Pre-mixed cement-free concrete taking waste silty-fine sand as main material and preparation method of pre-mixed cement-free concrete
By premixed cementless concrete with waste fine sand as the main material, combined with slag powder, fly ash and other materials with alkaline exciters, the problems of low utilization rate of fine sand and cement production pollution are solved, and high efficiency is achieved , environmentally friendly building materials applications meet the construction industry's demand for green and low-carbon development.
Patent Information
- Application Number
- CN202411282970.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-17
AI Technical Summary
The large amount of fine sand produced in traditional excavation projects has not been effectively utilized, resulting in water pollution and waste of mineral resources. At the same time, harmful gas emissions in traditional cement production process are emitted, and the application technology of environmentally friendly gelling materials is lacking.
Premixed cementless concrete with waste powder and fine sand as the main material is used, and the combination of slag powder, fly ash, gravel, quicklime powder and basalt chopped fibers and alkaline exciters (water glass and sodium hydroxide) are used as Solid and liquid additives are used to prepare green gelling materials with high strength and durability, replacing traditional cement.
It improves the utilization rate of fine sand, reduces engineering costs, and realizes the resource utilization of industrial solid waste. It has low energy consumption, low pollution and excellent mechanical properties. It is suitable for roads, slope protection and waterway management and other fields.
Smart Images

Figure CN119143467A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a concrete for waste utilization and new building materials and a preparation method thereof, in particular to a premixed cement-free concrete with waste fine sand as main material, which can improve the utilization rate of a large amount of fine sand produced by excavation in water system connection projects and the like, and a preparation method thereof. Background Art
[0002] In recent years, in the context of protecting the environment and saving resources, the traditional way of mining stones from mountains has been restricted. At the same time, the overall amount of sand coming from rivers, lakes and reservoirs has continued to decrease, the gap in sand and gravel resources is large, and the contradiction between the supply and demand of sand and gravel materials has become increasingly prominent, which has brought certain adverse effects to the construction industry. At the same time, various waterway and river dredging projects in my country produce a large amount of fine sand every year. According to surveys, the annual output of fine sand dredged from the main stream of the Yangtze River alone has reached 10 to 30 million cubic meters. For such a large amount of dredged fine sand, the traditional way of disposing of this dredged fine sand is to throw it out on the water. This disposal method will not only cause water pollution and affect the underwater ecological environment, but also is a great waste of mineral resources.
[0003] In addition, the traditional cementitious material cement will emit a large amount of harmful gases containing carbon and sulfur elements due to its production process of "two grindings and one burning". The new alkali-activated cementitious material is formed by using aluminum-silica materials such as slag powder and fly ash under alkaline medium conditions. It has the advantages of good mechanical properties, strong durability, and high temperature resistance. At the same time, alkali-activated cementitious materials are different from ordinary silicate cement. They have abundant raw material resources, low energy consumption, and almost no pollution during the production process. They are environmentally friendly green cementitious materials that are in line with the national green and low-carbon development strategy. At present, the existing technology lacks a technical means that can combine waste fine sand with new alkali-activated cementitious materials to overcome the above-mentioned defects. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a premixed cement-free concrete with waste fine sand as the main material, which can improve the utilization rate of a large amount of fine sand produced by excavation in water system connection projects, canal waterway projects, water resource allocation projects, etc., and improve the resource utilization rate of bulk industrial solid waste such as granulated blast furnace slag powder and fly ash, and a preparation method thereof.
[0005] The present invention is achieved through the following technical solutions:
[0006] The present invention comprises a premixable cement-free concrete with waste fine sand as the main material, the concrete is composed of solid premix and liquid additive, the solid premix is composed of the following components by mass: 15-25 parts of slag powder, 10-15 parts of fly ash, 40-45 parts of fine sand, 15-20 parts of crushed stone, 1.5-2 parts of quicklime powder, and 1-1.5 parts of chopped basalt fibers;
[0007] The liquid additive is composed of the following components by weight: 8 to 18 parts of alkaline activator and 5 to 15 parts of water.
