Leak-stopping grout for low-pressure, severely leaking formations, its preparation method and application

By using a plugging slurry composed of modified walnut shells and other components, the problem of easy aggregation of plugging materials in low-pressure, high-risk formations was solved, achieving effective plugging in low-density window formations and avoiding well leakage caused by increased density.

CN119490830BActive Publication Date: 2026-11-10PETROCHINA CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311025230.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-15
Publication Date
2026-11-10
Estimated Expiration
2043-08-15

AI Technical Summary

Technical Problem

In existing technologies, conventional plugging slurries tend to accumulate in low-pressure, severely leaky formations, resulting in poor plugging effects and increased density, which further leads to well leakage, creating a vicious cycle of more plugging and more leakage.

Method used

The sealing slurry is composed of modified walnut shells, bentonite, xanthan gum, rubber particles, and lignin sulfonate. The walnut shells are modified to prevent particle aggregation, and the slurry is treated with silane coupling agents and polyethylene to reduce viscosity and prevent solid particles from agglomerating, thereby improving dispersion performance.

Benefits of technology

It effectively prevents the aggregation of plugging slurry particles in low-density window formations, achieving good plugging results, reducing material consumption, and avoiding well leakage problems caused by increased density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004395235820000081
    Figure BDA0004395235820000081
  • Figure BDA0004395235820000091
    Figure BDA0004395235820000091
Patent Text Reader

Abstract

This invention discloses a sealing slurry for low-pressure, severely leaking formations, comprising water, bentonite, xanthan gum, modified walnut shell, rubber particles, and lignin sulfonate. The dispersion-type sealing slurry provided by this invention, suitable for low-density windows, effectively improves the dispersion performance of solid particles in the sealing slurry by modifying the sealing material, walnut shell. Therefore, it is not necessary to add a large amount of sealing material; only a small amount of modified walnut shell is needed to achieve a good sealing effect, making it very suitable for sealing formations with low-density windows.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of petroleum drilling chemical agents technology, and relates to a plugging slurry for low-pressure severe leakage formations. This invention also relates to a method for preparing the above-mentioned plugging slurry for low-pressure severe leakage formations, and to the application of the above-mentioned plugging slurry for low-pressure severe leakage formations. Background Technology

[0002] Low-pressure, severe leakage formations are a common problem in oil drilling, characterized by a low drilling fluid density window. A low density window means that the drilling fluid has a very small density range to choose from when drilling a particular formation. This situation easily leads to drilling complications; if the drilling fluid density exceeds this range, it causes well leakage; if it falls below, it causes wellbore collapse and spalling. When well leakage occurs, plugging slurry is often used for plugging. However, for low-density window formations in low-pressure, severe leakage formations, the amount of plugging material in the slurry should not be excessive. Otherwise, the density of the plugging slurry will increase, potentially fracturing the wellbore and causing even more severe leakage. This is because conventional plugging materials tend to aggregate. Once aggregated, the plugging material becomes larger and cannot easily penetrate the formation fractures for plugging. At this point, new plugging material needs to be added, which also tends to aggregate, creating a vicious cycle. The more new plugging material is added, the greater the density of the plugging slurry becomes, resulting in a situation where plugging only exacerbates the leakage. Therefore, it is necessary to provide a plugging grout for low-pressure, severely leaking formations to solve the above-mentioned technical problems. Summary of the Invention

[0003] The purpose of this invention is to provide a plugging grout for low-pressure, severely leaking formations, which solves the problem that conventional plugging grouts in the prior art are not easy to disperse, thus causing leakage to increase the more they are plugged in low-pressure, severely leaking formations.

[0004] Another object of the present invention is to provide a method for preparing the above-mentioned plugging grout for low-pressure, severely leaking formations.

[0005] Another object of the present invention is to provide the application of the above-mentioned plugging grout for low-pressure, severely leaking formations.

[0006] The technical solution adopted in this invention is a plugging grout for low-pressure, severely leaking formations, which is composed of the following components: based on 100 parts by weight of water, 3 to 6 parts by weight of bentonite, 5 to 8 parts by weight of xanthan gum, 14 to 16 parts by weight of modified walnut shell, 8 to 10 parts by weight of rubber particles, and 6 to 9 parts by weight of lignin sulfonate.

