A porous composite medium, its preparation method and application
By using a variety of high-molecular polymer fibers sintered to form porous composite media, the problems of insufficient flux and mechanical strength are solved, and a porous composite media with high flux and excellent mechanical properties is realized, which is suitable for filtration and adsorption materials.
Patent Information
- Application Number
- CN202411382750.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-09-30
AI Technical Summary
Existing porous polymer composite media suffer from low flux and insufficient mechanical strength during preparation, making it difficult to maintain efficient filtration and adsorption performance under harsh environments.
At least two types of high-molecular polymer fibers, including polyethylene and polymer A (such as polypropylene, polyethylene terephthalate, etc.), are used to form a porous structure by sintering, forming aggregates to improve porosity and mechanical strength. The SEM average diameter of the polymer fibers and the characteristics of the aggregates are measured by scanning electron microscopy.
It achieves high throughput and excellent mechanical strength, is suitable for gas and liquid filtration, has high porosity and pressure resistance, can effectively trap micron-sized impurities, and extends service life.
Smart Images

Figure CN119303380B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer materials technology, specifically to a porous composite medium, its preparation method, and its application. Background Technology
[0002] Porous polymeric composite media are porous composite media prepared from high molecular weight polymers (such as polyolefins and polyesters). They can be used as filter materials (such as filter cartridges), adsorbents, and various carriers (such as catalyst carriers). Porous polymeric composite media also possess resistance to acid, alkali, and other organic solvents, as well as high strength and good temperature resistance, enabling them to maintain efficient filtration and adsorption performance even in harsh environments. These properties make porous polymeric composite media important components in equipment used in water treatment and gas treatment, and they can also be used as carriers and scaffolds in biomedical engineering, as well as as carriers, filter materials, and adsorbents in the chemical industry, showing broad application prospects.
[0003] One major preparation method for porous polymer composite media is powder sintering. The main steps involve pressing powder into a compact and heating it to a temperature below the melting point of the main components. Due to physicochemical reactions such as bonding between particles, the desired strength and properties of the material or product are obtained. CN102553353A discloses a microporous filter medium, which is formed by adding a composite material to high-molecular-weight polyethylene powder and sintering it. The composite material forms a flexible mesh between the high-molecular-weight polyethylene powder particles, supporting the bonded structure of the polyethylene powder. Compared to porous composite media materials prepared by methods such as phase inversion, sintering can typically produce porous composite media materials with complex shapes and structures, higher mechanical strength, and a more uniform microstructure, reducing defects and impurities. However, the porosity of the resulting porous filter element is relatively low, generally only 20-40%, resulting in lower flux and slower filtration speed. Furthermore, it is prone to powder shedding, affecting cleanliness.
[0004] Another common preparation process for porous polymer composite media is the preparation of multilayer polymer materials by hot pressing or ultrasonic pressing. For example, CN101559326A provides a nanofiber ultrafiltration membrane and its preparation method, which includes the following steps: (1) one or two polymer spinning solutions are sprayed onto a horizontally moving receiving roller through one or two spinnerets for electrospinning. During the spinning process, the weight concentration of the spinning solution gradually decreases to obtain an electrospun nonwoven fabric; (2) then hot pressing is performed to obtain a nanofiber ultrafiltration membrane. This preparation method can produce materials with high porosity, but the mechanical strength is poor, the industrial applicability is poor, and the application scenarios are severely limited.
[0005] Therefore, it is urgent to develop a porous composite medium with high throughput and excellent mechanical strength. Summary of the Invention
[0006] The purpose of this invention is to overcome the above-mentioned problems existing in the prior art and provide a porous composite medium that can combine high throughput and excellent mechanical strength (high hardness and pressure resistance), and is suitable for use as a porous composite medium for gas filtration and liquid filtration, with broad application prospects.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: a porous composite medium comprising polymer fibers for forming a porous structure, wherein the polymer constituting the polymer fibers comprises polyethylene (PE) and polymer A, wherein polymer A comprises at least one of polypropylene (PP), polyethylene terephthalate (PET), polyamide (PA), polybutylene terephthalate (PBT), and polypropylene terephthalate (PTT), and the SEM average diameter of the polymer fibers is 5μm-40μm (e.g., 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm);
[0008] The porous composite medium contains several aggregates formed by sintering the polymer fibers; the average pore size (PMI) of the porous composite medium is 0.1 μm-5 μm (e.g., 0.1 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm), and the porosity is 40%-80% (e.g., 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%).
[0009] The porous composite medium of this invention is sintered from polymer fibers. Compared to powder sintering, the medium formed by fiber sintering is more conducive to obtaining higher porosity and higher flux. Furthermore, instead of using a single polymer, at least two polymers are selected as raw materials. Specifically, the polymers constituting the polymer fibers include polyethylene (PE) and polymer A, where PE acts as a binder and polymer A acts as a supporting framework. This composition facilitates the formation of aggregates (while single polymers are unlikely to form the aggregates required by this invention), resulting in a product with excellent flux (air permeability or liquid flux) and mechanical strength. It also solves the problem of poor heat shrinkage resistance of single polymers such as pure PP.
[0010] Moreover, compared to single polymers, polymer A in the composition of composite media can impart different properties to the product, making it suitable for various application scenarios. For example, when polymer A is PP, the porous composite media will have higher temperature resistance and wear resistance; while compared to PP, when polymer A is PET, combining it with PE is more conducive to further improving the hardness of the composite media. Combining PA with PE can prepare composite media that have both the softness and chemical resistance of PE and the high strength and wear resistance of PA. PBT is a variant of PET, with similar chemical stability and thermoplasticity, although some physical properties are slightly different. Composite media containing PE / PBT may combine the flexibility of PE with the specific performance advantages of PBT. PTT has excellent heat resistance, chemical resistance, and good elasticity, and the porous composite media obtained by combining it with PE has even higher heat resistance and elasticity. It should be understood that, for performance improvement, inorganic fibers such as glass fiber and carbon fiber can also be doped into the porous composite media to prepare composite media with high strength, high modulus, or special functions.
[0011] The average pore size (PMI) can reflect the overall pore size of a porous composite medium to some extent; a larger PMI value indicates a larger overall pore size. This value significantly affects the flux and impurity retention efficiency of the porous composite medium. In this invention, the composite medium sintered from at least two polymer raw materials has an average PMI pore size of 0.1 μm-5 μm, meaning it is a micron-level porous composite medium with relatively large, but not excessively large, pores. Its performance is fundamentally different from nano-level porous composite media and fabrics with visible pores. The average PMI pore size can be obtained using a PMI pore size meter. The porous composite medium of this invention can be cylindrical, cuboid, or other shapes required by the customer. This porous composite medium includes two end faces (outer surfaces), and the average PMI pore size is measured from one end face to the other.
[0012] The porosity testing method of this invention is mercury porosimetry. Those skilled in the art can also obtain porosity through other measurement methods; the aforementioned measurement methods are for reference only. Mercury porosimetry testing shows that the porosity of the porous composite medium of this invention is 40%-80%, indicating that the composite medium has a relatively large porosity and a large number of pores, which is beneficial for the overall high flux of the porous composite medium. Under the synergistic effect of the average pore size (PMI) and porosity of the composite medium, a high flux and fast filtration speed are ensured, along with a high dirt-holding capacity, enabling it to trap and accommodate a large number of impurity particles and resulting in a long service life.
[0013] Generally, if the pores of a porous composite medium are large and the porosity is high, its mechanical strength is usually low, especially under high pressure, the pores are prone to shrinkage or collapse, resulting in a short service life. However, in this invention, it was found that the composite medium, while having high porosity and large pore size, also possesses high mechanical strength (both its hardness and compressive strength are high). Upon observation of its microstructure, several agglomerates (at least two agglomerates) were unexpectedly discovered within the porous composite medium. The appearance of these agglomerates is likely due to the bonding at the contact points between polymer fibers during sintering, based on the use of at least two fiber raw materials. This causes the originally dispersed fibers to tightly bind together and gradually expand to form relatively dense sintered agglomerates. The relatively dense sintered agglomerates significantly enhance the mechanical properties of the porous composite medium. Furthermore, the presence of these agglomerates makes the composite medium less prone to stratification, reducing the likelihood of powder, fiber, or particle shedding, resulting in high product quality stability and greatly ensuring the cleanliness of the filtered material.
[0014] In the porous composite medium of the present invention, under the synergistic effect of aggregates and free fibers of a certain thickness (there are a certain number of aggregates and a certain number of relatively free polymer fibers in the composite medium), non-directional tortuous pathways are formed (the non-directional tortuous pathways refer to randomly oriented groove structures and / or discretely distributed pore structures, and each non-directional tortuous pathway is interconnected), ensuring that the composite medium can fully and effectively retain impurity particles of a certain size (mainly micron-sized impurities), with high retention efficiency.
[0015] The average diameter of polymer fibers in the composite medium via SEM and other features of the aggregates can be characterized by scanning electron microscopy of the cross-section of the composite medium, followed by measurement and calculation using computer software (such as Matlab, NIS-Elements, etc.) or by hand.
[0016] In actual measurement, the cross-section (thickness direction) of the composite medium can be characterized using an electron microscope to obtain the corresponding SEM image. Since the distribution of polymer fibers and aggregates is roughly uniform, a certain area, such as 1 mm², can be selected. 2 (1mm x 1mm) or 10000μm 2 (100μm x 100μm), the specific area size depends on the actual situation. Then, the diameter of the polymer fiber and the various characteristics of the agglomerate on this area are measured by appropriate computer software or manually. Several tests are performed (preferably more than 10 times, the specific number depends on the situation), and the average value is taken to obtain the average SEM diameter of the polymer fiber and the average value of various characteristics of the agglomerate. Of course, those skilled in the art can also obtain the above parameters by other measurement methods. The above measurement methods are for reference only.
