A wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene and its preparation process

By combining modified graphene nanosheets with polyester fibers to form a composite structure, the limitations of polyester fibers in terms of antibacterial properties and abrasion resistance are solved, resulting in school uniform fabrics with high abrasion resistance, long-lasting antibacterial effect, excellent moisture absorption and aging resistance, thus meeting consumers' demand for functional textiles.

CN119433796BActive Publication Date: 2026-11-10JIANGSU HAVLIN GARMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411780510.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-05
Publication Date
2026-11-10
Estimated Expiration
2044-12-05

AI Technical Summary

Technical Problem

Existing polyester fibers have limitations in terms of antibacterial properties and abrasion resistance, which restricts their application in certain special fields, and ordinary textiles are unable to meet consumer demands in terms of functionality.

Method used

Modified graphene nanosheets are combined with polyester fibers, and a composite structure is formed through specific dispersants and short-cut carbon fibers to enhance the fabric's abrasion resistance and antibacterial properties. Titanium dioxide particles form a heterojunction structure on the nanosheet surface to improve oxidative antibacterial performance, while optimizing moisture absorption, perspiration wicking, and aging resistance.

Benefits of technology

It achieves high abrasion resistance, long-lasting antibacterial properties, excellent moisture absorption and aging resistance of the fabric, improves the mechanical properties and stability of the fabric, and meets consumers' demand for functional textiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005172663100000151
    Figure BDA0005172663100000151
Patent Text Reader

Abstract

This application relates to the textile field, and more particularly to a wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene, and its preparation process. The wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene, by weight, comprises: 60-80 parts polyester fiber, 2-6 parts modified graphene nanosheets, 0.3-0.8 parts antibacterial agent, 2-4 parts dispersant, 0.5-1 part antioxidant, 1-2 parts stabilizer, 1-3 parts softener, 2-4 parts crosslinking agent, and 5-15 parts carbon fiber. The wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene in this application not only possesses excellent wear resistance and antibacterial properties, but also further improves its moisture absorption and wicking, aging resistance, and corrosion resistance, effectively meeting consumer demands for existing textiles, possessing greater functionality, and showing excellent application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the textile field, and more particularly to a wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene and its preparation process. Background Technology

[0002] With the development of technology and changes in consumer demand, textiles not only need to meet basic requirements for wearing comfort, but also increasingly incorporate more functional needs, such as abrasion resistance and antibacterial properties. This is especially true in fields such as medical health and sports leisure, where the demand for antibacterial, odor-resistant, and abrasion-resistant functions is growing.

[0003] Polyester fibers are widely used in the textile industry due to their excellent physical properties (such as high strength, good elasticity, and corrosion resistance) as well as good processability and dyeability. However, ordinary polyester fibers have certain limitations in terms of antibacterial properties and abrasion resistance, which restricts their application in some special fields. In recent years, graphene, as a novel two-dimensional material, has shown great application potential in many fields due to its unique physicochemical properties (such as high strength, good conductivity, and high thermal stability). Introducing graphene into textiles can not only significantly improve the physical properties of fabrics, such as increasing abrasion resistance and conductivity, but also endow fabrics with new functional properties, such as antibacterial and UV protection capabilities.

[0004] Combining the advantages of polyester fibers and graphene, the development of a novel antibacterial and abrasion-resistant fabric has become a research hotspot. This fabric not only effectively resists bacterial growth and reproduction, reducing odor, but also maintains high abrasion resistance, extending the lifespan of clothing. Furthermore, through appropriate processing methods, the fabric's hand feel, breathability, and moisture-wicking properties can be further optimized, making it more ergonomically designed.

[0005] Therefore, in order to provide a more stable, moisture-wicking, aging-resistant, corrosion-resistant, and anti-pilling school uniform fabric with better wear resistance and antibacterial properties, this application provides a fabric based on polyester fiber and graphene and its preparation method. The fabric material finally obtained by this application can effectively meet consumers' needs for existing textiles, has more functionality, and has excellent application prospects. Summary of the Invention

[0006] To address the aforementioned issues, the first aspect of this application provides a wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene. By weight, the raw materials are: 60-80 parts polyester fiber, 2-6 parts modified graphene nanosheets, 0.3-0.8 parts antibacterial agent, 2-4 parts dispersant, 0.5-1 part antioxidant, 1-2 parts stabilizer, 1-3 parts softener, 2-4 parts crosslinking agent, and 5-15 parts carbon fiber.

