A catalyst, preparation method and efficient method for synthesizing 3-methylpyridine
By preparing S-doped Ni-Al composite layered metal oxide/SiO2 composite supported W/Cu oxide catalyst, the problems of easy catalyst deactivation and high production cost in the prior art were solved, realizing an efficient, simplified synthesis route and high selectivity for 3-methylpyridine.
Patent Information
- Application Number
- CN202411528073.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-10-30
AI Technical Summary
Existing technologies for preparing 3-methylpyridine suffer from problems such as easy catalyst deactivation, numerous byproducts, high production costs, and unsuitability for continuous production. Furthermore, the catalyst preparation process is complex and unsuitable for industrial applications.
A catalyst using S-doped Ni-Al composite layered metal oxide/SiO2 composite supported on W/Cu oxide was prepared and loaded with Pt via co-precipitation to form Niδ+-S active centers and W/Cu catalytic active centers. The catalyst performance was enhanced by combining the sol-gel reaction.
The highly selective synthesis of 3-methylpyridine was achieved, simplifying the synthetic route, improving the activity and stability of the catalyst, reducing production costs, and making it suitable for industrial mass production.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of organic synthesis technology, specifically to a catalyst, a preparation method, and a method for the efficient synthesis of 3-methylpyridine. Background Technology
[0002] Methylpyridine, also known as β-methylpyridine or 3-picolinine, is an organic synthesis intermediate and solvent. It is a colorless, oily liquid with an unpleasant odor. It is miscible with water, ethanol, and ether. It is flammable when exposed to open flames, high temperatures, or oxidizing agents; it produces toxic nitrogen oxide gas when heated. In pesticides, it is used as an intermediate in the synthesis of the insecticides imidacloprid and acetamiprid, for the next intermediate, 3-methylpyridine-N-oxide. It can also be used as a pharmaceutical intermediate, dye intermediate, and resin intermediate.
[0003] Patents GB1488335A, US4521602A, CN101990532A, and CN107365257A all use 2-methylglutaronitrile as a starting material. Under the catalysis of metallic Ni, Pd / Al₂O₃, or Raney nickel or Raney cobalt doped with other elements, they react to produce 2-methyl-1,5-pentanediamine, 3-methylpiperidine, and 3-methylpyridine. In the presence of nickel-based or cobalt-based catalysts, the reaction products mainly consist of 2-methyl-1,5-pentanediamine and 3-methylpiperidine, with additional secondary and tertiary amine byproducts. Furthermore, nickel-based and cobalt-based catalysts are generally used in reaction vessels, making them unsuitable for continuous industrial production. Under the action of metal Pd, the products obtained are all composed of 3-methylpiperidine and 3-methylpyridine, with an overall yield of about 83%. However, Pd is prone to deactivation in the hydrogenation reaction of 2-methylglutaronitrile. Frequent catalyst regeneration will reduce catalyst activity and is not conducive to reducing production costs.
[0004] Chinese patent CN107983398B discloses a method for producing a nano-attapulgite composite catalyst for the preparation of 3-methylpyridine. The steps are as follows: Nano-attapulgite ore is added to a hydrochloric acid aqueous solution for separation and washing, then washed with silver nitrate solution, and then boiled with distilled water, followed by centrifugation and washing to obtain acid-modified nano-attapulgite; this is then mixed evenly with zeolite molecular sieves, dried, ground, and calcined at high temperature to obtain a nano-attapulgite composite support; the composite support is then added to silica sol for full adsorption, dried, and ground to obtain the nano-attapulgite composite catalyst. This invention has a complex process and high cost, making it unsuitable for industrial production. Summary of the Invention
[0005] The purpose of this invention is to provide a catalyst, preparation method, and efficient method for synthesizing 3-methylpyridine. Using 2-methylpentanilide as a raw material, 3-methylpyridine is directly obtained by hydrogenation and dehydrogenation reactions under the action of the same catalyst. The synthetic route is simple and efficient, with high product selectivity and no intermediate by-products or impurities generated. Moreover, the metal element doped in the catalyst system is economical, efficient, and readily available, and the catalyst has extremely high activity. Compared with other technologies, it does not require complex distillation and separation purification processes, which greatly improves economic efficiency and allows for industrial mass production.