[0008] Furthermore, in the present invention, the alkaline activator comprises water glass and sodium hydroxide, wherein the sodium hydroxide is solid, flake-shaped, industrial grade, and has a purity greater than 96%, and the water glass modulus is 2 to 3.5 and the Baume degree is 30 to 60 Be.
[0009] Furthermore, in the present invention, the modulus of the alkaline activator is in the range of 1 to 1.5, and the modulus of the solution needs to be adjusted by adding sodium hydroxide to the water glass. The mass of the sodium hydroxide solid to be added is calculated according to the following formula:
[0010]
[0011] Among them, G is the mass of sodium hydroxide to be added, in kg; G1 is the mass of water glass to be adjusted, in kg; N is the content of Na2O in water glass, in %; m1 is the initial modulus of water glass, m2 is the final modulus of water glass, and the recommended value is 0.5-1.5; P is the purity of the added sodium hydroxide, in %;
[0012] The mass of Na2O in the alkaline activator is 3% to 6% of the mass of the slag powder and fly ash, that is,
[0013]
[0014] in, is the mass of Na2O in kg; m 水玻璃 is the mass of water glass, in kg; m 氢氧化钠 is the mass of sodium hydroxide, in kg; m 矿渣粉 is the mass of slag powder, in kg; m 粉煤灰 is the mass of fly ash, in kg.
[0015] Furthermore, in the present invention, the specific preparation steps of the alkaline activator are: weighing the mass of sodium hydroxide and water glass according to the above calculation steps to obtain the alkaline activator of the designed modulus, and injecting a certain amount of water, wherein the injected water is in the form of water vapor. Solid sodium hydroxide and water glass are placed in a ceramic reactor in proportion and sealed, and then water vapor is passed into the reactor. A flow sensor is provided in the reactor to ensure that the mass of the water vapor passed is the same as the mass of the required water. After the water vapor is passed, the materials are stirred evenly at a speed of 5 to 20 rpm in the reactor, and the stirring time is not less than 30 minutes, and then the reactor is cooled naturally or water is passed to cool the alkaline activator to room temperature. Adding water vapor during the alkaline activator configuration process can not only shorten the configuration time of the alkaline activator solution, accelerate the dissolution rate of solid sodium hydroxide, but also reduce the crystal precipitation phenomenon caused by temperature changes during the subsequent transportation and storage of the alkaline activator.
[0016] Furthermore, in the present invention, the slag powder is of S95 grade or S105 grade, the main chemical components include SiO2, CaO and Al2O3, and the specific surface area is not less than 400m 2 / kg, in line with the requirements of GB / T 18046.
[0017] Furthermore, in the present invention, the fly ash is Grade II, the main chemical components include SiO2, Al2O3 and Fe2O3, and the carbon content shall not exceed 10%, which complies with the provisions of DL / T 2297-2021.
[0018] Furthermore, in the present invention, the main chemical components of the fine sand include SiO2, Al2O3, K2O, Fe2O3, TiO2, etc., the fineness modulus is between 0.5 and 1.5, and the mud content (particle size is less than 0.075mm) is generally not more than 5%; the crushed stone is a stone with a particle size of 5-20mm and uniform gradation. The water content of the fine sand and crushed stone does not exceed 6%.
[0019] Furthermore, in the present invention, the water is city tap water, and after being added externally, the water-cement ratio of the fresh concrete is 0.52-0.54, that is,
[0020] m 外掺水(包括水蒸气) +m 水玻璃中的液体含量 +m 骨料中的水分含量
[0021] =0.52~0.54(m 矿渣粉 +m 粉煤灰 )
[0022] Among them, m 外掺水(包括水蒸气) is the mass of external water (including water vapor), in kg; m 水玻璃中的液体含量 is the mass of liquid in water glass, in kg; m骨料中的水分含量 is the water mass in the aggregate, in kg; m 矿渣粉 is the mass of slag powder, in kg; m 粉煤灰 is the mass of fly ash, in kg.
[0023] Furthermore, in the present invention, the quicklime is industrial grade, has a calcium content of more than 90%, and is in white or gray granular form; the specifications of the basalt chopped fibers include 6mm, 8mm, 10mm, and 12mm.
