluoride may be diluted to about 100:1 prior to cleaning. Optional cleaning may be performed in a deposition chamber. Alternatively, optional cleaning may be performed in a separate process prior to providing to the deposition chamber.

[0058] Once the substrate is provided in the deposition chamber, a metal layer is formed in the feature in operation 303. The metal layer including a tungsten layer or a molybdenum layer may be deposited by co-flow CVD, pulsed CVD, or ALD.

[0059] In co-flow CVD, a metal halide precursor and a reducing agent are continuously pulsed so that the substrate is continuously exposed to the metal halide precursor and the reducing agent, the metal halide precursor including but not limited to tungsten hexafluoride, tungsten pentachloride, molybdenum hexafluoride or molybdenum pentachloride. The pulsed delivery can be continuous until a metal layer with a predetermined thickness is formed. Alternatively, the metal halide precursor and the reducing agent can be pulsed to co-flow with a carrier gas (e.g., an inert gas is purged between co-flow pulses). In a pulsed CVD process, the reducing agent can flow continuously while the metal halide precursor flows in pulses, and the intervals between the pulses expose the substrate to the precursor during the pulses. In an ALD process, the metal halide precursor, the reducing agent and the carrier gas can be pulsed sequentially to form a cycle. In some embodiments, the pulsed delivery cycle may include a pulsing sequence of a metal halide precursor, a carrier gas, a reducing agent and a carrier gas.

[0060] In some embodiments, the pulsed delivery may include more than one pulsed delivery step. For example, more than one metal halide precursor and / or reducing agent may be pulsed sequentially in multiple pulsed delivery steps. In the first pulsed delivery step, the substrate may be exposed to a first precursor and a first reducing agent to form a first metal layer on the substrate. In the second pulsed delivery step, the substrate may be exposed to a second precursor and a second reducing agent to form a second metal layer on the first metal layer formed in the first pulsed delivery step. In some embodiments, the metal layer may be formed conformally with the bottom crystalline silicon. In some embodiments, the metal layer may be about 2nm-20nm thick. In some embodiments, the metal layer may be about 2nm-10nm thick, 3nm-7nm thick, or 3nm-5nm thick.

[0061] During the formation of the metal layer, the temperature of the substrate and the pressure of the chamber can be controlled. For co-flow CVD and pulsed CVD, the substrate can be heated to between 250°C–350°C. In some embodiments, the chamber can be pressurized to at least 10 Torr, such as at least 30 Torr, or at least 50 Torr. For ALD processes, in some embodiments, the substrate can be heated to between 300°C-500°C, such as between 350°C-450°C. In some embodiments, the chamber can be pressurized to at least 10 Torr, such as at least 30 Torr, or at least 50 Torr.

[0062] In operation 304, after the metal layer is selectively deposited on the silicon surface, the feature is annealed to convert the metal layer into a metal silicide layer. In some embodiments, the metal layer can be annealed by rapid thermal annealing. In some embodiments, the thickness of the metal silicide layer can be in the range of about 2nm-10nm after annealing. Annealing is usually carried out between 500°C and 800°C, for example, between 500°C and 700°C. The metal layer can be annealed in situ in the deposition chamber where the metal layer is formed, without exposing the metal layer to the ambient atmosphere. In some embodiments, the substrate comprising the metal layer is transferred from one pedestal to another pedestal for annealing. After the metal silicide layer is formed, a barrier layer (or bottom electrode) can be formed on the metal silicide layer and the sidewall.

[0063] Figures 4A-4B Schematic diagram showing the formation of a tungsten layer by the reaction between WF6 / H2 and Si according to various embodiments. For some embodiments, in a CVD or ALD process, when a metal halide precursor (e.g., tungsten hexafluoride (WF6)) and a reducing agent (e.g., hydrogen (H2)) reach crystalline silicon ( Figure 4A ), the following reactions (1) and (2) will occur to form a W layer on Si.

[0064] 2WF6 (g) + 3Si (s) → 2W (s) + 3SiF4 (g) (1)

[0065] WF6 (g) + 3H2 (g) → W (s) + 6HF (g) (2)

[0066] Reaction (1) may occur first, followed by reaction (2). Alternatively, reactions (1) and (2) may occur substantially simultaneously with each other. According to reaction (1), WF6(g) reacts with silicon to form tungsten and SiF4 as a gas phase byproduct. As the tungsten layer is formed, one or more layers of silicon atoms are consumed downward from the silicon surface. As reaction (1) proceeds, the thickness of the silicon decreases while the thickness of the tungsten layer increases. Because the tungsten layer forms a diffusion barrier between silicon and WF6, the rate of reaction (1) may slow down until the diffusion layer prevents further reaction between silicon and WF6. The tungsten layer may grow until the layer thickness reaches a self-limiting thickness, which in some embodiments may be about 10 nm (or more). ).

[0067] In some embodiments, the reactivity of reaction (1) may be sufficient to cause excessive consumption of crystalline silicon. As a result, the growth of the tungsten metal layer may result in the formation of defects, such as Figure 4BA "wormhole" is shown. A wormhole defect can form from localized, non-uniform erosion of silicon. Wormhole defects can result in the formation of needles of tungsten that penetrate the crystalline silicon, which can cause a device short. Wormhole defects can also create non-uniform tungsten layer thickness in a feature, which can increase contact resistance variations in a device.