[0006] The technical solution of this invention is implemented as follows: This invention provides a method for preparing a catalyst, the method of which is as follows: S1. Preparation of S-doped Ni-Al composite layered metal oxide: Nickel nitrate, aluminum nitrate and thiourea were dissolved in water, alkaline solution was added dropwise, heated to crystallize, filtered, washed, dried and calcined to obtain S-doped Ni-Al composite layered metal oxide; S2. Preparation of S-doped Ni-Al composite layered metal oxide / SiO2 composite: Tetraethyl orthosilicate was added to ethanol, then S-doped Ni-Al composite layered metal oxide was added, stirred and mixed evenly, ammonia was added dropwise, heated and reacted, filtered, washed and dried to obtain S-doped Ni-Al composite layered metal oxide / SiO2 composite. S3. S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide: Concentrated nitric acid and copper nitrate were added to water to prepare mixture A. The S-doped Ni-Al composite layered metal oxide / SiO2 complex and ammonium tungstate were added to water and stirred to dissolve to prepare mixture B. Mixture A was added dropwise to mixture B and stirred to carry out co-precipitation reaction. The mixture was filtered, washed, dried and calcined to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide. S4. Reduction: The S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu oxide is reduced by low-temperature hydrogen gas to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu. S5. Catalyst preparation: The S-doped Ni-Al composite layered metal oxide / SiO2 complex supported on W / Cu was added to anhydrous ethanol, followed by the addition of an ethanol solution of chloroplatinic acid. The mixture was stirred at room temperature, and then polyvinylpyrrolidone and sodium borohydride were added. The mixture was stirred and reacted, washed, and dried to obtain the catalyst.
[0007] As a further improvement of the present invention, the molar ratio of nickel nitrate, aluminum nitrate and thiourea in step S1 is 1:1:0.05-0.1, the pH value of the solution is adjusted to 7.5-8.5 by adding alkaline solution, the temperature of the heating crystallization is 85-95℃ and the time is 20-40 min, and the temperature of the calcination is 500-600℃ and the time is 2-4 h.
[0008] As a further improvement of the present invention, the mass ratio of tetraethyl orthosilicate, S-doped Ni-Al composite layered metal oxide, and ammonia in step S2 is 10-12:17-25:2-3, and the heating reaction temperature is 40-50℃ for 10-12 hours.
[0009] As a further improvement of the present invention, the concentration of concentrated nitric acid in step S3 is 5.5-6 mol / L, the mass ratio of concentrated nitric acid to copper nitrate is 1-2:7-10, the mass ratio of S-doped-Ni-Al composite layered metal oxide / SiO2 composite to ammonium tungstate is 10-12:5-7, the co-precipitation reaction time is 0.5-1 h, and the calcination temperature is 300-400℃ for 1-3 h.
[0010] As a further improvement of the present invention, the low-temperature hydrogen reduction in step S4 is carried out by a strong drainage and permeable tubular furnace at 650-750°C for 2-4 hours with hydrogen flow rate of 15-20 L / min.
[0011] As a further improvement of the present invention, in step S5, the mass ratio of the S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu, chloroplatinic acid, polyvinylpyrrolidone and sodium borohydride is 15-20:3-5:1.2-1.5:1.9-2.2, and the stirring reaction time is 3-5 h.
[0012] As a further improvement to the present invention, the specific steps include: S1. Preparation of S-doped Ni-Al composite layered metal oxide: Dissolve 1 molar equivalent of nickel nitrate, 1 molar equivalent of aluminum nitrate, and 0.05-0.1 molar equivalent of thiourea in water, add 10-15 wt% NaOH solution to adjust the pH of the solution to 7.5-8.5, heat to 85-95℃, crystallize for 20-40 min, filter, wash, dry, and calcine at 500-600℃ for 2-4 h to obtain S-doped Ni-Al composite layered metal oxide; S2. Preparation of S-doped Ni-Al composite layered metal oxide / SiO2 composite: 10-12 parts by weight of tetraethyl orthosilicate were added to ethanol, and 17-25 parts by weight of S-doped Ni-Al composite layered metal oxide were added. The mixture was stirred and mixed evenly. 2-3 parts by weight of ammonia water were added dropwise. The mixture was heated to 40-50℃ and reacted for 10-12 h. The mixture was filtered, washed, and dried to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 composite. S3. S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide: 1-2 parts by weight of 5.5-6 mol / L concentrated nitric acid and 7-10 parts by weight of copper nitrate were added to water to prepare mixture A. 10-12 parts by weight of S-doped Ni-Al composite layered metal oxide / SiO2 complex and 5-7 parts by weight of ammonium tungstate were added to water and stirred to dissolve to prepare mixture B. Mixture A was added dropwise to mixture B and stirred to carry out a co-precipitation reaction for 0.5-1 h. The mixture was then filtered, washed, dried, and calcined at 300-400℃ for 1-3 h to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide. S4. Reduction: The S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu oxide was reduced by hydrogen gas at 650-750℃ for 2-4 hours in a tube furnace with strong drainage and permeability, with a hydrogen gas flow rate of 15-20 L / min, to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu. S5. Catalyst preparation: 15-20 parts by weight of S-doped Ni-Al composite layered metal oxide / SiO2 complex supported on W / Cu were added to anhydrous ethanol, followed by the addition of an ethanol solution containing 3-5 parts by weight of chloroplatinic acid. The mixture was stirred at room temperature for 0.5-1 h, then 1.2-1.5 parts by weight of polyvinylpyrrolidone and 1.9-2.2 parts by weight of sodium borohydride were added. The mixture was stirred for 3-5 h, washed, and dried to obtain the catalyst.
