Method for manufacturing semiconductor device
By forming a resin film that reacts with water on the semiconductor wafer, the problem of cutting objects adhesion during the cutting process is solved, and a higher quality semiconductor chip production is achieved.
Patent Information
- Application Number
- CN202380036860.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-11
- Filing Date
- 2023-10-06
- Publication Date
- 2024-12-06
AI Technical Summary
During the cutting process of semiconductor wafers, fine cutting objects adhere to the circuit forming surface, resulting in poor connection problems, which are difficult to effectively solve in the prior art.
A resin film which is low molecular weight by reacting with water is formed on the semiconductor wafer, and is used as a protective film. After cutting, it is reacted with water to remove the resin film to prevent the cutting from adhesion.
It effectively prevents the adhesion of cutting objects, improves the production quality and connection stability of semiconductor chips, and simplifies the removal process of resin film.
Smart Images

Figure CN119096328A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a semiconductor device. Background Art
[0002] Semiconductor devices are usually manufactured through the following steps. First, a semiconductor wafer is attached to a dicing tape and the semiconductor wafer is singulated into semiconductor chips in this state (dicing step). After that, a pickup step of picking up the semiconductor chip and a semiconductor chip bonding step of bonding the picked-up semiconductor chip and supporting components by thermal compression bonding with an adhesive (die bonding film) are performed to manufacture a semiconductor device.
[0003] In the dicing process, sometimes fine cuttings (chips) generated by cutting the semiconductor wafer adhere to the circuit formation surface of the semiconductor wafer, causing poor connection in the subsequent process. Therefore, the following process is being studied: the dicing process is performed after a resin film (protective film) is provided on the semiconductor wafer, and the resin film (protective film) is removed after dicing (for example, Patent Documents 1 and 2).
[0004] Previous technical literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2014-172932
[0007] Patent Document 2: Japanese Patent Application Publication No. 2018-129365 Summary of the invention
[0008] Technical issues to be solved by the invention
[0009] An object of the present invention is to provide a novel method for manufacturing a semiconductor device including a step of forming a resin film on a semiconductor wafer.
[0010] Means for solving technical problems
[0011] The present invention provides a method for manufacturing a semiconductor device according to [1] and [2].
[0012] [1] A method for manufacturing a semiconductor device, comprising:
[0013] A resin film forming step, forming a resin film including a resin that is reduced in molecular weight by reacting with water on a semiconductor wafer; a semiconductor chip manufacturing step with a resin film sheet, manufacturing a single-piece semiconductor chip with a resin film sheet by cutting the semiconductor wafer with the resin film formed thereon with a cutting blade; and a resin film sheet removing step, causing the resin in the resin film sheet of the semiconductor chip with the resin film sheet to react with water and removing the resin film sheet from the semiconductor chip with the resin film sheet.
[0014] [2] The method for manufacturing a semiconductor device according to [1], wherein:
[0015] The resin film removal step is performed by immersing the resin film of the semiconductor chip with the resin film in water.
[0016] Effects of the Invention
[0017] According to the present invention, there is provided a novel method for manufacturing a semiconductor device including a step of forming a resin film on a semiconductor wafer. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device. Figure 1 middle, Figure 1 (a) Figure 1 (b) Figure 1 (c) and Figure 1 (d) is a diagram showing each process.
[0019] Figure 2 is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device. Figure 2 middle, Figure 2 (a) Figure 2 (b) and Figure 2 (c) is a diagram showing each process. DETAILED DESCRIPTION
[0020] Hereinafter, the present embodiment will be described in detail with reference to the accompanying drawings. However, the present invention is not limited to the following embodiments. In the following embodiments, the constituent elements (including steps, etc.) are not necessary except for the cases specifically indicated. The same symbols are marked on the same or equivalent parts, and repeated descriptions are omitted. Regarding the positional relationship such as up, down, left, and right, unless otherwise specified, they are based on the positional relationship shown in the accompanying drawings. The sizes of the constituent elements in each figure are conceptual, and the relative relationship between the sizes of the constituent elements is not limited to those shown in the figures.
