By introducing amino silicone oil and aromatic ring modification during the preparation of silica aerogel, a multi-crosslinked structure is formed, which solves the problem of structural instability of silica aerogel under high temperature environment, improves its high temperature resistance, thermal insulation and mechanical properties, and expands its application range.

CN119100405BActive Publication Date: 2026-11-17JIANGSU YUAN NING NEW MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411402210.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2026-11-17
Estimated Expiration
2044-10-09

AI Technical Summary

Technical Problem

Existing silica aerogels are prone to damage to their nanoporous structure under high-temperature conditions, leading to performance degradation and shortened lifespan, which limits their application in high-temperature environments.

Method used

Amino silicone oil was introduced into the silica aerogel preparation process to participate in the condensation reaction, forming an amino-modified wet gel. The gel was then modified with trimethylchlorosilane solution and aromatic ring-terminated isocyanate group compound solution to form hydrophobic silicon-oxygen bonds and urea bonds, thereby enhancing the thermal and chemical stability of the material.

Benefits of technology

It significantly improves the high temperature resistance, thermal insulation and mechanical properties of silica aerogel, meeting the requirements for use in specific high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119100405B_ABST
    Figure CN119100405B_ABST
Patent Text Reader

Abstract

This invention relates to a silica aerogel thermal insulation composite material and its preparation method, belonging to the technical field of silica aerogel composite materials. The preparation method includes the following steps: acidic hydrolysis of a silicon source, anhydrous ethanol, and water to obtain a hydrolysate; adjusting the pH of the hydrolysate to neutral using ammonia and adding amino silicone oil, then further adjusting the pH to alkaline to carry out a condensation reaction to obtain a wet gel; aging the wet gel, replacing it with anhydrous ethanol, and then placing it in a trimethylchlorosilane solution for a first modification to obtain a first wet gel; placing the first wet gel in a solution of an aromatic ring-terminated isocyanate compound for a second modification to obtain a second wet gel, etc. The silica aerogel thermal insulation composite material provided by this invention has excellent high-temperature resistance, thermal insulation performance, and mechanical properties, which can meet the application requirements in certain specific high-temperature environments and make up for the shortcomings of existing silica aerogels.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of thermal insulation materials technology, and in particular to a silica aerogel thermal insulation composite material and its preparation method. Background Technology

[0002] Silica aerogels, with their unique nanoporous structure, exhibit excellent thermal insulation properties and lightweight characteristics, making them widely applicable in various high-tech and consumer fields such as aerospace, building insulation, and new energy. Currently, the sol-gel method is the mainstream technology for preparing silica aerogels. This process involves a series of meticulous steps, starting with the selection of precursors (such as methyl orthosilicate, tetraethyl orthosilicate, and other silanolates), followed by hydrolysis and condensation reactions to form a wet gel, and then aging, washing, displacement, and drying, ultimately yielding high-performance silica aerogel products.

[0003] However, while existing silica aerogels exhibit remarkable performance at room temperature, their performance often deteriorates significantly at high temperatures, severely limiting their application in certain high-temperature fields. Specifically, under high-temperature conditions, the nanoporous structure of existing silica aerogels is easily damaged, resulting in a generally high average linear shrinkage rate. This structural instability not only affects the material's properties such as thermal insulation but also shortens its lifespan. This, to some extent, hinders the further application and promotion of silica aerogels in higher-temperature and harsher environments.

[0004] Therefore, in order to address the above problems, it is particularly important to develop a silica aerogel thermal insulation composite material with excellent high-temperature resistance, thermal stability and thermal insulation properties. This is of great significance for promoting the advancement of silica aerogel technology and expanding its application fields. Summary of the Invention

[0005] To address the above problems, this invention provides a silica aerogel thermal insulation composite material and its preparation method.