[0013] This invention further protects a catalyst prepared by the above-described preparation method.
[0014] This invention further protects a method for the efficient synthesis of 3-methylpyridine, which involves subjecting 2-methylpentanonitrile to a hydrogenation-dehydrogenation reaction under the action of the above-mentioned catalyst to obtain the product 3-methylpyridine, with amino-3-methylpyridine as a byproduct.
[0015] As a further improvement of the present invention, the reaction temperature is 250-300℃, the hydrogen-to-nitrogen ratio is 1000-1400, and the 2-methylpentanilonitrile is 2-methylpentanilonitrile with a purity >99.9%.
[0016] The present invention has the following beneficial effects: 1. This invention uses a co-precipitation method to prepare a composite metal layered oxide, doped with sulfur (S). S atoms occupy the octahedral interstices of the active metal Ni particles, breaking the continuous Ni sites while simultaneously absorbing electrons from Ni, thus constructing a surface-isolated Ni layer. δ+ -S active centers, thus exhibiting excellent activity, selectivity, and stability in hydrogenation reactions. Meanwhile, Ni... δ+ The -S active center promotes hydrogen molecule activation, and the intermediates are adsorbed via weak π bonds, making them easy to desorb from the active site and improving dehydrogenation activity. Furthermore, coating the surface with a layer of silica using a sol-gel reaction not only significantly improves the catalyst's mechanical properties but also increases its specific surface area, enhances reaction sites, and promotes catalytic activity. The silica on the surface can also form hydrogen bonds, allowing for the uniform adsorption of tungsten copper oxide. After reduction, W / Cu catalytic active centers are obtained, and further reaction allows for Pt loading. The larger specific surface area increases the Pt loading, prevents Pt aggregation and detachment, and also promotes catalytic activity and durability. 2. The catalyst prepared by this invention has high Pt loading, strong action, which helps to prevent the agglomeration and shedding of active metals, improves the durability of the catalyst, and has high catalytic activity. It maintains good catalytic activity even after repeated catalysis, has good dispersibility, and has broad application prospects. 3. This invention uses 2-methylpentanilide as a raw material to directly produce 3-methylpyridine through hydrogenation and dehydrogenation reactions under the same catalyst. The synthetic route is simple and efficient, with high product selectivity and no intermediate by-products or impurities are generated. Moreover, the metal elements doped in the catalyst system are economical, efficient and easy to obtain, and the catalyst has extremely high activity. Compared with other technologies, there is no need for complex distillation and separation purification processes, which greatly improves economic efficiency and can be industrialized for mass production. Detailed Implementation
[0017] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0018] Example 1 A method for preparing a catalyst includes the following steps: S1. Preparation of S-doped Ni-Al composite layered metal oxide: 20 mmol nickel nitrate, 20 mmol aluminum nitrate and 1 mmol thiourea were dissolved in 200 mL water, and 10 wt% NaOH solution was added dropwise to adjust the pH of the solution to 7.5. The solution was heated to 85 °C and crystallized for 20 min. The solution was filtered, washed, dried and calcined at 500 °C for 2 h to obtain S-doped Ni-Al composite layered metal oxide. S2. Preparation of S-doped Ni-Al composite layered metal oxide / SiO2 composite: 10g of tetraethyl orthosilicate was added to 100mL of ethanol, 17g of S-doped Ni-Al composite layered metal oxide was added, the mixture was stirred and mixed for 10min, 2g of ammonia was added dropwise, the mixture was heated to 40℃ and reacted for 10h, filtered, washed and dried to obtain S-doped Ni-Al composite layered metal oxide / SiO2 composite. S3. S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide: 0.1 g of 5.5 mol / L concentrated nitric acid and 0.7 g of copper nitrate were added to 20 mL of water to prepare mixture A. 1 g of S-doped Ni-Al composite layered metal oxide / SiO2 complex and 0.5 g of ammonium tungstate were added to 80 mL of water and stirred to dissolve to prepare mixture B. Mixture A was added dropwise to mixture B and stirred to carry out a co-precipitation reaction for 0.5 h. The mixture was then filtered, washed, dried, and calcined at 300 °C for 1 h to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide. S4. Reduction: The S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu oxide was reduced by hydrogen gas at 650°C for 2 hours in a tube furnace with strong drainage and permeability. The hydrogen gas flow rate was 15 L / min, to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu. S5. Catalyst preparation: 15g of S-doped Ni-Al composite layered metal oxide / SiO2 complex supported on W / Cu was added to 200mL of anhydrous ethanol, followed by 50mL of ethanol solution containing 3g of chloroplatinic acid. The mixture was stirred at room temperature for 0.5h, then 1.2g of polyvinylpyrrolidone and 1.9g of sodium borohydride were added. The mixture was stirred for 3h, washed, and dried to obtain the catalyst.