[0021] The same is true for the numerical value and its range in the present invention, and the present invention is not limited thereto. In this specification, the numerical range represented by "~" represents the range including the numerical values recorded before and after "~" as the minimum and maximum values, respectively. In the numerical range recorded in stages in this specification, the upper limit or lower limit recorded in a numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In the numerical range recorded in this specification, the upper limit or lower limit of its numerical range can also be replaced by the value shown in the embodiment.
[0022] In this specification, the term "layer" includes not only a structure of a shape formed on the entire surface but also a structure of a shape formed on a part when viewed from a top view. In this specification, the term "process" includes not only an independent process but also a process that can achieve the desired effect of the process even if it cannot be clearly distinguished from other processes.
[0023] In this specification, "(meth)acryloyl" refers to at least one of acryloyl and methacryloyl. In this specification, "(poly)oxyalkylene" refers to at least one of oxyalkylene and polyoxyalkylene. Polyoxyalkylene is a group in which two or more alkylene groups are linked by an ether bond. The same applies to other similar expressions such as "(poly)oxyethylene".
[0024] Each component and material exemplified in the present specification may be used alone or in combination of two or more unless otherwise specified.
[0025] [Method for manufacturing semiconductor device]
[0026] A method for manufacturing a semiconductor device according to one embodiment of the present invention relates to a method for manufacturing a semiconductor device including a step of forming a resin film (protective film) on a semiconductor wafer. The method for manufacturing a semiconductor device includes a resin film (protective film) forming step, a semiconductor chip manufacturing step with a resin film (protective film), and a resin film (protective film) sheet removing step. Figure 1 and Figure 2 This is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device.
[0027] <Resin film forming step>
[0028] In this process, a resin film 3 including a resin that is reduced in molecular weight by reacting with water (hereinafter, sometimes referred to as "resin A") is formed on the semiconductor wafer 1. Resin A is a resin that has the property of being reduced in molecular weight by reacting with water, thereby increasing its solubility in water. The resin film 3 can function as a protective film that prevents fine cuttings (chips) generated by cutting the semiconductor wafer from adhering to the circuit formation surface of the semiconductor wafer.
[0029] In one embodiment, the resin A may be a resin containing an ester bond and a basic functional group. The resin containing an ester bond and a basic functional group is a resin that undergoes a hydrolysis reaction of the ester bond in the presence of a basic functional group by reacting with water to reduce the molecular weight. The resin film 3 may be formed, for example, by curing the resin A or a composition containing the resin A, or by reacting and curing a precursor of the resin A.
[0030] Examples of the basic functional group in the resin A include -NH- and -NH2.
[0031] Resin A can be formed using a resin film forming material comprising the following compounds: compound A, which comprises two or more first groups and has an ester bond; and compound B, which comprises two or more second groups capable of forming a bond with the first group and can form a resin comprising an ester bond and a basic functional group by reacting with compound A.
[0032] Compound A may include an ester bond in the first group, and may include an ester bond as a functional group different from the first group. Examples of the first group in compound A include (meth)acryloyloxy; isocyanate; cyclic ether group (oxirane group (oxiranyl group, epoxy group), oxetanyl group (oxetanyl group), tetrahydrofuranyl group, tetrahydropyranyl group, etc.); ethylenically unsaturated group (C=C), etc. The number of the first group in the molecule of compound A1 is 2 or more, 3 or more, or 4 or more, and may be 10 or less, 8 or less, 6 or less, or 5 or less.
[0033] Compound A may be a compound comprising a linking group that links two or more first groups and these first groups. Regarding the linking group, for example, it may include a (poly)oxyalkylene group. As the (poly)oxyalkylene group, a (poly)oxyethylene group may be cited. The linking group may include at least one skeleton selected from the group consisting of a pentaerythritol skeleton, a trimethylolpropane skeleton, and an isocyanurate skeleton.
[0034] The molecular weight or number average molecular weight of compound A may be 150 or more, 500 or more, or 1000 or more, and may be 50000 or less, 10000 or less, or 2000 or less. In this specification, the "number average molecular weight" is a polystyrene conversion value obtained by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene.
[0035] Compound A may be a compound containing two first groups or a compound containing two (meth)acryloyloxy groups. When containing two first groups, the time required for resin A to dissolve in water tends to be longer than when containing two first groups.