[0068] As reaction (1) slows down over time, reaction (2) may dominate and eventually replace reaction (1). In reaction (2), WF6(g) is reduced by a reducing agent (e.g., H2) to form a tungsten metal layer. Hydrogen fluoride (HF) may be a gas phase byproduct. The tungsten metal formed by reaction (2) can be selectively formed on the tungsten metal layer formed according to reaction (1). That is, the tungsten is formed on the tungsten below and not on the dielectric sidewalls. In addition, the tungsten metal layer according to reaction (2) does not substantially cause any defects (e.g., wormholes that may be observed in reaction (1)) to form. In some embodiments, after reactions (1) and (2), the thickness of the tungsten layer and the remaining silicon may be less than the thickness of the silicon before the reaction.

[0069] Although the reactions of Si and WF6 and H2 and WF6 are described above for the purpose of illustrating the competing reactions, the above description is also applicable to other metal halide precursors and reducing agents.

[0070] Figure 5 Schematic examples of metal layer formation according to various embodiments are shown. Figure 5 It is described that a metal halide precursor and a reducing agent (e.g., WF6 and H2) can be provided to a deposition chamber to form a tungsten layer on the bottom silicon in a substrate using an ALD or CVD process. The tungsten layer 504 can be selectively formed on the upper surface of the crystalline silicon 502, but not on the dielectric sidewalls 506. During the formation of the tungsten layer, the substrate can be exposed to continuous co-flowing WF6 and H2. Alternatively, WF6 can be pulsed and H2 is continuously flowing. Alternatively, WF6 and H2 are pulsed sequentially without any overlap. The flow sequence of the precursor, reducing agent, and carrier gas according to various embodiments is as follows: Figures 8A-8D Detailed description is given in further detail in .

[0071] Although WF6 is shown as an example of a metal halide precursor for tungsten layer deposition, other metal halide precursors such as WCl6 or WCl5 can be pulsed with hydrogen (H2). To form molybdenum, MoF6, MoCl6, or MoCl5 can be used as a precursor. In some embodiments, hydrogen (H2), silane (SiH4), or a mixture thereof can be used as a reducing agent.

[0072] In some embodiments, the gas flow rates of the metal halide precursor (e.g., WF6, WCl6, or WCl5) and the reducing agent (e.g., H2 or SiH4) can be controlled during the formation of the tungsten layer. In some embodiments, the flow rate of the reducing agent is at least 10 times higher than the flow rate of the metal halide precursor. For example, the gas flow rate of H2 can be controlled to be at least 10 times higher than the gas flow rate of WF6 to achieve high H2 flow rate conditions. In some embodiments, the gas flow rate of H2 to WF6 can be set to 10:1-10,000:1.

[0073] This high H2 flow rate condition can also be applied to form a molybdenum layer. The gas flow rate of H2 can be at least 10 times higher than the gas flow rate of the molybdenum halide precursor (e.g., MoF6, MoCl6, or MoCl5). In some embodiments, the gas flow rate of H2 to MoF6 is 10:1-10,000:1.

[0074] Under such high H2 flow rate conditions, the rates of reactions (1) and (2) can be controlled so that reaction (1) continues for only a limited time before reaction (2) becomes dominant. In the case where reaction (1) is quickly replaced, the formation of wormholes or other defects can be minimized or significantly suppressed. Reaction (2) forms a tungsten layer on the tungsten formed by the aforementioned reaction (1) without forming wormholes or other defects. In some embodiments, under high H2 flow rate conditions, the resulting tungsten layer may contain a significantly reduced number of wormholes or other defects, which is beneficial for reducing short circuits and / or resistance changes, thereby improving device life and reliability.

[0075] Fig. 6A and 6B A schematic illustration of forming a tungsten metal layer on a bottom Si by combining two sequential steps of providing different sets of reactants according to various embodiments is shown. Fig. 6A In the first step shown, the substrate is exposed to WF6 and SiH4. In some embodiments, WF6 and SiH4 can be delivered in pulses or in a continuous co-flow. Alternatively, WF6 and SiH4 can be delivered in pulses in sequence. A tungsten layer 604 can be selectively formed on the upper surface of the crystalline silicon 602 without forming tungsten on the dielectric sidewalls 606. The flow rate of SiH4 to WF6 in the first gas mixture can be controlled to be at least 10:1. In some embodiments, the flow rate of SiH4 to WF6 can be set in the range of 10:1 to 10,000:1.

[0076] In some embodiments, it may be advantageous to introduce SiH4 as a reducing agent at a high flow rate because the bottom crystalline silicon consumption in the SiH4 reduction may not be as reactive as the silicon consumption in reaction (1) using only H2 as a reducing agent. Thus, the formation of wormholes or other defects may be suppressed or prevented compared to reaction (1), while still forming a tungsten layer on the crystalline silicon.

[0077] In some embodiments, more than one reducing agent may be pulsed in the first step. For example, a mixture of SiH4 and H2 having a predetermined flow rate ratio may be used instead of SiH4. Adding H2 to SiH4 may change the reactivity of WF6 with silicon. The flow rate of (SiH4+H2) to WF6 may be controlled to be at least 10:1. In some embodiments, the flow rate of (SiH4+H2) to WF6 may be set in the range of 10:1 to 10,000:1.

[0078] After the first step is completed, the first gas mixture is purged to remove any gaseous reactants such as WF6 and SiH4 (or SiH4+H2) remaining in the deposition chamber. Figure 6B In the second step shown, WF6 and H2 may be introduced to further form a tungsten layer on the tungsten layer previously formed in the first step. The flow rate of H2 to WF6 in the second step may be controlled to be at least 10:1. In some embodiments, the flow rate of H2 to WF6 may be set within a range of 10:1 to 10,000:1. Although Fig. 6A and 6B The steps for forming a tungsten layer with minimized or suppressed wormholes or other defects are described, but may also be based on Fig. 6A and 6B The embodiment shown is used to form molybdenum. For example, MoF6, SiH4 and H2 can be pulsed to form a molybdenum layer on crystalline silicon.