[0006] In a first aspect, the present invention provides a method for preparing a silica aerogel thermal insulation composite material, the method comprising the following steps:

[0007] Acidic hydrolysis reaction was carried out with silicon source, anhydrous ethanol and water to obtain hydrolysate;

[0008] The pH of the hydrolysate was adjusted to neutral using ammonia water, and amino silicone oil was added. The pH was then adjusted to alkaline to carry out a condensation reaction, resulting in a wet gel.

[0009] The wet gel was aged, replaced with anhydrous ethanol, and then placed in a trimethylchlorosilane solution for the first modification to obtain the first wet gel.

[0010] The first wet gel was placed in a solution of a compound containing an aromatic ring-terminated isocyanate group for a second modification to obtain a second wet gel;

[0011] The second wet gel was washed in anhydrous ethanol and then dried to obtain the silica aerogel thermal insulation composite material.

[0012] Furthermore, the operating conditions of the acidic hydrolysis reaction include: the molar ratio of the silicon source, the anhydrous ethanol, and the water is (1-2):(10-17):(3-7); the pH of the acidic hydrolysis reaction is adjusted to 2-4 using an acid, which includes oxalic acid; the acidic hydrolysis reaction time is 2-3 hours; and the pH of the condensation reaction is 9-10.

[0013] Furthermore, the molar ratio of the silicon source to the amino silicone oil is 1:(1-2).

[0014] Furthermore, the preparation method of the amino silicone oil includes the following steps:

[0015] Hydroxyl-terminated silicone oil, amino coupling agent, and alkaline catalyst in a molar ratio of (2-2.3):1:(0.01-0.05) were stirred evenly, and then the mixture was stirred at a constant temperature of 80-85℃ for 2-3 hours to obtain a mixture.

[0016] The mixture is heated to 105–110°C, then vacuumed. When the viscosity of the system is 4–6 × 10⁻⁶... 3 Stop vacuuming at mPa·s, cool to room temperature, and obtain the amino silicone oil;

[0017] The hydroxyl-terminated silicone oil includes WS62M from Wacker Chemie AG, Germany; the amino coupling agent is N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane; and the alkaline catalyst includes potassium hydroxide.

[0018] Furthermore, the silicon source includes at least one of methyl orthosilicate and ethyl orthosilicate; the aromatic ring-terminated isocyanate compound includes at least one of toluene diisocyanate, diphenylmethane diisocyanate and naphthyl diisocyanate.

[0019] Furthermore, the properties of the trimethylchlorosilane solution include: the solvent is n-hexane, and the volume ratio of the trimethylchlorosilane to the n-hexane is 1:(5-10); the properties of the aromatic ring-terminated isocyanate compound solution include: the solvent is n-hexane, and the mass-volume ratio of the aromatic ring-terminated isocyanate compound to the n-hexane is (10-20):1, expressed in g / L.

[0020] Further, the working conditions for the first modification include: a weight ratio of the wet gel to the trimethylchlorosilane solution of 1:(10-20) in g / mL, a temperature of 30-40°C, and a time of 1-2 hours; the working conditions for the second modification include: a weight ratio of the first wet gel to the terminal isocyanate compound solution of 1:(20-30) in g / mL, a temperature of 30-40°C, and a time of 60-90 minutes.

[0021] Furthermore, the aging working conditions parameters include: a temperature of 45–55°C and a time of 35–55 hours; the drying method includes atmospheric pressure drying.

[0022] In a second aspect, the present invention provides a silica aerogel thermal insulation composite material, wherein the silica aerogel thermal insulation composite material is prepared by the preparation method of the silica aerogel thermal insulation composite material described in any one of the first aspects.