[0007] As a preferred embodiment, the mass ratio of the polyester fiber, modified graphene nanosheets, and carbon fiber is (70-75):(4-5.5):(8-10).

[0008] As a preferred embodiment, the modified graphene nanosheets have a mass ratio of dispersant to crosslinking agent of (4-5.5):(2.5-3):(3-3.5).

[0009] As a preferred embodiment, the polyester fiber has a fineness of 0.5 to 1.5 denier.

[0010] As a preferred embodiment, the polyester fiber has a fineness of 0.6 to 0.8 denier.

[0011] As a preferred embodiment, the average length of the polyester fiber is 30-60 mm.

[0012] As a preferred embodiment, the average length of the polyester fiber is 40-50 mm.

[0013] As a preferred embodiment, the polyester fiber has a Y-shaped cross-section or a pentagonal cross-section.

[0014] As a preferred embodiment, the polyester fiber has a pentagonal cross-section.

[0015] As a preferred embodiment, the preparation method of the modified graphene nanosheets specifically includes the following steps: S1: Graphene nanosheets and titanium dioxide are mixed and added to a DMF solution, heated to 70-75℃, succinic anhydride is added, and the reaction is maintained at this temperature for 2-3 hours. After completion, the nanosheets are washed, filtered, and dried to obtain pretreated nanosheets; S2: Titanium dioxide and anhydrous aluminum chloride are mixed and added to a mixed solution of DMF and deionized water, stirred at 100-120 rpm for 10-15 minutes, and then terephthalic acid and 2-aminoterephthalic acid are added. A mixed DMF solution of acid was stirred at 100–120 rpm for 10–15 min to form a homogeneous solution. The reaction vessel was sealed, and the temperature was raised to 130–150 °C under nitrogen protection, and the reaction was maintained at this temperature for 14–16 h. S3: After the reaction was completed, the mixture was naturally cooled to 70–80 °C, and then the pretreated nanosheets were added. The mixture was kept at this temperature for another 4–6 h. After the reaction was completed, triethanolamine was added to adjust the pH value to 7.5–8. The product was then filtered, washed 2–3 times with deionized water and acetone, and then dried under vacuum at 70–80 °C. The product was then obtained.

[0016] As a preferred embodiment, in S1, the mass ratio of graphene nanosheets, titanium dioxide, and succinic anhydride is (6-8):(0.8-1.4):(1.5-2).

[0017] As a preferred embodiment, in S2 and S3, the mass ratio of titanium dioxide, anhydrous aluminum chloride, terephthalic acid, 2-aminoterephthalic acid and pretreated nanosheets is (0.5-0.8):(2.5-3.5):(1.4-2):(1-1.4):(1-2).

[0018] As a preferred embodiment, in S2 and S3, the mass ratio of titanium dioxide, anhydrous aluminum chloride, terephthalic acid, 2-aminoterephthalic acid and pretreated nanosheets is (0.6-0.7):(2.5-3):(1.4-1.8):(1.1-1.3):(1-1.5).

[0019] As a preferred embodiment, the titanium dioxide has an average particle size of 10–20 nm.

[0020] As a preferred embodiment, the mass ratio of DMF to deionized water in the mixed solution of DMF and deionized water is (2-3):1.

[0021] As a preferred embodiment, the graphene nanosheets have 5 to 10 layers.

[0022] As a preferred embodiment, the lateral dimensions of the graphene nanosheets are 3–5 μm.

[0023] The addition of modified graphene nanosheets in this application not only effectively improves the wear resistance and antibacterial properties of the fabric material, but also significantly enhances its moisture absorption, wicking, aging resistance, and corrosion resistance. The added modified graphene nanosheets, using titanium dioxide as a particle medium, form a framework of particles on the surface and sides of the nanosheets through group interactions, resulting in a sheet-like composite structure based on graphene nanosheets. This structure creates a good heterojunction structure, which, under light exposure, promotes the formation of more electron-hole pairs on the surface titanium dioxide particles. Furthermore, by extending the electron movement path and widening the band gap, holes and electrons accumulate for extended periods, significantly improving the oxidative antibacterial properties and preventing electron backflow. This results in excellent long-lasting antibacterial effects during long-term use. The addition of short-cut carbon fibers further enhances this effect, and the resulting linear-surface composite structure significantly strengthens the bonding force under external forces, thereby improving the fabric's mechanical properties. Furthermore, the resulting modified graphene nanosheet composite structure exhibits good structural stability. In particular, the addition of framework particles, which serve as surface support sites, provides excellent intermolecular structural stability. This ensures that the overall orderliness of the fabric surface molecular structure remains excellent even in long-term abrasion-resistant environments, thereby achieving superior abrasion resistance.

