Plasma cladding FeAl intermetallic compound coating and preparation method thereof

Through plasma cladding technology and the addition of VC, NbC nanoparticles and Cr elements, the problem of poor plasticity and hydrogen embrittlement of FeAl intermetallic compound coating at room temperature is solved, and the coating performance with high hardness and hydrogen embrittlement resistance is achieved.

CN119615043APending Publication Date: 2025-03-14CHINA-UKRAINE INST OF WELDING GUANGDONG ACAD OF SCI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411544384.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2025-03-14

AI Technical Summary

Technical Problem

The FeAl intermetallic compound coating has poor plasticity and wear resistance at room temperature, resulting in cracking of the coating, reducing its protective effect on the matrix metal, and the hydrogen embrittlement problem has not been effectively solved.

Method used

FeAl intermetallic compound coating was prepared by plasma cladding technology, VC and NbC nanoparticles were added, and Cr elements were added to form a high hardness, hydrogen embrittlement-resistant coating.

Benefits of technology

The room temperature plasticity and hydrogen embrittlement resistance of FeAl intermetallic compound coating are significantly improved, and its resistance to high-temperature oxidation and corrosion are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005113438650000111
    Figure BDA0005113438650000111
  • Figure BDA0005113438650000121
    Figure BDA0005113438650000121
Patent Text Reader

Abstract

The invention discloses a plasma cladding FeAl intermetallic compound coating and a preparation method thereof. According to the composite metal powder of the FeAl intermetallic compound coating, iron powder, aluminum powder, ferrochrome powder, VC particles and NbC particles are subjected to ball milling and powder mixing under the protection of inert atmosphere, and the composite metal powder of the FeAl intermetallic compound coating is obtained. The FeAl intermetallic compound material provided by the invention is prepared through plasma cladding, so that the room-temperature plasticity of a FeAl intermetallic compound coating is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to the technical field of welding materials, and in particular to a plasma cladding FeAl intermetallic compound coating and a preparation method thereof. Background technology:

[0002] With the needs of national economic development, especially the adjustment of energy structure and the improvement of environmental protection requirements, gas turbines, as a clean, efficient and flexible power generation equipment, have gradually become the first choice of major power companies, regional energy suppliers and industrial users, and are an important part of my country's power system. Gas turbine blades are important components of gas turbines. They are mainly used to push the blades to generate power by mixing fuel and air. However, this key component has been in service for a long time in complex working environments such as high temperature, high pressure and strong corrosion, and needs to have good high-temperature mechanical properties and anti-oxidation corrosion ability. The performance of traditional metal materials and ceramic materials is not enough to meet the working requirements of gas turbine blades, so it is necessary to seek new high-performance materials to make up for their shortcomings.

[0003] FeAl intermetallic coatings are widely used due to their excellent oxidation resistance and corrosion resistance at high temperatures, as well as their relatively low material density (5.76–6.32 g / cm 3 ) and good mechanical properties, it has become one of the important materials for the surface protection of gas turbine blades. However, the plasticity and wear resistance of FeAl intermetallic compounds are poor at room temperature, which may cause the FeAl alloy coating to crack and reduce its protective effect on the base metal, which has become the main obstacle to the promotion and application of FeAl intermetallic compounds. Studies have shown that the contact of FeAl intermetallic compounds with moisture in the air induces hydrogen embrittlement, which is one of the main reasons for its low room temperature plasticity. Hydrogen in the air easily penetrates and gathers near the crystal defects of the FeAl metal matrix. Under the action of external forces, hydrogen atoms will move with the crystal defects to the stress concentration area and enrich, which promotes plastic deformation in this area, making it easy to generate cracks and expand, resulting in brittle fracture. Generally, the formation of hydrogen embrittlement at the grain boundary or the diffusion of hydrogen can be suppressed by reducing the grain size or adding suitable alloying elements.

[0004] Patent CN113444961A discloses a method for carbon nanotube fiber reinforcement of FeAl intermetallic compounds. A large number of uniformly dispersed carbon nanotube fiber particles are introduced into FeAl alloy through ultrasonic vibration and high-energy ball milling. Under the action of external force, on the one hand, the carbon nanotubes can play a bearing role, and on the other hand, the FeAl alloy matrix can bond the carbon nanotubes and transfer the load. This greatly improves the oxidation resistance of FeAl intermetallic compounds at a high temperature of 600°C, greatly reduces oxidation weight gain, and increases room temperature hardness. However, the problem of poor room temperature plasticity of FeAl intermetallic compounds has not been significantly improved.