[0079] Fig. 7A and 7B Schematic illustration of forming a tungsten layer on a bottom Si by combining two sequential steps of providing different sets of reactants according to various embodiments. Fig. 7A In the first step shown, a substrate containing features to be formed therein of tungsten is exposed to a first set of reactants containing WF6 and H2. WF6 and H2 may be pulsed or co-flowed continuously. Alternatively, WF6 and H2 may be pulsed sequentially. Tungsten layer 704 may be selectively formed on the upper surface of crystalline silicon 702 without forming tungsten on dielectric sidewalls 706. In some embodiments, the flow rate of H2 to WF6 may be controlled to be at least 10:1. In some embodiments, the flow rate of H2 to WF6 may be 10:1 to 10,000:1.

[0080] Under such high flow rate H2 conditions, the formation of wormholes or other defects can be substantially suppressed or prevented. After completing the first step, the remaining WF6 and H2 in the gas phase can be purged to remove any unwanted reactions in the deposition chamber. Figure 7BIn the second step shown, a second set of reactants can be introduced into the deposition chamber. The second set of reactants can be different from the first set of reactants. For example, the second set of reactants can include tungsten pentachloride (WCl5) and H2. Chloride precursors such as WCl5 may be superior to fluoride precursors such as WF6 because the incorporation of fluorine (F) ions into tungsten increases its resistivity. Similar to the flow rate of the first set of reactants, the flow rate of H2 to WCl5 can be controlled at least 10:1. In some embodiments, the flow rate of H2 to WCl5 can be set in the range of 10:1 to 10,000:1. In some embodiments, tungsten hexachloride (WCl6) can be used to replace tungsten pentachloride (WCl5) in the second step while maintaining the flow rate of H2 to WCl6. Using a tungsten chloride precursor such as tungsten pentachloride (WCl5) or tungsten hexachloride (WCl6) under high flow rate H2 conditions can also be beneficial in suppressing the formation of wormholes or other defects.

[0081] In some embodiments, WCl5 (or another WCl x Reactants) and H2 can be pulsed or continuously co-flowed to form a tungsten layer on the substrate without using WF6 or other gaseous reactants. Forming a tungsten layer from only WCl5 and H2 at the beginning of the deposition process may be beneficial in preventing the formation of defects such as wormholes.

[0082] It should be noted that Fig. 7A and 7B The embodiment shown forms a molybdenum layer. For example, MoF6 and H2 can be co-flowed into the deposition chamber continuously or sequentially. After an optional sweep cleaning, MoCl5 (or MoCl6) and H2 can be pulsed to form molybdenum on the molybdenum formed by the reaction between MoF6 and H2.

[0083] After forming a metal layer such as tungsten or molybdenum on crystalline silicon according to various embodiments, the metal layer is annealed to convert the metal layer into a metal silicide layer. The annealing may be a rapid thermal annealing between about 500°C-800°C. In some embodiments, the annealing may be performed in situ in a deposition chamber previously used to form the metal layer without breaking the vacuum. A chamber pressure of 1 Torr-100 Torr may be used. For in-situ annealing in a deposition chamber having multiple pedestals, a substrate in which a metal layer is to be formed may be positioned in one pedestal to form the metal layer. After forming the metal layer, the substrate with the metal layer may be transferred to another pedestal in the same deposition chamber without breaking the vacuum. Alternatively, the substrate with the metal layer may be removed from the deposition chamber for subsequent annealing in different annealing chambers. In-situ annealing may be beneficial in preventing any undesirable oxide layer from being formed on the metal layer before annealing, compared to removing the substrate from the deposition chamber.

[0084] Fig. 8AAn example of a pulsed CVD timing sequence for depositing metals according to various embodiments is shown. Fig. 8A In the example of , H2 flows continuously. Although H2 can flow alone, in some embodiments, a carrier gas such as nitrogen (N2), argon (Ar), helium (He), or other inert gas can co-flow with H2. For some embodiments, H2 or a mixture of H2 and a carrier gas co-flows continuously. To form tungsten, WF6 is pulsed into a deposition chamber containing a substrate on which tungsten is to be deposited. WF6 is pulsed at intervals between pulses. These intervals are labeled "sweep" because the continuous flow of H2 (or H2 / Ar) has the effect of clearing WF6 from the chamber to the outside. In some embodiments, the pressure during pulsed CVD can be less than 20 Torr, such as 10 Torr, or less than 10 Torr. The temperature during the pulsed CVD process may be the same as the temperature during thermal decomposition of the precursor, i.e., 250°C–350°C.

[0085] Figure 8B An example of a timing sequence for co-flow CVD for depositing metals according to various embodiments is shown. The substrate temperature during the co-flow CVD process can be 250°C–350°C. For the formation of tungsten, the WF6 precursor and H2 are pulsed so that they co-flow continuously into a deposition chamber in which a substrate to be formed of tungsten is placed. When a tungsten layer having a predetermined thickness is formed, the co-flow can end after a certain time. Although H2 can flow alone, in some embodiments, argon (Ar) or other inert gases can co-flow with H2. In some embodiments, the flow rate of H2 to WF6 is controlled to be at least 10:1. In some embodiments, the flow rate of H2 to WF6 can be 10:1-10,000:1. The thickness of tungsten can be monitored in situ. Alternatively, a separate measurement can be performed to determine the thickness of tungsten.