[0023] The technical solutions provided in the embodiments of the present invention have at least the following advantages compared with the prior art:

[0024] This invention provides a silica aerogel thermal insulation composite material and its preparation method. The silica aerogel thermal insulation composite material of this invention introduces amino silicone oil into the silica aerogel preparation process to participate in the condensation reaction, obtaining an amino-modified silica wet gel. Subsequently, it undergoes a first modification in a trimethylchlorosilane solution, where trimethylchlorosilane reacts with the hydroxyl groups on the gel surface to form hydrophobic silicon-oxygen bonds, improving the material's hydrophobicity and chemical stability. A second modification is then performed in a solution of a compound containing aromatic ring-terminated isocyanate groups, where the amino groups react rapidly with the terminal isocyanate groups to form urea bonds, introducing an aromatic ring structure and further enhancing the material's thermal stability. Finally, a multi-crosslinked silica aerogel thermal insulation composite material is obtained, significantly improving its high-temperature resistance, thermal insulation performance, and mechanical properties, thereby meeting the application requirements in certain specific high-temperature environments and overcoming the shortcomings of existing silica aerogels. Attached Figure Description

[0025] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0026] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0027] Figure 1 This is a schematic flowchart illustrating a method for preparing a silica aerogel thermal insulation composite material according to an embodiment of the present invention. Detailed Implementation

[0028] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0029] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.

[0030] In a first aspect, the present invention provides a method for preparing a silica aerogel thermal insulation composite material, such as... Figure 1 As shown, the preparation method includes the following steps:

[0031] Acidic hydrolysis reaction was carried out with silicon source, anhydrous ethanol and water to obtain hydrolysate;

[0032] The pH of the hydrolysate was adjusted to neutral using ammonia water, and amino silicone oil was added. The pH was then adjusted to alkaline to carry out a condensation reaction, resulting in a wet gel.

[0033] The wet gel was aged, replaced with anhydrous ethanol, and then placed in a trimethylchlorosilane solution for the first modification to obtain the first wet gel.

[0034] The first wet gel was placed in a solution of a compound containing an aromatic ring-terminated isocyanate group for a second modification to obtain a second wet gel;

[0035] The second wet gel was washed in anhydrous ethanol and then dried to obtain the silica aerogel thermal insulation composite material.

[0036] This invention provides a method for preparing a silica aerogel thermal insulation composite material. During the silica aerogel preparation process, amino silicone oil is introduced to participate in the condensation reaction, obtaining an amino-modified silica wet gel. Subsequently, a first modification is performed in a trimethylchlorosilane solution, where trimethylchlorosilane reacts with the hydroxyl groups on the gel surface to form hydrophobic silicon-oxygen bonds, improving the material's hydrophobicity and chemical stability. A second modification is then performed in a solution of a compound containing aromatic ring-terminated isocyanate groups, where the amino group reacts rapidly with the terminal isocyanate group to form urea bonds, introducing an aromatic ring structure and further enhancing the material's thermal stability. Finally, a multi-crosslinked silica aerogel thermal insulation composite material is obtained, significantly improving its high-temperature resistance, thermal insulation performance, and mechanical properties, thereby meeting the application requirements in certain specific high-temperature environments and overcoming the shortcomings of existing silica aerogels.

[0037] In some specific embodiments, the concentration of the ammonia water is 20-30% by volume percentage.

[0038] In some specific embodiments, the operating conditions of the acidic hydrolysis reaction include: the molar ratio of the silicon source, the anhydrous ethanol, and the water is (1-2):(10-17):(3-7); the pH of the acidic hydrolysis reaction is adjusted to 2-4 using acid, the acid including oxalic acid, and the molar concentration of the oxalic acid is 0.1-5 mol / L; the acidic hydrolysis reaction time is 2-3 hours; and the pH of the condensation reaction is 9-10.

[0039] In some specific embodiments, the molar ratio of the silicon source and the amino silicone oil is 1:(1-2), preferably 1:1.5.

[0040] In some specific embodiments, the preparation method of the amino silicone oil includes the following steps:

[0041] Hydroxyl-terminated silicone oil, amino coupling agent, and alkaline catalyst in a molar ratio of (2-2.3):1:(0.01-0.05) were stirred evenly, and then the mixture was stirred at a constant temperature of 80-85℃ for 2-3 hours to obtain a mixture.