[0005] Patent CN111230118A discloses a method for preparing a FeAl intermetallic compound, the main components of which are as follows: Fe72.75-74.25wt.%, Al24.25-24.75wt.%, Si1-3wt.%. The addition of Si can inhibit the violent exothermic reaction between Fe and liquid Al during high temperature and induce a self-propagating reaction. The product prepared has excellent high-temperature mechanical properties, good corrosion resistance and high-temperature oxidation resistance, and has no deformation, cracking, uneven organizational composition, etc.

[0006] The article "Effect of C, Ti, Zr and B alloying on fracture mechanisms in hot-rolled Fe–40 (at.%) Al" points out that the plasticity of FeAl alloy can be improved by adding elements such as C, Ti, Zr, and B. Among them, the addition of Zr and B elements has the most obvious effect on the improvement of high-temperature plasticity of FeAl alloy. At up to 600°C, its fracture mechanism is mainly transgranular cleavage fracture, showing excellent plasticity. However, the addition of these elements has no obvious effect on the room temperature plasticity of FeAl alloy, and FeAl alloy still exhibits brittle fracture at room temperature.

[0007] As a high-temperature structural material and stainless steel substitute, FeAl intermetallic compounds have broad application prospects. Although they have been studied in many aspects at home and abroad, the room temperature brittleness problem induced by hydrogen embrittlement has not been solved. Therefore, it is necessary to design and optimize the composition of FeAl intermetallic compounds and strive to develop new FeAl alloys with good room temperature plasticity. Summary of the invention:

[0008] The present invention solves the problems existing in the prior art, provides a FeAl intermetallic compound coating and a preparation method thereof, and greatly improves the room temperature plasticity of the FeAl intermetallic compound coating. The FeAl intermetallic compound material proposed in the present invention is prepared by plasma cladding, which has the characteristics of high efficiency, low cost, excellent coating quality, etc.

[0009] The first object of the present invention is to provide a composite metal powder with a FeAl intermetallic compound coating, wherein iron powder, aluminum powder, ferrochrome powder, VC particles and NbC particles are ball-milled and mixed under the protection of an inert atmosphere to obtain the composite metal powder with a FeAl intermetallic compound coating.

[0010] Preferably, in terms of mass percentage, the iron powder contains Fe≥99%, the aluminum powder contains Al≥99%, and the ferrochrome powder contains Cr≥68%.

[0011] The Fe and Al proposed in the present invention are the basic constituent elements of the FeAl intermetallic compound matrix, and elements such as Si and Mn are impurity elements. Within the Al content range, a FeAl phase matrix with a B2 structure will be formed. The VC and NbC particles added to the FeAl intermetallic compound coating have the characteristics of high hardness, good chemical stability, high melting point, good high temperature performance, etc., which can greatly improve the hardness of the FeAl intermetallic compound coating.

[0012] Preferably, the composite metal powder comprises, by mass percentage, 23%-30% Al, 3%-8% Cr, <0.1% Si, <0.1% Mn, 0.5%-1% VC, 0.5%-1% NbC, and the balance is Fe.

[0013] Preferably, the average particle size of iron powder, aluminum powder and ferrochrome powder is 60-100 mesh, and the average particle size of VC particles and NbC particles is 100 nm.

[0014] Preferably, the specific conditions of ball milling are: ball-to-material ratio 4-6:1, ball milling forward rotation 0.5-1.5h, reverse rotation 0.5-1.5h, and rotation speed 280-320r / min.

[0015] Further preferably, the specific conditions of the ball milling are: ball-to-material ratio 5:1, ball milling forward rotation for 1 hour, reverse rotation for 1 hour, and rotation speed of 300 r / min.

[0016] The second object of the present invention is to provide a method for preparing a FeAl intermetallic compound coating by plasma cladding, wherein the composite metal powder of the FeAl intermetallic compound coating is deposited on the surface of a metal substrate by plasma cladding to form a FeAl intermetallic compound coating.