[0086] Figure 8C Another timing example of co-flow CVD for depositing metals according to various embodiments is shown. In some embodiments, a gas mixture containing WF6 and H2 can be pulsed with intervals between pulses, and then a carrier gas for tungsten deposition is pulsed to clear the WF6 and H2 of the gas phase. In some embodiments, WF6 and H2 can form a gas mixture with a predetermined flow rate ratio. The flow rate of H2 to WF6 in the gas mixture during co-flow CVD can be controlled to be at least 10:1. In some embodiments, the flow rate of H2 to WF6 can be 10:1-10,000:1.

[0087] When a gas mixture (e.g., WF6 and H2) is pulsed to expose the substrate to WF6 and H2, WF6 can react with silicon to form tungsten and SiF4 in the gas phase. Thereafter, WF6 can react with H2 to form tungsten and HF in the gas phase on the tungsten formed by the reaction between WF6 and Si. At the end of the pulsed delivery of the gas mixture, the co-flow of WF6 and H2 stops, and tungsten is no longer formed. The deposition chamber may contain unreacted H2 and / or WF6. An inert gas such as argon (Ar) may be pulsed for a predetermined time to purge any remaining gas from the deposition chamber, thereby preventing any undesirable gaseous reactions that may occur later. After the inert gas purge, a gas mixture containing WF6 and H2 is pulsed again to expose the substrate to WF6 and H2, thereby forming additional tungsten and HF in the gas phase. In some embodiments, the reaction between WF6 and silicon may not be complete in the first pulsed delivery of WF6 / H2. Instead, the reaction may continue during subsequent pulse delivery.

[0088] The sequence of WF6 / H2 pulses and carrier gas pulses may be repeated until a tungsten layer having a predetermined thickness is formed. The tungsten layer thickness may be monitored in situ during the tungsten layer formation. Alternatively, a separate measurement may be made to determine the tungsten thickness. The substrate temperature during co-flow CVD may be 250°C–350°C.

[0089] Fig.8D An example of a timing sequence for ALD for depositing metals according to various embodiments is shown. The ALD process is a surface-mediated deposition technique in which doses of reactants (eg, precursors and reducing agents) and a sweep carrier gas are sequentially introduced into a deposition chamber. Fig.8D A timing chart showing tungsten deposition, where a WF6 precursor and a reducing agent (e.g., H2) can be alternately pulsed into the deposition chamber. Fig.8D In the process, H2 is first pulsed to expose the substrate to H2 in the deposition chamber. Subsequently, the carrier gas is pulsed to remove H2 from the chamber that is not at or near the substrate surface. During the carrier gas pulse delivery, the deposition chamber may be at a pressure of about 1 Torr. After the sweep is completed, the WF6 precursor is pulsed to expose the substrate on which tungsten metal will be formed to the WF6 precursor. WF6 can react with silicon to form tungsten on the silicon surface. SiF4 can be released in the gas phase. In some embodiments, WF6 can react chemically with H2 at or near the substrate to form tungsten and gas-phase HF on the tungsten formed by the reaction between WF6 and H2. After the WF6 pulse delivery is completed, the carrier gas is pulsed again to purge the deposition chamber to remove any gas-phase WF6 and H2. In some embodiments, the flow rate of H2 to WF6 can be controlled to be at least 10:1. In some embodiments, the flow rate of H2 to WF6 can be 10:1-10,000:1.

[0090] In some embodiments, instead of pulsing H2 first, WF6 is first pulsed to expose the substrate to WF6, whereby a reaction occurs between WF6 and silicon, and tungsten is first formed on the surface of silicon. The carrier gas can then be pulsed to remove any WF6 that is not at or near the silicon. After the carrier gas is pulsed, H2 is pulsed to expose the substrate to H2. In some embodiments, WF6 can continue to react with Si in the presence of H2 to form tungsten and gas-phase SiF4. In some embodiments, WF6 can react with H2 to form tungsten and gas-phase HF on the tungsten formed by the reaction between WF6 and Si. The H2 pulse delivery step is followed by a carrier gas pulse delivery to remove any gas phase that is not on or near the Si surface. In some embodiments, the flow rate of H2 to WF6 can be controlled to be at least 10:1. In some embodiments, the flow rate of H2 to WF6 can be 10:1-10,000:1.

[0091] It should be noted that Figures 8A-8D The y-axes in the timing examples are not necessarily to the same scale; rather, the timing is presented to show the relative sequential times of the pulses and sweeps. Fig. 8A , 8C Any purge:dose continuity times in the timing examples in 8D do not necessarily reflect the actual continuity times; rather, any purge:dose continuity times demonstrate the timing between the metal halide precursor, the reducing agent, and the carrier gas.

[0092] It should also be noted that Figures 8A-8D The timing example in FIG. 1 can be used to form a molybdenum (Mo) layer. For example, the Mo metal layer can be formed by Fig. 8A The Mo metal layer can be formed by a pulsed CVD process using a MoF6 precursor and H2. Figure 8B The co-flow CVD process is formed by continuously pulsing MoF6 and H2. In another example, the Mo metal layer can be formed according to Figure 8C The co-flow CVD process is formed by continuously pulsing MoF6 and H2 and sequentially purging with a carrier gas between the pulses of MoF6 / H2. In another example, the Mo metal layer can be formed by Fig.8D The ALD process is formed by alternately and sequentially pulsing MoF6, H2 and carrier gas.

[0093] According to various embodiments, the following one or more advantages can be achieved by the method described herein. In some embodiments, the formation of wormholes or other defects between the metal layer and the following crystalline silicon is significantly suppressed while forming a metal layer such as a tungsten or molybdenum layer. Controlling these defects helps to improve the reliability of the equipment. In some embodiments, after the metal layer is formed, the substrate with the metal layer can be annealed in the same chamber without being exposed to the ambient atmosphere, thereby preventing the pollution and oxidation of the metal layer. This in-situ annealing provides the additional advantage of not needing multiple process steps (comprising deposition of covering metal, annealing, stripping of covering metal, deposition of barrier metal or pre-cleaning before the bottom electrode of the capacitor). This in-situ annealing also improves output and reduces manufacturing costs.