[0024] Furthermore, in the present invention, fly ash, slag powder, fine sand, crushed stone, quicklime and basalt fiber are all in a dry state.
[0025] The present invention also includes a method for preparing premixed cement-free concrete using waste fine sand as a main material, comprising the following steps:
[0026] S1. Prepare alkaline stimulator 24 hours in advance:
[0027] S2. Weigh the raw materials of each component of the solid premix by mass: 15-25 parts of slag powder, 10-15 parts of fly ash, 40-45 parts of fine sand, 15-20 parts of crushed stone, 1.5-2 parts of quicklime powder, and 1-1.5 parts of basalt chopped fibers;
[0028] S3, material mixing and stirring: add weighed crushed stone, fine sand, slag powder, fly ash, quicklime powder, and basalt chopped fibers to the concrete mixer in order and stir until uniform. The stirring time is 2 to 3 minutes to obtain a solid premix;
[0029] S4. Obtaining a mixture: adding the prepared alkaline activator and water to the uniformly mixed solid premix and stirring until uniform. The stirring time is 3 to 5 minutes to obtain fresh concrete.
[0030] S5. Forming concrete: Pour the freshly mixed concrete into the mold and place it on a concrete vibration table to fully vibrate. After smoothing the sample, cure it in a standard curing box for 24 hours, then remove the mold, and then perform standard curing again to obtain solidified concrete.
[0031] Compared with the prior art, the beneficial effects of the present invention are:
[0032] First, the cement-free concrete prepared by the present invention uses waste fine sand as the main raw material to prepare concrete to replace ordinary concrete for use in the fields of roads, slope protection, waterway management, etc., which alleviates the shortage of natural sand and stone materials, reduces engineering costs, and provides an effective way to recycle fine sand.
[0033] Second, the new green alkali-activated cementitious material has excellent properties such as high strength, acid and alkali resistance, high temperature resistance, and good durability. It can replace cement. In addition, the preparation process of the cementitious material does not require high-temperature calcination, and has the advantages of low energy consumption, low emissions, and low pollution, which is in line with the national green and low-carbon development strategy;
[0034] Thirdly, the concrete product produced by the present invention with fine sand as the main material is easy to spread and compact, has good fluidity, cohesion and water retention, and has a greatly improved pouring construction efficiency compared with ordinary concrete. At the same time, it has excellent mechanical properties, which is conducive to engineering promotion;
[0035] Fourth, the raw materials required by the present invention are widely available, and many large-scale industrial solid wastes rich in aluminum and silicon can be used as raw materials, which can realize the dual waste utilization of construction waste fine sand and industrial waste slag;
[0036] Fifth, the present invention can apply the premixed cement-free concrete with waste fine sand as the main material to the commercial concrete industry in the form of premixing, thereby realizing the productization and automation of the production and preparation process of the premixed cement-free concrete with waste fine sand as the main material, and has considerable economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 is a flow chart of an embodiment of the present invention. DETAILED DESCRIPTION
[0038] In order to make the contents of the present invention easier to understand, the technical solutions of the present invention are further explained below in combination with specific implementation methods. The examples are only used to illustrate the present invention, but the present invention is not limited to the contents.
[0039] Example 1
[0040] The present invention discloses a premixed cement-free concrete with waste fine sand as main material, according to which 1m 3 According to the mass ratio of each raw material, the mass ranges of each material of the concrete are: 800-900kg of dredged fine sand, 300-400kg of crushed stone, 200-300kg of water, 250-360kg of slag powder, 200-300kg of fly ash, 80-130kg of alkaline activator, 20-30kg of basalt chopped fiber, and 30-40kg of quicklime powder.
[0041] The present invention discloses a method for preparing premixed cement-free concrete using waste fine sand as main material, comprising the following steps:
[0042] Step 1, prepare the alkaline activator. Prepare the alkaline activator 24 hours in advance. Take 108kg of industrial-grade sodium water glass (modulus is 2.4, Baume degree is 50), 11kg of industrial-grade flaky sodium hydroxide (purity is 99%), and 30kg of water, wherein the water is in the form of water vapor. Put the solid sodium hydroxide and water glass into a ceramic reactor according to the above proportions and seal it. Then, pass water vapor into the reactor. A flow sensor is installed in the reactor to ensure that the mass of the water vapor passed is the same as the mass of the required water. After the water vapor is passed, stir the materials evenly at a speed of 5 to 20rpm in the reactor. The stirring time is not less than 30min. Then cool the reactor naturally or pass water to cool the alkaline activator to room temperature.