[0017] VC and NbC particles have high temperature stability. During the cooling process of plasma cladding, nano-sized VC and NbC particles tend to be enriched at the grain boundaries, pinning the grain boundaries to move, inhibiting grain growth, thereby refining the grains and increasing the grain boundary density. This can reduce the effective diffusion coefficient of hydrogen in the air in the FeAl intermetallic compound coating to a certain extent, inhibit hydrogen embrittlement, and improve room temperature plasticity. Both VC and NbC have a body-centered cubic (BCC) crystal structure. Their nanoparticles have a semi-coherent interface relationship with the FeAl alloy with a B2 structure. There is a high density of misfit dislocations at the coherent interface, and the hydrogen absorption energy near the core of the misfit dislocation is low, which makes it easier to absorb and capture the hydrogen diffused there, prompting the uniformly dispersed VC and NbC nanoparticles to become deep hydrogen traps, thereby reducing the hydrogen diffusion coefficient, greatly improving the FeAl alloy's resistance to hydrogen embrittlement, and further improving room temperature plasticity. The Cr element added to the FeAl intermetallic compound coating can be dissolved into the FeAl matrix with B2 structure, thereby improving the strength and hardness of the alloy. In addition, after the Cr element comes into contact with air, it is easy to form a dense Cr2O3 oxide film on the surface of the coating, which can inhibit or delay the contact between the metal in the coating and hydrogen, thereby reducing the possibility of hydrogen embrittlement.

[0018] Preferably, the process parameters of the plasma cladding are: current 130-150A, voltage 30-40V, welding speed 28-32mm / min, powder feeding amount 2-5L / min, plasma gas flow rate 2.5L / min, and shielding gas flow rate 20L / min.

[0019] The preparation method of the FeAl intermetallic compound coating provided by the present invention is simple to operate, easy to implement, and low in cost. The prepared FeAl intermetallic compound coating has the advantages of low density, high strength, good room temperature plasticity, high temperature oxidation resistance, good corrosion resistance, and the like.

[0020] The present invention also protects the FeAl intermetallic compound coating obtained by the preparation method. The present invention optimizes the addition of Cr elements and VC and NbC nanoparticles to obtain a solidification structure with significantly refined grains, which has excellent high-temperature performance and excellent hydrogen embrittlement resistance, thereby improving the room temperature plasticity of the FeAl intermetallic compound coating.

[0021] The present invention also protects the FeAl intermetallic compound coating for surface protection of high-temperature structural parts, including gas turbine blades, waste incinerators, and the like.

[0022] Compared with the prior art, the present invention has the following advantages:

[0023] 1. The present invention optimizes the addition of Cr elements and VC and NbC nanoparticles to obtain a solidification structure with significantly refined grains. While having excellent high-temperature performance, it also has excellent hydrogen embrittlement resistance and improves the room temperature plasticity of the FeAl intermetallic compound coating.

[0024] 2. The Cr, VC and NbC added in combination in the present invention can improve the strength and hardness of the FeAl intermetallic compound.

[0025] 3. The addition of Cr is conducive to the formation of dense Cr2O3 oxide film, and its combined effect with Al2O3 film will further improve high-temperature oxidation resistance and corrosion resistance;

[0026] 4. The preparation method of the FeAl intermetallic compound coating provided by the present invention is simple to operate, easy to implement, and low in cost. The prepared FeAl intermetallic compound coating has the advantages of low density, high strength, good room temperature plasticity, resistance to high temperature oxidation and good corrosion resistance. Specific implementation method:

[0027] The following examples are provided to further illustrate the present invention, rather than to limit the present invention.

[0028] Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the experimental materials and reagents herein are conventional commercial products in the art.

[0029] Example 1

[0030] A composite metal powder suitable for preparing a FeAl intermetallic compound coating by plasma cladding, wherein the composite metal powder has the following composition weight ratios: Al 23%, Cr 3%, Si <0.1%, Mn <0.1%, VC 0.5%, NbC 0.5%, and the balance is Fe.

[0031] The specific preparation steps of plasma cladding FeAl intermetallic compound coating are as follows:

[0032] S1. According to the above proportions, iron powder, aluminum powder, ferrochrome powder and VC and NbC particles with an average particle size of 100 nm are ball-milled under the protection of an argon atmosphere to obtain FeAl intermetallic compound composite metal powder with uniformly dispersed VC and NbC particles; the ball-to-material ratio during the ball milling process is 5:1, the ball mill is rotated forward for 1 hour, reversed for 1 hour, and the rotation speed is 300r / min.