[0042] The mixture is heated to 105–110°C, then vacuumed. When the viscosity of the system is 4–6 × 10⁻⁶... 3 Stop vacuuming at mPa·s, cool to room temperature, and obtain the amino silicone oil;

[0043] The hydroxyl-terminated silicone oil includes WS62M from Wacker Chemie AG, Germany; the amino coupling agent is N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane; and the alkaline catalyst includes potassium hydroxide.

[0044] In some specific embodiments, the silicon source includes at least one of methyl orthosilicate and ethyl orthosilicate; the aromatic ring-terminated isocyanate compound includes at least one of toluene diisocyanate, diphenylmethane diisocyanate and naphthyl diisocyanate.

[0045] In some specific embodiments, the property parameters of the trimethylchlorosilane solution include: the solvent is n-hexane, and the volume ratio of the trimethylchlorosilane to the n-hexane is 1:(5-10); the property parameters of the aromatic ring-terminated isocyanate compound solution include: the solvent is n-hexane, and the mass-volume ratio of the aromatic ring-terminated isocyanate compound to the n-hexane is (10-20):1, calculated in g / L.

[0046] In some specific embodiments, the working conditions for the first modification include: a weight ratio of the wet gel to the trimethylchlorosilane solution of 1:(10-20) in g / mL, a temperature of 30-40°C, and a time of 1-2 hours; the working conditions for the second modification include: a weight ratio of the first wet gel to the terminal isocyanate compound solution of 1:(20-30) in g / mL, a temperature of 30-40°C, and a time of 60-90 minutes.

[0047] In some specific embodiments, the aging working conditions parameters include: a temperature of 45-55°C and a time of 35-55 hours; the drying method includes atmospheric pressure drying.

[0048] Secondly, based on the same inventive concept, the present invention provides a silica aerogel thermal insulation composite material, which is prepared by the preparation method of silica aerogel thermal insulation composite material described in any one of the first aspects.

[0049] The silica aerogel thermal insulation composite material provided in this embodiment of the invention is achieved based on the preparation method of the silica aerogel thermal insulation composite material according to any one of the first aspects, and therefore has at least the beneficial effects of the silica aerogel thermal insulation composite material according to any one of the first aspects, which will not be elaborated here.

[0050] It should be noted that, unless otherwise specified or described, the raw materials involved in the silica aerogel thermal insulation composite material and its preparation method provided in the embodiments of the present invention can be directly made from commercially available products or by using existing publicly disclosed preparation methods; at the same time, unless otherwise specified or described, the steps and parameters involved can be carried out according to the existing processing technology of silica aerogel thermal insulation composite material or directly using existing equipment, and will not be described in detail in this document.

[0051] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Experimental methods in the following embodiments, unless otherwise specified, are generally performed according to national standards. If no corresponding national standard exists, then generally accepted international standards, conventional conditions, or conditions recommended by the manufacturer are followed.

[0052] Example 1

[0053] This example provides a silica aerogel thermal insulation composite material, the preparation method of which includes the following steps:

[0054] Step (1): Acidic hydrolysis reaction is carried out on silicon source, anhydrous ethanol and water to obtain hydrolysate; wherein, the silicon source is methyl orthosilicate; the working conditions of the acidic hydrolysis reaction include: the molar ratio of silicon source, anhydrous ethanol and water is 1.5:14:5, the pH of the acidic hydrolysis reaction is adjusted to 2.6 using acid, the acid is oxalic acid, and the acidic hydrolysis reaction time is 2.5 hours;