[0094] In some embodiments, the metal silicide layer may be W or The product may be formed in a four-station module (QSM) of Halo (available from Lam Research Corp. (Fremont, California)), or in any of a variety of other commercially available processing systems. These products may include a deposition chamber with multiple pedestals. In some embodiments, the deposition station may include four pedestals, and the first pedestal, the second pedestal, and the third pedestal may be used to selectively form a metal layer, while the fourth pedestal may be used to anneal the metal to form a metal silicide. This product configuration may maximize the productivity of the process by reducing process integration steps and manufacturing costs.

[0095] Fig. 9 A schematic diagram of an embodiment of a processing station 900 having a processing chamber 902 for maintaining a low pressure environment is depicted. In some embodiments, multiple processing stations may be included in a common low pressure processing tool environment. For example, Fig. 10A An embodiment of a processing tool 1000 is described. In some embodiments, one or more hardware parameters of the processing station 900, including those discussed in detail below, can be programmatically adjusted by one or more computer controllers, such as 950. In other embodiments, the processing chamber can be a single-station chamber.

[0096] In some embodiments, the processing station 900 can include an ALD processing station and is in fluid communication with a reactant delivery system 901a to deliver process gases to a distribution showerhead 906. The reactant delivery system 901a includes a mixing vessel 904 for mixing and / or conditioning process gases, such as a W-containing precursor gas, a Mo-containing precursor gas, a hydrogen-containing gas, an argon gas or other carrier gas, or other reactant-containing gas, for delivery to the showerhead 906. One or more mixing vessels 920 can control the introduction of process gases into the mixing vessel 904. In various embodiments, deposition of a W layer or a Mo layer is performed in the processing station 900, and in some embodiments, other operations such as in-situ cleaning can be performed in the same or another station of a processing tool 1000 including multiple stations, as described below with respect to Fig. 10A Further description of.

[0097] As an example, Fig. 9 Embodiments include vaporization point 903, which is used to vaporize liquid reactants to be supplied to mixing container 904. In some embodiments, vaporization point 903 can be a heated vaporizer. In some embodiments, liquid precursors or liquid reactants can be vaporized at a liquid injector (not shown). For example, a liquid injector can inject a pulse of liquid reactants into a carrier gas flow upstream of mixing container 904. In one embodiment, a liquid injector can vaporize reactants by flashing liquid from a higher pressure to a lower pressure. In another example, a liquid injector can atomize liquid into dispersed droplets that are then vaporized in a heated delivery pipe. Smaller droplets can vaporize faster than larger droplets, thereby reducing the delay between liquid injection and completion of vaporization. Faster vaporization can reduce the length of the pipeline downstream of vaporization point 903. In one embodiment, a liquid injector can be directly mounted to mixing container 904. In another embodiment, a liquid injector can be directly mounted to a spray head 906.

[0098] In some embodiments, a liquid flow controller (LFC) can be set upstream of the vaporization point 903 to control the mass flow rate of the liquid used for vaporization and delivered to the processing chamber 902. For example, the LFC can include a thermal mass flow meter (MFM) located downstream of the LFC. The plunger valve of the LFC can then be adjusted in response to a feedback control signal provided by a proportional integral differential (PID) controller that is electrically in communication with the MFM. However, it can take one second or more to use feedback control to stabilize the liquid flow. This can extend the time for dosing liquid reactants. Therefore, in some embodiments, the LFC can dynamically switch between feedback control mode and direct control mode. In some embodiments, this can be performed by disabling the sensing pipeline and PID controller of the LFC.

[0099] The showerhead 906 distributes process gases toward the substrate 912. Fig. 9In the illustrated embodiment, substrate 912 is positioned below showerhead 906 and is shown resting on pedestal 908. Showerhead 906 may have any suitable shape and may have any suitable number and arrangement of ports to distribute process gases to substrate 912.

[0100] In some embodiments, the pedestal 908 can be raised or lowered to expose the substrate 912 to the volume between the substrate 912 and the showerhead 906. In some embodiments, the pedestal 908 can be temperature controlled by a heater 910. The pedestal 908 can be set to any suitable temperature during operation for performing the various disclosed embodiments, such as a temperature between about 300° C. and about 500° C. It should be understood that in some embodiments, the pedestal height can be adjusted programmatically via a suitable controller 950. At the end of a process stage, the pedestal 908 can be lowered during another substrate transfer stage to allow the substrate 912 to be removed from the pedestal 908.

[0101] In some embodiments, the position of the showerhead 906 can be adjusted relative to the base 908 to change the volume between the substrate 912 and the showerhead 906. In addition, it should be understood that the vertical position of the base 908 and / or the showerhead 906 can be changed by any suitable mechanism within the scope of the present disclosure. In some embodiments, the base 908 may include a rotation axis for rotating the orientation of the substrate 912. It should be understood that in some embodiments, one or more of these exemplary adjustments can be performed programmatically by one or more appropriate controllers (e.g., computer controller 950). The controller 950 may include the following about Fig. 9 Any features described for controller 950.