[0033] S2. Plasma cladding is used to prepare FeAl intermetallic compound coatings from uniformly mixed composite metal powders on the polished stainless steel surface. The process parameters are: current 130A, voltage 30V, welding speed 28mm / min, powder feeding 2L / min, plasma gas flow 2.5L / min, shielding gas flow 20L / min. High-purity argon is used as shielding gas and ionizing gas in the whole process of coating preparation.

[0034] Example 2

[0035] A composite metal powder suitable for preparing a FeAl intermetallic compound coating by plasma cladding, wherein the composite metal powder has the following composition ratio by mass: Al 25%, Cr 5%, Si<0.1%, Mn<0.1%, VC 0.75%, NbC 0.5%, and the balance is Fe.

[0036] The specific preparation steps of plasma cladding FeAl intermetallic compound coating are as follows:

[0037] S1. According to the above proportions, iron powder, aluminum powder, ferrochrome powder and VC and NbC particles with an average particle size of 100 nm are ball-milled under the protection of an argon atmosphere to obtain FeAl intermetallic compound composite powders in which VC and NbC particles are uniformly dispersed; the ball-to-material ratio during the ball milling process is 5:1, the ball mill is rotated forward for 1 hour, reversed for 1 hour, and the rotation speed is 300 r / min.

[0038] S2. Plasma cladding technology is used to prepare FeAl intermetallic compound coatings from uniformly mixed metal powders on the polished stainless steel surface. The process parameters are: current 140A, voltage 35V, welding speed 30mm / min, powder feeding 3L / min, plasma gas flow 2.5L / min, shielding gas flow 20L / min. The entire coating preparation process is carried out under the protection of high-purity argon.

[0039] Example 3

[0040] A composite metal powder suitable for preparing a FeAl intermetallic compound coating by plasma cladding, wherein the composite metal powder has the following composition weight ratios: Al 27%, Cr 6%, Si <0.1%, Mn <0.1%, VC 1%, NbC 0.5%, and the balance is Fe.

[0041] The specific preparation steps of plasma cladding FeAl intermetallic compound coating are as follows:

[0042] S1. According to the above proportions, iron powder, aluminum powder, ferrochrome powder and VC and NbC particles with an average particle size of 100 nm are ball-milled under the protection of an argon atmosphere to obtain FeAl intermetallic compound composite powders in which VC and NbC particles are uniformly dispersed; the ball-to-material ratio during the ball milling process is 5:1, the ball mill is rotated forward for 1 hour, reversed for 1 hour, and the rotation speed is 300 r / min.

[0043] S2. Plasma cladding technology is used to prepare FeAl intermetallic compound coatings from uniformly mixed metal powders on the polished stainless steel surface. The process parameters are: current 150A, voltage 40V, welding speed 32mm / min, powder feeding 5L / min, plasma gas flow 2.5L / min, shielding gas flow 20L / min. The entire coating preparation process is carried out under the protection of high-purity argon.

[0044] Example 4

[0045] A composite metal powder suitable for preparing a FeAl intermetallic compound coating by plasma cladding, wherein the composite metal powder has the following composition mass ratios: Al 28%, Cr 7%, Si<0.1%, Mn<0.1%, VC 0.5%, NbC 0.75%, and the balance is Fe.

[0046] The specific preparation steps of plasma cladding FeAl intermetallic compound coating are as follows:

[0047] S1. According to the above proportions, iron powder, aluminum powder, ferrochrome powder and VC and NbC particles with an average particle size of 100 nm are ball-milled under the protection of an argon atmosphere to obtain FeAl intermetallic compound composite powders in which VC and NbC particles are uniformly dispersed; the ball-to-material ratio during the ball milling process is 5:1, the ball mill is rotated forward for 1 hour, reversed for 1 hour, and the rotation speed is 300 r / min.

[0048] S2. Plasma cladding technology is used to prepare FeAl intermetallic compound coatings from uniformly mixed metal powders on the polished stainless steel surface. The process parameters are: current 140A, voltage 35V, welding speed 30mm / min, powder feeding 3L / min, plasma gas flow 2.5L / min, shielding gas flow 20L / min. The entire coating preparation process is carried out under the protection of high-purity argon.

