A method for preparing a bio-based epoxy resin anti-corrosion coating
By preparing a bio-based epoxy resin anticorrosive coating of COFs-AA and galangin-based epoxy resin, the dispersibility and compatibility problems of bio-based coatings were solved, the anticorrosive and aging resistance of the coatings were improved, and an environmentally friendly and efficient protective effect was achieved.
Patent Information
- Application Number
- CN202411776209.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-05
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-12-05
AI Technical Summary
Existing bio-based coatings suffer from internal dispersion and compatibility issues in the field of corrosion protection, leading to internal defects, reduced barrier properties, and micropore formation due to interfacial incompatibility, which affects protective performance.
COFs materials were prepared by Schiff base reaction and anti-corrosion fillers were prepared by condensation reaction with AA. Epoxy resin was prepared by combining galangin and then mixed to prepare a bio-based epoxy resin anti-corrosion coating. The synergistic anti-corrosion properties of COFs-AA and epoxy resin were utilized to enhance the compatibility and barrier properties of the coating.
It improves the environmental friendliness and safety of the coating, enhances its hydrophobicity and corrosion resistance, improves its aging resistance and substrate adhesion, and provides better protection.
Abstract
Description
Technical Field
[0001] This invention relates to the field of anti-corrosion coating preparation technology, and more particularly to a method for preparing a bio-based epoxy resin anti-corrosion coating. Background Technology
[0002] Anti-corrosion coatings are widely used in modern industry, transportation, and marine engineering. The market is primarily dominated by organic coatings, making organic solvents a major component of coating formulations. In recent years, increasingly stringent policies and regulations have begun to control VOC emissions, promoting the development of high-solids coatings, UV-cured coatings, and water-based coatings. With growing emphasis on sustainable development, the development of bio-based raw materials for coatings, partially or completely replacing petrochemical-derived raw materials, is becoming a hot research topic in the anti-corrosion coatings industry.
[0003] Therefore, the preparation of bio-based coating components and their functionalization modification methods are crucial to the development of bio-based coatings. Bio-based coatings also face challenges related to dispersion and compatibility between multiple phases within the system. For example, filler agglomeration and precipitation lead to significant internal defects in the coating, reduced barrier properties, and ultimately, decreased protective performance. Incompatibility between the filler and the resin matrix results in phase separation within the coating, creating noticeable micropores, which also ultimately reduces its protective performance. Therefore, developing high-performance bio-based protective coatings is a significant need in the field of corrosion protection. Summary of the Invention
[0004] The purpose of this invention is to provide a method for preparing a bio-based epoxy resin anti-corrosion coating. This bio-based epoxy resin anti-corrosion coating mainly consists of the anti-corrosion filler COFs-AA, bio-based epoxy resin, and a curing agent. This bio-based epoxy resin anti-corrosion coating is composed of biomass-based components and features green, environmentally friendly, non-toxic, excellent hydrophobicity, and good anti-corrosion performance. This bio-based epoxy resin anti-corrosion coating can be applied to the protection of corrosive environments for various metals, wood, and other materials.
[0005] The objective of this invention is achieved through the following technical solution: A method for preparing a bio-based epoxy resin anticorrosive coating includes the following steps: First, COFs materials are prepared according to the Schiff base reaction; then, the COFs are condensed with AA to prepare an anticorrosive filler with excellent barrier properties and good compatibility; second, an epoxy resin is prepared by epoxidation using galangin as a raw material, which has excellent antioxidant properties and can synergistically prevent corrosion with the anticorrosive filler during service; finally, the resin, filler, and curing agent are mixed in a certain proportion to prepare the bio-based epoxy resin anticorrosive coating. The specific scheme is as follows: Step 1. In a three-necked flask, monomers 1,3,5-trialdehyde phloroglucinol (0.2 mmol), 2,5-dihydroxyterephthalohydrazide (0.3 mmol), solvent (tris(methylbenzene) / tetrahydrofuran, 4 mL / 4 mL), and catalyst (acetic acid, 0.8 mL, 6 M) were mixed and heated at 120 °C for 72 h to prepare COFs. Subsequently, the precipitate in the reactor was collected, washed 3-6 times by centrifugation with acetone, and then dried under vacuum at 50 °C to constant weight to obtain COFs.