[0043] Step 2: Prepare the mixed dry materials. Add 300kg crushed stone, 900kg fine sand, 240kg fly ash, 360kg slag powder, 35kg quicklime powder, and 30kg basalt fiber to the concrete mixer in proportion, dry mix for 2 minutes, then slowly add the prepared alkaline activator and 222kg water, and continue stirring for 3 minutes to ensure that the materials are evenly mixed.
[0044] Step 3: Forming concrete: The fluid mixture is placed into a customized mold, placed on a concrete vibrating table for compaction, and then the surface is smoothed, sealed with a special curing film, and sent to a standard curing room for curing.
[0045] Step 4: demoulding and curing. The concrete specimens are demoulded immediately after 24 hours of standard curing. After demoulding, the concrete specimens are tightly wrapped with curing film and sent to the standard curing room for regular curing. The final concrete is obtained after curing to the standard age.
[0046] According to the provisions of the Standard for Test Methods of Mechanical Properties of Ordinary Concrete (GB / T50081-2002), the compressive strength of the concrete specimens prepared in Example 1 was tested at room temperature using a universal testing machine. The test results are shown in Table 1.
[0047] Table 1 Compressive strength of concrete at different ages in Example 1
[0048]
[0049] In accordance with the provisions of the Standard for Test Methods for Performance of Ordinary Concrete Mixtures (GB / T50080-2002), the setting time and slump of the concrete prepared in Example 1 were tested using a concrete penetrometer and a slump cone. The test results are shown in Table 2.
[0050] Table 2 Example 1 Concrete setting time and slump test
[0051] Test piece number Curing temperature / ℃ Initial setting time / min Final setting time / min Slump / mm Example 1 18-22 194 277 211
[0052] According to the provisions of the "Code for Design of Concrete Structures" (GB50010-2010), the strength grade of concrete in Example 1 reaches the standard of C45; according to the provisions of the "Concrete Quality Control Standard" (GB50164-2011), the slump grade of the fresh concrete mixture in Example 1 reaches S4 grade, and the flowability is excellent; the setting time conforms to the provisions of the "General Portland Cement" (GB175-2020); according to the provisions of the "Urban Road Engineering Design Code" (CJJ 37-2012), the concrete in Example 1 has met the strength requirements of road surface concrete for urban expressways, trunk roads, heavy traffic and the like.
[0053] Example 2
[0054] The present invention discloses a premixed cement-free concrete with waste fine sand as main material, according to which 1m 3 According to the mass ratio of each raw material, the mass ranges of each material of the concrete are: 800-900kg of dredged fine sand, 300-400kg of crushed stone, 200-300kg of water, 250-360kg of slag powder, 200-300kg of fly ash, 80-130kg of alkaline activator, 20-30kg of basalt chopped fiber, and 30-40kg of quicklime powder.
[0055] The present invention discloses a method for preparing premixed cement-free concrete using waste fine sand as main material, comprising the following steps:
[0056] Step 1, prepare the alkaline activator. Prepare the alkaline activator 24 hours in advance. The alkaline activator includes 72 kg of industrial-grade sodium water glass (modulus 2.4, Baume degree 50), 17 kg of industrial-grade flaky sodium hydroxide (purity 99%), and 10 kg of water, wherein the water is in the form of water vapor. According to the above proportions, solid sodium hydroxide and water glass are placed in a ceramic reactor and sealed, and then water vapor is introduced into the reactor. A flow sensor is installed in the reactor to ensure that the mass of the water vapor introduced is the same as the mass of the required water. After the water vapor is introduced, the materials are stirred evenly in the reactor at a speed of 5 to 20 rpm, and the stirring time is not less than 30 minutes. Then the reactor is cooled naturally or water is passed to cool the alkaline activator to room temperature.