[0017] As a further improvement of the present invention, the SEM average diameter of the polymer fiber is 8μm-35μm; and / or, the PMI average pore size of the porous composite medium is 0.3μm-3.5μm;
[0018] And / or, the porosity of the porous composite medium is 45%-75%.
[0019] Fibers of suitable thickness provide mechanical strength to porous composite media and also offer a certain adsorption effect, further improving retention efficiency and fully capturing various substances. The thickness of the polymer fibers affects the stability of the pores in the porous composite media. When the fiber diameter is larger, it has higher mechanical strength, especially under higher pressure, it is less prone to breakage or deformation, avoiding pore shrinkage or collapse, thus ensuring high throughput during long-term use and extending the product's service life. When the PMI (Polymer Mixture Index) of the porous composite media, its average pore size, porosity, and fiber diameter all meet certain ranges simultaneously, their synergistic effect allows the composite media to effectively retain impurity particles of a certain size (mainly micron-sized impurities), further improving the retention efficiency and throughput stability of the porous composite media. Simultaneously, it ensures excellent mechanical properties, significantly improving the hardness and compressive strength of the porous composite media.
[0020] As a further improvement of the present invention, the average SEM area of the aggregates in the cross-section of the porous composite medium is 3000 μm. 2 -50000μm 2 For example, 3000μm 2 5000μm 2 10000μm 2 20000μm 2 30000μm 240000μm 2 50000μm 2 ;
[0021] And / or, in the cross-section of the porous composite medium, the density of the aggregates is 3-70 aggregates / mm. 2 For example, 3 per 1mm 2 10 pieces / 1mm 2 20 pieces / 1mm 2 30 pieces / 1mm 2 40 pieces / 1mm 2 50 pieces / 1mm 2 60 pieces / 1mm 2 70 pieces / 1mm 2 .
[0022] In this invention, some small aggregates exist in the porous composite medium. To facilitate statistical analysis of the aggregates in the SEM images, aggregates with an SEM area of less than 500 μm are excluded. 2 Aggregates were ignored in the calculation; only SEM areas of 500 μm were considered. 2 The above aggregates.
[0023] Aggregates are relatively dense regions inside porous composite media. It is the presence of aggregates that improves the overall mechanical strength of porous composite media. Further research has found that the area and density (the number within a certain area) of aggregates also affect the pore distribution of porous composite media. When their area is too large or too small, the average pore size and porosity of the porous composite media may not be able to reach the ranges mentioned above, thus affecting the various performance characteristics of the product. If the agglomerates are too small in area or too few in number (too low in density), the mechanical strength (hardness and compressive strength) of the porous composite medium will still be relatively poor and will not be significantly improved. Furthermore, when used under high pressure, there is still a risk of stratification within the porous composite medium. Conversely, if the number of agglomerates is too large or the area is too large, it may mean a reduction in the number of free fibers, which not only easily leads to a lower overall porosity and flux of the composite medium, but also affects the retention efficiency of various impurities, resulting in lower dirt holding capacity and a shorter product lifespan. Therefore, agglomerates of a certain density and size can ensure that the composite medium as a whole has high flux and mechanical strength, while also efficiently retaining various impurities, resulting in high dirt holding capacity and a long service life.
[0024] In this invention, the SEM average area and density of the aggregates can be obtained by characterizing the cross-section of the composite medium using a scanning electron microscope, then selecting a certain area (the specific area size depends on the actual situation), and then measuring it using computer software (such as Matlab, NIS-Elements, etc.) or manually to obtain the area and number of aggregates in that area. Further calculations are then performed to obtain the SEM average area and corresponding density of the aggregates.
[0025] As a further improvement of the present invention, on the cross section of the porous composite medium, with the thickness direction of the porous composite medium as the y-axis, the average SEM size d1 of the aggregate along the y-axis direction is 50μm-500μm, for example, 50μm, 100μm, 200μm, 300μm, 400μm, 500μm;
[0026] And / or, the average SEM size d2 perpendicular to the y-axis direction is 60μm-800μm, for example, 60μm, 100μm, 200μm, 400μm, 600μm, 800μm.
[0027] When using porous composite media for filtration, the material to be filtered often moves along the thickness direction of the composite media, meaning filtration occurs in this direction. Therefore, higher requirements are placed on the mechanical strength of the composite media in this direction. Research has found that when the agglomerates are flat, i.e., d1 is too small, the mechanical strength in the thickness direction is low, and under high pressure, the porous composite media is more prone to stratification. Sintered agglomerates with a suitable d1 in the thickness direction ensure that the porous composite media is less prone to stratification during filtration, improving its retention performance and service life while also exhibiting higher mechanical properties. When both d1 and d2 are within a suitable range, the agglomerate size is appropriate, and the connection methods between different agglomerates within the porous composite media are varied. This results in suitable non-directional tortuous pathways, reducing the proportion of closed pores. While ensuring high mechanical properties, this also provides higher retention efficiency and dirt-holding capacity, thus extending the filtration life of the porous composite media.
[0028] As a further improvement of the present invention, the ratio of d1 to the thickness T of the porous composite medium, d1 / T, is 1.5%-20%, for example, 1.5%, 2%, 5%, 10%, 15%, 20%, preferably 2%-15%.
[0029] And / or, in the thickness direction of the cross section of the porous composite medium, the ratio of the sum of the agglomerates d1 to the thickness T of the porous composite medium is 20%-60%, for example, 20%, 30%, 40%, 50%, 60%.
[0030] The proportion of individual agglomerates and the sum of agglomerate thicknesses to the thickness of the porous composite medium in the thickness direction affects the size and number of agglomerates. With a fixed thickness, larger individual agglomerates can accommodate fewer agglomerates, potentially leading to excessively large sums of agglomerate thicknesses. This hinders the formation of non-directional tortuous pathways and negatively impacts the uniformity of thickness and mechanical strength. Under high pressure, this increases the risk of breakage or damage, resulting in lower porosity and the formation of closed pores, reducing the flux and contaminant holding capacity of the porous composite medium and shortening its lifespan. Conversely, when the proportion of individual agglomerate thickness is too small, closed pores are also easily formed, creating more ineffective pores, further reducing the flux and contaminant holding capacity of the porous composite medium and shortening its lifespan. Furthermore, it increases the risk of internal stratification within the porous composite medium, and also reduces its mechanical properties. When it meets the aforementioned range, it is conducive to the formation of non-directional tortuous channels and improves the mechanical strength of the product, thereby having a positive impact on the filtration and air permeability of the product; at the same time, it is also conducive to improving the stability and thickness uniformity of the product, avoiding tearing, breakage, flaking, damage and delamination.
[0031] As a further improvement of the present invention, the ratio of the SEM average diameter of the polymer fiber to d1 is 1:2-10, for example, 1:2, 1:4, 1:6, 1:8, or 1:10;
[0032] And / or, d1 / d2 is 1:1.2-8, for example, 1:1.2, 1:2, 1:4, 1:6, 1:8, preferably 1:1.5-5.
[0033] The diameter of polymer fibers affects the formation and stability of aggregates. For example, if the fiber diameter is too large, its mechanical strength is relatively high, and it is not easy to bond together during sintering. Even if aggregates are formed, they are easy to disperse under pressure during high-pressure filtration, resulting in a short lifespan of the composite medium. If the diameter is too small, it is easy to form excessively large aggregates, which is not conducive to improving the mechanical strength, flux, and dirt holding capacity of the composite medium. When the ratio of fiber diameter to d1 of aggregates meets this range, the free fibers and aggregates can be kept in a good ratio, which is conducive to the formation of non-directional tortuous channels. The composite medium has higher mechanical properties, higher flux, and higher dirt holding capacity.
[0034] When d1 / d2 is within the above range, the cross-section of the aggregates is more of a near rectangle with a small length-to-width ratio, which is conducive to improving the mechanical strength of the product and the formation of non-directional tortuous channels, reducing the generation of closed pores, and giving the composite medium good filtration performance. At the same time, when the ratio of fiber diameter to aggregate d1 is within the range, the composite medium can have excellent mechanical and filtration performance, ensuring that it can maintain a high throughput level for a long time during filtration, and giving the product a long service life.
[0035] As a further improvement of the present invention, the surface of the porous composite medium was subjected to infrared absorption spectroscopy testing using the ATR method, and the results were obtained at 710 cm⁻¹. -1 -730cm -1 There is a first peak at 2910 cm. -1 -2930cm -1 A second peak exists, and the ratio of the peak area of the first peak to the peak area of the second peak is the relative peak area X of polyethylene. The relative peak area X of polyethylene is 0.01-4, for example, 0.01, 0.05, 0.1, 0.5, 1, 2, 3, 4; the SEM average diameter of the polymer fiber is 10μm-30μm, for example, 10μm, 15μm, 20μm, 25μm, 30μm.