[0019] Example 2 A method for preparing a catalyst includes the following steps: S1. Preparation of S-doped Ni-Al composite layered metal oxide: 20 mmol nickel nitrate, 20 mmol aluminum nitrate and 2 mmol thiourea were dissolved in 200 mL water, and 15 wt% NaOH solution was added dropwise to adjust the pH of the solution to 8.5. The solution was heated to 95 °C and crystallized for 40 min. After filtration, washing and drying, the solution was calcined at 600 °C for 4 h to obtain S-doped Ni-Al composite layered metal oxide. S2. Preparation of S-doped Ni-Al composite layered metal oxide / SiO2 composite: 12g of tetraethyl orthosilicate was added to 100mL of ethanol, 25g of S-doped Ni-Al composite layered metal oxide was added, the mixture was stirred and mixed for 10min, 3g of ammonia was added dropwise, the mixture was heated to 50℃ and reacted for 12h, filtered, washed and dried to obtain S-doped Ni-Al composite layered metal oxide / SiO2 composite. S3. S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide: 0.2 g of 6 mol / L concentrated nitric acid and 1 g of copper nitrate were added to 20 mL of water to prepare mixture A. 1.2 g of S-doped Ni-Al composite layered metal oxide / SiO2 complex and 0.7 g of ammonium tungstate were added to 80 mL of water and stirred to dissolve to prepare mixture B. Mixture A was added dropwise to mixture B and stirred to carry out a co-precipitation reaction for 1 h. The mixture was then filtered, washed, dried, and calcined at 400 °C for 3 h to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide. S4. Reduction: The S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu oxide was reduced by hydrogen gas at 750°C for 4 hours in a tube furnace with strong drainage and permeability. The hydrogen gas flow rate was 20 L / min, to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu. S5. Catalyst preparation: 20g of S-doped Ni-Al composite layered metal oxide / SiO2 complex supported on W / Cu was added to 200mL of anhydrous ethanol, followed by 50mL of ethanol solution containing 5g of chloroplatinic acid. The mixture was stirred at room temperature for 1h, then 1.5g of polyvinylpyrrolidone and 2.2g of sodium borohydride were added. The mixture was stirred for 5h, washed, and dried to obtain the catalyst.
[0020] Example 3 A method for preparing a catalyst includes the following steps: S1. Preparation of S-doped Ni-Al composite layered metal oxide: 20 mmol nickel nitrate, 20 mmol aluminum nitrate and 1.5 mmol thiourea were dissolved in 200 mL water, and 12 wt% NaOH solution was added dropwise to adjust the pH of the solution to 8. The solution was heated to 90 °C and crystallized for 30 min. After filtration, washing and drying, the solution was calcined at 550 °C for 3 h to obtain S-doped Ni-Al composite layered metal oxide. S2. Preparation of S-doped Ni-Al composite layered metal oxide / SiO2 composite: 11g of tetraethyl orthosilicate was added to 100mL of ethanol, 20g of S-doped Ni-Al composite layered metal oxide was added, the mixture was stirred and mixed for 10min, 2.5g of ammonia was added dropwise, the mixture was heated to 45℃ and reacted for 11h, filtered, washed and dried to obtain S-doped Ni-Al composite layered metal oxide / SiO2 composite; S3. S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide: 0.15 g of 5.7 mol / L concentrated nitric acid and 0.85 g of copper nitrate were added to 50 mL of water to prepare mixture A. 1.1 g of S-doped Ni-Al composite layered metal oxide / SiO2 complex and 0.6 g of ammonium tungstate were added to 80 mL of water and stirred to dissolve to prepare mixture B. Mixture A was added dropwise to mixture B and stirred to carry out a co-precipitation reaction for 1 h. The mixture was then filtered, washed, dried, and calcined at 350 °C for 2 h to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide. S4. Reduction: The S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu oxide was reduced by hydrogen gas at 700℃ for 3 hours in a tube furnace with strong drainage and permeability. The hydrogen gas flow rate was 17 L / min, to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu. S5. Catalyst preparation: 17g of S-doped Ni-Al composite layered metal oxide / SiO2 complex supported on W / Cu was added to 200mL of anhydrous ethanol, followed by 50mL of ethanol solution containing 4g of chloroplatinic acid. The mixture was stirred at room temperature for 1h, then 1.35g of polyvinylpyrrolidone and 2g of sodium borohydride were added. The mixture was stirred for 4h, washed, and dried to obtain the catalyst.