[0055] Step (2): Adjust the pH of the hydrolysate obtained in step (1) to neutral using ammonia and add amino silicone oil. Then, continue to adjust the pH to 9 to carry out a condensation reaction to obtain a wet gel. The preparation method of the amino silicone oil includes the following process: stirring the terminal hydroxyl silicone oil, amino coupling agent and alkaline catalyst in a molar ratio of 2.1:1:0.03 evenly, and then stirring at 82°C for 2.5 hours to obtain a mixture; heating the mixture to 108°C and then vacuuming it. When the viscosity of the system is 5×10⁻⁶, the mixture is then heated to 108°C and vacuumed. 3 The vacuum was stopped at mPa·s, and the mixture was cooled to room temperature to obtain the amino silicone oil. The hydroxyl-terminated silicone oil included WS62M from Wacker Chemie AG, Germany. The amino coupling agent was N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane. The alkaline catalyst was potassium hydroxide. The molar ratio of the silicon source to the amino silicone oil was 1:1.5.

[0056] Step (3): The wet gel obtained in step (2) is aged at 50°C for 40 hours and replaced twice with anhydrous ethanol. Then, it is placed in a trimethylchlorosilane solution for the first modification to obtain the first wet gel. The properties of the trimethylchlorosilane solution include: the solvent is n-hexane, and the volume ratio of trimethylchlorosilane to n-hexane is 1:10. The working conditions of the first modification include: the weight ratio of the wet gel to the trimethylchlorosilane solution is 1:15 (g / mL), the temperature is 35°C, and the time is 1.5 hours.

[0057] Step (4): The first wet gel obtained in step (3) is placed in a solution of a compound containing an aromatic ring terminal isocyanate group for a second modification to obtain a second wet gel; wherein, the property parameters of the compound containing an aromatic ring terminal isocyanate group include: the solvent is n-hexane, and the mass-volume ratio of the compound containing an aromatic ring terminal isocyanate group to the n-hexane is 15:1, and the compound containing an aromatic ring terminal isocyanate group is naphthyl diisocyanate; the working conditions parameters of the second modification include: the mass-volume ratio of the first wet gel to the compound containing terminal isocyanate group is 1:25, the temperature is 35℃, and the time is 75 minutes;

[0058] Step (5): The second wet gel obtained in step (4) is washed in anhydrous ethanol and then dried at 65°C under normal pressure for 24 hours to obtain the silica aerogel thermal insulation composite material.

[0059] Example 2

[0060] This example provides a silica aerogel thermal insulation composite material, the preparation method of which includes the following steps:

[0061] Step (1): Acidic hydrolysis reaction is carried out on silicon source, anhydrous ethanol and water to obtain hydrolysate; wherein, the silicon source is tetraethyl orthosilicate; the working conditions of the acidic hydrolysis reaction include: the molar ratio of silicon source, anhydrous ethanol and water is 2:17:7, the pH of the acidic hydrolysis reaction is adjusted to 2.2 by acid, the acid is oxalic acid, and the acidic hydrolysis reaction time is 2 hours;

[0062] Step (2): Adjust the pH of the hydrolysate obtained in step (1) to neutral using ammonia and add amino silicone oil. Then, continue to adjust the pH to 9 to carry out a condensation reaction to obtain a wet gel. The preparation method of the amino silicone oil includes the following process: stirring the terminal hydroxyl silicone oil, amino coupling agent and alkaline catalyst in a molar ratio of 2.3:1:0.05 evenly, and then stirring at 80°C for 3 hours to obtain a mixture; heating the mixture to 108°C and then vacuuming it. When the viscosity of the system is 4×10 3 The vacuum was stopped at mPa·s, and the mixture was cooled to room temperature to obtain the amino silicone oil. The hydroxyl-terminated silicone oil included WS62M from Wacker Chemie AG, Germany. The amino coupling agent was N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane. The alkaline catalyst was potassium hydroxide. The molar ratio of the silicon source to the amino silicone oil was 1:1.