[0049] Example 5

[0050] A composite metal powder suitable for preparing a FeAl intermetallic compound coating by plasma cladding. The composite metal powder has the following composition weight ratios: Al 30%, Cr 8%, Si <0.1%, Mn <0.1%, VC 0.5%, NbC 1%, and the balance Fe.

[0051] The specific preparation steps of plasma cladding FeAl intermetallic compound coating are as follows:

[0052] S1. According to the above proportions, iron powder, aluminum powder, ferrochrome powder and VC and NbC particles with an average particle size of 100 nm are ball-milled under the protection of an argon atmosphere to obtain FeAl intermetallic compound composite powders in which VC and NbC particles are uniformly dispersed; the ball-to-material ratio during the ball milling process is 5:1, the ball mill is rotated forward for 1 hour, reversed for 1 hour, and the rotation speed is 300 r / min.

[0053] S2. Plasma cladding technology is used to prepare FeAl intermetallic compound coatings from uniformly mixed metal powders on the polished stainless steel surface. The process parameters are: current 150A, voltage 40V, welding speed 32mm / min, powder feeding 5L / min, plasma gas flow 2.5L / min, shielding gas flow 20L / min. The entire coating preparation process is carried out under the protection of high-purity argon.

[0054] Example 6

[0055] A composite metal powder suitable for preparing a FeAl intermetallic compound coating by plasma cladding, wherein the composite metal powder has the following composition weight ratios: Al 30%, Cr 8%, Si <0.1%, Mn <0.1%, VC 1%, NbC 1%, and the balance is Fe.

[0056] The specific preparation steps of plasma cladding FeAl intermetallic compound coating are as follows:

[0057] S1. According to the above proportions, iron powder, aluminum powder, ferrochrome powder and VC and NbC particles with an average particle size of 100 nm are ball-milled under the protection of an argon atmosphere to obtain FeAl intermetallic compound composite powders in which VC and NbC particles are uniformly dispersed; the ball-to-material ratio during the ball milling process is 5:1, the ball mill is rotated forward for 1 hour, reversed for 1 hour, and the rotation speed is 300 r / min.

[0058] S2. Plasma cladding technology is used to prepare FeAl intermetallic compound coatings from uniformly mixed metal powders on the polished stainless steel surface. The process parameters are: current 150A, voltage 40V, welding speed 32mm / min, powder feeding 5L / min, plasma gas flow 2.5L / min, shielding gas flow 20L / min. The entire coating preparation process is carried out under the protection of high-purity argon.

[0059] Comparative Example 1

[0060] Refer to Example 1, except that VC and NbC nanoparticles are not added to the composite metal powder. Other steps are the same as in Example 1.

[0061] Comparative Example 2

[0062] Refer to Example 1, except that no VC nanoparticles are added to the composite metal powder, and the mass fraction of NbC particles is 1%. Other steps are the same as in Example 1.

[0063] Comparative Example 3

[0064] Refer to Example 1, except that no NbC nanoparticles are added to the composite metal powder, and the mass fraction of VC particles is 1%. Other steps are the same as in Example 1.

[0065] Comparative Example 4

[0066] Refer to Example 1, except that VC and NbC nanoparticles are not added to the composite metal powder, the mass fraction of Cr is 8%, and the other steps are the same as in Example 1.

[0067] Comparative Example 5

[0068] Refer to Example 1, except that no ferrochrome powder and NbC nanoparticles are added to the composite metal powder, and the mass fraction of VC is 0.5%. Other steps are the same as in Example 1.

[0069] Comparative Example 6

[0070] Refer to Example 1, except that no ferrochrome powder and VC nanoparticles are added to the composite metal powder, and the mass fraction of NbC is 0.5%. Other steps are the same as in Example 1.

[0071] Example 7

[0072] The same as Example 2, except that: a composite metal powder suitable for preparing a FeAl intermetallic compound coating by plasma cladding, the composition mass ratio of the composite metal powder is: Al 23%, Cr 3%, Si<0.1%, Mn<0.1%, VC 0.5%, NbC 0.5%, and the balance is Fe.

[0073] Example 8

[0074] The same as Example 2, except that: a composite metal powder suitable for preparing a FeAl intermetallic compound coating by plasma cladding, the composition mass ratio of the composite metal powder is: Al 27%, Cr 6%, Si<0.1%, Mn<0.1%, VC 1%, NbC 0.5%, and the balance is Fe.