[0024] On the other hand, the modified graphene nanosheets added in this application can also form a guiding path for water molecules through the selected specific dispersant and chopped carbon fibers. The dispersant can enhance the surface stability of the modified graphene nanosheets and chopped carbon fibers in the mixed fabric, and when in contact with water, it can guide and adsorb water through a large number of surface hydrophilic clusters. The more complex peak-valley surface can form grooves to lock in surface water and limit its migration effect, thereby achieving a continuous hydration layer region, accelerating the passage of water, and thus effectively achieving the function of moisture absorption and perspiration, with excellent moisture absorption. In addition, the addition of carbon fibers can significantly enhance the surface free radical activity of the modified graphene nanosheets and limit the penetration of active groups into the fabric coating, thereby effectively protecting the fibers and obtaining excellent aging resistance and corrosion resistance.

[0025] As a preferred embodiment, the antibacterial agent is at least one selected from silver chloride, zinc oxide, hexadecyltrimethylammonium bromide, potassium sorbate, and sodium benzoate.

[0026] As a preferred embodiment, the antibacterial agent is hexadecyltrimethylammonium bromide.

[0027] As a preferred embodiment, the dispersant is a composition of polyethylene glycol fatty acid ester, lauryl alcohol polyoxyethylene ether, and cocamidopropyl betaine.

[0028] As a preferred embodiment, the mass ratio of the polyethylene glycol fatty acid ester, lauryl alcohol polyoxyethylene ether and cocamidopropyl betaine is (6-10):(2-4):(2-4).

[0029] As a preferred embodiment, the mass ratio of the polyethylene glycol fatty acid ester, lauryl alcohol polyoxyethylene ether, and cocamidopropyl betaine is (8-9):(2.5-3):(3.5-4).

[0030] As a preferred embodiment, the hydroxyl value of the lauryl alcohol polyoxyethylene ether is 160–190 mg KOH / g.

[0031] As a preferred embodiment, the antioxidant is at least one of antioxidant 1010, antioxidant 1076, antioxidant 168, or antioxidant 626.

[0032] As a preferred embodiment, the antioxidant is antioxidant 1010 or antioxidant 1076.

[0033] As a preferred embodiment, the stabilizer is a combination of dibutyltin dilaurate and UV-531.

[0034] As a preferred embodiment, the mass ratio of dibutyltin dilaurate to UV-531 is (3-5):(1-1.5).

[0035] As a preferred embodiment, the mass ratio of dibutyltin dilaurate to UV-531 is (3.8–4.2):(1.2–1.4).

[0036] As a preferred embodiment, the softener is a composition of hexadecyltrimethylammonium chloride, amino silicone oil, and glyceryl stearate.

[0037] As a preferred embodiment, the mass ratio of hexadecyltrimethylammonium chloride, amino silicone oil, and glyceryl stearate is (1-1.5):(5-6):(0.3-0.5).

[0038] As a preferred embodiment, the crosslinking agent is a composition of diphenylmethane diisocyanate, toluene diisocyanate, and γ-aminopropyltriethoxysilane.

[0039] As a preferred embodiment, the mass ratio of diphenylmethane diisocyanate, toluene diisocyanate, and γ-aminopropyltriethoxysilane is (4-5):(2-3):(0.2-0.6).

[0040] As a preferred embodiment, the mass ratio of diphenylmethane diisocyanate, toluene diisocyanate, and γ-aminopropyltriethoxysilane is (4.5–5):(2–2.2):(0.3–0.4).

[0041] As a preferred embodiment, the carbon fiber is short-cut carbon fiber.

[0042] As a preferred embodiment, the average diameter of the chopped carbon fibers is 5–8 μm; the average length of the chopped carbon fibers is 7–12 mm.