[0102] In some embodiments, instructions for controller 950 may be provided via input / output control (IOC) sequencing instructions. In one example, instructions for setting the conditions of a process stage may be included in the corresponding recipe stage of a process recipe. In some cases, the process recipe stages may be arranged in order so that all instructions for a process stage are executed simultaneously with the process stage. In some embodiments, instructions for setting one or more reactor parameters may be included in the recipe stage. For example, the first recipe stage may include instructions for setting the flow rate of an inert gas and / or a reaction gas (e.g., a W or Mo precursor, H2, or SiH4, etc.), instructions for setting the flow rate of a carrier gas (e.g., argon), and time delay instructions for the first recipe stage. The subsequent second recipe stage may include instructions for adjusting or stopping the flow rate of an inert gas and / or a reaction gas, instructions for adjusting the flow rate of a carrier gas or a purge gas, and time delay instructions for the second recipe stage. The third recipe stage may include instructions for adjusting the flow rate of a second reaction gas such as H2, instructions for adjusting the flow rate of a carrier gas or a purge gas, and time delay instructions for the third recipe stage. A subsequent fourth recipe stage may include instructions for adjusting or stopping the flow rates of the inert gas and / or the reactant gas, and instructions for adjusting the flow rates of the carrier gas or the purge gas, and time delay instructions for the fourth recipe stage. It should be understood that within the scope of the present disclosure, these recipe stages may be further subdivided and / or repeated in any suitable manner.

[0103] Additionally, in some embodiments, pressure control for processing station 900 may be provided by butterfly valve 918. Fig. 9 In the embodiment shown in FIG. 1 , butterfly valve 918 throttles the vacuum provided by a downstream vacuum pump (not shown). However, in some embodiments, pressure control of process station 900 can also be adjusted by changing the flow rate of one or more gases introduced into process station 900.

[0104] Fig. 10A and Fig. 10B An example of a processing system is shown. Fig. 10A An example of a processing tool including multiple stations is shown. The processing tool 1000 includes a transfer module 1003. The transfer module 1003 provides a clean vacuum environment to minimize the risk of contamination of the substrate being processed when it moves between the various modules. Mounted on the transfer module 1003 is a chamber 1009 (e.g., a multi-station chamber) capable of performing the above-mentioned in-situ cleaning and / or ALD processes.

[0105] Chamber 1009 may include a plurality of stations 1011, 1013, 1015, and 1017, which may perform operations in sequence according to the disclosed embodiments. For example, chamber 1009 may be configured such that stations 1011 and 1013 perform in-situ cleaning of the substrate using dilute hydrofluoride, and subsequent metal layer deposition. For example, a tungsten layer may be formed using a WF6 precursor and H2. Thus, stations 1011 and 1013 may be configured to process the substrate in parallel, with each station performing cleaning and deposition processes in turn. Stations 1015 and 1017 may be configured to receive a substrate having a metal layer formed in stations 1011 and 1013, respectively, to perform annealing to convert the metal layer into a metal silicide layer without contaminating the substrate with the ambient atmosphere. In another example, chamber 1009 may be configured such that station 1011 performs in-situ cleaning, stations 1013 and 1015 perform metal layer deposition, and station 1017 performs metal layer annealing. In another example, chamber 1009 can be configured so that stations 1011, 1013, and 1015 process substrates in parallel, with each station sequentially performing multiple processes including in-situ cleaning and metal deposition. After depositing the metal layer in stations 1011, 1013, and 1015, station 1017 can receive the substrate from stations 1013, 1015, and 1017 for annealing.

[0106] A multi-station chamber may contain two or more stations, for example 2-6, with operations appropriately distributed. For example, a two-station chamber may be configured to perform substrate cleaning in the first station followed by metal layer deposition in the second station. A station may contain a heated susceptor or substrate support, one or more gas inlets or showerheads, or a dispersion plate.

[0107] Module 1007 may also be mounted on transfer module 1003. In some embodiments, a pre-clean as described above may be performed in module 1007 before the substrate is transferred to another module (not shown) similar to module 1007 or chamber 1009 under vacuum for ALD.

[0108] The processing tool 1000 also includes one or more wafer source modules 1001, which are storage locations for wafers before and after processing. An atmospheric robot (not shown) in an atmospheric transfer chamber 1019 can first move wafers from the source module 1001 to a load lock 1021. Wafer transfer equipment (usually a robot arm unit) in the transfer module 1003 then moves the wafers from the load lock 1021 to and between modules mounted on the transfer module 1003.

[0109] Fig. 10B is an embodiment of a processing tool 1000, as described in 10A. Fig. 10BThe processing tool 1000 has a wafer source module 1001, a transfer module 1003, an atmospheric transfer chamber 1019 and a load lock 1021, as described above with reference to Fig. 10A described. Fig. 10B The system in has three single station modules 1057A-1057C. The processing tool 1000 can be configured to perform operations in sequence according to the disclosed embodiments. For example, the station modules can be configured so that a single station module 1057A performs a cleaning operation, a single station module 1057B performs metal formation using, for example, a metal halide precursor, and a single station module 1057C performs an in-situ anneal. The station modules can include a heated pedestal or substrate support, one or more gas inlets or showerheads or dispersion plates, as described above with reference to Fig. 9 described.

[0110] In various embodiments, a controller 1029 (e.g., a system controller) is used to control process conditions during deposition. The controller 1029 will typically include one or more memory devices and one or more processors. The processor may include a CPU or computer, analog and / or digital input / output connections, a stepper motor controller board, etc.

[0111] The controller 1029 can control all device activities. The system controller 1029 runs system control software, which includes instruction sets for controlling timing, gas mixture, chamber pressure, chamber temperature, wafer temperature, radio frequency (RF) power level, wafer chuck or pedestal position, and other parameters of a particular process. In some embodiments, other computer programs stored on a memory device associated with the controller 1029 may be used.