[0063] Step (3): The wet gel obtained in step (2) is aged at 50°C for 40 hours and replaced twice with anhydrous ethanol. Then, it is placed in a trimethylchlorosilane solution for the first modification to obtain the first wet gel. The properties of the trimethylchlorosilane solution include: the solvent is n-hexane, and the volume ratio of trimethylchlorosilane to n-hexane is 1:5. The working conditions of the first modification include: the weight ratio of the wet gel to the trimethylchlorosilane solution is 1:10 (g / mL), the temperature is 30°C, and the time is 2 hours.

[0064] Step (4): The first wet gel obtained in step (3) is placed in a solution of a compound containing an aromatic ring terminal isocyanate group for a second modification to obtain a second wet gel; wherein, the property parameters of the compound containing an aromatic ring terminal isocyanate group include: the solvent is n-hexane, and the mass-volume ratio of the compound containing an aromatic ring terminal isocyanate group to the n-hexane is 10:1, and the compound containing an aromatic ring terminal isocyanate group is toluene diisocyanate; the working conditions parameters of the second modification include: the mass-volume ratio of the first wet gel to the compound containing the terminal isocyanate group is 1:25, the temperature is 35℃, and the time is 75 minutes;

[0065] Step (5): The second wet gel obtained in step (4) is washed in anhydrous ethanol and then dried at 65°C under normal pressure for 24 hours to obtain the silica aerogel thermal insulation composite material.

[0066] Example 3

[0067] This example provides a silica aerogel thermal insulation composite material, the preparation method of which includes the following steps:

[0068] Step (1): Acidic hydrolysis reaction is carried out on silicon source, anhydrous ethanol and water to obtain hydrolysate; wherein, the silicon source is tetraethyl orthosilicate; the working conditions of the acidic hydrolysis reaction include: the molar ratio of silicon source, anhydrous ethanol and water is 1:10:3, the pH of the acidic hydrolysis reaction is adjusted to 2.8 using acid, the acid is oxalic acid, and the acidic hydrolysis reaction time is 3 hours;

[0069] Step (2): Adjust the pH of the hydrolysate obtained in step (1) to neutral using ammonia and add amino silicone oil. Then, continue to adjust the pH to 9 to carry out a condensation reaction to obtain a wet gel. The preparation method of the amino silicone oil includes the following process: stirring the terminal hydroxyl silicone oil, amino coupling agent and alkaline catalyst in a molar ratio of 2.3:1:0.05 evenly, and then stirring at 80°C for 3 hours to obtain a mixture; heating the mixture to 108°C and then vacuuming it. When the viscosity of the system is 6×103 The vacuum was stopped at mPa·s, and the mixture was cooled to room temperature to obtain the amino silicone oil. The hydroxyl-terminated silicone oil included WS62M from Wacker Chemie AG, Germany. The amino coupling agent was N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane. The alkaline catalyst was potassium hydroxide. The molar ratio of the silicon source to the amino silicone oil was 1:1.

[0070] Step (3): The wet gel obtained in step (2) is aged at 50°C for 40 hours and replaced twice with anhydrous ethanol. Then, it is placed in a trimethylchlorosilane solution for the first modification to obtain the first wet gel. The properties of the trimethylchlorosilane solution include: the solvent is n-hexane, and the volume ratio of trimethylchlorosilane to n-hexane is 1:5. The working conditions of the first modification include: the weight ratio of the wet gel to the trimethylchlorosilane solution is 1:10 (g / mL), the temperature is 30°C, and the time is 2 hours.

[0071] Step (4): The first wet gel obtained in step (3) is placed in a solution of a compound containing an aromatic ring terminal isocyanate group for a second modification to obtain a second wet gel; wherein, the property parameters of the compound containing an aromatic ring terminal isocyanate group solution include: the solvent is n-hexane, and the mass-volume ratio of the compound containing an aromatic ring terminal isocyanate group to the n-hexane is 10:1, and the compound containing an aromatic ring terminal isocyanate group is diphenylmethane diisocyanate; the working conditions parameters of the second modification include: the mass-volume ratio of the first wet gel to the compound containing terminal isocyanate group solution is 1:25, the temperature is 35℃, and the time is 75 minutes;

[0072] Step (5): The second wet gel obtained in step (4) is washed in anhydrous ethanol and then dried at 65°C under normal pressure for 24 hours to obtain the silica aerogel thermal insulation composite material.