[0043] The second aspect of this application provides a preparation process for the aforementioned wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene, specifically including the following steps: S1: Modified graphene nanosheets and a dispersant are mixed and added to deionized water, and ultrasonically dispersed into a stable suspension. Then, an antibacterial agent, a dispersant, an antioxidant, a stabilizer, a softener, and a crosslinking agent are added sequentially. After each addition, the mixture is stirred at 100-200 rpm for 20-30 minutes to ensure that all components are mixed evenly, resulting in a mixed solution; S2: Polyester fiber and carbon fiber are stirred, mixed, and impregnated into the mixed solution. The mixture is stirred at 300-400 rpm for 30-35 minutes. Then, the impregnated fibers are dried at 130-150°C for 20-25 minutes to remove excess moisture and promote the curing of the coating, resulting in mixed fibers; S3: The mixed fibers are ring-spun into yarn. A suitable weaving method is selected according to the requirements of the final fabric, and the density of the warp and weft yarns is adjusted to achieve the required fabric thickness and strength, thus completing the process.

[0044] The beneficial effects of this application are:

[0045] 1. The wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene provided in this application not only has good wear resistance and antibacterial properties, but also can further improve its moisture absorption and wicking, aging resistance and corrosion resistance properties, effectively meeting consumers' needs for existing textiles, having more functionality and having excellent application prospects.

[0046] 2. This application provides a wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene. The modified graphene nanosheets added can form a framework particle synthesis and intercalation on the surface and sides of the nanosheets through group interaction with titanium dioxide as the particle medium, thereby realizing a sheet-like composite structure based on graphene nanosheets. The presence of this structure can form a good heterojunction structure. Under light, it can promote the formation of more hole-electron pairs on the surface titanium dioxide particles, and can widen the band gap by extending the electron movement path, thereby allowing holes and electrons to accumulate for a long time. This not only greatly improves its oxidation and antibacterial properties, but also avoids electron backflow, thus achieving excellent long-term antibacterial effect during long-term use. In particular, the addition of short-cut carbon fibers significantly improves this effect, and the formed linear-surface composite structure greatly enhances its connection force under external force, thereby improving the mechanical properties of the fabric.

[0047] 3. The wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene provided in this application, wherein the modified graphene nanosheets can form a guiding path for water molecules through the selected specific dispersant and short-cut carbon fibers, the dispersant can enhance the surface stability of the modified graphene nanosheets and short-cut carbon fibers in the mixed fabric, and when in contact with water, it can guide and adsorb water through a large number of surface hydrophilic clusters, and the more complex peak-valley surface can form grooves to lock surface water and limit its migration effect, thereby realizing a continuous hydration layer area, accelerating the passage of water, and thus effectively achieving the function of moisture absorption and perspiration, with excellent moisture absorption; and the addition of carbon fibers can significantly enhance the surface free radical activity of the modified graphene nanosheets and limit the penetration of active groups into the fabric coating, thereby effectively protecting the fibers and obtaining excellent aging resistance and corrosion resistance. Detailed Implementation

[0048] The following will further illustrate and demonstrate the technical solutions described above in this application through specific implementation schemes. Furthermore, the following embodiments are merely practical examples used to illustrate and explain the content of the technical solutions in the specification, and should not limit the scope of the claims to be protected by this application. All technical products based on the technical solutions described in this application should be covered within the scope of protection of this application.

[0049] In the following embodiments, unless otherwise specified, the raw materials are all commercially available products or can be prepared by methods known to those skilled in the art.

[0050] Example 1

[0051] Example 1: The first aspect provides a wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene. By weight, the raw materials are: 72.5 parts polyester fiber, 5.2 parts modified graphene nanosheets, 0.4 parts antibacterial agent, 2.8 parts dispersant, 0.8 parts antioxidant, 1.4 parts stabilizer, 1.8 parts softener, 3.2 parts crosslinking agent, and 9 parts carbon fiber.

[0052] The polyester fiber has a fineness of 0.8 denier; the average length of the polyester fiber is 45 mm; the cross-section of the polyester fiber is a pentagonal cross-section; the polyester fiber was purchased from Taian Haosong Fiber Co., Ltd. of China and is of the corresponding specification.

[0053] The preparation method of modified graphene nanosheets specifically includes the following steps: S1: 7.2 parts of graphene nanosheets and 1.1 parts of titanium dioxide are mixed and added to 200 parts of DMF solution. The temperature is raised to 75℃, 1.8 parts of succinic anhydride are added, and the reaction is maintained at this temperature for 2.5 h. After completion, the nanosheets are washed, filtered, and dried to obtain pretreated nanosheets; S2: 0.6 parts of titanium dioxide and 2.8 parts of anhydrous aluminum chloride are mixed and added to a mixed solution of DMF and deionized water (the mass ratio of DMF to deionized water is 3:1, totaling 150 parts). The mixture is stirred at 120 rpm for 12 min. Then, a mixed DMF solution of 1.6 parts terephthalic acid and 1.2 parts 2-aminoterephthalic acid (60 parts in total) was added, and the mixture was stirred at 120 rpm for 15 min to form a homogeneous solution. The reaction vessel was sealed, and the temperature was raised to 140℃ under nitrogen protection and kept at this temperature for 15 h. S3: After the reaction was completed, the mixture was naturally cooled to 75℃, and then 1.3 parts of pretreated nanosheets were added. The mixture was kept at this temperature for another 6 h. After the reaction was completed, triethanolamine was added to adjust the pH value to 7.8. The product was then filtered, washed three times with deionized water and acetone, and then dried under vacuum at 80℃ to obtain the final product.