[0057] Step 2: Prepare the mixed dry materials. Add 400kg crushed stone, 800kg fine sand, 360kg fly ash, 240kg slag powder, 40kg quicklime powder, and 30kg basalt fiber to the concrete mixer in proportion, dry mix for 2 minutes, then slowly add the prepared alkaline activator and 250kg water, and continue stirring for 3 minutes to ensure that the materials are evenly mixed.
[0058] Step 3: Forming concrete: The fluid mixture is placed into a customized mold, placed on a concrete vibrating table for compaction, and then the surface is smoothed, sealed with a special curing film, and sent to a standard curing room for curing.
[0059] Step 4: demoulding and curing. The concrete specimens are demoulded immediately after 24 hours of standard curing. After demoulding, the concrete specimens are tightly wrapped with curing film and sent to the standard curing room for regular curing. The final concrete is obtained after curing to the standard age.
[0060] According to the provisions of the Standard for Test Methods of Mechanical Properties of Ordinary Concrete (GB / T50081-2002), the compressive strength of the concrete specimens prepared in Example 2 was tested at room temperature using a universal testing machine. The test results are shown in Table 3.
[0061] Table 3 Compressive strength of concrete in Example 2 at different ages
[0062]
[0063]
[0064] In accordance with the provisions of the Standard for Test Methods for Performance of Ordinary Concrete Mixtures (GB / T50080-2002), the setting time and slump of the concrete prepared in Example 2 were tested using a concrete penetrometer and a slump cone. The test results are shown in Table 4.
[0065] Table 4 Concrete setting time and slump test of Example 1
[0066] Test piece number Curing temperature / ℃ Initial setting time / min Final setting time / min Slump / mm Example 2 18-22 204 296 219
[0067] According to the provisions of the "Code for Design of Concrete Structures" (GB50010-2010), the strength grade of concrete in Example 1 reaches the standard of C35; according to the provisions of the "Concrete Quality Control Standard" (GB50164-2011), the slump grade of the fresh concrete mixture in Example 1 reaches S4, and the flowability is excellent; the setting time conforms to the provisions of the "General Portland Cement" (GB175-2020); according to the provisions of the "Urban Road Engineering Design Code" (CJJ 37-2012), the concrete in Example 2 has met the strength requirements of road surface concrete for urban expressways, trunk roads, heavy traffic, etc.
[0068] Example 3
[0069] The present invention discloses a premixed cement-free concrete with waste fine sand as main material, according to which 1m 3According to the mass ratio of each raw material, the mass ranges of each material of the concrete are: 800-900kg of dredged fine sand, 300-400kg of crushed stone, 200-300kg of water, 250-360kg of slag powder, 200-300kg of fly ash, 80-130kg of alkaline activator, 20-30kg of basalt chopped fiber, and 30-40kg of quicklime powder.
[0070] The present invention discloses a method for preparing premixed cement-free concrete using waste fine sand as main material, comprising the following steps:
[0071] Step 1, prepare the alkaline activator. Prepare the alkaline activator 24 hours in advance. Take 135kg of industrial-grade sodium water glass (modulus is 2.4, Baume degree is 50), 14kg of industrial-grade flaky sodium hydroxide (purity is 99%), and 20kg of water as the alkaline activator, wherein the water is in the form of water vapor. Put the solid sodium hydroxide and water glass into a ceramic reactor according to the above proportions and seal it, then pass water vapor into the reactor, and set a flow sensor in the reactor to ensure that the mass of the water vapor passed is the same as the mass of the required water. After the water vapor is passed, stir the materials evenly at a speed of 5 to 20rpm in the reactor, and the stirring time shall not be less than 30min, then cool the reactor naturally or pass water to cool the alkaline activator to room temperature.
[0072] Step 2: Prepare the mixed dry materials. Add 300kg crushed stone, 900kg fine sand, 360kg fly ash, 240kg slag powder, 30kg quicklime powder, and 30kg basalt fiber to the concrete mixer in proportion, dry mix for 2 minutes, then slowly add the prepared alkaline activator and 205kg water, and continue stirring for 3 minutes to ensure that the materials are evenly mixed.