[0036] Research has revealed that PE exhibits a high infrared spectrum at 720 cm⁻¹ in composite media. -1 The location exhibits a crystallization absorption peak, the value of which is influenced by various factors such as PE content, PE crystallization status, and crystal form. Furthermore, the magnitude of this value significantly affects the mechanical strength, heat resistance, and other properties of the porous composite medium. Specifically, at 720 cm⁻¹... -1 The size of the crystal absorption peak near the location can, to some extent, characteristically reflect the presence, content, and crystallization status of PE in the composite medium. The peak size at 2920 cm⁻¹... -1 The second peak near the first peak serves as the internal standard peak (standard peak) for PE. It corresponds to the unique methylene asymmetric stretching vibration of PE, which avoids interference from polymer A absorption; therefore, it is used as the internal standard peak for PE. The ratio of the peak areas of the first and second peaks reflects the relative peak area X of PE (the reason for using a ratio is that research has found that only 720 cm⁻¹ is needed). -1The size of the absorption peak near the location of the crystallization can vary greatly and cannot accurately represent the various properties of the composite medium. To a certain extent, it can reflect the comprehensive factors such as the PE content range in the composite medium and the crystallization of PE after sintering. Furthermore, the relative peak area X of polyethylene is 0.01-4. When X is too high or too low, it means that the PE content as a binder is too high or too low, and the crystallinity is too high or too low. These are not conducive to the formation of agglomerates, and the stability of the formed agglomerates will also be deviated (agglomerates formed with fibers are easily separated under high pressure). When X is within this range, and at the same time the average SEM diameter of the polymer fibers is 10-30μm, it is conducive to the formation of agglomerates of appropriate size, and the composite medium has a suitable degree of crystallinity, thereby improving the mechanical properties and filtration performance of the product.
[0037] As a further improvement of the present invention, when polymer A contains polypropylene, the surface of the porous composite medium is subjected to infrared absorption spectroscopy testing using the ATR method, and the result is obtained at 965 cm⁻¹. -1 -975cm -1 A third peak exists at 2940 cm⁻¹. -1 -2960cm -1 A fourth peak exists, and the ratio of the peak area of the third peak to the peak area of the fourth peak is the relative peak area Y of polypropylene. The relative peak area Y of polypropylene is 0.1-0.8, for example, 0.1, 0.2, 0.4, 0.6, 0.8.
[0038] Preferably, X / Y is 0.01-1, such as 0.01, 0.05, 0.1, 0.5, or 1.
[0039] Similar to PE, a characteristic peak in the infrared spectrum can reflect the content, crystallinity, and crystal form of polymer A in the composite medium. However, the characteristic absorption peaks in the infrared spectrum differ depending on the type of polymer A. Specifically, for polymer A containing PP, studies have found that the characteristic absorption peak at 973 cm⁻¹... -1 The location exhibits a crystallization absorption peak that characteristically reflects the PP content and crystallization status in the composite medium. The peak at 2949 cm⁻¹ is... -1 The fourth peak near the location is an internal standard peak for PP, corresponding to the unique methyl asymmetric stretching vibration of PP. This vibration avoids interference from PE absorption, hence it is used as the internal standard peak for PP. Compared to the peak area of the third peak, the ratio of the peak areas of the third and fourth peaks, i.e., the relative peak area Y of PP, more accurately reflects the content range of PP in the composite medium and the crystallization status of PP after sintering.
[0040] The study also found that the values of X and Y differed in composite media containing different polymers A. When polymer A was PP, Y was 0.1-0.8. If X and Y were too high or too low, it meant that the content of PP and PE was too high or too low, and the crystallinity was too high or too low, which was not conducive to the formation of agglomerates. Furthermore, the mechanical properties of the composite media would deviate, and the stability of the pores would also deviate (collapse or shrinkage may occur). When X and Y met the specified range, especially when X / Y was 0.01-1, it was more conducive to the formation of stable agglomerates and non-directional tortuous pathways, giving the composite media excellent mechanical and filtration properties.
[0041] As a further improvement of the present invention, when polymer A contains polyethylene terephthalate (PET), the surface of the porous composite medium is subjected to infrared absorption spectroscopy testing using the ATR method, and the infrared absorption spectrum is measured at 838 cm⁻¹. -1 -858cm -1 A fifth peak exists at 1709 cm⁻¹. -1 -1729cm -1 A sixth peak exists, and the ratio of the peak area of the fifth peak to the peak area of the sixth peak is the relative peak area Z of polyethylene terephthalate. The relative peak area Z of polyethylene terephthalate is 0.01-0.5, for example, 0.01, 0.05, 0.1, 0.5; preferably, X / Z is 20-40, for example, 20, 25, 30, 35, 40.
[0042] For polymer A containing PET, the study found that at 848cm -1 The location exhibits a characteristic absorption peak at 1719 cm⁻¹, reflecting the PP content and crystallization status of the composite medium. -1 The sixth peak near the position is the internal standard peak of PET, corresponding to the unique ester carbonyl stretching vibration of PET. Avoiding interference from PE absorption, it is therefore used as the internal standard peak of PET. Compared to the peak area of the fifth peak, the ratio of the peak areas of the fifth and sixth peaks, i.e., the relative peak area Z of PET, can more accurately reflect the content range of PET in the composite medium and the crystallization state of PET after sintering. In a similar case to PP, when polymer A is PET, Z is 0.01-0.5. If X and Z are too high or too low, it means that the content of PET and PE is too high or too low, and the crystallinity is too high or too low, both of which are unfavorable for the formation of agglomerates. Furthermore, the mechanical properties of the composite medium will deviate, and the stability of the pores will also deviate (collapse or shrinkage may occur). When X and Z meet the specified range, especially when X / Z is further satisfied at 20-40, it is more conducive to the formation of stable agglomerates and non-directional tortuous pathways, giving the composite medium excellent mechanical and filtration properties.
[0043] It should be understood that during infrared testing, multiple points on the sample can be selected for testing, and then values that deviate too much can be removed before calculating the average value.
[0044] As a further improvement of the present invention, the difference between the maximum pore size and the minimum pore size in the porous composite medium is 100nm-800nm, for example, 100nm, 200nm, 400nm, 600nm, or 800nm.
[0045] And / or, the thickness of the porous composite medium is 1mm-8mm, for example, 1mm, 2mm, 3mm, 4mm, 5mm, 6mm, 7mm, 8mm; and / or, the DSC crystallinity of the porous composite medium is 20%-50%, for example, 20%, 30%, 40%, 50%.
[0046] The difference between the maximum and minimum pore size can be measured using a PMI pore size analyzer; DSC crystallinity can be determined using differential scanning calorimetry (DSC).
[0047] The porous composite medium described in this invention is a micron-sized porous composite medium with a wide pore size distribution when the difference between the maximum and minimum pore sizes is 100nm-800nm. This results in a high specific surface area and permeability, which helps promote the flow of materials within the composite medium and improves filtration efficiency. Simultaneously, the wide pore size distribution of the porous composite medium can more effectively separate particles of different sizes, as larger pores can capture larger impurities, while smaller pores can intercept finer particles, thereby improving the filtration selectivity of the porous composite medium. Furthermore, the larger pores can serve as stress concentration release points and buffer zones for microcrack propagation, helping to disperse the stress on the porous composite medium, thus improving its overall stability and mechanical strength. This reduces wear, deformation, or breakage caused by external factors (such as pressure and temperature) during use, increases dirt holding capacity, reduces clogging problems, extends service life, and lowers maintenance costs.
[0048] In this field, as the thickness of the filter medium increases, its flux decreases, which is detrimental to improving the filtration rate. Therefore, the thickness of the filter medium needs to be controlled at the micrometer level, typically below 500 μm, and it is undesirable for the thickness to reach the millimeter level. The composite medium in this invention is characterized by high porosity, thus providing a porous composite medium with a thickness reaching the millimeter level, expanding the application scenarios of composite media. Increased thickness provides higher mechanical strength, and when combined with a suitable pore size, it can further improve the retention efficiency of the porous composite medium. A thicker specification combined with a wider pore size distribution can retain particles of different sizes, increasing the dirt-holding capacity, broadening the application range, and extending the service life.
[0049] DSC crystallinity reflects the proportion of crystalline regions in the composite medium to a certain extent. The higher the DSC crystallinity, the more crystalline regions there are, the better the orientation of the lattice molecules, and the better the mechanical strength. The present invention has the above-mentioned DSC crystallinity based on the above-mentioned pore size and porosity, indicating that the porous composite medium does not have the problems of excessively high or low crystallinity, that is, it does not have problems such as low bonding strength or powder inclusion. The aggregates in the composite medium are more tightly bonded, the non-directional tortuous pathways are more interconnected, and it is not easy to delaminate. At the same time, it has higher mechanical strength, stronger heat resistance and greater porosity. When combined with thickness, it can further improve the stability of the composite medium, making it less prone to delamination and slag shedding.
[0050] As a further improvement of the present invention, the surface of the porous composite medium includes a plurality of mold wall contact areas; the SEM average width of the mold wall contact areas is 30μm-200μm, for example, 30μm, 50μm, 80μm, 100μm, 150μm, 200μm, preferably 50μm-150μm; the area ratio of the mold wall contact areas is 20%-80%, for example, 20%, 30%, 40%, 50%, 60%, 70%, 80%.
[0051] In this invention, the mold wall contact area is formed when the raw material melts and contacts the inner wall of the mold during sintering. The average SEM width of the mold wall contact area reflects, to some extent, the size of the skeleton material serving as the surface of the porous composite medium. A suitable skeleton base is beneficial for improving the compressive strength of the porous composite medium. Simultaneously, the area ratio of the mold wall contact area represents the solid portion of the contact between the raw material and the mold during sintering; therefore, the area ratio of the mold wall contact area also affects the compressive strength of the composite medium surface during application. The area ratio of the mold wall contact area is calculated as: (SEM average area of the mold wall contact area / SEM average area of the porous composite medium surface), equivalent to 1 minus the surface pore area ratio (surface pore area ratio). When it falls within this range, the compressive strength of the porous composite medium and, for example, the surface compressive strength under various practical application conditions can be further improved.