[0036] The compound A including two (meth)acryloyloxy groups may include a structure represented by the following formula (a1).
[0037]
[0038] In formula (a1), R represents a hydrogen atom or a methyl group. 1 The number of carbon atoms in the alkylene group may be, for example, 2 or more, and may be 10 or less, 6 or less, 4 or less, or 3 or less. The alkylene group may be, for example, ethylene (-CH2-CH2-).
[0039] n represents an integer greater than or equal to 1. For example, n may be greater than or equal to 1, greater than or equal to 5, greater than or equal to 10, greater than or equal to 15, or greater than or equal to 20, and may be less than or equal to 50, less than or equal to 45, less than or equal to 40, less than or equal to 35, less than or equal to 30, or less than or equal to 25.
[0040] Examples of commercially available products of compound A containing two (meth)acryloyloxy groups include NK ester A-1000 (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #1000 diacrylate), A-600 (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #600 diacrylate), A-400 (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #400 diacrylate), A-200 (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #200 diacrylate), 2G (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: diethylene glycol dimethacrylate), 3G (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: diethylene glycol dimethacrylate), Co., Ltd., chemical name: triethylene glycol dimethacrylate), 4G (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #200 dimethacrylate), 9G (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #400 dimethacrylate), 14G (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #600 dimethacrylate), 23G (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #1000 dimethacrylate), Light Acrylate 3EGA (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: triethylene glycol dimethacrylate), Light Acrylate 4EG-A (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: polyethylene glycol #200 dimethacrylate), Light Acrylate 9EG-A (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: polyethylene glycol #400 diacrylate), Light Acrylate 14EG-A (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: polyethylene glycol #600 diacrylate), Light Acrylate EG (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: ethylene glycol dimethacrylate), Light Acrylate 2EG (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: ethylene glycol dimethacrylate),, chemical name: diethylene glycol dimethacrylate), light ester 3EG (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: triethylene glycol dimethacrylate), light ester 4EG (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: polyethylene glycol #200 dimethacrylate), light ester 9EG (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: polyethylene glycol #400 dimethacrylate), light ester 14EG (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: polyethylene glycol #600 dimethacrylate), FANCRYL FA-222A (manufactured by Showa Denko Materials Co., Ltd., chemical name: diethylene glycol diacrylate), FANCRYL FA-232A (manufactured by Showa Denko Materials Co., Ltd., chemical name: diethylene glycol diacrylate), FANCRYL FA-220A, FA-230A, FA-240A, FA-260A, FA-2100A and FA-2200A (all manufactured by Showa Denko Materials Co., Ltd., chemical name: polyethylene glycol diacrylate), FANCRYL FA-222M (manufactured by Showa Denko Materials Co., Ltd., chemical name: diethylene glycol dimethacrylate), FANCRYL FA-232M (manufactured by Showa Denko Materials Co., Ltd., chemical name: diethylene glycol dimethacrylate), and FANCRYL FA-220M, FA-230M, FA-240M, FA-260M, FA-2100M and FA-2200M (all manufactured by Showa Denko Materials Co., Ltd., chemical name: polyethylene glycol dimethacrylate). .
[0041] The compound A may be a compound containing three or more first groups, or may be a compound containing three or more (meth)acryloyloxy groups.
[0042] The compound A including three or more (meth)acryloyloxy groups may be, for example, a compound represented by the following formula (a2).
[0043]
[0044] In formula (a2), R represents a hydrogen atom or a methyl group, and X 2represents an alkylene group. a, b, c and d are each independent and represent an integer greater than or equal to 0 or 1. Multiple Rs may be the same or different. 2 The carbon number of the alkylene group represented by may be 2 or more, and may be 10 or less, 6 or less, or 3 or less. 2 The alkylene represented by X may be, for example, ethylene (-CH2-CH2-). 2 When there are multiple numbers, they may be the same or different. The total of a, b, c and d, a+b+c+d, may be, for example, 1 or more, 5 or more, 10 or more, 15 or more, 20 or more, 25 or more, or 30 or more, and may be 60 or less, 55 or less, 50 or less, 45 or less, or 40 or less.