[0073] Step 3: Forming concrete: The fluid mixture is placed into a customized mold, placed on a concrete vibrating table for compaction, and then the surface is smoothed, sealed with a special curing film, and sent to a standard curing room for curing.
[0074] Step 4: demoulding and curing. The concrete specimens are demoulded immediately after 24 hours of standard curing. After demoulding, the concrete specimens are tightly wrapped with curing film and sent to the standard curing room for regular curing. The final concrete is obtained after curing to the standard age.
[0075] According to the provisions of the Standard for Test Methods of Mechanical Properties of Ordinary Concrete (GB / T50081-2002), the compressive strength of the concrete specimens prepared in Example 3 was tested at room temperature using a universal testing machine. The test results are shown in Table 5.
[0076] Table 5 Compressive strength of concrete of Example 3 at different ages
[0077]
[0078] In accordance with the provisions of the Standard for Test Methods for Performance of Ordinary Concrete Mixtures (GB / T50080-2002), the setting time and slump of the concrete prepared in Example 3 were tested using a concrete penetrometer and a slump cone. The test results are shown in Table 6.
[0079] Table 6 Concrete setting time and slump test of Example 3
[0080] Test piece number Curing temperature / ℃ Initial setting time / min Final setting time / min Slump / mm Example 3 18-22 138 287 218
[0081] According to the provisions of the "Code for Design of Concrete Structures" (GB50010-2010), the strength grade of the concrete in Example 1 reaches the C30 standard; according to the provisions of the "Concrete Quality Control Standard" (GB50164-2011), the slump grade of the fresh concrete mixture in Example 1 reaches S4 grade, and the flowability is excellent; the setting time conforms to the provisions of the "General Portland Cement" (GB175-2020); according to the provisions of the "Urban Road Engineering Design Code" (CJJ 37-2012), the concrete in Example 3 has met the strength requirements of road surface concrete for urban expressways, trunk roads, heavy traffic, etc.
[0082] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A premixed cement-free concrete with waste fine sand as main material, characterized in that It is composed of solid premix and liquid additive; The solid premix is composed of the following components by mass: 15-25 parts of slag powder, 10-15 parts of fly ash, 40-45 parts of fine sand, 15-20 parts of crushed stone, 1.5-2 parts of quicklime powder, and 1-1.5 parts of basalt chopped fibers; The liquid additive is composed of the following components by mass: 8 to 18 parts of alkaline activator and 5 to 15 parts of water.
2. The premixed cement-free concrete with waste fine sand as main material according to claim 1, characterized in that The alkaline activator comprises water glass and sodium hydroxide, wherein the sodium hydroxide is solid, flaky, industrial grade, and has a purity greater than 90%, the water glass modulus is 2-3.5, and the Baume degree is 30-60 Be.
3. The premixed cement-free concrete with waste fine sand as main material according to claim 1, characterized in that The modulus of the alkaline activator is in the range of 1 to 1.
5. The modulus of the solution needs to be adjusted by adding sodium hydroxide to the water glass. The mass of the sodium hydroxide solid to be added is calculated according to the following formula: Among them, G is the mass of sodium hydroxide to be added, in kg; G1 is the mass of water glass to be adjusted, in kg; N is the content of Na2O in water glass, in %; m1 is the initial modulus of water glass, m2 is the final modulus of water glass, and the recommended value is 0.5-1.5; P is the purity of the added sodium hydroxide, in %; The mass of Na2O in the alkaline activator is 3% to 6% of the mass of the slag powder and fly ash, that is, in, is the mass of Na2O in kg; m 水玻璃 is the mass of water glass, in kg; m 氢氧化钠 is the mass of sodium hydroxide, in kg; m 矿渣粉 is the mass of slag powder, in kg; m 粉煤灰 is the mass of fly ash, in kg.
4. The premixed cement-free concrete with waste fine sand as main material according to claim 1, characterized in that: The slag powder is of S95 or S105 grade, and its main chemical components include SiO2, CaO and Al2O3, and its specific surface area is not less than 400m 2 / kg, in line with the requirements of GB / T 18046.