[0021] Comparative Example 1 The difference from Example 3 is that thiourea was not added in step S1.
[0022] Specifically as follows: S1. Preparation of Ni-Al composite layered metal oxide: 20 mmol nickel nitrate and 20 mmol aluminum nitrate were dissolved in 200 mL of water, and 12 wt% NaOH solution was added dropwise to adjust the pH of the solution to 8. The solution was heated to 90 °C and crystallized for 30 min. After filtration, washing, drying, and calcination at 550 °C for 3 h, Ni-Al composite layered metal oxide was obtained.
[0023] Comparative Example 2 The difference from Example 3 is that step S2 was not performed.
[0024] A method for preparing a catalyst includes the following steps: S1. Preparation of S-doped Ni-Al composite layered metal oxide: 20 mmol nickel nitrate, 20 mmol aluminum nitrate and 1.5 mmol thiourea were dissolved in 200 mL water, and 12 wt% NaOH solution was added dropwise to adjust the pH of the solution to 8. The solution was heated to 90 °C and crystallized for 30 min. After filtration, washing and drying, the solution was calcined at 550 °C for 3 h to obtain S-doped Ni-Al composite layered metal oxide. S2. S-doped Ni-Al composite layered metal oxide loaded with W / Cu oxide: 0.15 g of 5.7 mol / L concentrated nitric acid and 0.85 g of copper nitrate were added to 50 mL of water to prepare mixture A. 1.1 g of S-doped Ni-Al composite layered metal oxide and 0.6 g of ammonium tungstate were added to 80 mL of water and stirred to dissolve to prepare mixture B. Mixture A was added dropwise to mixture B and stirred to carry out a co-precipitation reaction for 1 h. The mixture was then filtered, washed, dried, and calcined at 350 °C for 2 h to obtain S-doped Ni-Al composite layered metal oxide loaded with W / Cu oxide. S3. Reduction: The S-doped Ni-Al composite layered metal oxide loaded with W / Cu oxide was reduced by hydrogen gas at 700°C for 3 hours in a tube furnace with strong drainage and permeability. The hydrogen gas flow rate was 17 L / min, to obtain the S-doped Ni-Al composite layered metal oxide loaded with W / Cu. S4. Catalyst preparation: 17g of S-doped Ni-Al composite layered metal oxide supported on W / Cu was added to 200mL of anhydrous ethanol, followed by 50mL of ethanol solution containing 4g of chloroplatinic acid. The mixture was stirred at room temperature for 1h, then 1.35g of polyvinylpyrrolidone and 2g of sodium borohydride were added. The mixture was stirred for 4h, washed, and dried to obtain the catalyst.
[0025] Comparative Example 3 The difference from Example 3 is that steps S3 and S4 were not performed.
[0026] A method for preparing a catalyst includes the following steps: S1. Preparation of S-doped Ni-Al composite layered metal oxide: 20 mmol nickel nitrate, 20 mmol aluminum nitrate and 1.5 mmol thiourea were dissolved in 200 mL water, and 12 wt% NaOH solution was added dropwise to adjust the pH of the solution to 8. The solution was heated to 90 °C and crystallized for 30 min. After filtration, washing and drying, the solution was calcined at 550 °C for 3 h to obtain S-doped Ni-Al composite layered metal oxide. S2. Preparation of S-doped Ni-Al composite layered metal oxide / SiO2 composite: 11g of tetraethyl orthosilicate was added to 100mL of ethanol, 20g of S-doped Ni-Al composite layered metal oxide was added, the mixture was stirred and mixed for 10min, 2.5g of ammonia was added dropwise, the mixture was heated to 45℃ and reacted for 11h, filtered, washed and dried to obtain S-doped Ni-Al composite layered metal oxide / SiO2 composite; S3. Catalyst preparation: 17g of S-doped Ni-Al composite layered metal oxide / SiO2 complex was added to 200mL of anhydrous ethanol, followed by 50mL of ethanol solution containing 4g of chloroplatinic acid. The mixture was stirred at room temperature for 1h, then 1.35g of polyvinylpyrrolidone and 2g of sodium borohydride were added. The mixture was stirred for 4h, washed, and dried to obtain the catalyst.
[0027] Comparative Example 4 The difference from Example 3 is that step S4 was not performed.