[0045] Examples of commercially available products of compound A containing three or more (meth)acryloyloxy groups include NK ester ATM-35E (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated pentaerythritol tetraacrylate), NK ester A-TMPT-9EO (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated trimethylolpropane triacrylate), NK ester AT-20E (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated trimethylolpropane triacrylate), NK ester A-GLY-3E (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated glycerol triacrylate), NK ester A-GLY-9E (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated trimethylolpropane triacrylate). Co., Ltd., chemical name: ethoxylated glycerol triacrylate), NK ester A-GLY-20E (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated glycerol triacrylate) and A-DPH-12E (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated dipentaerythritol polyacrylate).
[0046] Compound A may be a compound showing solubility in water. The solubility of compound A in 100 g of water at 25° C. may be 1 g or more, 5 g or more, or 10 g or more. The upper limit of the solubility is not particularly limited.
[0047] The content of compound A may be 80 parts by mass or more, 85 parts by mass or more, or 90 parts by mass or more, and may be 99 parts by mass or less, 95 parts by mass or less, or 90 parts by mass or less, based on 100 parts by mass of the total content of compound A and compound B.
[0048] The second group in compound B is appropriately selected according to the type of the first group. Regarding the combination of the first group and the second group, for example, it can be a combination of at least one first group selected from the group consisting of a (meth)acryloyloxy group, an isocyanate group, a cyclic ether group (oxirane group (oxiranyl group, epoxy group), oxetane group (oxetanyl group), tetrahydrofuranyl group, tetrahydropyranyl group, etc.) and an ethylenically unsaturated group (C=C) and at least one second group selected from the group consisting of an amino group, a substituted amino group (for example, a monosubstituted amino group (-NH-)) and a mercapto group (-SH), or a combination of a (meth)acryloyloxy group and an amino group.
[0049] The number of the second groups in the compound B1 molecule is 2 or more, and may be 10 or less, 8 or less, 6 or less, 4 or less, or 3 or less, or 2. The number of the second groups in the compound B1 molecule may be the same as or different from the number of the first groups in the compound A1 molecule, or may be less than the number of the first groups in the compound A1 molecule.
[0050] Compound B may contain a functional group other than the second group. Examples of the functional group other than the second group include an alkylene group and -NH-(imino) group.
[0051] Compound B may be a compound containing two or more second groups and an alkylene group, a compound containing two or more second groups, an alkylene group, and -NH-, or a compound containing two or more amino groups, an alkylene group, and -NH-.
[0052] The compound B may be, for example, a compound represented by the following formula (b).
[0053] H2N—Y—NH2((b)
[0054] Y represents a divalent group including an alkylene group. The divalent group including an alkylene group represented by Y may include -NH-. As for compound B, for example, a compound represented by the following formula (b1) may be used.
[0055]
[0056] In formula (b), Z represents an alkylene group. The number of carbon atoms in the alkylene group may be 1 or more, 2 or more, or 3 or more, and may be 10 or less, 8 or less, 6 or less, or 4 or less.
[0057] Examples of compound B include bis(3-aminopropyl)amine, norbornanediamine, ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyetheramine, 4,4′-diaminodiphenyl sulfone, 3,3′-diaminodiphenyl sulfone, 4,4′-diaminodiphenyl ether, 1,3-bis(3-aminophenoxy)benzene, dianiline, aminobenzylamine, and polyoxypropylenediamine.
[0058] Compound B may be a compound showing solubility in water. The solubility of compound B in 100 g of water at 25° C. may be 1 g or more, 5 g or more, or 10 g or more. The upper limit of the solubility is not particularly limited.
[0059] The ratio (B / A) of the number of moles of the second group (e.g., amino group) in compound B to the number of moles of the first group (e.g., (meth)acryloyl group) in compound A may be 0.20 or more, 0.40 or more, 0.60 or more, 0.80 or more, or 1.00 or more. The ratio of the number of moles of compound B to the number of moles of compound A (the number of moles of compound B / the number of moles of compound A) may be, for example, 10.00 or less, 8.00 or less, 6.00 or less, 4.00 or less, 3.00 or less, 2.50 or less, or 2.20 or less.