[0073] Comparative Example 1

[0074] This example provides a silica aerogel thermal insulation composite material and its preparation method. The only difference from Example 1 is that the aromatic ring-containing terminal isocyanate group compound is adjusted to a terminal isocyanate group compound whose side chain does not contain an aromatic ring (specifically, hexamethylene diisocyanate); the remaining steps and parameters are the same.

[0075] Comparative Example 2

[0076] This example provides a silica aerogel thermal insulation composite material and its preparation method. The only difference from Example 1 is that the amino coupling agent is changed to γ-piperazinylpropylmethyldimethoxysilane; the remaining steps and parameters are the same.

[0077] Test case

[0078] In this example, the performance of the silica aerogel thermal insulation composite materials obtained in Examples 1-3 and Comparative Examples 1-2 was tested.

[0079] High temperature resistance test method: The silica aerogel thermal insulation composite material sample was placed in a high temperature environment of 1000℃ for 2 hours. Then the average linear shrinkage rate (%) of the silica aerogel thermal insulation composite material sample was measured and calculated. The lower the average linear shrinkage rate (%), the better its high temperature resistance performance. The test results are shown in Table 1.

[0080] Table 1

[0081] Test sample Average linear shrinkage rate (%) Example 1 3.8 Example 2 9.1 Example 3 7.6 Comparative Example 1 27.4 Comparative Example 2 16.2

[0082] As shown in Table 1, compared with Comparative Examples 1 and 2, the silica aerogel thermal insulation composite material provided in the embodiments of the present invention has a lower average linear shrinkage rate (all below 10%) in an environment of 1000℃, with a minimum of 3.8%, and has excellent high-temperature stability.

[0083] In addition, the present invention also tested the thermal insulation performance and mechanical properties of the silica aerogel thermal insulation composite materials obtained in Examples 1 to 3, and the test results are shown in Table 2.

[0084] Table 2

[0085] Test sample Thermal conductivity (W / m·K) Compressive strength (MPa) Example 1 0.0138 0.98 Example 2 0.0146 0.79 Example 3 0.0143 0.84

[0086] As shown in Table 2, the silica aerogel thermal insulation composite material provided in the embodiments of the present invention has excellent thermal insulation and mechanical properties.

[0087] In summary, the embodiments of the present invention provide a silica aerogel thermal insulation composite material and its preparation method. During the preparation of silica aerogel, amino silicone oil is introduced to participate in the condensation reaction, obtaining an amino-modified silica wet gel. Subsequently, a first modification is performed in a trimethylchlorosilane solution, where trimethylchlorosilane reacts with the hydroxyl groups on the gel surface to form hydrophobic silicon-oxygen bonds, improving the hydrophobicity and chemical stability of the material. A second modification is then performed in a solution of a compound containing aromatic ring-terminated isocyanate groups, where the amino group reacts rapidly with the terminal isocyanate group to form urea bonds, introducing an aromatic ring structure and further enhancing the thermal stability of the material. Finally, a multi-crosslinked silica aerogel thermal insulation composite material is obtained, significantly improving its high-temperature resistance, thermal insulation performance, and mechanical properties, thereby meeting the application requirements in certain specific high-temperature environments and overcoming the shortcomings of existing silica aerogels.

[0088] Various embodiments of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of the invention; therefore, it should be considered that the range description has specifically disclosed all possible subranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed subranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the range referred to.