[0028] A method for preparing a catalyst includes the following steps: S1. Preparation of S-doped Ni-Al composite layered metal oxide: 20 mmol nickel nitrate, 20 mmol aluminum nitrate and 1.5 mmol thiourea were dissolved in 200 mL water, and 12 wt% NaOH solution was added dropwise to adjust the pH of the solution to 8. The solution was heated to 90 °C and crystallized for 30 min. After filtration, washing and drying, the solution was calcined at 550 °C for 3 h to obtain S-doped Ni-Al composite layered metal oxide. S2. Preparation of S-doped Ni-Al composite layered metal oxide / SiO2 composite: 11g of tetraethyl orthosilicate was added to 100mL of ethanol, 20g of S-doped Ni-Al composite layered metal oxide was added, the mixture was stirred and mixed for 10min, 2.5g of ammonia was added dropwise, the mixture was heated to 45℃ and reacted for 11h, filtered, washed and dried to obtain S-doped Ni-Al composite layered metal oxide / SiO2 composite; S3. S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide: 0.15 g of 5.7 mol / L concentrated nitric acid and 0.85 g of copper nitrate were added to 50 mL of water to prepare mixture A. 1.1 g of S-doped Ni-Al composite layered metal oxide / SiO2 complex and 0.6 g of ammonium tungstate were added to 80 mL of water and stirred to dissolve to prepare mixture B. Mixture A was added dropwise to mixture B and stirred to carry out a co-precipitation reaction for 1 h. The mixture was then filtered, washed, dried, and calcined at 350 °C for 2 h to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide. S4. Catalyst preparation: 17g of S-doped Ni-Al composite layered metal oxide / SiO2 complex supported on W / Cu oxide was added to 200mL of anhydrous ethanol, followed by 50mL of ethanol solution containing 4g of chloroplatinic acid. The mixture was stirred at room temperature for 1h, then 1.35g of polyvinylpyrrolidone and 2g of sodium borohydride were added. The mixture was stirred for 4h, washed, and dried to obtain the catalyst.
[0029] Comparative Example 5. The difference from Example 3 is that step S5 was not performed.
[0030] A method for preparing a catalyst includes the following steps: S1. Preparation of S-doped Ni-Al composite layered metal oxide: 20 mmol nickel nitrate, 20 mmol aluminum nitrate and 1.5 mmol thiourea were dissolved in 200 mL water, and 12 wt% NaOH solution was added dropwise to adjust the pH of the solution to 8. The solution was heated to 90 °C and crystallized for 30 min. After filtration, washing and drying, the solution was calcined at 550 °C for 3 h to obtain S-doped Ni-Al composite layered metal oxide. S2. Preparation of S-doped Ni-Al composite layered metal oxide / SiO2 composite: 11g of tetraethyl orthosilicate was added to 100mL of ethanol, 20g of S-doped Ni-Al composite layered metal oxide was added, the mixture was stirred and mixed for 10min, 2.5g of ammonia was added dropwise, the mixture was heated to 45℃ and reacted for 11h, filtered, washed and dried to obtain S-doped Ni-Al composite layered metal oxide / SiO2 composite; S3. S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide: 0.15 g of 5.7 mol / L concentrated nitric acid and 0.85 g of copper nitrate were added to 50 mL of water to prepare mixture A. 1.1 g of S-doped Ni-Al composite layered metal oxide / SiO2 complex and 0.6 g of ammonium tungstate were added to 80 mL of water and stirred to dissolve to prepare mixture B. Mixture A was added dropwise to mixture B and stirred to carry out a co-precipitation reaction for 1 h. The mixture was then filtered, washed, dried, and calcined at 350 °C for 2 h to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide. S4. Reduction: The S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu oxide was reduced by hydrogen gas at 700℃ for 3 hours in a tube furnace with strong drainage and permeability. The hydrogen gas flow rate was 17 L / min. The resulting S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu was used as the catalyst.
[0031] Test Example 1 The specific surface area and total pore volume of the catalysts prepared in Examples 1-3 and Comparative Examples 1-5 were determined using a 3-FLEX 3500 multi-station high-throughput gas adsorption analyzer. The results are shown in Table 1.
[0032] Table 1
[0033] As can be seen from the table above, the catalysts prepared in Examples 1-3 of this invention have a large specific surface area and total pore volume.
[0034] Catalyst testing: 1.0 g of the above solid catalyst was weighed and reacted in a micro fixed-bed reactor at a reaction temperature of 250-300℃ to synthesize 3-methylpyridine; the sample was analyzed by an Agilent 7820 gas chromatograph, and the results are shown in Table 2 below.