[0060] The content of compound B may be 1 part by mass or more, 5 parts by mass or more, 8 parts by mass or more, or 10 parts by mass or more relative to 100 parts by mass of the total content of compound A and compound B. The content of compound B may be 20 parts by mass or less, 15 parts by mass or less, 10 parts by mass or less, or 8 parts by mass or less relative to 100 parts by mass of the total content of compound A and compound B.
[0061] The resin A, which is a reaction product of compound A and compound B, can be obtained by mixing or kneading these compounds. Mixing and kneading can be performed by appropriately combining a common disperser such as a stirrer, a pestle, a three-roll mill, a ball mill, or a bead mill.
[0062] The reaction may be carried out while heating as required. The reaction temperature when reacting compound A and compound B may be, for example, 0°C or more, 10°C or more, or 20°C or more, and may be 100°C or less, 85°C or less, or 70°C or less. The time for maintaining the reaction temperature may be, for example, 1.0 minute or more, and may be 60 minutes or less, 30 minutes or less, 10 minutes or less, 5 minutes or less, or 3 minutes or less.
[0063] The resin film 3 may further include components (other components) other than the resin A. As other components, for example, plasticizers; adhesiveness imparting agents such as tackifiers; antioxidants; leuco dyes; sensitizers; adhesion improvers such as coupling agents; polymerization inhibitors; light stabilizers; defoamers; fillers; chain transfer agents; thixotropy imparting agents; flame retardants; mold release agents; surfactants; lubricants; antistatic agents and other additives can be used for these additives. Known additives can be used. When the resin film 3 includes other components, the total amount of the content of the other components is based on the total amount of the resin film 3, and can be 0 to 95% by mass, 0.01 to 50% by mass, or 0.1 to 10% by mass.
[0064] Resin A can be diluted with an organic solvent and used as a varnish. Examples of the organic solvent include aromatic hydrocarbons such as toluene, xylene, mesitylene, cumene, and p-cymene; aliphatic hydrocarbons such as hexane and heptane; cycloalkanes such as methylcyclohexane; cyclic ethers such as tetrahydrofuran and 1,4-dioxane; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and 4-hydroxy-4-methyl-2-pentanone; esters such as methyl acetate, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, and γ-butyrolactone; carbonates such as ethylene carbonate and propylene carbonate; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone (NMP). The solid content in the varnish, that is, the content other than the organic solvent in the varnish, can be 10 to 95% by mass, 15 to 70% by mass, or 20 to 50% by mass based on the total amount of the varnish.
[0065] The resin film forming step may include, for example, a step of preparing the semiconductor wafer 1 (see Figure 1 (a)); and forming a resin film 3 comprising a resin A on a semiconductor wafer 1 (reference Figure 1 (b)).
[0066] Examples of the semiconductor wafer 1 include single crystal silicon, polycrystalline silicon, various ceramics, and compound semiconductors such as gallium arsenide. The semiconductor wafer 1 may have a circuit formation surface.
[0067] The thickness of the semiconductor wafer 1 may be, for example, 10 to 1000 μm, 20 to 900 μm, or 30 to 800 μm.
[0068] As a method for forming a resin film on a semiconductor wafer, for example, a method including the following steps can be used: applying resin A or a composition containing resin A on a semiconductor wafer by spin coating, slit coating, etc.; and forming a resin film by curing the applied resin A or the composition containing resin A. The resin film can be arranged on a circuit formation surface on a semiconductor wafer, for example. The resin can be cured at room temperature.
[0069] As a method for forming a resin film on a semiconductor wafer, a method comprising the following steps can also be used: placing a curable composition comprising resin A or a precursor of resin A on a semiconductor wafer; and curing the curable composition placed on the semiconductor wafer. As a method for placing a curable composition on a semiconductor wafer, a method of laminating or stacking the curable composition can be cited. The laminating or stacking method of the curable composition can be carried out under heating or at room temperature. Regarding the precursor of resin A, for example, it can be a mixture of compounds that react by heating or the like to form resin A.