[0089] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A method for preparing a silica aerogel thermal insulation composite material, characterized in that, The preparation method includes the following steps: Acidic hydrolysis reaction was carried out with silicon source, anhydrous ethanol and water to obtain hydrolysate; The pH of the hydrolysate was adjusted to neutral using ammonia water, and amino silicone oil was added. The pH was then adjusted to alkaline to carry out a condensation reaction, resulting in a wet gel. The wet gel was aged, replaced with anhydrous ethanol, and then placed in a trimethylchlorosilane solution for the first modification to obtain the first wet gel. The first wet gel was placed in a solution of a compound containing an aromatic ring-terminated isocyanate group for a second modification to obtain a second wet gel; The second wet gel was washed in anhydrous ethanol and then dried to obtain the silica aerogel thermal insulation composite material. The preparation method of the amino silicone oil includes the following steps: Hydroxyl-terminated silicone oil, amino coupling agent and alkaline catalyst in a molar ratio of (2~2.3):1:(0.01~0.05) were stirred evenly, and then the mixture was stirred at a constant temperature of 80~85℃ for 2~3 hours to obtain a mixture. The mixture is heated to 105-110°C, and then vacuumized, and when the viscosity of the system is 4-6*10 3 mPa·s, the vacuumization is stopped, and the mixture is cooled to room temperature to obtain the amino silicone oil. The hydroxyl-terminated silicone oil includes WS62M from Wacker Chemie AG, Germany; the amino coupling agent is N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane; and the alkaline catalyst includes potassium hydroxide.

2. The method of claim 1, wherein the silica aerogel thermal insulation composite is prepared by the steps of: The operating conditions for the acidic hydrolysis reaction include: the molar ratio of the silicon source, the anhydrous ethanol, and the water is (1~2):(10~17):(3~7); the pH of the acidic hydrolysis reaction is adjusted to 2~4 using acid, which includes oxalic acid; the acidic hydrolysis reaction time is 2~3 hours; and the pH of the condensation reaction is 9~10.

3. The method of claim 1, wherein the silica aerogel thermal insulation composite is prepared by the steps of: The molar ratio of the silicon source to the amino silicone oil is 1:(1~2).

4. The method of claim 1, wherein the silica aerogel thermal insulation composite is prepared by the steps of: The silicon source includes at least one of methyl orthosilicate and ethyl orthosilicate; the aromatic ring-terminated isocyanate compound includes at least one of toluene diisocyanate, diphenylmethane diisocyanate and naphthyl diisocyanate.

5. The method of claim 1, wherein the silica aerogel thermal insulation composite is prepared by the steps of: The properties of the trimethylchlorosilane solution include: the solvent is n-hexane, and the volume ratio of the trimethylchlorosilane to the n-hexane is 1:(5~10); the properties of the aromatic ring-terminated isocyanate compound solution include: the solvent is n-hexane, and the mass-volume ratio of the aromatic ring-terminated isocyanate compound to the n-hexane is (10~20):1, expressed in g / L.

6. The method of claim 1, wherein the silica aerogel thermal insulation composite is prepared by the steps of: The working conditions for the first modification include: a weight ratio of 1:(10~20) of the wet gel to the trimethylchlorosilane solution (g / mL), a temperature of 30~40℃, and a time of 1~2 hours; the working conditions for the second modification include: a weight ratio of 1:(20~30) of the first wet gel to the terminal isocyanate compound solution (g / mL), a temperature of 30~40℃, and a time of 60~90 minutes.

7. The method of claim 1, wherein the silica aerogel thermal insulation composite is prepared by the steps of: The aging working conditions include: a temperature of 45~55℃ and a time of 35~55 hours; the drying method includes atmospheric pressure drying.

8. A silica aerogel thermal insulation composite material, characterized in that, The silica aerogel thermal insulation composite material is prepared by the preparation method described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Fire-class reinforced aerogel compositions

    CN112512679A

  • Method for producing organically modified, permanently hydrophobic aerogels

    WO1998023367A2