[0054] The average particle size of titanium dioxide is 16 nm.

[0055] The graphene nanosheets have 8 to 10 layers and an average lateral dimension of 4.2 μm. They were purchased from Henan Liugong Graphite Co., Ltd. in China and were products of the corresponding specifications.

[0056] The antibacterial agent is hexadecyltrimethylammonium bromide.

[0057] The dispersant is a composition of polyethylene glycol fatty acid ester, lauryl alcohol polyoxyethylene ether and cocamidopropyl betaine, with a mass ratio of 8.5:2.6:3.6.

[0058] The hydroxyl value of lauryl alcohol polyoxyethylene ether is 180 mg KOH / g, and it is a MOA-3 product purchased from China Haian Guo Chemical Co., Ltd.

[0059] The antioxidant is antioxidant 1010.

[0060] The stabilizer is a combination of dibutyltin dilaurate and UV-531 in a mass ratio of 4:1.2.

[0061] The softener is a composition of hexadecyltrimethylammonium chloride, amino silicone oil and glyceryl stearate, in a mass ratio of 1.2:5.5:0.3.

[0062] The crosslinking agent is a composition of diphenylmethane diisocyanate, toluene diisocyanate and γ-aminopropyltriethoxysilane, in a mass ratio of 4.8:2.1:0.3.

[0063] The carbon fiber is short-cut carbon fiber with an average diameter of 7.5 μm and an average length of 10.5 mm, and was purchased from Shanghai Lishuo Composite Materials Co., Ltd. for the corresponding specifications.

[0064] The second aspect of this embodiment provides a preparation process for the above-mentioned wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene, specifically including the following steps: S1: Modified graphene nanosheets and dispersant are mixed and added to deionized water, and ultrasonically dispersed into a stable suspension. Then, antibacterial agent, dispersant, antioxidant, stabilizer, softener and crosslinking agent are added sequentially. After each addition, the mixture is stirred at 180 rpm for 25 minutes to ensure that all components are mixed evenly, resulting in a mixed solution; S2: Polyester fiber and carbon fiber are stirred and mixed and impregnated into the mixed solution. The mixture is stirred at 400 rpm for 30 minutes. Then, the impregnated fiber is dried at 140°C for 22 minutes to remove excess moisture and promote the curing of the coating, resulting in mixed fiber; S3: The mixed fiber is ring spun into yarn. According to the requirements of the final fabric, a suitable weaving method is selected, and the density of the warp and weft yarns is adjusted to achieve the required fabric thickness and strength, thus completing the process.

[0065] Example 2

[0066] The specific implementation method of this embodiment is basically the same as that of Embodiment 1, except that: the wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene, by weight, consists of: 75 parts polyester fiber, 4 parts modified graphene nanosheets, 0.4 parts antibacterial agent, 2.5 parts dispersant, 0.8 parts antioxidant, 1.4 parts stabilizer, 1.8 parts softener, 3 parts crosslinking agent, and 10 parts carbon fiber.

[0067] The dispersant is a composition of polyethylene glycol fatty acid ester, lauryl alcohol polyoxyethylene ether, and cocamidopropyl betaine, with a mass ratio of 6:4:4.

[0068] The stabilizer is a combination of dibutyltin dilaurate and UV-531 in a mass ratio of 5:1.

[0069] The softener is a composition of hexadecyltrimethylammonium chloride, amino silicone oil and glyceryl stearate, in a mass ratio of 1.5:5:0.5.

[0070] The crosslinking agent is a composition of diphenylmethane diisocyanate, toluene diisocyanate and γ-aminopropyltriethoxysilane, in a mass ratio of 4:3:0.6.