[0052] In this invention, the relevant SEM features can be obtained by taking images of the porous composite medium using a scanning electron microscope, and then taking multiple points to measure using computer software (such as Matlab, NIS-Elements, etc.) or manually, and taking the average value; of course, it is understood that those skilled in the art can also obtain the above parameters by other measurement methods.
[0053] As a further improvement of the present invention, the flux of the porous composite medium is 0.5-8 L / min@7 kPa, for example, 0.5 L / min@7 kPa, 1 L / min@7 kPa, 2 L / min@7 kPa, 4 L / min@7 kPa, 6 L / min@7 kPa, or 8 L / min@7 kPa;
[0054] And / or; the porous composite medium has a retention efficiency of more than 95% for impurity particles with a particle size of 0.1-10μm (preferably 0.1-5μm), such as 95%, 96%, 97%, 98%, 99% or above;
[0055] And / or, the Shore A hardness of the porous composite medium is not less than 90HA, for example, 90HA, 92HA, 96HA, or 98HA;
[0056] And / or, the compressive strength of the porous composite medium is not less than 65N@1mm, such as 65N@1mm, 70N@1mm, 75N@1mm, 80N@1mm or above.
[0057] Retention and flux tests demonstrate that the composite medium of the present invention not only has efficient retention of various fine impurities, but also excellent flux.
[0058] The flux of the porous composite medium can be tested using an air permeability tester. Adjust the air pressure to the test pressure of 7 kPa, read and record the corresponding flux (test multiple times, preferably more than 3 times, and take the average value). The air permeability area of the porous composite medium is controlled to be within 1 cm². 2 Under the conditions.
[0059] Shore A hardness can be tested using a Shore A hardness tester, and the average value is taken after three tests.
[0060] The compressive strength of porous composite media can be tested by cutting a 1cm wide and 3cm long domed sample of the porous composite media and placing it on a compression testing machine.
[0061] The porous composite medium of the present invention is a hydrophobic material, but it can also be modified to a hydrophilic material by means of a suitable hydrophilic modification process as needed.
[0062] A second aspect of the present invention provides a method for preparing a porous composite medium as described above, the method comprising the following steps:
[0063] (1) A layered material consisting of at least two layers of polymer fibers is pressed to obtain a pressed material, wherein the pressing conditions are such that the compression amount based on the thickness is 50-80% (e.g., 50%, 55%, 60%, 65%, 70%, 75%, 80%).
[0064] (2) The material after pressing is subjected to a first sintering and a second sintering to obtain the sintered material;
[0065] (3) Cool the sintered material to produce a porous composite medium;
[0066] The polymer fiber is composed of polyethylene and polymer A, wherein polymer A contains at least one of polypropylene, polyethylene terephthalate, polyamide, polybutylene terephthalate, and polypropylene terephthalate.
[0067] The conditions for the first sintering include: a temperature of 100-140℃ (e.g., 100℃, 110℃, 120℃, 130℃, 140℃), and a holding time of 10-30min (e.g., 10min, 15min, 20min, 25min, 30min).
[0068] The conditions for the second sintering include: a temperature of 150-180℃ (e.g., 150℃, 160℃, 170℃, 180℃) and a holding time of 10-30min (e.g., 10min, 15min, 20min, 25min, 30min);
[0069] Cooling conditions include a cooling rate of 5-15℃ / min (e.g., 5℃ / min, 8℃ / min, 10℃ / min, 12℃ / min, 15℃ / min).
[0070] The present invention can prepare the porous composite medium described in the first aspect (i.e., the composite medium is formed by sintering multiple layered structures, including two end faces (outer surfaces)) using a layered material containing two polymer fibers by compression sintering. In this invention, controlling the amount of compression is beneficial to the bonding between fibers and the formation of agglomerates during the sintering process, while affecting the formation of pores and porosity (excessive compression will lead to a significant reduction in the porosity of the product), thereby improving the mechanical and physical properties of the product.
[0071] In this invention, the compression percentage (%) refers to 100% minus the thickness of the multilayered material after compression / the thickness of the multilayered material before compression.
[0072] As sintering progresses, during the first sintering process, the PE (polyethylene) in the polymer fibers begins to melt and gradually adheres together over time, initially forming pores of a certain size and number. By controlling the sintering time, incomplete sintering is avoided in the first sintering process, preventing over-sintering during the second sintering process, which significantly reduces porosity. During the second sintering process, with increasing temperature and time, polymer decomposition and rearrangement and bonding of inter-fiber particles occur, forming aggregates. Therefore, the sintering temperature and holding time are key factors affecting the microstructure, causing changes in fiber diameter and the formation of aggregates, which simultaneously influence porosity and complexity. The overall pore size of the composite medium; through appropriate compression and the synergistic effect of two sintering processes, it is beneficial to ensure that the porous composite medium has high throughput and mechanical strength, and the porous composite medium is not prone to stratification inside, enabling high-pressure filtration for a long time and efficient capture of various impurities; in addition, research has found that the cooling rate during the cooling process will further cause different stresses and microstructure changes inside the porous composite medium (the stability of the composite medium pores, the fibers are firmly bonded together to form agglomerates, and further, the agglomerates with the ideal shape in this invention are formed), thereby synergistically affecting the mechanical properties of the porous composite medium and giving it a long service life.
[0073] Specifically, as a further improvement of the present invention, the basis weight of the layered raw material is 50-200 g / m³. 2 For example, 50g / m 2 80g / m 2 100g / m 2 120g / m 2 150g / m 2 180g / m 2 200g / m 2 ;
[0074] And / or, the thickness of the layered material is 0.1-1 mm, for example, 0.1 mm, 0.2 mm, 0.4 mm, 0.6 mm, 0.8 mm, or 1 mm; and / or, the porosity of the layered material is 70-90%, for example, 70%, 75%, 80%, 85%, or 90%; and / or, the moisture content in the layered material is less than 5 wt%, for example, 5 wt%, 4 wt%, 3 wt%, 2 wt%, 1 wt%, or less, preferably less than 1 wt%.
[0075] The layered material can be a conventional material in the field, such as nonwoven fabric. When selecting layered raw materials, research has found that parameters such as basis weight, thickness, and porosity directly affect the structural performance, filtration efficiency, mechanical strength, and application performance of the final product. For example, basis weight refers to the mass of the layered raw material per unit area. Basis weight directly affects the fiber density of the product (which significantly influences the formation of aggregates) and is a key factor determining the strength and durability of the porous composite medium. Generally, the higher the basis weight, the better the strength and impact resistance of the porous composite medium, and the greater the tensile and compressive forces it can withstand (but excessively high basis weight can negatively impact the filtration performance and air permeability of the product). Porosity affects the porosity and aggregate formation in the porous composite medium, thus affecting the flux and mechanical strength of the porous composite medium, and consequently, its practical application. Thickness affects the mechanical stability and durability of the porous composite medium. By compressing and sintering multiple layers of raw materials of a certain thickness, a porous composite medium of ideal thickness is ultimately formed. Simultaneously, the porous composite medium is not prone to delamination under high pressure, and there is almost no particle shedding, ensuring cleanliness.
[0076] The moisture content of the layered material described in this invention can be obtained by drying the material, for example, drying it at a temperature of 50-80℃ for 0.5-2 hours, as long as the moisture content reaches this range. The presence of moisture affects sintering; if the moisture content is too high, the non-uniformity of the pores in the composite medium will be too large, and the porosity will be too low. When the moisture content is within this range, it is beneficial to improve the uniformity of the pores in the porous composite medium and obtain a product with a larger porosity.
[0077] As a further improvement of the present invention, the number of layers of the layered raw material is 5-25, for example, 5, 10, 12, 15, 18, 20 and 25, preferably 10-20;
[0078] And / or, the polymer fiber comprises a bicomponent fiber, preferably also comprising a single-component fiber, wherein the polymer of the single-component fiber is at least one selected from polypropylene, polyethylene terephthalate, polyamide, polybutylene terephthalate, and polypropylene terephthalate.
[0079] The number of layers and the composition of polymer fibers determine the thickness of the porous composite medium and the formation of agglomerates and pores therein, and affect its stability. By combining the two, a porous composite medium with appropriate thickness, suitable agglomerates of appropriate size and suitable pore size distribution can be obtained.
[0080] The structure of the bicomponent fiber can be a conventional structure in the art, such as a core-sheath structure, where the sheath contains PE and the core contains polymer A; it can also be a parallel structure, such as PE and polymer A arranged side by side. The polymer fiber can also contain single-component fibers, that is, both bicomponent and single-component fibers are present, in which case a product with higher strength can be obtained. During the research, it was found that during the sintering process, after the melting point of PE is reached, the PE in the sheath melts first, and the fiber diameter decreases after melting; due to the melting of PE, the fibers that were originally tightly wrapped together in the layered material will bond into larger clumps and then form aggregates; the fibers that are not in contact with other fibers have smaller fiber diameters and are in a dispersed state, while the polymer A in the core basically retains its original properties and shape, providing the necessary mechanical properties and modulus support for the porous composite medium.