[0112] Typically, there will be a user interface associated with the controller 1029. The user interface may include a display screen, a graphical software display of the device and / or process conditions, and a user input device such as a pointing device, keyboard, touch screen, microphone, or the like.

[0113] The system control logic may be configured in any suitable manner. In general, the logic may be designed or configured in hardware and / or software. The instructions for controlling the drive circuit may be hard-coded or provided as software. The instructions may be provided by "programming". Such programming is understood to include any form of logic including hard-coded logic in digital signal processors, application specific integrated circuits, and other devices having specific algorithms implemented as hardware. Programming is also understood to include software or firmware instructions that can be executed on a general purpose processor. The system control software may be encoded in any suitable computer readable programming language.

[0114] The computer program code for controlling the Mo precursor pulses, hydrogen pulses and argon gas flow and other processes in the process sequence can be written in any conventional computer readable programming language: for example, assembly language, C, C++, Pascal, Fortran or others. The compiled object code or script is executed by the processor to perform the tasks identified in the program. As also indicated, the program code can be hard-coded.

[0115] Controller parameters relate to process conditions such as, for example, process gas composition and flow rate, temperature, pressure, cooling gas pressure, substrate temperature and chamber wall temperature. These parameters are provided to the user in the form of a recipe and can be input using a user interface.

[0116] Signals for monitoring the process may be provided through analog and / or digital input connections of the controller 1029. Signals for controlling the process may be output through analog and digital output connections of the deposition apparatus.

[0117] The system software can be designed or configured in many different ways. For example, multiple chamber component subroutines or control objects can be written to control the operation of chamber components required to perform deposition processes according to the disclosed embodiments. Examples of programs or program segments for this purpose include substrate positioning code, process gas control code, pressure control code, and heater control code.

[0118] In some implementations, the controller 1029 is part of a system, which can be part of the above examples. Such a system can include a semiconductor processing device, which includes one or more processing tools, one or more chambers, one or more platforms for processing, and / or specific processing components (wafer pedestals, gas flow systems, etc.). These systems can be integrated with electronic devices for controlling their operation before, during, and after the processing of semiconductor wafers or substrates. The electronic device can be referred to as a "controller", which can control various components or subcomponents of one or more systems. Depending on the processing requirements and / or the type of system, the controller 1029 can be programmed to control any process disclosed herein, including the delivery of process gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings in some systems, RF matching circuit settings, frequency settings, flow rate settings, fluid delivery settings, position and operation settings, wafer transfer in and out tools and other transfer tools and / or load locks connected or docked with a specific system.

[0119] Broadly speaking, a controller can be defined as an electronic device having various integrated circuits, logic, memory, and / or software that receive instructions, issue instructions, control operations, enable cleaning operations, enable endpoint measurements, etc. The integrated circuit can include a chip in the form of firmware that stores program instructions, a digital signal processor (DSP), a chip defined as an application specific integrated circuit (ASIC), and / or one or more microprocessors or microcontrollers that execute program instructions (e.g., software). The program instructions can be instructions sent to the controller in the form of various individual settings (or program files) that define operating parameters for performing a specific process on or for a semiconductor wafer or system. In some embodiments, the operating parameters can be part of a recipe defined by a process engineer to complete one or more processing steps during the manufacture of one or more (kinds of) layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or dies of a wafer.

[0120] In some implementations, the controller 1029 may be part of or coupled to a computer that is integrated with the system, coupled to the system, otherwise networked to the system, or a combination thereof. For example, the controller 1029 may be in the "cloud" or may be all or part of a wafer fab host system that may allow remote access to wafer processing. The computer may enable remote access to the system to monitor the current progress of a manufacturing operation, check the history of past manufacturing operations, check trends or performance criteria for multiple manufacturing operations, change parameters of a current process, set processing steps to follow the current process, or start a new process. In some examples, a remote computer (e.g., a server) may provide a process recipe to the system via a network (which may include a local network or the Internet). The remote computer may include a user interface that enables input or programming of parameters and / or settings, which are then sent from the remote computer to the system. In some examples, the controller receives instructions in the form of data that specify parameters for each processing step to be performed during one or more operations. The parameters may be specific to the type of process to be performed and the type of tool that the controller is configured to interface with or control. Thus, as described above, the controller may be distributed, for example, by including one or more discrete controllers networked together and working toward a common purpose, such as the processes and controls described herein. An example of a distributed controller for such a purpose is one or more integrated circuits on a chamber that communicate with one or more integrated circuits remotely (e.g., at a platform level or as part of a remote computer), which combine to control the process on the chamber.

[0121] Example systems may include, but are not limited to, plasma etch chambers or modules, deposition chambers or modules, spin rinse chambers or modules, metal plating chambers or modules, cleaning chambers or modules, chamfer edge etch chambers or modules, PVD chambers or modules, CVD chambers or modules, ALD chambers or modules, atomic layer etch (ALE) chambers or modules, ion implantation chambers or modules, track chambers or modules, and any other semiconductor processing system that may be associated with or used in the manufacture and / or preparation of semiconductor wafers.

[0122] As described above, depending on one or more processing steps to be performed by the tool, the controller can communicate with one or more other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, neighboring tools, tools located throughout the factory, a host computer, another controller, or tools used in material transport to transport wafer containers to and from tool locations and / or load ports in a semiconductor manufacturing facility.