[0071] Example 3

[0072] The specific implementation method of this embodiment is basically the same as that of Embodiment 1, except that: the wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene, by weight, consists of: 70 parts polyester fiber, 5.5 parts modified graphene nanosheets, 0.4 parts antibacterial agent, 3 parts dispersant, 0.8 parts antioxidant, 1.4 parts stabilizer, 1.8 parts softener, 3.5 parts crosslinking agent, and 8 parts carbon fiber.

[0073] The dispersant is a composition of polyethylene glycol fatty acid ester, lauryl alcohol polyoxyethylene ether and cocamidopropyl betaine, in a mass ratio of 10:2:3.

[0074] The stabilizer is a combination of dibutyltin dilaurate and UV-531 in a mass ratio of 3:1.4.

[0075] The softener is a composition of hexadecyltrimethylammonium chloride, amino silicone oil and glyceryl stearate, in a mass ratio of 1:6:0.3.

[0076] The crosslinking agent is a composition of diphenylmethane diisocyanate, toluene diisocyanate and γ-aminopropyltriethoxysilane, in a mass ratio of 5:2:0.3.

[0077] Comparative Example 1

[0078] The specific implementation method of this comparative example is basically the same as that of Example 1, except that: the wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene, by weight, consists of: 80 parts polyester fiber, 8.5 parts modified graphene nanosheets, 0.4 parts antibacterial agent, 1.5 parts dispersant, 0.8 parts antioxidant, 1.4 parts stabilizer, 1.8 parts softener, 2.1 parts crosslinking agent, and 9 parts carbon fiber.

[0079] The dispersant is a composition of polyethylene glycol fatty acid ester, lauryl alcohol polyoxyethylene ether and cocamidopropyl betaine, with a mass ratio of 5:0:1.

[0080] Comparative Example 2

[0081] The specific implementation method of this comparative example is basically the same as that of Example 1, except that: the wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene, by weight, contains the following raw materials: 70.5 parts polyester fiber, 6.2 parts modified graphene nanosheets, 0.4 parts antibacterial agent, 2.8 parts dispersant, 0.8 parts antioxidant, 1.4 parts stabilizer, 1.8 parts softener, 3.2 parts crosslinking agent, and 9 parts carbon fiber.

[0082] The dispersant is a composition of polyethylene glycol fatty acid ester, lauryl alcohol polyoxyethylene ether and cocamidopropyl betaine, in a mass ratio of 2:6:1.

[0083] Comparative Example 3

[0084] The specific implementation method of this comparative example is basically the same as that of Example 1, except that the cross-section of the polyester fiber is a triangular cross-section.

[0085] Comparative Example 4

[0086] The specific implementation method of this comparative example is basically the same as that of Example 1, except that the dispersant is a composition of cetearyl alcohol polyoxyethylene ether and sodium dodecylbenzene sulfonate, with a mass ratio of 3:1.

[0087] Comparative Example 5

[0088] The specific implementation method of this comparative example is basically the same as that of Example 1, except that the preparation method of modified graphene nanosheets specifically includes the following steps: S1: 9.5 parts of graphene nanosheets and 0.5 parts of titanium dioxide are mixed and added to 300 parts of DMF solution, heated to 75°C, 2.5 parts of succinic anhydride are added, and the reaction is maintained at this temperature for 2.5 hours. After completion, the mixture is washed, filtered, and dried to obtain pretreated nanosheets; S2: 0.2 parts of titanium dioxide and 2.8 parts of anhydrous aluminum chloride are mixed and added to a mixed solution of DMF and deionized water (the mass ratio of DMF to deionized water is 3:1, totaling 150 parts), 1 Stir at 20 rpm for 12 min, then add 1.6 parts of a mixed DMF solution of terephthalic acid and 1.2 parts of 2-aminoterephthalic acid (60 parts in total), stir at 120 rpm for 15 min to form a homogeneous solution, seal the reaction vessel, heat to 140℃ under nitrogen protection, and keep the reaction at this temperature for 15 h; S3: After the reaction is completed, cool naturally to 75℃, then add 1.3 parts of pretreated nanosheets, continue to keep the temperature for 6 h, add triethanolamine to adjust the pH to 7.8 after the reaction is completed, then filter the product, wash it three times with deionized water and acetone, and then dry it under vacuum at 80℃ to obtain the final product.