[0070] As a method for forming a resin film on a semiconductor wafer, for example, a method including the following steps can also be used: a step of disposing a curable composition on a substrate to form a curable composition layer; a step of heating the substrate and the curable composition layer to cure the curable composition layer, and forming a resin film containing a cured product of the curable composition on the substrate to produce a first laminate having a substrate and a resin film; a step of laminating or stacking the semiconductor wafer and the first laminate in a manner that the semiconductor wafer and the resin film are in contact during heating or at room temperature to produce a second laminate having a semiconductor wafer, a resin film and a substrate in sequence; and a step of peeling the substrate from the second laminate to produce a third laminate having a semiconductor wafer and a resin film. The curing of the curable composition before laminating or stacking can be in a semi-cured state without being completely cured, and completely cured after laminating or stacking.
[0071] The thickness of the resin film 3 may be, for example, 1 to 1000 μm, 3 to 500 μm, or 5 to 200 μm.
[0072] In this way, the resin film 3 including the resin A can be formed on the semiconductor wafer 1 .
[0073] <Process for manufacturing semiconductor chips with resin films>
[0074] In this step, the semiconductor wafer 1 on which the resin film 3 is formed is diced by a dicing blade 9 to produce individual semiconductor chips 7 with resin film sheets.
[0075] The process of manufacturing a semiconductor chip with a resin film sheet may include, for example, a step of preparing a laminate 10 having a dicing tape 5, a semiconductor wafer 1, and a resin film 3 in this order (see Figure 1 and in the laminate 10, at least the semiconductor wafer 1 and the resin film 3 are cut by a dicing blade 9 to obtain a single-piece semiconductor chip 7 with a resin film (reference Figure 1 (d)).
[0076] As the dicing tape 5, for example, plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, polyimide film, etc. can be cited. The dicing tape 5 can also be subjected to surface treatments such as primer coating, UV treatment, corona discharge treatment, grinding treatment, etching treatment, etc. as needed. The dicing tape 5 can have adhesiveness. This dicing tape 5 can impart adhesiveness to the above-mentioned plastic film, or it can be a dicing tape with a pressure-sensitive adhesive layer provided on one side of the above-mentioned plastic film. The pressure-sensitive adhesive layer can be formed by a UV-curable or UV-non-curable pressure-sensitive pressure-sensitive adhesive, and there is no particular limitation as long as it has sufficient adhesive force to prevent the semiconductor elements from flying apart during dicing, and a previously known pressure-sensitive adhesive layer can be used.
[0077] The thickness of the dicing tape 5 may be, for example, 10 to 1000 μm, 30 to 500 μm, or 50 to 300 μm.
[0078] The laminated body 10 can be obtained by attaching the dicing tape 5 to the semiconductor wafer 1 on which the resin film 3 is formed.
[0079] Next, in the stacked body 10, at least the semiconductor wafer 1 and the resin film 3 (and a portion of the dicing tape 5) are cut by a dicing blade 9 and are separated into individual pieces. The dicing by the dicing blade 9 can be performed using a commercially available device. The dicing by the dicing blade 9 is performed, for example, in a grating-shaped dicing pattern in a plan view on the semiconductor wafer 1 and the resin film 3.
[0080] From the viewpoint of suppressing the temperature rise of the contact portion between the semiconductor wafer 1 or the resin film 3 and the dicing blade 9, the dicing by the dicing blade 9 can be performed while spraying cooling water (cutting water) on these contact portions. This further suppresses the cutting material (chips) from adhering to the circuit formation surface of the semiconductor wafer.
[0081] In this manner, the semiconductor wafer 1 and the resin film 3 can be singulated separately to obtain the semiconductor chip 7 with the resin film sheet including the semiconductor chip 1 a and the resin film sheet 3 a .
[0082] The shape of the semiconductor chip 1a in plan view may be, for example, a square or a rectangle. The area of the semiconductor chip 1a may be, for example, 1 to 250 mm. 2 , 4~200mm 2 , or 9~150mm 2 The length of one side of the semiconductor chip 1 a may be greater than 1 mm, greater than 2 mm, or greater than 3 mm, and may be less than 20 mm, less than 18 mm, or less than 15 mm. The thickness of the semiconductor chip 1 a may be the same as the thickness of the semiconductor wafer 1 .