[0035] Example 4 2-Methylpentanilonitrile was subjected to a hydrogenation-dehydrogenation reaction in the presence of a catalyst at a temperature of 250°C and a hydrogen-to-nitrile ratio of 1000. The 2-methylpentanilonitrile was 2-methylpentanilonitrile with a purity >99.9%. The liquid hourly space velocity was 2 / h. The catalyst was the one prepared in Example 1 and was added at 50% of the total system volume. The product obtained was 3-methylpyridine, and the byproduct was amino-3-methylpyridine.
[0036] Example 5 2-Methylpentanilonitrile was subjected to a hydrogenation-dehydrogenation reaction in the presence of a catalyst at a temperature of 300°C and a hydrogen-to-nitrile ratio of 1400. The 2-methylpentanilonitrile was 2-methylpentanilonitrile with a purity >99.9%. The liquid hourly space velocity was 2 / h. The catalyst was the one prepared in Example 2 and was added at 50% of the total system volume. The product obtained was 3-methylpyridine, and the byproduct was amino-3-methylpyridine.
[0037] Example 6 This embodiment provides a method for the efficient synthesis of 3-methylpyridine. 2-methylpentanilide is subjected to a hydrogenation-dehydrogenation reaction under the action of a catalyst at a temperature of 280°C and a hydrogen-to-nitrile ratio of 1300. The 2-methylpentanilide is 2-methylpentanilide with a purity >99.9%. The liquid hourly space velocity is 2 / h. The catalyst is the one prepared in Example 3, and its addition amount is 1 wt% of the total system mass. The product obtained is 3-methylpyridine, and the byproduct is amino-3-methylpyridine.
[0038] Comparative Example 6 The difference from Example 6 is that the catalyst used is the catalyst prepared in Comparative Example 1.
[0039] Comparative Example 7 The difference from Example 6 is that the catalyst used is the catalyst prepared in Comparative Example 2.
[0040] Comparative Example 8 The difference from Example 6 is that the catalyst used is the catalyst prepared in Comparative Example 3.
[0041] Comparative Example 9 The difference from Example 6 is that the catalyst used is the catalyst prepared in Comparative Example 4.
[0042] Comparative Example 10 The difference from Example 6 is that the catalyst used is the catalyst prepared in Comparative Example 5.
[0043] Test Example 2 The methods for preparing 3-methylpyridine in Examples 4-6 and Comparative Examples 6-10 were analyzed. The results are shown in Table 2.
[0044] Table 2
[0045] As can be seen from the table above, the methods in Examples 4-6 of this invention have a high conversion rate of 2-methylpentanilide and good selectivity in the production of 3-methylpyridine.
[0046] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a catalyst, characterized in that, The catalyst is prepared as follows: S1. Preparation of S-doped Ni-Al composite layered metal oxide: Nickel nitrate, aluminum nitrate and thiourea were dissolved in water, alkaline solution was added dropwise, heated to crystallize, filtered, washed, dried and calcined to obtain S-doped Ni-Al composite layered metal oxide; S2. Preparation of S-doped Ni-Al composite layered metal oxide / SiO2 composite: Tetraethyl orthosilicate was added to ethanol, then S-doped Ni-Al composite layered metal oxide was added, stirred and mixed evenly, ammonia was added dropwise, heated and reacted, filtered, washed and dried to obtain S-doped Ni-Al composite layered metal oxide / SiO2 composite. S3. S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide: Concentrated nitric acid and copper nitrate were added to water to prepare mixture A. The S-doped Ni-Al composite layered metal oxide / SiO2 complex and ammonium tungstate were added to water and stirred to dissolve to prepare mixture B. Mixture A was added dropwise to mixture B and stirred to carry out co-precipitation reaction. The mixture was filtered, washed, dried and calcined to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide. S4. Reduction: The S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu oxide is reduced by low-temperature hydrogen gas to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu. S5. Catalyst preparation: The S-doped Ni-Al composite layered metal oxide / SiO2 complex supported on W / Cu was added to anhydrous ethanol, followed by the addition of an ethanol solution of chloroplatinic acid. The mixture was stirred at room temperature, and then polyvinylpyrrolidone and sodium borohydride were added. The mixture was stirred and reacted, washed, and dried to obtain the catalyst.
2. The method according to claim 1, characterized in that, In step S1, the molar ratio of nickel nitrate, aluminum nitrate, and thiourea is 1:1:0.05-0.1; the pH of the solution is adjusted to 7.5-8.5 by adding alkali solution; the temperature for heating and crystallization is 85-95℃ and the time is 20-40 min; and the temperature for calcination is 500-600℃ and the time is 2-4 h.
3. The method according to claim 1, characterized in that, In step S2, the mass ratio of tetraethyl orthosilicate, S-doped Ni-Al composite layered metal oxide, and ammonia is 10-12:17-25:2-3, and the heating reaction temperature is 40-50℃ for 10-12 hours.