[0089] Comparative Example 6

[0090] The specific implementation method of this comparative example is basically the same as that of Example 1, except that the preparation method of modified graphene nanosheets specifically includes the following steps: S1: 7.2 parts of graphene nanosheets and 1.1 parts of titanium dioxide are mixed and added to 200 parts of DMF solution, heated to 75°C, 1.8 parts of succinic anhydride are added, and the reaction is maintained at this temperature for 2.5 hours. After completion, the mixture is washed, filtered, and dried to obtain pretreated nanosheets; S2: 1.5 parts of titanium dioxide and 2.8 parts of anhydrous aluminum chloride are mixed and added to a mixed solution of DMF and deionized water (the mass ratio of DMF to deionized water is 3:1, totaling 150 parts), 1 Stir at 20 rpm for 12 min, then add 1.6 parts of a mixed DMF solution of terephthalic acid and 1.2 parts of 2-aminoterephthalic acid (60 parts in total), stir at 120 rpm for 15 min to form a homogeneous solution, seal the reaction vessel, heat to 140℃ under nitrogen protection, and keep the reaction at this temperature for 15 h; S3: After the reaction is completed, cool naturally to 75℃, then add 0.5 parts of pretreated nanosheets, continue to keep the temperature for 6 h, add triethanolamine to adjust the pH to 7.8 after the reaction is completed, then filter the product, wash it three times with deionized water and acetone, and then dry it under vacuum at 80℃ to obtain the final product.

[0091] Comparative Example 7

[0092] The specific implementation method of this comparative example is basically the same as that of Example 1, except that the average particle size of titanium dioxide is 45 nm. The number of graphene nanosheets is 15 to 20 layers, the average lateral size is 6.5 μm, and the corresponding specifications of the product were purchased from Henan Liugong Graphite Co., Ltd. in China.

[0093] Performance Evaluation

[0094] Abrasion resistance test: The fabrics prepared in the examples and comparative examples were tested for abrasion resistance in accordance with the standard ASTM D3383. The abrasion wheel was H18 and the number of tests was 5000. The percentage of weight loss before and after the test was recorded. The test value was taken as the average value of 50 tests and recorded in Table 1. The surface condition of the fabric after the test was recorded. If there was no change in color, no pilling, no fuzzing, and no obvious wear, it was considered as qualified. Otherwise, it was considered as unqualified. Each group was tested 50 times and the pass rate was recorded in Table 1.

[0095] Antimicrobial testing: Fabrics prepared according to the AATCC 100 examples and comparative examples were subjected to antimicrobial testing. The test strain was Staphylococcus aureus, and the bacterial suspension concentration was 10. 5 The final antibacterial rate was obtained by testing at CFU / mL, 37℃, for 24 hours. The average value of 10 tests was recorded in Table 1.

[0096] Moisture absorption test: The fabrics prepared in the examples and comparative examples were subjected to a standard moisture regain test in accordance with ISO 139:2017. The test values ​​were the average of 10 tests and recorded in Table 1.

[0097] Aging and corrosion resistance test: The fabrics prepared in the examples and comparative examples were made into strips of fabric measuring 25mm × 100mm. These strips were then sprayed with 5wt% NaCl at a slant at 62±2℃ and 80±2% humidity at a spray rate of 1mL / 80cm. 2 / h, test for 72h. After 72h, take it out and observe whether there is any damage, pilling, fuzzing and discoloration. If there is, it is recorded as unqualified, otherwise it is qualified. Each group has 50 tests, and the pass rate is recorded in Table 1.

[0098] Table 1 Performance Test Results

[0099]

[0100] From the embodiments and comparative examples of this application, as well as the data results in Table 1, it can be seen that embodiments 1-3 of this application have significant advantages over comparative examples 1-7 in terms of wear resistance, antibacterial properties, moisture absorption and wicking, and resistance to aging and corrosion. This is mainly due to the combined effect of the modified graphene nanosheets, specific dispersant combinations, and other cooperating technical solutions specified in this application. In contrast, comparative examples 1-7 did not adopt the technical solutions specified in this application, resulting in significant disadvantages in the above performance tests. This further proves the necessity of the technical solutions specified in this application for the technical effects of this application and for solving technical problems.