[0081] During the research, it was found that, as a further improvement of the present invention, based on controlling the compression amount to 50%-80%, the compression treatment conditions include: a pressure of 0.1MPa-0.6MPa, such as 0.1MPa, 0.2MPa, 0.3MPa, 0.4MPa, 0.5MPa, and 0.6MPa. This is beneficial for controlling the spacing between layered materials, resulting in a tighter arrangement between fibers and an increased contact area between fibers. This is conducive to the bonding between fibers during sintering, thereby affecting the formation of non-directional tortuous pathways during sintering. This relatively tight arrangement and bonding helps to obtain suitable agglomerates and pores during sintering, thereby improving the density, strength, and corrosion resistance of the product, and avoiding delamination or powder inclusion in the product obtained after subsequent sintering. However, further increasing the compression amount and excessive pressure will also lead to a decrease in the porosity of the product. Too low a porosity may also affect the throughput and retention efficiency of the product. Too low a compression amount or too low a pressure will affect the subsequent sintering process, leading to a decrease in the crystallinity of the porous composite medium and the existence of powder inclusion.
[0082] Sintering temperature is a key factor affecting the microstructure of porous composite media. The holding time affects the degree of sintering, the diameter and degree of fiber breakage, and thus the formation of agglomerates. During the experiment, it was found that as the sintering temperature increased, polyethylene with a lower melting point began to melt, and the fibers began to bond together, gradually forming sintering necks that gradually increased in size over time. The bonds between the fibers became tighter, and agglomerates were formed during the secondary sintering process.
[0083] During the first sintering process, controlling the temperature range and holding it at that temperature for a period of time allows for a more uniform temperature distribution in the polymer fibers, which is beneficial for the melting of PE and the more uniform distribution of the polymer A skeleton. During the first sintering process, PE melts and initially bonds, but polymer A melting is minimal. This facilitates subsequent sintering to obtain pores of ideal size and quantity, as well as agglomerates, avoiding over-sintering, powder inclusion, or delamination. If the temperature is too low, PE cannot melt and bond, which is detrimental to the subsequent agglomerate formation. If the temperature is too high, over-sintering during the second sintering process is likely to occur, causing excessive polymer decomposition and significantly thinning of the fiber diameter. As a further improvement of this invention, the heating rate for the first sintering is 10-15℃ / min, for example, 10℃ / min, 11℃ / min, 12℃ / min, 13℃ / min, 14℃ / min, or 15℃ / min. This heating rate ensures efficiency while minimizing the temperature difference between different polymer fibers, which is beneficial for subsequent sintering processes.
[0084] The second sintering temperature is controlled at 150-180℃. At this temperature, the already bonded polymer fiber surfaces further fuse together due to the movement and diffusion of molecular chain segments, resulting in a stable and firm bond. Combined with controlled holding time, suitable non-directional tortuous pathways can be generated while forming appropriate agglomerates, ultimately forming an ideal porous composite medium. If the temperature is too low or the time is too short, it is not conducive to the formation of agglomerates; if the temperature is too high or the time is too long, over-sintering will occur, resulting in a significant reduction in the number of pores. Ultimately, the porosity and flux of the composite medium are too low, and the mechanical strength is poor. As a further improvement of this invention, the heating rate of the second sintering is 5-10℃ / min, for example, 5℃ / min, 6℃ / min, 7℃ / min, 8℃ / min, 9℃ / min, or 10℃ / min. When the heating rate is within this range, the sintering process can proceed smoothly, avoiding problems such as excessive temperature gradients and stress concentration caused by excessively rapid heating. The heating rate of the first sintering can be greater than that of the second sintering, which helps to further alleviate problems such as excessive temperature gradient and stress concentration.
[0085] Furthermore, research has found that if only the first sintering is performed, the fibers may only form sintering necks without significant fusion, resulting in the inability to form aggregates in the resulting porous composite medium. If only the second sintering is performed, the melting of PE can cause significant fusion between the fibers, but this can lead to over-sintering, powder inclusion, and other problems. Additionally, polymer fibers are prone to diameter shrinkage and breakage, both of which are detrimental to the formation of aggregates and pores, resulting in poor mechanical and filtration properties of the prepared porous composite medium. Moreover, if the sintering temperature is too high, it may cause the polymer A to melt, leading to fiber diameter shrinkage or breakage, and even the formation of micropores, cracks, or granular structures. This further hinders aggregate formation and results in excessively thin free fibers, impacting the filtration and mechanical properties of the porous composite medium. Excessively high sintering temperatures can also lead to over-sintering, causing cracks and deformation, ultimately reducing product performance.
[0086] The study also found that even with controlled compression and secondary sintering processes, the resulting composite medium may still exhibit varying degrees of crystallinity. Cooling rate can lead to different stresses and microstructure changes within the product. Rapid cooling can reduce the crystallinity and hardness of the porous composite medium and increase its tensile strength. Slow cooling, on the other hand, may result in more complete crystallization of the porous composite medium, but may reduce its toughness. When the cooling rate is 5-15℃ / min, the crystallinity of the porous composite medium is controlled within a suitable range. This results in tighter bonding between aggregates in the composite medium, better connectivity of non-directional tortuous pathways, and less delamination, which helps the porous composite medium to possess both good toughness and tensile strength.
[0087] The third aspect of the present invention provides the application of the porous composite medium as described above as a porous filter medium for liquid filtration or gas filtration.
[0088] The porous composite medium described in this invention features high porosity and strong chemical and physical resistance, making it suitable as a porous filter medium. Specifically, liquid filtration can be used to filter solid particles or suspended matter from liquids, such as in water treatment (e.g., for water purification and seawater desalination in microfiltration, ultrafiltration, and reverse osmosis systems), oil filtration, chemical processing, the food and beverage industry (e.g., for filtering beverages, beer, and juice to remove impurities and microorganisms), the fine chemical industry (e.g., for filtering emulsions and creams in the production of cosmetics and personal care products), the pharmaceutical industry (e.g., for removing impurities), the electronics manufacturing industry (for filtering chemical cleaning agents, detergents, and ultrapure water), mining and mineral processing (for filtering mineral slurries and tailings), and agriculture (for filtering irrigation water to remove soil particles and other impurities).
[0089] Gas filtration can be applied in the chemical and manufacturing industries to remove harmful gases or vapors, such as acid gases, solvent vapors, and other harmful emissions. It can also be used as a filter medium in air purification systems, such as HVAC systems, to improve indoor air quality and remove odors, bacteria, and viruses. Furthermore, it can be used in medical equipment, such as ventilators, anesthesia machines, and other medical devices, to provide sterile air or filter out the air exhaled by patients. In the automotive industry, it can be used in vehicle emission control systems to reduce pollutant emissions from exhaust gases. In the painting and coating industry, it can be used for air filtration in paint booths to remove excess paint particles and dust. In the nuclear industry, it can be used to filter radioactive gases and dust, protecting the environment and worker safety. It can also be used in fragrance diffusers and air fresheners to control fragrance release. Finally, it is used in various industrial processes to collect and filter generated dust to protect the working environment and reduce pollution.
[0090] The present invention, by adopting the above technical solution, has the following beneficial effects:
[0091] The porous composite medium of the present invention is obtained by sintering polymer fibers containing at least two polymers. It has the advantages of high throughput and high mechanical properties, and has the advantages of high filtration efficiency, long service life, corrosion resistance and high temperature resistance. Its unique porous structure and material properties enable it to maintain stable filtration performance in various harsh environments.
[0092] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and should be understood to include values close to those ranges or values. For numerical ranges, endpoint values of various ranges, endpoint values of various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. In this document, unless otherwise specified, data ranges include endpoints. Attached Figure Description
[0093] Figure 1 The image shown is a SEM image of a longitudinal section perpendicular to the end face of the porous composite medium prepared in Example 1 of the present invention, with a magnification of 50×.
[0094] Figure 2 The image shown is an SEM image of one end face of the porous composite medium prepared in Example 1 of the present invention, with a magnification of 100×.
[0095] Figure 3 The image shown is a SEM image of a longitudinal section perpendicular to the end face of the porous composite medium prepared in Example 2 of the present invention, with a magnification of 100×.
[0096] Figure 4The image shown is a SEM image of a longitudinal section perpendicular to the end face of the porous composite medium prepared in Example 6 of the present invention, with a magnification of 100×. Detailed Implementation
[0097] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.
[0098] Unless otherwise defined, all scientific and technical terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art.
[0099] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0100] Unless otherwise specified, all materials and reagents used in the following examples are commercially available.
[0101] The present invention will now be described in detail with reference to specific embodiments, which are intended to understand rather than limit the invention.
[0102] Example 1
[0103] This embodiment provides a method for preparing the porous composite medium described in this invention.
[0104] S1. The nonwoven fabric raw material composed of polymer fibers is heated and dried at a temperature of 70°C for 1 hour, so that the moisture content of the nonwoven fabric raw material is below 1 wt%. The basis weight of the nonwoven fabric raw material is 130 g / m². 2 The single-layer thickness is 0.7 mm, the porosity is 75%, and the polymer fiber has a core-sheath structure, with the sheath being PE and the core being PP.
[0105] S2. Cut the non-woven fabric treated in S1 into neat and regular non-woven fabric sheets. Take 16 layers of sheets and lay them flat into the board sintering mold. The sheets should be flat and wrinkle-free. Close the pressing mold and perform pressing treatment. Control the pressure to 0.4 MPa and the compression amount based on thickness to be 65%.
[0106] S3. Place the sintering mold flat in the sintering equipment, set the first sintering process parameters, start heating from room temperature, set the heating rate to 12℃ / min, set the first sintering temperature to 130℃, and set the holding time to 20min; then set the second sintering process parameters, set the heating rate to 8℃ / min, set the temperature to 165℃, and set the holding time to 20min.