[0123] The controller 1029 may include different programs. The substrate positioning program may include program code for controlling chamber components for loading the substrate onto a pedestal or chuck and controlling the spacing between the substrate and other components of the chamber, such as a gas inlet and / or a target. The process gas control program may include code for controlling gas composition, flow rate, pulse time, and optionally for flowing gas into the chamber to stabilize the pressure in the chamber before deposition. The pressure control program may include code for controlling the pressure in the chamber by adjusting, for example, a throttle valve in an exhaust system in the chamber. The heater control program may include code for controlling the current of a heating unit for heating the substrate. Alternatively, the heater control program may control the delivery of a heat transfer gas, such as helium, to a wafer chuck.

[0124] Examples of chamber sensors that can be monitored during deposition include mass flow controllers, pressure sensors such as manometers, and thermocouples located in the pedestal or chuck. Appropriately programmed feedback and control algorithms can be used with data from these sensors to maintain desired processing conditions.

[0125] The foregoing describes embodiments of the present invention implemented in a single-chamber or multi-chamber semiconductor processing tool. The apparatus and processes described herein can be used in conjunction with a lithographic patterning tool or process, for example, for preparing or manufacturing semiconductor devices, displays, LEDs, photovoltaic panels, etc. Typically, although not necessarily, these tools / processes will be used or operated together in a common manufacturing facility. The lithographic patterning of a film typically includes some or all of the following steps, each of which enables multiple feasible tools: (1) applying a photoresist to a workpiece, i.e., a substrate, using a spin coating or spray coating tool; (2) curing the photoresist using a hot plate or heating furnace or a UV curing tool; (3) exposing the photoresist to visible light or UV light or X-rays using a tool such as a wafer stepper; (4) developing the resist so as to selectively remove the resist and thereby patterning it using a tool such as a wet cleaning station; (5) transferring the resist pattern to an underlying film or workpiece by using a dry or plasma assisted etching tool; and (6) removing the resist using a tool such as a radio frequency or microwave plasma resist stripper.

Claims

1. A method comprising: Providing a feature having a feature bottom and a feature sidewall, wherein the feature bottom comprises a crystalline silicon surface and the feature sidewall comprises an oxide or nitride surface; exposing the feature to a metal halide precursor flow comprising a metal halide precursor and a reducing agent flow comprising a reducing agent, thereby selectively forming a metal layer on the crystalline silicon surface, wherein the metal halide precursor flow and the reducing agent flow have a flow rate ratio of at least 10:1; and The metal layer is annealed to form a metal silicide layer.

2. The method according to claim 1, further comprising: The feature bottom and the feature sidewalls are cleaned prior to exposing the feature to the metal halide precursor flow. The method of claim 1 , wherein the metal halide precursor comprises a metal chloride or a metal fluoride.

4. The method according to claim 3, wherein the metal halide precursor comprises tungsten hexafluoride, tungsten pentachloride, molybdenum hexafluoride, or molybdenum pentachloride. The method of claim 1 , wherein the metal layer comprises tungsten or molybdenum. The method of claim 1 , wherein the reducing agent comprises hydrogen, silane, or a combination thereof.

7. The method of claim 1, wherein the flow rate ratio is in a range of about 10:1 to about 10,000:

1. The method of claim 1 , wherein the metal layer has a thickness in a range between approximately 2 nm and 20 nm. 9 . The method according to claim 1 , wherein the crystalline silicon on the surface of the crystalline silicon is a doped or undoped single crystal silicon crystal or a doped or undoped polycrystalline silicon crystal.

10. The method of claim 1, wherein the annealing of the metal layer is performed between about 500°C-800°C.

11. The method of claim 1, wherein the annealing of the metal layer is performed at a pressure range between approximately 1 Torr-100 Torr.

12. The method of claim 1, wherein the flow of the metal halide precursor and the flow of the reducing agent are alternated to form the metal layer by atomic layer deposition.

13. The method of claim 1, wherein the metal halide precursor flow and the reducing agent flow co-flow to form the metal layer by chemical vapor deposition.

14. The method of claim 1, wherein the flow of the metal halide precursor is pulsed and the flow of the reducing agent is continuous to form the metal layer by pulsed chemical vapor deposition.

15. The method of claim 1, wherein the metal silicide layer forms an ohmic contact with the crystalline silicon surface. The method of claim 1 , wherein the metal silicide layer comprises tungsten silicide or molybdenum silicide.

17. A method comprising: Providing a feature having a feature bottom and a feature sidewall, wherein the feature bottom comprises a crystalline silicon surface and the feature sidewall comprises an oxide or nitride surface; exposing the feature to a first metal halide precursor flow and a first reducing agent flow, the first metal halide precursor flow comprising a first metal halide precursor and the first reducing agent flow comprising a first reducing agent, thereby selectively forming a first metal layer on the crystalline silicon surface, wherein the first metal halide precursor flow and the first reducing agent flow have a flow rate ratio of at least 10:1; providing a second metal halide precursor flow and a second reducing agent flow to the first metal layer, the second metal halide precursor flow comprising a second metal halide precursor and the second reducing agent flow comprising a second reducing agent, thereby forming a second metal layer, wherein the second metal halide precursor flow and the second reducing agent flow have a flow rate ratio of at least 10:1; and The second metal layer is annealed to form a metal silicide layer.

18. The method of claim 17, wherein the first metal halide precursor and the second metal halide precursor are selected from tungsten hexafluoride, tungsten pentachloride, molybdenum hexafluoride, and molybdenum pentachloride, respectively.

19. The method of claim 17, wherein the first reducing agent and the second reducing agent are each selected from hydrogen, silane, or a combination thereof.

20. The method of claim 17, wherein the metal silicide layer comprises tungsten silicide or molybdenum silicide. 21 . The method of claim 17 , wherein the first and second metal halide precursors and the first and second reducing agents are supplied by chemical vapor deposition or atomic layer deposition.