[0007] The invention is further characterized by:

[0008] The preparation method of modified walnut shells is as follows:

[0009] S1. Grind the walnut shells and pass them through an 80-mesh sieve to obtain walnut shell powder;

[0010] S2. Soak the walnut shell powder obtained in step S1 in anhydrous ethanol, heat and stir, then remove it, wash it with deionized water and drain it to obtain the first processed product.

[0011] S3. Pour deionized water into the container, add hydrochloric acid solution to adjust the pH value to 4-5, add silane coupling agent, place the first processed product obtained in step S2 into the container, heat and stir, then take it out, wash it with deionized water and drain it to obtain the second processed product.

[0012] S4. The second processed material is mixed with polyethylene and ball-milled to obtain the third processed material;

[0013] S5. Place the third processed product in an oven and bake it to obtain the fourth processed product;

[0014] S6. Grind the fourth processed material and pass it through a 60-mesh sieve to obtain the final product.

[0015] In step S2, the heating temperature is 40-50℃ and the stirring time is 10-15 minutes.

[0016] In step S3, the mass ratio of the first processed material to the silane coupling agent is 1:0.4-0.6.

[0017] In step S3, the heating temperature is 60-70℃ and the stirring time is 20-30 minutes.

[0018] In step S4, the ratio of the second processed material to polyethylene is 1:2-2.4.

[0019] In step S5, the baking temperature is 100-110℃ and the baking time is 80-100 minutes.

[0020] Another technical solution adopted in this invention is a method for preparing plugging grout for low-pressure, severely leaking formations. The preparation method is as follows:

[0021] S101: Based on 100 parts by weight of water, weigh out 3-6 parts by weight of bentonite, 5-8 parts by weight of xanthan gum, 14-16 parts by weight of modified walnut shell, 8-10 parts by weight of rubber granules, and 6-9 parts by weight of lignin sulfonate.

[0022] S201: Mix the ingredients weighed in S101 and then stir to obtain the final product.

[0023] The invention is further characterized by the application of plugging slurry in low-pressure, severely leaking formations for plugging leaks in oil and gas wells with low safety density drilling fluid windows.

[0024] The beneficial effects of this invention are:

[0025] The sealing slurry for low-pressure, severely leaking formations provided by this invention modifies the sealing material, walnut shells. First, the oil and sugar in the walnut shells are removed by soaking in anhydrous ethanol to prevent the aggregation of walnut shell particles. Then, the silanol produced by the dissolution of the silane coupling agent reacts with the OH groups on the walnut shells to form Si-O-Si and Si-OC bonds, which hardens the clay in the sealing slurry to a certain extent, thereby reducing its viscosity and effectively preventing the aggregation of solid particles in the sealing slurry. Finally, the surface of the walnut shell powder is treated with polyethylene to make it hydrophobic, further preventing particle aggregation and effectively improving the dispersion performance of solid particles in the sealing slurry. Therefore, it does not require a large amount of sealing material; only a small amount of modified walnut shells is needed to achieve a good sealing effect, making it very suitable for sealing formations with low-density windows. Detailed Implementation

[0026] The present invention will now be described in detail with reference to specific embodiments.

[0027] The plugging grout used in low-pressure, severely leaking formations is composed of the following components: based on 100 parts by weight of water, 3-6 parts by weight of bentonite, 5-8 parts by weight of xanthan gum, 14-16 parts by weight of modified walnut shell, 8-10 parts by weight of rubber particles, and 6-9 parts by weight of lignin sulfonate.

[0028] The preparation method of modified walnut shells is as follows:

[0029] S1. Grind the walnut shells and pass them through an 80-mesh sieve to obtain walnut shell powder;

[0030] S2. Soak the walnut shell powder obtained in step S1 in anhydrous ethanol, heat and stir, then take it out, wash it with deionized water and drain it to obtain the first processed product. The purpose of this step is to remove the oil and sugar in the walnut shell to prevent the walnut shell particles from agglomerating.