[0006] Step 2. Dissolve 8 g of arachidonic acid (AA) in 80 mL of dichloromethane solution, then add 2 g of COFs, stir well, and then add an appropriate amount of 10 mol / L H2SO4 solution dropwise. Stir at 70 ℃ (300 r / min) for 4 h. After the reaction is complete, remove excess solvent by rotary evaporation of the mixture. Wash the remaining mixture with deionized water by centrifugation until neutral. Finally, dry the solid under vacuum at 50 ℃ to constant weight to obtain the corrosion-resistant filler COFs-AA.
[0007] Step 3. Dissolve 20 g of galangin in 200 g of DMSO, then add 200 g of epichlorohydrin and 2 g of tetrabutylammonium bromide. After stirring thoroughly, transfer the mixture to a three-necked flask and reflux at 70 °C with stirring (260 r / min) for 3 h. Then, add 40 g of NaOH solution (50%) dropwise to the mixture and stir at 60 °C for 2 h to obtain a dark-colored reaction mixture. Rotary evaporate the mixture to remove unreacted epichlorohydrin, yielding galangin-based epoxy resin.
[0008] Step 4. Take 10 g of bio-based epoxy resin and dilute it with 2.5 g of deionized water. Then pour it into a ball mill jar and add an appropriate amount of anti-corrosion filler COFs-AA. Ball mill the mixture to fully disperse the filler. Then add 2.5 g of amino curing agent (AQ419) and stir with a magnetic stirrer at 1000 r / min until it is uniformly mixed to obtain the bio-based epoxy resin anti-corrosion coating.
[0009] Preferably, the mass ratio of AA to COFs is 4:1; Preferably, the mass of the 10 mol / L H2SO4 solution added as a catalyst is 3% to 7% of the mass of COFs.
[0010] Preferably, the mass ratio of galangin to epichlorohydrin is 1:10; Preferably, NaOH solution is added during the preparation of bio-based epoxy resin to make the pH of the mixture 8.
[0011] Preferably, the bio-based material galangin can be replaced or partially replaced with curcumin. Preferably, the amount of anti-corrosion filler added during the preparation of the bio-based epoxy resin anti-corrosion coating is 0.5% to 3.0% of the resin mass.
[0012] The beneficial effects of this invention are: 1. This patent uses galangin as a resin raw material, which is green, environmentally friendly, non-toxic and pollution-free. Galangin also has a certain antioxidant capacity. After epoxidation, it can work synergistically with two-dimensional COFs materials for corrosion protection as a bio-based resin. In addition, it has excellent aging resistance and good matrix adhesion.
[0013] 2. The anti-corrosion functional filler COFs-AA of this patent uses two-dimensional COFs as the main material. Through a condensation reaction, arachidonic acid (AA) with hydrophobic alkyl chains is successfully introduced into the bio-based coating, which reduces the hydrophilicity of COFs and retains the barrier ability unique to two-dimensional materials. At the same time, compared with inorganic fillers, this filler has better interfacial compatibility with the resin matrix, thereby maximizing the anti-corrosion ability of the coating.