[0107] S4. After sintering, the material automatically enters the cooling device at a rate of 10℃ / min. Once cooled to room temperature, the material is opened by the mold-opening device, and the sintered fiberboard is removed. The fiberboard is then flattened in a punching machine and punched into the required specifications using a specific punching die, thus creating a porous composite medium.
[0108] SEM images of the prepared porous composite media are shown below. Figure 1 As shown in the figure, from Figure 1 As can be seen, the porous composite medium contains several agglomerates formed by the sintering of the polymer fibers. These agglomerates are interconnected, and free fibers are present around and inside the agglomerates. In the cross-section of the porous composite medium, the agglomerates appear rectangular or circular. Figure 2 As shown, the surface of the porous composite medium includes several mold wall contact areas, and the average SEM width of the mold wall contact areas is in the range of 50μm-150μm; the area ratio of the mold wall contact areas is in the range of 20%-80%.
[0109] The prepared porous composite medium was measured to have a thickness T of 3.8 mm, an average fiber SEM diameter of 20 μm, an average PMI pore size of 1.5 μm, a difference between the maximum and minimum pore sizes of 500 nm, and a porosity of 60%. In the thickness direction of the porous composite medium's cross-section, the average SEM area of the aggregates was 25,000 μm². 2 The density is 24 particles / mm 2 The d1 is 150 μm, the d2 is 200 μm, the d1 / d2 ratio is 1:1.33, the d1 / T ratio is 3.95%, the sum of d1 of the aggregates is 38.6% of the ratio of T, and the average diameter of the fiber by SEM is 1:7.5.
[0110] The surface of the porous composite medium was subjected to infrared absorption spectroscopy using the ATR method, with the results obtained at 710 cm⁻¹. -1 -730cm -1 There is a first peak at 2910 cm. -1 -2930cm -1 A second peak exists, and the ratio of the peak area of the first peak to the peak area of the second peak is the relative peak area X of polyethylene, where the relative peak area X of polyethylene is 0.23; at 965 cm⁻¹ -1 -985cm-1 A third peak exists at 2940 cm⁻¹. -1 -2960cm -1 A fourth peak is present. The ratio of the peak area of the third peak to the peak area of the fourth peak is the relative peak area Y of polypropylene, which is 0.38; X / Y is 0.61. The DSC crystallinity of the porous composite medium is 36%.
[0111] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 1.
[0112] Example 2
[0113] This embodiment provides a method for preparing the porous composite medium described in this invention.
[0114] S1. The nonwoven fabric raw material composed of polymer fibers is heated and dried at a temperature of 70°C for 1 hour, so that the moisture content of the nonwoven fabric raw material is below 1 wt%. The basis weight of the nonwoven fabric raw material is 180 g / m². 2 The single-layer thickness is 1mm, the porosity is 70%, and the polymer fiber has a core-sheath structure, with the sheath being PE and the core being PET.
[0115] S2. Cut the non-woven fabric treated in S1 into neat and regular non-woven fabric sheets. Take 12 layers of sheets and lay them flat into the board sintering mold. The sheets should be flat and wrinkle-free. Close the pressing mold and perform pressing treatment. Control the pressure to 0.6 MPa and the compression amount based on thickness to be 80%.
[0116] S3. Place the sintering mold flat in the sintering equipment, set the first sintering process parameters, start heating from room temperature, set the heating rate to 11℃ / min, set the first sintering temperature to 140℃, and set the holding time to 25min; then set the second sintering process parameters, set the heating rate to 6℃ / min, set the temperature to 180℃, and set the holding time to 30min.
[0117] S4. After sintering, the material automatically enters the cooling device at a rate of 8°C / min. Once cooled to room temperature, the mold is opened by the mold-opening device, and the sintered fiberboard is removed. The fiberboard is then flattened in a punching machine and punched into the required specifications using a specific punching die, thus creating a porous composite medium.
[0118] SEM image of the longitudinal section of the prepared porous composite medium is shown below. Figure 3As shown in the figure, the porous composite medium contains several agglomerates formed by the sintering of the polymer fibers. These agglomerates are interconnected, and free fibers are present around and inside the agglomerates. In the cross-section of the porous composite medium, each agglomerate is approximately rectangular. The surface of the porous composite medium includes several mold wall contact areas, with an average SEM width of 50 μm-150 μm; the area of these mold wall contact areas accounts for 20%-80% of the total surface area.
[0119] The prepared porous composite medium was measured to have a thickness T of 2.2 mm, an average fiber SEM diameter of 35 μm, an average PMI pore size of 0.3 μm, a difference between the maximum and minimum pore sizes of 150 nm, and a porosity of 45%. In the thickness direction of the porous composite medium's cross-section, the average SEM area of the aggregates was 37,000 μm². 2 The density is 15 particles / mm 2 The d1 is 150 μm, the d1 / T is 9.09%, the sum of d1 of the aggregates is 58.5% to T, and the average diameter of the fiber by SEM is 1:5.7.
[0120] The surface of the porous composite medium was subjected to infrared absorption spectroscopy using the ATR method, with the results obtained at 710 cm⁻¹. -1 -730cm -1 There is a first peak at 2910 cm. -1 -2930cm -1 A second peak exists, and the ratio of the peak area of the first peak to the peak area of the second peak is the relative peak area X of polyethylene, where the relative peak area X of polyethylene is 2.23; at 838 cm⁻¹ -1 -858cm -1 A fifth peak exists at 1709 cm⁻¹. -1 -1729cm -1 A sixth peak is present. The ratio of the peak area of the fifth peak to the peak area of the sixth peak is the relative peak area Z of polyethylene terephthalate (PET), which is 0.084; X / Z is 26.5. The DSC crystallinity of the porous composite medium is 48%.
[0121] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 1.
[0122] Example 3
[0123] This embodiment provides a method for preparing the porous composite medium described in this invention.
[0124] S1. The nonwoven fabric raw material composed of polymer fibers is heated and dried at a temperature of 70°C for 1 hour, so that the moisture content of the nonwoven fabric raw material is below 1 wt%. The basis weight of the nonwoven fabric raw material is 60 g / m². 2 The single-layer thickness is 0.4 mm, the porosity is 85%, and the polymer fiber has a core-sheath structure, with the sheath being PE and the core being PBT.
[0125] S2. Cut the non-woven fabric treated in S1 into neat and regular non-woven fabric sheets. Take 20 layers of sheets, lay them flat and put them into the board sintering mold. The sheets should be flat and wrinkle-free. Close the pressing mold and press them together. Control the pressure to 0.2 MPa and the compression amount based on the thickness to be 50%.
[0126] S3. Place the sintering mold flat in the sintering equipment, set the first sintering process parameters, start heating from room temperature, set the heating rate to 14℃ / min, set the first sintering temperature to 110℃, and set the holding time to 15min; then set the second sintering process parameters, set the heating rate to 10℃ / min, set the temperature to 150℃, and set the holding time to 15min.
[0127] S4. After sintering, the material automatically enters the cooling device at a rate of 14℃ / min. Once cooled to room temperature, the mold is opened by the mold-opening device, and the sintered fiberboard is removed. The fiberboard is then flattened in a punching machine and punched into the required specifications using a specific punching die, thus creating a porous composite medium.
[0128] The porous composite medium contains several agglomerates formed by sintering the polymer fibers. These agglomerates are interconnected, and free fibers are present around and within the agglomerates. In the cross-section of the porous composite medium, each agglomerate is approximately rectangular. The surface of the porous composite medium includes several mold wall contact areas, with an average SEM width of 50 μm-150 μm. The area of these mold wall contact areas accounts for 20%-80% of the total surface area.
[0129] The prepared porous composite medium was measured to have a thickness T of 3.8 mm, an average fiber SEM diameter of 10 μm, an average PMI pore size of 3.5 μm, a difference between the maximum and minimum pore sizes of 750 nm, and a porosity of 75%. In the thickness direction of the porous composite medium's cross-section, the average SEM area of the aggregates was 0.8 million μm². 2 The density is 45 particles / mm 2 The d1 is 80 μm, the d1 / T is 2.11%, the sum of d1 of the aggregates is 25.9% to T, and the average diameter of the fiber by SEM is 1:8.
[0130] The surface of the porous composite medium was subjected to infrared absorption spectroscopy using the ATR method, with the results obtained at 710 cm⁻¹. -1 -730cm -1 There is a first peak at 2910 cm. -1 -2930cm -1 A second peak exists, and the ratio of the peak area of the first peak to the peak area of the second peak is the relative peak area X of polyethylene, wherein the relative peak area X of polyethylene is 0.75, and the DSC crystallinity of the porous composite medium is 30%.
[0131] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 1.
[0132] Example 4
[0133] This embodiment provides a method for preparing the porous composite medium described in this invention.
[0134] S1. The nonwoven fabric raw material composed of polymer fibers is heated and dried at a temperature of 70°C for 1 hour, so that the moisture content of the nonwoven fabric raw material is below 1 wt%. The basis weight of the nonwoven fabric raw material is 90 g / m². 2 The single-layer thickness is 0.8 mm, the porosity is 80%, and the polymer fiber has a core-sheath structure, with the sheath being PE and the core being PP.
[0135] S2. Cut the non-woven fabric treated in S1 into neat and regular non-woven fabric sheets. Take 18 layers of sheets, lay them flat and put them into the board sintering mold. The sheets should be flat and wrinkle-free. Close the pressing mold and press them together. Control the pressure to 0.3 MPa and the compression amount based on the thickness to be 60%.