[0031] S3. Pour deionized water into the container, add hydrochloric acid solution to adjust the pH to 4-5, and add silane coupling agent. The purpose of this step is that the silanol produced after the silane coupling agent dissolves reacts with the OH groups on the walnut shell to generate Si-O-Si and Si-OC bonds, which hardens the clay in the sealing grout to a certain extent, thereby reducing its viscosity and effectively preventing the aggregation of solid particles in the sealing grout. Place the first processed material obtained in step S2 into the container, heat and stir, then take it out, wash it with deionized water and drain it to obtain the second processed material.

[0032] S4. The second processed material is mixed with polyethylene and ball-milled to obtain the third processed material. The purpose of this step is to use polyethylene to perform hydrophobic treatment on the surface of the walnut shell powder, further preventing particle aggregation, thereby effectively improving the dispersion performance of solid particles in the plugging slurry.

[0033] S5. Place the third processed product in an oven and bake it to obtain the fourth processed product;

[0034] S6. Grind the fourth processed material and pass it through a 60-mesh sieve to obtain the final product.

[0035] In step S2, the heating temperature is 40-50℃ and the stirring time is 10-15 minutes.

[0036] In step S3, the mass ratio of the first processed material to the silane coupling agent is 1:0.4-0.6.

[0037] In step S3, the heating temperature is 60-70℃ and the stirring time is 20-30 minutes.

[0038] In step S4, the ratio of the second processed material to polyethylene is 1:2-2.4.

[0039] In step S5, the baking temperature is 100-110℃ and the baking time is 80-100 minutes.

[0040] The preparation method of plugging grout for low-pressure, severely lost circulation formations is as follows:

[0041] S101: Based on 100 parts by weight of water, weigh out 3-6 parts by weight of bentonite, 5-8 parts by weight of xanthan gum, 14-16 parts by weight of modified walnut shell, 8-10 parts by weight of rubber granules, and 6-9 parts by weight of lignin sulfonate.

[0042] S201: Mix the ingredients weighed in S101 and then stir to obtain the final product.

[0043] The application of plugging slurry in low-pressure, severely leaking formations is used for plugging leaks in oil and gas wells with low safety density drilling fluid windows.

[0044] Example 1

[0045] Place 100 parts by weight of water in an enamel measuring cup, add 6 parts by weight of bentonite, 8 parts by weight of xanthan gum, 16 parts by weight of modified walnut shell G1, 10 parts by weight of rubber granules and 9 parts by weight of lignin sulfonate to the water, and stir to obtain the plugging grout A1 for low-pressure severe leakage formations.

[0046] The modified walnut shell G1 was prepared as follows:

[0047] S1. Grind the walnut shells and pass them through an 80-mesh sieve to obtain walnut shell powder;

[0048] S2. Soak the walnut shell powder obtained in step S1 in anhydrous ethanol, heat it to 45°C and stir for 13 minutes, take it out, wash it with deionized water and drain it to obtain the first processed product.

[0049] S3. Pour deionized water into a three-necked flask, add hydrochloric acid solution to adjust the pH to 4.5, add silane coupling agent, place the first processed product obtained in step S2 into the three-necked flask, and the mass ratio of the first processed product to the silane coupling agent is 1:0.5. Heat to 65°C and stir for 25 minutes. Take it out, wash it with deionized water and drain it to obtain the second processed product.

[0050] S4. The second processed material and polyethylene are placed together in a planetary ball mill at a mass ratio of 1:2.2 and ball milled to obtain the third processed material.

[0051] S5. Place the third processed material in a boat dish and bake it in an oven at 105°C for 90 minutes to obtain the fourth processed material in block form.

[0052] S6. Grind the fourth processed material and pass it through a 60-mesh sieve to obtain modified walnut shell G1.

[0053] Example 2

[0054] Place 100 parts by weight of water in an enamel measuring cup, add 6 parts by weight of bentonite, 8 parts by weight of xanthan gum, 16 parts by weight of modified walnut shell G2, 10 parts by weight of rubber granules and 9 parts by weight of lignin sulfonate to the water, and stir to obtain the plugging grout A2 for low-pressure, severe leakage formations.