[0014] 3. This patent constructs coating components based on bio-based materials, which greatly improves the environmental friendliness and safety of the coating. This will help promote the research process of bio-based coatings and provide new ideas for the development of bio-based coatings. Detailed Implementation
[0015] The present invention is further described below through specific embodiments, but the present invention is not limited to the following embodiments. Modifications, combinations, or substitutions made to the present invention within the scope of the present invention or without departing from the content, spirit, and scope of the present invention will be obvious to those skilled in the art and are included within the scope of the present invention. Example 1
[0016] A bio-based epoxy resin anticorrosive coating (named A1) comprises the following preparation steps: 10 g of bio-based epoxy resin is taken and diluted with 2.5 g of deionized water, then poured into a ball mill jar, and 0.1 g of anticorrosive filler COFs-AA is added. The mixture is ball-milled to fully disperse the filler, and then 2.5 g of amino curing agent (AQ419) is added. The mixture is stirred with a magnetic stirrer at 1000 r / min until homogeneous, thus obtaining the bio-based epoxy resin anticorrosive coating. Example 2
[0017] A bio-based epoxy resin anticorrosive coating (named A2) comprises the following preparation steps: 10 g of bio-based epoxy resin is taken and diluted with 2.5 g of deionized water, then poured into a ball mill jar, and 0.1 g of anticorrosive filler COFs is added. The mixture is ball-milled to fully disperse the filler, and then 2.5 g of amino curing agent (AQ419) is added. The mixture is stirred with a magnetic stirrer at 1000 r / min until homogeneous, thus obtaining the bio-based epoxy resin anticorrosive coating. Example 3
[0018] A bio-based epoxy resin anticorrosive coating (named A3) comprises the following preparation steps: 10 g of bio-based epoxy resin is taken and diluted with 2.5 g of deionized water, then poured into a ball mill jar, and 0.1 g of a mixed filler of COFs and AA (0.2 g of COFs and 0.8 g of AA) is added. The mixture is ball-milled to fully disperse the filler, and then 2.5 g of amino curing agent (AQ419) is added. The mixture is stirred with a magnetic stirrer at 1000 r / min until homogeneous, thus obtaining the bio-based epoxy resin anticorrosive coating. Example 4
[0019] A bio-based epoxy resin anticorrosive coating (A4) comprises the following preparation steps: 10 g of commercially available bio-based epoxy lignin resin is taken and diluted with 2.5 g of deionized water, then poured into a ball mill jar, and 0.1 g of anticorrosive filler COFs-AA is added. The mixture is ball-milled to fully disperse the filler, and then 2.5 g of amino curing agent (AQ419) is added. The mixture is stirred with a magnetic stirrer at 1000 r / min to make it uniform, thus obtaining the bio-based epoxy resin anticorrosive coating.
[0020] The bio-based epoxy resin anti-corrosion coatings prepared in the above embodiments were sprayed onto the surface of a Q235 low-carbon steel substrate. After the coating was cured for one week, its static contact angle, adhesion and resistance to neutral salt spray (5.0 wt.% NaCl solution) were tested. The test results are shown in Table 1.
[0021] As can be seen from the test results in Table 1, the patented product exhibits the largest static contact angle and relatively good hydrophobicity. No blistering was observed after 240 hours of neutral salt spray testing, and the adhesion reached grade 0, demonstrating excellent barrier and protective properties. For component A2, the static contact angle is only 70°, mainly because the functional filler consists only of COFs, which are hydrophilic. This results in poorer water resistance in the composite coating compared to component A1, leading to blistering after 240 hours of neutral salt spray testing. For component A3, the anti-corrosion filler is a mixture of COFs and AA. These two components are distributed in the composite coating through physical blending without chemical bonding. Due to uneven distribution and the hydrophilic effect of COFs, localized compositional inconsistencies occur, resulting in a relatively small static contact angle. Simultaneously, barrier properties and adhesion also decrease, leading to significant blistering after 240 hours of neutral salt spray testing. For component A4, the addition of the functional filler (COFs-AA) prepared in this patent to epoxidized lignin exhibits good protective properties and adhesion, indicating that the functional filler prepared in this patent is not only suitable for the epoxidized galangin matrix of this patent, but also suitable for other resin matrices to a certain extent.
[0022] Table 1. Test results of corrosion resistance of epoxy composite coating Component Name static contact angle Resistance to neutral salt spray Adhesion A1 93° 240 h No foaming Level 0 A2 70° Foaming occurred after 240 hours. Level 0 A3 64° Obvious bubbling occurred after 240 hours. Level 1 A4 89° 240 h No foaming Level 0 Test methods Droplet method GB / T 9286-1988 GB / Y 9286-2021 .