4. The method according to claim 1, characterized in that, In step S3, the concentration of concentrated nitric acid is 5.5-6 mol / L, the mass ratio of concentrated nitric acid to copper nitrate is 1-2:7-10, the mass ratio of S-doped Ni-Al composite layered metal oxide / SiO2 composite to ammonium tungstate is 10-12:5-7, the co-precipitation reaction time is 0.5-1 h, and the calcination temperature is 300-400℃ for 1-3 h.
5. The method according to claim 1, characterized in that, The low-temperature hydrogen reduction in step S4 is carried out in a forced-drainage permeable tubular furnace at 650-750℃ for 2-4 hours with hydrogen flow rate of 15-20 L / min.
6. The method according to claim 1, characterized in that, In step S5, the mass ratio of the S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu, chloroplatinic acid, polyvinylpyrrolidone, and sodium borohydride is 15-20:3-5:1.2-1.5:1.9-2.2, and the stirring reaction time is 3-5 hours.
7. The method according to claim 1, characterized in that, Specifically, the following steps are included: S1. Preparation of S-doped Ni-Al composite layered metal oxide: Dissolve 1 molar equivalent of nickel nitrate, 1 molar equivalent of aluminum nitrate, and 0.05-0.1 molar equivalent of thiourea in water, add 10-15 wt% NaOH solution to adjust the pH of the solution to 7.5-8.5, heat to 85-95℃, crystallize for 20-40 min, filter, wash, dry, and calcine at 500-600℃ for 2-4 h to obtain S-doped Ni-Al composite layered metal oxide; S2. Preparation of S-doped Ni-Al composite layered metal oxide / SiO2 composite: 10-12 parts by weight of tetraethyl orthosilicate were added to ethanol, and 17-25 parts by weight of S-doped Ni-Al composite layered metal oxide were added. The mixture was stirred and mixed evenly. 2-3 parts by weight of ammonia water were added dropwise. The mixture was heated to 40-50℃ and reacted for 10-12 h. The mixture was filtered, washed, and dried to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 composite. S3. S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide: 1-2 parts by weight of 5.5-6 mol / L concentrated nitric acid and 7-10 parts by weight of copper nitrate were added to water to prepare mixture A. 10-12 parts by weight of S-doped Ni-Al composite layered metal oxide / SiO2 complex and 5-7 parts by weight of ammonium tungstate were added to water and stirred to dissolve to prepare mixture B. Mixture A was added dropwise to mixture B and stirred to carry out a co-precipitation reaction for 0.5-1 h. The mixture was then filtered, washed, dried, and calcined at 300-400℃ for 1-3 h to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 complex loaded with W / Cu oxide. S4. Reduction: The S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu oxide was reduced by hydrogen gas at 650-750℃ for 2-4 hours in a tube furnace with strong drainage and permeability, with a hydrogen gas flow rate of 15-20 L / min, to obtain the S-doped Ni-Al composite layered metal oxide / SiO2 composite loaded with W / Cu. S5. Catalyst preparation: 15-20 parts by weight of S-doped Ni-Al composite layered metal oxide / SiO2 complex supported on W / Cu were added to anhydrous ethanol, followed by the addition of an ethanol solution containing 3-5 parts by weight of chloroplatinic acid. The mixture was stirred at room temperature for 0.5-1 h, then 1.2-1.5 parts by weight of polyvinylpyrrolidone and 1.9-2.2 parts by weight of sodium borohydride were added. The mixture was stirred for 3-5 h, washed, and dried to obtain the catalyst.
8. A catalyst prepared by the method according to any one of claims 1-7.
9. A method for the efficient synthesis of 3-methylpyridine, characterized in that, 2-Methylpentanilide is subjected to a hydrogenation-dehydrogenation reaction under the action of the catalyst described in claim 8 to obtain the product 3-methylpyridine, and the byproduct is amino-3-methylpyridine.
10. The method according to claim 9, characterized in that, The reaction temperature is 250-300℃, the hydrogen-to-nitrogen ratio is 1000-1400, and the 2-methylpentanilonitrile is 2-methylpentanilonitrile with a purity >99.9%.
Citation Information
Patent Citations
Method for making methylpentamethylene diamine and methylpiperidine
CN101990532A
Method for preparing 2-methyl pentamethylene diamine and 3-methylpiperidine by hydrogenation of 2-methyl-pentanedinitrile
CN107365257A
A method for producing a nano-attapulgite composite catalyst for the preparation of 3-methylpyridine
CN107983398B
Preparation of pyridines or pyrroles from alpha , omega -dinitriles
US4521602A
Non-amphoteric, quaternisable and water-soluble polymers for modifying the surface charge of solid particles
CN107075712A