[0055] The modified walnut shell G2 was prepared as follows:

[0056] S1. Grind the walnut shells and pass them through an 80-mesh sieve to obtain walnut shell powder;

[0057] S2. Soak the walnut shell powder obtained in step S1 in anhydrous ethanol, heat it to 40°C and stir for 10 minutes. Take it out, wash it with deionized water and drain it to obtain the first processed product.

[0058] S3. Pour deionized water into a three-necked flask, add hydrochloric acid solution to adjust the pH value to 4, add silane coupling agent, place the first processed product obtained in step S2 into the three-necked flask, and the mass ratio of the first processed product to the silane coupling agent is 1:0.4. Heat to 60°C and stir for 20 minutes. Take it out, wash it with deionized water and drain it to obtain the second processed product.

[0059] S4. The second processed material and polyethylene are placed together in a planetary ball mill at a mass ratio of 1:2 and ball milled to obtain the third processed material.

[0060] S5. Place the third processed material in a boat dish and bake it in an oven at 100°C for 80 minutes to obtain the fourth processed material in block form.

[0061] S6. Grind the fourth processed material and pass it through a 60-mesh sieve to obtain modified walnut shell G2.

[0062] Example 3

[0063] Place 100 parts by weight of water in an enamel measuring cup, add 6 parts by weight of bentonite, 8 parts by weight of xanthan gum, 16 parts by weight of modified walnut shell G3, 10 parts by weight of rubber granules and 9 parts by weight of lignin sulfonate to the water, and stir to obtain the plugging grout A3 for low-pressure, severe leakage formations.

[0064] The modified walnut shell G3 was prepared as follows:

[0065] S1. Grind the walnut shells and pass them through an 80-mesh sieve to obtain walnut shell powder;

[0066] S2. Soak the walnut shell powder obtained in step S1 in anhydrous ethanol, heat to 50°C and stir for 15 minutes, take it out, wash it with deionized water and drain it to obtain the first processed product.

[0067] S3. Pour deionized water into a three-necked flask, add hydrochloric acid solution to adjust the pH value to 5, add silane coupling agent, place the first processed product obtained in step S2 into the three-necked flask, and the mass ratio of the first processed product to the silane coupling agent is 1:0.6. Heat to 70°C and stir for 30 minutes. Take it out, wash it with deionized water and drain it to obtain the second processed product.

[0068] S4. The second processed material and polyethylene are placed together in a planetary ball mill at a mass ratio of 1:2.4 and ball milled to obtain the third processed material.

[0069] S5. Place the third processed material in a boat dish and bake it in an oven at 110°C for 100 minutes to obtain the fourth processed material in block form.

[0070] S6. Grind the fourth processed material and pass it through a 60-mesh sieve to obtain modified walnut shell G3.

[0071] Example 4

[0072] Place 100 parts by weight of water in an enamel measuring cup, add 6 parts by weight of bentonite, 8 parts by weight of xanthan gum, 16 parts by weight of modified walnut shell G4, 10 parts by weight of rubber granules and 9 parts by weight of lignin sulfonate to the water, and stir to obtain the plugging slurry A4 for low-pressure, severe leakage formations.

[0073] The modified walnut shell G4 was prepared as follows:

[0074] S1. Grind the walnut shells and pass them through an 80-mesh sieve to obtain walnut shell powder;

[0075] S2. Soak the walnut shell powder obtained in step S1 in anhydrous ethanol, heat it to 43°C and stir for 12 minutes, take it out, wash it with deionized water and drain it to obtain the first processed product.

[0076] S3. Pour deionized water into a three-necked flask, add hydrochloric acid solution to adjust the pH to 4.3, add silane coupling agent, place the first processed product obtained in step S2 into the three-necked flask, and the mass ratio of the first processed product to the silane coupling agent is 1:0.45. Heat to 63°C and stir for 23 minutes. Take it out, wash it with deionized water and drain it to obtain the second processed product.

[0077] S4. The second processed material and polyethylene are placed together in a planetary ball mill at a mass ratio of 1:2.1 and ball milled to obtain the third processed material.