Claims
1. A method for preparing a bio-based epoxy resin anti-corrosion coating, characterized in that, The bio-based epoxy resin anticorrosive coating is composed of anticorrosive functional fillers, bio-based epoxy resin, and a curing agent. The anticorrosive functional fillers are prepared by condensation of a two-dimensional covalent organic framework (COFs) and the bio-based material arachidonic acid. The bio-based epoxy resin is prepared by epoxidation using galangin, a bio-based material. The curing agent is a general-purpose curing agent. The bio-based anticorrosive coating includes the following preparation process: Step 1. Preparation of COFs: According to the Schiff base reaction, solvent, monomer 1,3,5-trialdehyde phloroglucinol, monomer 2,5-dihydroxyterephthalohydrazide and catalyst were added sequentially to a three-necked flask. After heating at 120℃ for 72 h, the precipitate in the reaction vessel was collected and washed with acetone by centrifugation 3-6 times. Then, it was dried under vacuum at 50℃ to constant weight to obtain COFs. Step 2. Preparation of corrosion-resistant filler COFs-AA: Arachidonic acid was dissolved in a three-necked flask using dichloromethane solution as solvent, then COFs were added, and the mixture was stirred evenly. The catalyst was then added dropwise, and the mixture was stirred at 70°C and 300 r / min for 4 h. After the reaction was completed, the mixture was rotary evaporated to remove excess solvent. The remaining mixture was washed with deionized water by centrifugation until neutral. Finally, the solid was vacuum dried at 50°C to constant weight to obtain corrosion-resistant filler COFs-AA. Step 3. Preparation of bio-based epoxy resin: Galangin was dissolved in a three-necked flask using dimethyl sulfoxide as solvent, and then epichlorohydrin and tetrabutylammonium bromide were added sequentially. The mixture was refluxed at 70°C and stirred at 260 r / min for 3 h. Then, NaOH solution was added dropwise to the mixture, and the mixture was stirred at 60°C for 2 h to obtain a dark-colored reaction mixture. The mixture was then rotary evaporated to remove unreacted epichlorohydrin, yielding galangin-based epoxy resin. Step 4. Take bio-based epoxy resin and dilute it with deionized water. Then pour it into a ball mill jar, add the anti-corrosion filler COFs-AA, and ball mill the mixture for 20 minutes to fully disperse the filler. Then add the amino curing agent and stir with a magnetic stirrer to mix it evenly to obtain the bio-based epoxy resin anti-corrosion coating.
2. The method for preparing a bio-based epoxy resin anti-corrosion coating according to claim 1, characterized in that, The molar ratio of the monomer 1,3,5-trialdehyde phloroglucinol to 2,5-dihydroxyterephthalohydrazide is 2:
3.
3. The method for preparing a bio-based epoxy resin anti-corrosion coating according to claim 1, characterized in that, The solvent is a mixed solution of mesitylene and tetrahydrofuran, wherein the volume ratio of mesitylene to tetrahydrofuran is 1:
1.
4. The method for preparing a bio-based epoxy resin anti-corrosion coating according to claim 1, characterized in that, The mass ratio of arachidonic acid to COFs is 4:
1.
5. The method for preparing a bio-based epoxy resin anti-corrosion coating according to claim 1, characterized in that, In Step 2, the catalyst is H2SO4 with a concentration of 10 mol / L, and the added mass is 3% to 7% of the mass of COFs.
6. The method for preparing a bio-based epoxy resin anti-corrosion coating according to claim 1, characterized in that, The mass ratio of galangin to epichlorohydrin is 1:
10.
7. The method for preparing a bio-based epoxy resin anti-corrosion coating according to claim 1, characterized in that, After adding NaOH solution, the pH value of the mixture is adjusted to 8.
Citation Information
Patent Citations
Self-healing coating based on covalent organic framework material and preparation method thereof
CN114539870A
Graphene oxide modified bio-based epoxy anticorrosive paint as well as preparation method and application thereof
CN117844336A