[0136] S3. Place the sintering mold flat in the sintering equipment, set the first sintering process parameters, start heating from room temperature, set the heating rate to 13℃ / min, set the first sintering temperature to 120℃, and set the holding time to 20min; then set the second sintering process parameters, set the heating rate to 8℃ / min, set the temperature to 155℃, and set the holding time to 20min.
[0137] S4. After sintering, the material automatically enters the cooling device at a rate of 6°C / min. Once cooled to room temperature, the mold is opened by the mold-opening device, and the sintered fiberboard is removed. The fiberboard is then flattened in a punching machine and punched into the required specifications using a specific punching die, thus creating a porous composite medium.
[0138] The porous composite medium contains several agglomerates formed by sintering the polymer fibers. These agglomerates are interconnected, and free fibers are present around and within the agglomerates. In the cross-section of the porous composite medium, each agglomerate is approximately rectangular. The surface of the porous composite medium includes several mold wall contact areas, with an average SEM width of 50 μm-150 μm. The area of these mold wall contact areas accounts for 20%-80% of the total surface area.
[0139] The prepared porous composite medium was measured to have a thickness T of 5.5 mm, an average fiber SEM diameter of 27 μm, an average PMI pore size of 2.4 μm, a difference between the maximum and minimum pore sizes of 600 nm, and a porosity of 68%. In the thickness direction of the porous composite medium's cross-section, the average SEM area of the aggregates was 14,000 μm². 2 The density is 37 particles / mm 2 The d1 is 130 μm, the d1 / T is 2.36%, the sum of d1 of the aggregates is 30.3% to T, and the average diameter of the fiber by SEM is 1:4.8.
[0140] The surface of the porous composite medium was subjected to infrared absorption spectroscopy using the ATR method, with the results obtained at 710 cm⁻¹. -1 -730cm -1 There is a first peak at 2910 cm. -1 -2930cm -1 A second peak exists, and the ratio of the peak area of the first peak to the peak area of the second peak is the relative peak area X of polyethylene, wherein the relative peak area X of polyethylene is 0.48, and the DSC crystallinity of the porous composite medium is 33%.
[0141] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 1.
[0142] Example 5
[0143] This embodiment provides a method for preparing the porous composite medium described in this invention.
[0144] The method described in Example 1 is followed, except that the polymer fibers of the nonwoven fabric are bicomponent fibers and monocomponent fibers, wherein the bicomponent fibers have a core-sheath structure, the sheath is PE, the core is PP, and the monocomponent fibers are PP.
[0145] The porous composite medium contains several agglomerates formed by sintering the polymer fibers. These agglomerates are interconnected, and free fibers are present around and within the agglomerates. In the cross-section of the porous composite medium, the agglomerates are approximately rectangular or circular. The surface of the porous composite medium includes several mold wall contact areas, with an average SEM width of 50 μm-150 μm; the area of the mold wall contact areas accounts for 20%-80% of the total surface area.
[0146] The prepared porous composite medium was measured to have a thickness T of 3.7 mm, an average fiber SEM diameter of 24 μm, an average PMI pore size of 1.5 μm, a difference between the maximum and minimum pore sizes of 600 nm, and a porosity of 59%. In the thickness direction of the porous composite medium's cross-section, the average SEM area of the aggregates was 28,000 μm². 2 The density is 22 particles / mm 2 The d1 is 170 μm, the d2 is 220 μm, the d1 / d2 ratio is 1:1.29, the d1 / T ratio is 4.59%, the sum of d1 of the aggregates is 40.5% of the ratio of T, and the average diameter of the fiber by SEM is 1:7.1.
[0147] The surface of the porous composite medium was subjected to infrared absorption spectroscopy using the ATR method, with the results obtained at 710 cm⁻¹. -1 -730cm -1 There is a first peak at 2910 cm. -1 -2930cm -1 A second peak exists, and the ratio of the peak area of the first peak to the peak area of the second peak is the relative peak area X of polyethylene, where the relative peak area X of polyethylene is 0.19; at 965 cm⁻¹ -1 -985cm -1 A third peak exists at 2940 cm⁻¹. -1 -2960cm -1 A fourth peak is present. The ratio of the peak area of the third peak to the peak area of the fourth peak is the relative peak area Y of polypropylene, which is 0.47; X / Y is 0.40. The DSC crystallinity of the porous composite medium is 38%.
[0148] The performance of the prepared porous composite medium was evaluated, and the results are shown in Table 1. The addition of single-component fibers significantly improved the Shore A hardness and compressive strength of the porous composite medium.
[0149] Example 6
[0150] This embodiment illustrates the preparation method of the porous composite medium described in this invention.
[0151] The operation was carried out according to the method described in Example 1, except that the heating rate of both the first sintering and the second sintering was 20°C / min.
[0152] SEM images of the prepared porous composite media are shown below. Figure 4 As shown in the figure, the area of the prepared aggregates is relatively small, with an average SEM area of 2000 μm. 2 On the cross-section of the porous composite medium, with the thickness direction of the porous composite medium as the y-axis, the average SEM size d1 of the aggregate along the y-axis direction is 62 μm.
[0153] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 1.
[0154] Example 7
[0155] This embodiment illustrates the preparation method of the porous composite medium described in this invention.
[0156] The operation was carried out according to the method described in Example 1, except that the heating rates of the first sintering and the second sintering were 5°C / min and 2°C / min, respectively.
[0157] The porosity of the prepared porous composite medium is 43%.
[0158] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 1.
[0159] Example 8
[0160] This embodiment illustrates the preparation method of the porous composite medium described in this invention.
[0161] The operation was carried out according to the method described in Example 1, except that the thickness of the nonwoven fabric was 1.4, the number of layers was 8, and the pressure during the pressing process was 0.05 MPa.
[0162] The prepared porous composite medium has a d1 of 80 μm and a d2 of 400 μm.
[0163] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 1.
[0164] Example 9
[0165] This embodiment illustrates the preparation method of the porous composite medium described in this invention.
[0166] The operation was carried out according to the method described in Example 1, except that the thickness of the nonwoven fabric was 0.7 mm, the number of layers was 20, and the heat preservation time for the second sintering was 5 minutes.
[0167] The prepared porous composite medium has a thickness T of 8.9 mm, a d1 of 110 μm, and a d1 / T ratio of 1.24%.
[0168] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 1.
[0169] Example 10
[0170] This embodiment illustrates the preparation method of the porous composite medium described in this invention.
[0171] The operation was carried out according to the method described in Example 1, except that the heating and drying conditions were such that the moisture content in the nonwoven fabric raw material was below 3 wt%, and the holding time for the first sintering was 5 min.
[0172] The surface of the porous composite medium was subjected to infrared absorption spectroscopy using the ATR method, with the results obtained at 710 cm⁻¹. -1 -730cm -1 There is a first peak at 2910 cm. -1 -2930cm -1 A second peak exists, and the ratio of the peak area of the first peak to the peak area of the second peak is the relative peak area X of polyethylene. The relative peak area X of polyethylene is 0.009, and nearly 20% of the products in the batch have a certain amount of powder shedding.
[0173] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 1.
[0174] Table 1
[0175] Group Flux L / min@7kpa Retention efficiency Shore A hardness / HA Compressive strength / N Example 1 4 For 1μm particles, greater than 95% 95 72 Example 2 1 For particles larger than 0.1μm, 95% 97 74 Example 3 6.5 For particles larger than 3μm, the percentage is greater than 95%. 92 68 Example 4 5 For 2μm particles, greater than 95% 94 70 Example 5 3.9 For 1μm particles, greater than 95% 99 81 Example 6 3.1 For 1μm greater than 90% 90 67 Example 7 3.3 For 1μm greater than 90% 94 70 Example 8 2.9 For 1μm greater than 90% 90 69 Example 9 3.4 For 1μm greater than 90% 92 67 Example 10 2.4 For 1μm greater than 90% 91 66
[0176] Comparative Example 1
[0177] This comparative example is used to illustrate the preparation method of the reference porous composite medium.
[0178] The operation is carried out according to the method described in Example 1, except that the polymer fiber is made of PP material.
[0179] Experiments revealed that the obtained porous composite medium did not contain agglomerates, and it was prone to stratification and had low mechanical strength.
[0180] Comparative Example 2
[0181] This comparative example is used to illustrate the preparation method of the reference porous composite medium.
[0182] The operation is carried out according to the method described in Example 1, except that the polymer fiber is made of PE material.
[0183] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 2.
[0184] Comparative Example 3
[0185] This comparative example is used to illustrate the preparation method of the reference porous composite medium.
[0186] The method described in Example 1 was followed, except that the pressure was controlled at 0.8 MPa and the compression amount was 95% during the pressing process. The results showed that the porosity of the prepared porous composite medium was low, at 29%.
[0187] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 2.
[0188] Comparative Example 4
[0189] This comparative example is used to illustrate the preparation method of the reference porous composite medium.
[0190] The operation was carried out according to the method described in Example 1, except that the pressure was controlled at 0.05 MPa and the compression amount was 30% during the pressing process.
[0191] The results showed that the average pore size of the prepared porous composite medium was 7.3 μm, the porosity was high at 72%, the agglomerates were too small, and it was easy to separate into layers.
[0192] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 2.
[0193] Comparative Example 5
[0194] This comparative example is used to illustrate the preparation method of the reference porous composite medium.
[0195] The procedure is performed according to the method described in Example 1, except that the basis weight of the nonwoven fabric is 400 g / m². 2 The first sintering temperature is 150℃, and the holding time is 50min.
[0196] The results showed that the average SEM diameter of the fibers in the prepared porous composite medium was 78 μm.