[0083] <Resin film removal process>
[0084] In this process, the resin in the resin film sheet 3a of the semiconductor chip with resin film 7 is reacted with water to remove the resin film sheet 3a from the semiconductor chip with resin film 7. From the viewpoint of reducing the molecular weight by reacting with water and thus improving the solubility in water, the resin A contained in the resin film sheet 3a can easily remove the resin film sheet 3a from the semiconductor chip with resin film 7 by water.
[0085] In one embodiment, the resin film sheet removal step may be a step of removing the resin film sheet 3a from the semiconductor chip 7 with the resin film sheet using an aqueous solvent. The resin A contained in the resin film sheet 3a can be reduced in molecular weight by reacting with water, thereby increasing its solubility in the aqueous solvent. Therefore, the resin film sheet 3a can be fully removed by washing with an aqueous solvent.
[0086] Examples of the aqueous solvent include water, a mixed solvent of water and a hydrophilic organic solvent, etc. In the mixed solvent of water and a hydrophilic organic solvent, the proportion of water can be, for example, 80% by mass or more. For example, a pH adjuster can be added to the aqueous solvent.
[0087] The aqueous solvent can be water. As water, for example, tap water, natural water, purified water, distilled water, ion exchanged water, pure water and ultrapure water (Milli-Q water, etc.) can be cited. Milli-Q water refers to ultrapure water obtained by the Milli-Q water manufacturing device of Merck Millipore (Merck KGaA). From the viewpoint of impurity reduction, water can be purified water, distilled water, ion exchanged water, pure water, or ultrapure water.
[0088] Examples of the hydrophilic organic solvent include alcohols such as methanol, ethanol, 2-propanol, and 1,2-propylene glycol; and glycol ethers such as ethylene glycol monomethyl ether, propylene glycol monomethyl ether, ethyl cellosolve, propylene glycol monopropyl ether, propylene glycol monoisopropyl ether, butyl cellosolve, ethylene glycol monoisobutyl ether, propylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, and dipropylene glycol monomethyl ether.
[0089] As the pH adjusting agent, inorganic acids, inorganic bases, organic acids, organic bases, etc. can be mentioned. As inorganic acids, nitric acid, sulfuric acid, hydrochloric acid, phosphoric acid, boric acid, etc. can be mentioned. As inorganic bases, sodium hydroxide, potassium hydroxide, calcium hydroxide, etc. can be mentioned. As organic acids, formic acid, acetic acid, propionic acid, butyric acid, acrylic acid, benzoic acid, picolinic acid, etc. can be mentioned. As organic bases, primary amines, secondary amines, tertiary amines, tetramethylammonium hydroxide, tetraethylammonium hydroxide, imidazole compounds, etc. can be mentioned.
[0090] The temperature of the water used to react the resin with water may be, for example, 5°C or higher, 10°C or higher, 15°C or higher, 20°C or higher, 25°C or higher, 35°C or higher, 45°C or higher, or 55°C or higher, and may be 80°C or lower, or 70°C or lower. By adjusting the temperature of the water used to react the resin with water, the time required for the resin film to dissolve in the water can be adjusted. By increasing the temperature of the water used to react the resin with water, the resin film tends to dissolve in the water in a shorter time.
[0091] The time for reacting the resin with water (the time for keeping the water at the temperature of the water) may be, for example, 5 minutes or more, 10 minutes or more, or 15 minutes or more, and 150 minutes or less or 120 minutes or less. The time for reacting the resin with water (the time for keeping the water at the temperature of the water) may be 15 to 120 minutes.
[0092] In one embodiment, the resin film removal step may be a step of immersing the resin film 3a of the semiconductor chip 7 with the resin film in an aqueous solvent 11 (see Figure 2 (a)) The resin contained in the resin film 3a can be reduced in molecular weight by reacting with water, thereby flowing out in the aqueous solvent 11, and the resin film 3a can be removed efficiently.
[0093] In this manner, a plurality of semiconductor chips 1a (see FIG. 1 ) in which adhesion of cut materials (chips) is sufficiently suppressed can be obtained from the semiconductor wafer 1. Figure 2 (b)).