Claims

1. A wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene, characterized in that: By weight, the raw materials are: 60-80 parts polyester fiber, 2-6 parts modified graphene nanosheets, 0.3-0.8 parts antibacterial agent, 2-4 parts dispersant, 0.5-1 part antioxidant, 1-2 parts stabilizer, 1-3 parts softener, 2-4 parts crosslinking agent, and 5-15 parts carbon fiber. The polyester fiber has a fineness of 0.5 to 1.5 denier; The average length of the polyester fiber is 30~60mm; The cross-section of the polyester fiber is a Y-shaped cross-section or a pentagonal cross-section; The preparation method of the modified graphene nanosheets specifically includes the following steps: S1: Graphene nanosheets and titanium dioxide are mixed and added to a DMF solution, heated to 70-75℃, succinic anhydride is added and the reaction is maintained for 2-3 hours. After completion, the nanosheets are washed, filtered, and dried to obtain pretreated nanosheets; S2: Titanium dioxide and anhydrous aluminum chloride are mixed and added to a mixed solution of DMF and deionized water, stirred at 100-120 rpm for 10-15 minutes, and then a mixture of terephthalic acid and 2-aminoterephthalic acid is added. MF solution: Stir at 100-120 rpm for 10-15 min to form a homogeneous solution. Seal the reaction vessel and heat to 130-150℃ under nitrogen protection. Maintain the temperature for 14-16 h. S3: After the reaction is complete, allow it to cool naturally to 70-80℃. Then add the pretreated nanosheets and continue to maintain the temperature for 4-6 h. After the reaction is complete, add triethanolamine to adjust the pH to 7.5-8. Then filter the product, wash it 2-3 times with deionized water and acetone, and then dry it under vacuum at 70-80℃. The product is now ready. In S1, the mass ratio of graphene nanosheets, titanium dioxide, and succinic anhydride is (6~8):(0.8~1.4):(1.5~2). In S2 and S3, the mass ratio of titanium dioxide, anhydrous aluminum chloride, terephthalic acid, 2-aminoterephthalic acid and pretreated nanosheets is (0.5~0.8):(2.5~3.5):(1.4~2):(1~1.4):(1~2). The modified graphene nanosheets have a dispersant to crosslinking agent mass ratio of (4~5.5):(2.5~3):(3~3.5). The average particle size of the titanium dioxide is 10~20 nm; The graphene nanosheets have 5 to 10 layers; the lateral dimensions of the graphene nanosheets are 3 to 5 μm. The carbon fiber is chopped carbon fiber; the average diameter of the chopped carbon fiber is 5~8μm; the average length of the chopped carbon fiber is 7~12mm.

2. The wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene according to claim 1, characterized in that: The mass ratio of the polyester fiber, modified graphene nanosheets and carbon fiber is (70~75):(4~5.5):(8~10).

3. The wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene according to claim 2, characterized in that: The antibacterial agent is at least one of silver chloride, zinc oxide, hexadecyltrimethylammonium bromide, potassium sorbate, and sodium benzoate.

4. The wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene according to claim 3, characterized in that: The dispersant is a composition of polyethylene glycol fatty acid ester, lauryl alcohol polyoxyethylene ether and cocamidopropyl betaine; the mass ratio of polyethylene glycol fatty acid ester, lauryl alcohol polyoxyethylene ether and cocamidopropyl betaine is (6~10):(2~4):(2~4).

5. The wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene according to claim 4, characterized in that: The antioxidant is at least one of antioxidant 1010, antioxidant 1076, antioxidant 168 or antioxidant 626.

6. A preparation process for a wear-resistant and antibacterial school uniform fabric based on polyester fiber and graphene according to any one of claims 1 to 5, characterized in that: Specifically, the following steps are included: S1: Modified graphene nanosheets and dispersant are mixed and added to deionized water, and ultrasonically dispersed into a stable suspension. Then, antibacterial agent, dispersant, antioxidant, stabilizer, softener and crosslinking agent are added sequentially. After each addition, the mixture is stirred at 100-200 rpm for 20-30 minutes to ensure that all components are mixed evenly, resulting in a mixed solution. S2: Polyester fiber and carbon fiber are stirred and mixed and impregnated into the mixed solution. The mixture is stirred at 300-400 rpm for 30-35 minutes. Then, the impregnated fiber is dried at 130-150℃ for 20-25 minutes to remove excess moisture and promote the curing of the coating, resulting in mixed fiber. S3: The mixed fiber is ring spun into yarn. According to the requirements of the final fabric, a suitable weaving method is selected, and the density of the warp and weft yarns is adjusted to achieve the required fabric thickness and strength.

Citation Information

Patent Citations

  • Wear resistant and antistatic polyamide composite material and preparation method thereof

    CN106967293A

  • Antibacterial terylene woven gray fabric and production process thereof

    CN114182524A

  • GO-TiO2at-MIL-68 (Al) composite material as well as preparation method and application thereof

    CN118513087A