5. The ready-mixed cement-free concrete with waste fine sand as main material according to claim 1, characterized in that: The fly ash is Grade II, and its main chemical components include SiO2, Al2O3 and Fe2O3. The carbon content shall not exceed 10%, which complies with the provisions of DL / T2297-2021.
6. The premixed cement-free concrete with waste fine sand as main material according to claim 1, characterized in that: The main chemical components of the fine sand include SiO2, Al2O3, K2O, Fe2O3, TiO2, the fineness modulus is between 0.5 and 1.5, the mud content of particles with a particle size less than 0.075 mm does not exceed 5%; the crushed stone is a stone with a particle size of 5 to 20 mm and uniform grading.
7. The premixed cement-free concrete with waste fine sand as main material according to claim 1, characterized in that: The water is city tap water, and after being mixed with water, the water-cement ratio of the fresh concrete is 0.52-0.54, that is, m 外掺水(包括水蒸气) +m 水玻璃中的液体含量 +m 骨料中的水分含量 =0.52~0.54(m 矿渣粉 +m 粉煤灰 ) Among them, m 外掺水(包括水蒸气) is the mass of external water (including water vapor), in kg; m 水玻璃中的液体含量 is the mass of liquid in water glass, in kg; m 骨料中的水分含量 is the water mass in the aggregate, in kg; m 矿渣粉 is the mass of slag powder, in kg; m 粉煤灰 is the mass of fly ash, in kg.
8. The premixed cement-free concrete with waste fine sand as main material according to claim 1, characterized in that: The quicklime is industrial grade, has a calcium content of more than 90%, and is in white or gray granular form; the fly ash, slag powder, fine sand, crushed stone, quicklime, and basalt fiber are all in a dry state, and the specifications of the basalt chopped fibers include 6mm, 8mm, 10mm, and 12mm.
9. A method for preparing premixed cement-free concrete with waste fine sand as main material according to claims 1 to 8, characterized in that: The following steps are involved: S1. Prepare alkaline stimulator 24 hours in advance: S2. Weigh the raw materials of each component of the solid premix by mass: 15-25 parts of slag powder, 10-15 parts of fly ash, 40-45 parts of fine sand, 15-20 parts of crushed stone, 1.5-2 parts of quicklime powder, and 1-1.5 parts of basalt chopped fibers; S3, material mixing and stirring: add weighed crushed stone, fine sand, slag powder, fly ash, quicklime powder, and basalt chopped fibers to the concrete mixer in order and stir until uniform. The stirring time is 2 to 3 minutes to obtain a solid premix; S4. Obtaining a mixture: adding the prepared alkaline activator and water to the uniformly mixed solid premix and stirring until uniform. The stirring time is 3 to 5 minutes to obtain fresh concrete. S5. Forming concrete: Pour the freshly mixed concrete into the mold and place it on a concrete vibration table to fully vibrate. After smoothing the sample, cure it in a standard curing box for 24 hours, then remove the mold, and then perform standard curing again to obtain solidified concrete.
10. A method for preparing premixed cement-free concrete with waste fine sand as main material according to claim 9, characterized in that: The preparation method of the alkaline activator in step S1 comprises the following steps: S101, placing solid sodium hydroxide and water glass in a ceramic reactor according to a proportion and sealing the reactor, and then introducing water vapor into the reactor, wherein a flow sensor is provided in the reactor to ensure that the mass of the introduced water vapor is the same as the mass of the required water; S102, after the water vapor is introduced, the materials are stirred evenly in the reactor at a speed of 5 to 20 rpm, and the stirring time is not less than 30 minutes; S103. After stirring, the reactor is cooled naturally or by passing water to cool the alkaline activator to room temperature.
Citation Information
Patent Citations
Alkali-activated cement utilizing abandoned clay brick powder and preparation method thereof
CN105399353A
Retarding geopolymer concrete and preparation method thereof
CN115321857A
Geopolymer concrete mix proportion design method based on dredged sand and artificial soft stone
CN115340324A
Method and system for recycling sodium silicate insoluble waste residues
CN117049556A
Fly ash based geopolymer grouting material and preparation method therefor
WO2018028225A1
Cited By
High folding pressure ratio dry hard road surface concrete based on large amount of fine sand and preparation method thereof