[0078] S5. Place the third processed material in a boat dish and bake it in an oven at 103°C for 85 minutes to obtain the fourth processed material in block form.

[0079] S6. Grind the fourth processed material and pass it through a 60-mesh sieve to obtain modified walnut shell G3.

[0080] Comparative Example 1

[0081] Except for the modified walnut shell, the other characteristics are the same as in Example 1. Ordinary walnut shells (60 mesh particle size, 16 parts by weight) are used instead of modified walnut shells to finally obtain the sealing slurry D1.

[0082] Comparative Example 2

[0083] Except for the modified walnut shell, the other characteristics are the same as in Example 2. Ordinary walnut shells (60 mesh particle size, 60 parts by weight) are used instead of modified walnut shells to finally obtain the sealing slurry D2.

[0084] The sealing performance of the sealing slurries obtained in the above embodiments and comparative examples was tested using a QD-2 type sealing instrument (with a joint length of 30 mm and a width of 1 mm). The results are as follows:

[0085]

[0086]

[0087] As can be seen from the data in the table above, the plugging slurry for low-pressure, severely leaking formations prepared by the method provided by this invention can achieve a pressure resistance of over 6 MPa when the amount of plugging material used is very small. However, if ordinary walnut shells are used as plugging material, a large amount is required to achieve the same plugging effect. But if the amount is large, the density of the plugging slurry will inevitably increase. Therefore, ordinary walnut shells are not suitable for plugging formations with low-density windows.

Claims

1. A plugging grout for low-pressure, severely leaking formations, characterized in that, It is composed of the following components: based on 100 parts by weight of water, 3 to 6 parts by weight of bentonite, 5 to 8 parts by weight of xanthan gum, 14 to 16 parts by weight of modified walnut shell, 8 to 10 parts by weight of rubber granules, and 6 to 9 parts by weight of lignin sulfonate. The method for preparing the modified walnut shell is as follows: S1. Grind the walnut shells and pass them through an 80-mesh sieve to obtain walnut shell powder; S2. Soak the walnut shell powder obtained in step S1 in anhydrous ethanol, heat and stir, then remove it, wash it with deionized water and drain it to obtain the first processed product. S3. Pour deionized water into the container, add hydrochloric acid solution to adjust the pH value to 4-5, add silane coupling agent, place the first processed product obtained in step S2 into the container, heat and stir, then take it out, wash it with deionized water and drain it to obtain the second processed product. S4. The second processed material is mixed with polyethylene and ball-milled to obtain the third processed material; S5. Place the third processed product in an oven and bake it to obtain the fourth processed product; S6. Grind the fourth processed material and pass it through a 60-mesh sieve to obtain the final product. In step S2, the heating temperature is 40-50℃ and the stirring time is 10-15 minutes; In step S3, the mass ratio of the first processed material to the silane coupling agent is 1:0.4-0.6; In step S3, the heating temperature is 60-70℃ and the stirring time is 20-30 minutes; In step S4, the ratio of the second processed material to polyethylene is 1:2-2.4; In step S5, the baking temperature is 100-110℃ and the baking time is 80-100 minutes.

2. The method for preparing the plugging grout for low-pressure, severely leaking formations as described in claim 1, characterized in that, The preparation method is as follows: S101: Based on 100 parts by weight of water, weigh out 3-6 parts by weight of bentonite, 5-8 parts by weight of xanthan gum, 14-16 parts by weight of modified walnut shell, 8-10 parts by weight of rubber granules, and 6-9 parts by weight of lignin sulfonate. S201: Mix the components weighed in S101 and then stir to obtain the final product.

3. The application of the plugging grout for low-pressure, severely leaking formations according to claim 1, characterized in that, Used for plugging leaks in oil and gas wells with low safety density drilling fluid windows.

Citation Information

Patent Citations

  • Nanometer plugging agent for drilling fluid and preparation method and application thereof

    CN109439293A

  • Basalt fiber leaking stoppage material suitable for granite cracks and preparation method of basalt fiber leaking stoppage material

    CN114395382A

  • Aqueous particulate slurries and methods of making the same

    US20180265773A1