[0075] Example 9

[0076] The same as Example 2, except that: a composite metal powder suitable for preparing a FeAl intermetallic compound coating by plasma cladding, the composition mass ratio of the composite metal powder is: Al 28%, Cr 7%, Si<0.1%, Mn<0.1%, VC 0.5%, NbC 0.75%, and the balance is Fe.

[0077] Example 10

[0078] The same as Example 2, except that: a composite metal powder suitable for preparing a FeAl intermetallic compound coating by plasma cladding, the mass ratio of the composite metal powder is: Al 30%, Cr 8%, Si<0.1%, Mn<0.1%, VC 0.5%, NbC 1%, and the balance is Fe.

[0079] Embodiment 11

[0080] The same as Example 2, except that: a composite metal powder suitable for preparing a FeAl intermetallic compound coating by plasma cladding, the mass ratio of the composite metal powder is: Al 30%, Cr 8%, Si<0.1%, Mn<0.1%, VC1%, NbC 1%, and the balance is Fe.

[0081] The performance of the plasma cladding FeAl intermetallic compound coatings prepared in Examples 1-11 and Comparative Examples 1-6 were tested respectively. The hardness test was carried out using a Vickers hardness tester. The tensile performance test method referred to GB / T 228.1-2021 "Tensile test of metallic materials Part 1: Room temperature test method". The test results are shown in Table 1.

[0082] Table 1 Hardness and room temperature tensile properties test results of Examples 1-11 and Comparative Examples 1-6

[0083]

[0084]

[0085] It can be seen from Table 1 that as the VC and NbC contents increase, the room temperature strength and plasticity of the FeAl alloy increase accordingly. When the NbC content is increased to 1% and the VC content is 0.5% (ie, Example 5), the room temperature plasticity of the FeAl alloy reaches a maximum value; but as the VC content continues to increase to 1% (Example 6), although the room temperature strength is improved, due to the excessive precipitation phases gathered at the grain boundaries, the precipitation phases will agglomerate and coarsen, which is harmful to the room temperature plasticity.

[0086] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A composite metal powder with a FeAl intermetallic compound coating, characterized in that: Iron powder, aluminum powder, ferrochrome powder, VC particles and NbC particles are mixed by ball milling under the protection of an inert atmosphere to obtain composite metal powder with a FeAl intermetallic compound coating.

2. The composite metal powder according to claim 1, characterized in that In terms of mass percentage, the iron powder contains Fe≥99%, the aluminum powder contains Al≥99%, and the ferrochrome powder contains Cr≥68%.

3. The composite metal powder according to claim 1 or 2, characterized in that: The composite metal powder comprises, by mass percentage, 23%-30% Al, 3%-8% Cr, <0.1% Si, <0.1% Mn, 0.5%-1% VC, 0.5%-1% NbC, and the balance is Fe.

4. The composite metal powder according to claim 1, characterized in that: The average particle size of iron powder, aluminum powder and ferrochrome powder is 60-100 meshes, and the average particle size of VC particles and NbC particles is 100 nm.

5. The composite metal powder according to claim 1, characterized in that: The specific conditions of ball milling are: ball-to-material ratio 4-6:1, ball mill forward rotation 0.5-1.5h, reverse rotation 0.5-1.5h, speed 280-320r / min.

6. The composite metal powder according to claim 5, characterized in that: The specific conditions of ball milling are: ball-to-material ratio 5:1, ball mill forward rotation for 1 h, reverse rotation for 1 h, and rotation speed of 300 r / min.

7. A method for preparing a FeAl intermetallic compound coating by plasma cladding, characterized in that: The composite metal powder of the FeAl intermetallic compound coating according to any one of claims 1 to 6 is deposited on the surface of a metal substrate by plasma cladding to form a FeAl intermetallic compound coating.

8. The preparation method according to claim 7, characterized in that: The process parameters of the plasma cladding are: current 130-150A, voltage 30-40V, welding speed 28-32mm / min, powder feeding amount 2-5L / min, plasma gas flow rate 2.5L / min, and shielding gas flow rate 20L / min.

9. The FeAl intermetallic compound coating obtained by the preparation method according to claim 7.

10. The FeAl intermetallic compound coating according to claim 9 is used for surface protection of high temperature structural parts.

Citation Information

Patent Citations

  • Lightweight anti-oxidation carbon nanotube reinforced iron-aluminum alloy and preparation method thereof

    CN113444961A