[0197] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 2.
[0198] Comparative Example 6
[0199] This comparative example is used to illustrate the preparation method of the reference porous composite medium.
[0200] The procedure is performed according to the method described in Example 1, except that the basis weight of the nonwoven fabric is 30 g / m². 2 The first sintering is not performed, and the cooling rate is 18℃ / min.
[0201] The results showed that the average SEM diameter of the fibers in the prepared porous composite medium was 4 μm.
[0202] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 2.
[0203] Comparative Example 7
[0204] This comparative example is used to illustrate the preparation method of the reference porous composite medium.
[0205] The procedure was performed according to the method described in Example 1, except that the second sintering temperature was 190°C and the holding time was 50 min.
[0206] The results showed that the average pore size of the prepared porous composite medium was 0.6 μm and the porosity was 35%.
[0207] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 2.
[0208] Comparative Example 8
[0209] This comparative example is used to illustrate the preparation method of the reference porous composite medium.
[0210] The procedure was performed according to the method described in Example 1, except that the second sintering temperature was 140°C and the holding time was 2 minutes.
[0211] The results showed that the average pore size of the prepared porous composite medium was 5.2 μm, the porosity was 71%, and there were basically no agglomerates, making it easy to separate into layers.
[0212] The performance of the prepared porous composite media was evaluated, and the results are shown in Table 2.
[0213] Table 2
[0214] Group Flux L / min@7kpa Shore A hardness / HA Compressive strength / N Example 1 4 95 72 Comparative Example 2 0.4 64 38 Comparative Example 3 0.5 85 59 Comparative Example 4 6.7 66 41 Comparative Example 5 0.7 / / Comparative Example 6 / 56 35 Comparative Example 7 0.8 / / Comparative Example 8 / 69 43
[0215] Note: / indicates not measured.
[0216] It should be noted that, in this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes that element. Furthermore, it should be noted that the scope of the methods and apparatuses in the embodiments of this application is not limited to performing functions in the order shown or discussed, but may also include performing functions substantially simultaneously or in the reverse order, depending on the functions involved. For example, the described methods may be performed in a different order than described, and various steps may be added, omitted, or combined. Additionally, features described with reference to certain examples may be combined in other examples.
[0217] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications or equivalent substitutions made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A porous composite medium, characterized in that, The porous composite medium comprises polymer fibers for forming a porous structure. The polymer constituting the polymer fibers comprises polyethylene and polymer A. Polymer A comprises at least one of polypropylene, polyethylene terephthalate, polyamide, polybutylene terephthalate, and polypropylene terephthalate. The SEM average diameter of the polymer fibers is 5 μm-40 μm. The porous composite medium contains several aggregates formed by sintering the polymer fibers; The average pore size of the porous composite medium is 0.1 μm-5 μm, and the porosity is 40%-80%. In a cross-section of the porous composite medium, the SEM average area of the agglomerates is 3000 μm 2 - 50000 μm 2 ; In a cross-section of the porous composite medium, the density of the agglomerates is 3-70 per 1 mm 2 .
2. The porous composite medium according to claim 1, characterized in that, The average diameter of the polymer fiber as measured by SEM is 8μm-35μm; And / or, the average pore size of the porous composite medium is 0.3 μm-3.5 μm; And / or, the porosity of the porous composite medium is 45%-75%.
3. The porous composite medium according to claim 1, characterized in that, On the cross-section of the porous composite medium, with the thickness direction of the porous composite medium as the y-axis, the average SEM size d1 of the aggregate along the y-axis direction is 50μm-500μm; And / or, the average SEM size d2 perpendicular to the y-axis direction is 60μm-800μm.
4. The porous composite medium according to claim 3, characterized in that, The ratio of d1 to the thickness T of the porous composite medium, d1 / T, is 1.5%-20%. And / or, in the thickness direction of the cross section of the porous composite medium, the ratio of the sum of d1 of the aggregates to the thickness T of the porous composite medium is 20%-60%.
5. The porous composite medium according to claim 4, characterized in that: The ratio of d1 to the thickness T of the porous composite medium, d1 / T, is 2%-15%.
6. The porous composite medium according to claim 3, 4, or 5, characterized in that, The ratio of the average SEM diameter of the polymer fiber to d1 is 1:2-10; And / or, d1 / d2 is 1:1.2-8.
7. The porous composite medium according to claim 6, characterized in that, The ratio of d1 / d2 is 1:1.5-5.
8. The porous composite medium according to claim 1, characterized in that, The surface of the porous composite medium was subjected to infrared absorption spectroscopy using the ATR method, with the results obtained at 710 cm⁻¹. -1 -730cm -1 There is a first peak at 2910 cm. -1 -2930cm -1 A second peak exists, and the ratio of the peak area of the first peak to the peak area of the second peak is the relative peak area X of polyethylene, wherein the relative peak area X of polyethylene is 0.01-4; the average SEM diameter of the polymer fiber is 10μm-30μm.
9. The porous composite medium according to claim 8, characterized in that, When polymer A contains polypropylene, the surface of the porous composite medium is subjected to infrared absorption spectroscopy using the ATR method, and the result is observed at 965 cm⁻¹. -1 -985cm -1 A third peak exists at 2940 cm⁻¹. -1 -2960cm -1 A fourth peak exists, and the ratio of the peak area of the third peak to the peak area of the fourth peak is the relative peak area Y of polypropylene, which is 0.1-0.
8.
10. The porous composite medium according to claim 9, characterized in that, X / Y is 0.01-1.
11. The porous composite medium according to claim 8, characterized in that, When polymer A contains polyethylene terephthalate, the surface of the porous composite medium is subjected to infrared absorption spectroscopy testing using the ATR method, and the result is at 838 cm⁻¹. -1 -858cm -1 A fifth peak exists at 1709 cm⁻¹. -1 -1729cm -1 A sixth peak exists, and the ratio of the peak area of the fifth peak to the peak area of the sixth peak is the relative peak area Z of polyethylene terephthalate, which is 0.01-0.
5.
12. The porous composite medium according to claim 11, characterized in that, X / Z is 20-40.
13. The porous composite medium according to claim 1, characterized in that, The difference between the maximum and minimum pore size in the porous composite medium is 100-800 nm. And / or, the thickness of the porous composite medium is 1mm-8mm; And / or, the DSC crystallinity of the porous composite medium is 20%-50%.
14. The porous composite medium according to claim 1, characterized in that, The surface of the porous composite medium includes several mold wall contact areas; the average SEM width of the mold wall contact areas is 30μm-200μm; and the area ratio of the mold wall contact areas is 20%-80%.
15. The porous composite medium according to claim 14, characterized in that, The average SEM width of the contact area between the mold wall and the mold wall is 50μm-150μm.
16. The porous composite medium according to claim 1, characterized in that, The flux of the porous composite medium is 0.5-8 L / min at 7 kPa; And / or; the porous composite medium has a retention efficiency of greater than 95% for impurity particles with a particle size of 0.1-10 μm; And / or, the Shore A hardness of the porous composite medium is not less than 90HA; And / or, the compressive strength of the porous composite medium is not less than 65 N@1 mm.
17. A method for preparing a porous composite medium according to any one of claims 1-16, characterized in that, The method includes the following steps: (1) A layered material consisting of at least two layers of polymer fibers is subjected to compression treatment to obtain a compressed material, wherein the compression conditions are such that the compression amount based on thickness is 50-80%; (2) The material after pressing is subjected to a first sintering and a second sintering to obtain the sintered material; (3) Cool the sintered material to produce a porous composite medium; The polymer fiber is composed of polyethylene and polymer A, wherein polymer A contains at least one of polypropylene, polyethylene terephthalate, polyamide, polybutylene terephthalate, and polypropylene terephthalate. The conditions for the first sintering include: a temperature of 100-140℃ and a holding time of 10-30 minutes. The conditions for the second sintering include: a temperature of 150-180℃ and a holding time of 10-30 minutes; Cooling conditions include a cooling rate of 5-15℃ / min.
18. The method according to claim 17, characterized in that, The weight of the layered material is 50-200 g / m³. 2 ; And / or, the thickness of the layered material is 0.1-1 mm; And / or, the porosity of the layered material is 70-90%; And / or, the moisture content in the layered material is less than 5 wt%.
19. The method according to claim 18, characterized in that, The moisture content in the layered material is less than 1 wt%.
20. The method according to claim 17, 18, or 19, characterized in that, The layered material has 5-25 layers; And / or, the polymer fiber comprises a bicomponent fiber, the bicomponent fiber comprising a core-sheath structure.
21. The method according to claim 20, characterized in that, The layered material has 10-20 layers.
22. The method according to claim 20, characterized in that, The polymer fiber also includes a single-component fiber, wherein the polymer of the single-component fiber is at least one selected from polypropylene, polyethylene terephthalate, polyamide, polybutylene terephthalate, and polypropylene terephthalate.
23. The method according to claim 17, characterized in that, The conditions for the pressing process include: a pressure of 0.1 MPa to 0.6 MPa; And / or, the heating rate for the first sintering is 10-15℃ / min; And / or, the heating rate for the second sintering is 5-10℃ / min.
24. The porous composite medium according to any one of claims 1-16 is used as a porous filter medium for liquid filtration or gas filtration.
Citation Information
Patent Citations
Nanofibre hyperfiltration membrane and preparation method thereof
CN101559326A
Microporous filter medium
CN102553353A
Bi-component polyester coarse fibre, filter material and preparation thereof
CN101302659A
Non-woven fabrics
GB1329132A