[0094] The manufacturing method of the semiconductor device of the present embodiment may further include: an ultraviolet irradiation process of irradiating ultraviolet rays to the pressure-sensitive adhesive layer of the dicing tape 5; a picking up process of picking up the semiconductor chip 1a; a semiconductor chip bonding process of bonding the picked up semiconductor chip 1a and the supporting component 13 by thermal compression bonding via an adhesive layer 15 (grain bonding film, etc.); and a thermal curing process of thermally curing the adhesive layer 15, etc.
[0095] <Ultraviolet irradiation process>
[0096] When the pressure-sensitive adhesive layer of the dicing tape 5 is composed of a UV-curable pressure-sensitive adhesive, the method for manufacturing the semiconductor device may include an ultraviolet irradiation step. In this step, the pressure-sensitive adhesive layer is irradiated with ultraviolet rays. In the ultraviolet irradiation, the wavelength of the ultraviolet rays may be 200 to 400 nm. In the ultraviolet irradiation conditions, the illumination and the irradiation amount may be 30 to 240 mW / cm 2 The range is 50~500mJ / cm 2 range.
[0097] <Pick-up process>
[0098] In this step, the individualized semiconductor chips 1 a are separated from each other, and the semiconductor chips 1 a pushed up from the dicing tape 5 side by the needles are sucked by a suction chuck and picked up from the dicing tape 5 .
[0099] The ultraviolet irradiation step and the pickup step may be performed after the resin film sheet removal step or may be performed before the resin film sheet removal step.
[0100] <Semiconductor chip bonding process>
[0101] In this step, the picked-up semiconductor chip 1a and the support member 13 are bonded by thermocompression via an adhesive layer 15 (die bonding film, etc.). The die bonding film can be a die bonding film used in this field. A plurality of semiconductor chips 1a can be bonded to the support member 13.
[0102] The heating temperature during the thermocompression bonding may be, for example, 80 to 160° C. The load during the thermocompression bonding may be, for example, 5 to 15 N. The heating time during the thermocompression bonding may be, for example, 0.5 to 20 seconds.
[0103] <Thermosetting process>
[0104] In this step, the adhesive layer 15 is thermally cured. The heating temperature can be appropriately changed according to the constituent components of the die bonding film. The heating temperature can be, for example, 60 to 200° C., 90 to 190° C., or 120 to 180° C. The heating time can be 30 minutes to 5 hours, 1 to 3 hours, or 2 to 3 hours. The temperature or pressure can be changed in stages.
[0105] In this manner, a semiconductor device 20 including a semiconductor chip 1a, a support member 13 on which the semiconductor chip 1a is mounted, and an adhesive layer 15 provided between the semiconductor chip 1a and the support member 13 for bonding the semiconductor chip 1a and the support member 13 can be manufactured (see Figure 2 (c)).
[0106] Explanation of symbols
[0107] 1-semiconductor wafer, 1a-semiconductor chip, 3-resin film, 3a-resin film sheet, 5-dicing tape, 7-semiconductor chip with resin film sheet, 9-dicing blade, 10-laminated body, 11-aqueous solvent, 13-support member, 15-adhesive layer, 20-semiconductor device.
Claims
1. A method for manufacturing a semiconductor device, comprising: a resin film forming step of forming a resin film including a resin reduced in molecular weight by reaction with water on the semiconductor wafer; a step of manufacturing a semiconductor chip with a resin film, wherein the semiconductor wafer with the resin film formed thereon is diced with a dicing blade to thereby manufacture individual semiconductor chips with a resin film; and The resin film sheet removing step causes the resin in the resin film sheet of the semiconductor chip with the resin film sheet to react with water, thereby removing the resin film sheet from the semiconductor chip with the resin film sheet.
2. The method for manufacturing a semiconductor device according to claim 1, in, The resin film removal step is performed by immersing the resin film of the semiconductor chip with the resin film in water.
Citation Information
Patent Citations
Composition for forming protective film of electronic component
JP2014172932A
Protective film substrate for dicing, protective film composition for dicing, protective sheet for dicing, and method for producing wafer to be processed