A modified ferrite pre-sintered material and its preparation method, and permanent magnet ferrite and its preparation method.

By growing a nano-silica shell in situ on the surface of the ferrite pre-sintered material for permanent magnets, the problems of uneven grain morphology and insufficient grain boundary strength were solved, improving magnetic properties and production efficiency, and achieving higher magnet performance and production efficiency.

CN119638447BActive Publication Date: 2026-11-17HENGDIAN GRP DMEGC MAGNETICS CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411702406.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-11-26
Publication Date
2026-11-17
Estimated Expiration
2044-11-26

AI Technical Summary

Technical Problem

In existing permanent magnet ferrite preparation processes, uneven grain morphology and insufficient grain boundary strength lead to reduced magnetic properties. Dry processes suffer from disordered grain growth and excessive internal stress, affecting magnet performance and production efficiency.

Method used

By growing a nano-silica shell in situ on the surface of a ferrite pre-sintered substrate, and by mixing a silicon source with a catalyst and ball milling, a nano-silica modification layer is formed to improve the grain morphology and strength. Furthermore, by optimizing the flux and lubricant, the grain growth and sintering process is controlled to improve the magnetic properties.

Benefits of technology

It improves the magnetic properties of permanent magnet ferrite, reduces the porosity and internal stress between grains, enhances grain boundary strength, and improves production efficiency and product competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005153669190000151
    Figure BDA0005153669190000151
Patent Text Reader

Abstract

This invention relates to a modified ferrite pre-sintered material and its preparation method, as well as permanent magnet ferrite and its preparation method, belonging to the field of magnetic materials technology. The preparation method of the modified ferrite pre-sintered material of this invention includes the following steps: Step 1, mixing a ferrite pre-sintered material substrate, a silicon source, and a solvent to obtain a mixture; the mass ratio of the ferrite pre-sintered material substrate to the silicon source is (500-3000):(10-100); Step 2, mixing the mixture with a catalyst and ball milling; the catalyst includes an aqueous solution of acid or an aqueous solution of alkali; Step 3, solid-liquid separation to obtain the modified ferrite pre-sintered material. This invention improves the magnetic properties of permanent magnet ferrite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of magnetic materials technology, specifically relating to a modified ferrite pre-sintered material and its preparation method, and a permanent magnet ferrite and its preparation method. Background Technology

[0002] Ferrites are abundant in raw materials and possess excellent chemical stability, leading to their rapid development since their application as magnetic materials. Permanent magnet ferrites, in particular, exhibit high permeability and stable magnetic properties, making them widely used in automotive, home appliance, and aerospace industries. Currently, domestic and international processes for preparing permanent magnet ferrites include dry and wet methods. Magnets prepared using the dry method are widely used in complex-shaped magnetic devices such as multipole magnetic rings and magnetic tiles due to their low raw material cost, simple equipment, and stable performance. Magnets prepared using the wet method can achieve higher magnetic properties, mainly due to the ease of magnetic domain movement leading to better orientation. However, the wet method requires the removal of a dispersion medium during forming, resulting in longer processing time, lower productivity, and higher operating costs. Therefore, the dry process has a wider range of applications.

[0003] Permanent magnet ferrites possess advantages such as abundant raw materials, low cost, simple preparation process, excellent oxidation resistance, and high remanent magnetization. After decades of development and improvement, ferrite materials have become a widely used and diverse class of functional materials, and are the preferred material in many fields. How to further improve the magnetic properties of permanent magnet ferrites is currently a key research focus. Summary of the Invention

[0004] Therefore, the present invention provides a modified ferrite pre-sintered material and its preparation method, and a permanent magnet ferrite and its preparation method, which further improves the magnetic properties of the permanent magnet ferrite.

[0005] To this end, the present invention provides the following technical solution.

[0006] In a first aspect, the present invention provides a method for preparing modified ferrite pre-sintered material, comprising the following steps:

[0007] Step 1: Mix the ferrite pre-sintered material substrate, silicon source, and solvent to obtain a mixture;

[0008] The mass ratio of the ferrite pre-sintered material to the silicon source is (500-3000):(10-100); for example, it can be 500:10, 500:40, 500:70, 500:100, 1000:10, 1000:40, 1000:70, 1000:100, 2000:10, 2000:40, 2000:70, 2000:100, 3000:10, 3000:40, 3000:70 or 3000:100, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably (1500-2500):(25-90).

[0009] Step 2: Mix the mixture with the catalyst and ball mill it;

[0010] The catalyst includes an aqueous solution of an acid or an aqueous solution of a base;

[0011] Step 3: Solid-liquid separation to obtain modified ferrite pre-calcined material.

[0012] Furthermore, step 1 satisfies at least one of the following conditions:

[0013] (1) The mass ratio of the silicon source to the solvent is (10-100):(3000-6000); for example, it can be 10:3000, 10:4000, 10:5000, 10:6000, 40:3000, 40:4000, 40:5000, 40:6000, 70:3000, 70:4000, 70:5000, 70:6000, 100:3000, 100:4000, 100:5000 or 100:6000, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably (25-90):(4000-5000);

[0014] (2) After mixing the ferrite pre-sintered material substrate, silicon source and solvent, ultrasonic dispersion is performed to obtain a mixture;

[0015] (3) The silicon source includes one or more of methyl orthosilicate, tetraethyl orthosilicate and sodium silicate; preferably tetraethyl orthosilicate;

[0016] (4) The solvent includes water and / or organic solvents;

[0017] Optionally, the organic solvent includes one or more of anhydrous ethanol, acetone, and toluene, preferably anhydrous ethanol.

[0018] Furthermore, step 2 satisfies at least one of the following conditions:

[0019] (1) The mass ratio of the silicon source to the catalyst is (10-100):(1-10), for example, it can be 10:1, 10:4, 10:7, 10:10, 40:1, 40:4, 40:7, 40:10, 70:1, 70:4, 70:7, 70:10, 100:1, 100:4 or 100:7, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable. Preferably, it is (25-90):(4-8).

[0020] (2) Aqueous solutions of acids include one or more of hydrochloric acid and selenic acid;

[0021] For example, it could be 1 mol / L hydrochloric acid;

[0022] (3) The aqueous solution of the alkali includes ammonia;

[0023] For example, it could be ammonia solution with a concentration of 12 mol / L;

[0024] (4) The rotational speed of the ball mill is 200 to 600 r / min, for example, it can be 200 r / min, 250 r / min, 300 r / min, 350 r / min, 400 r / min, 450 r / min, 500 r / min, 550 r / min or 600 r / min, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable. Preferably, it is 250 to 450 r / min.

[0025] (5) The ball milling time is 6 to 10 hours, for example, it can be 6 hours, 7 hours, 8 hours, 9 hours, or 10 hours, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable, with 7 to 8 hours being preferred.

[0026] Furthermore, step 3 includes drying the liquid product after solid-liquid separation;

[0027] Optionally, the drying method is air drying;

[0028] Optionally, step 3 further includes crushing and sieving the dried product; optionally, a sieve with a mesh size of 10 to 100 is used for sieving, such as 10, 20, 30, 40, 50, 60, 70, 80, 90 or 100 mesh, but not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably a sieve with a mesh size of 20 to 50.

[0029] Secondly, the present invention provides a modified ferrite pre-sintered material, which is prepared according to the above preparation method.

[0030] Thirdly, the present invention provides a method for preparing permanent magnet ferrite, which is prepared using the above-mentioned modified ferrite pre-sintered material.

[0031] Furthermore, the method for preparing the permanent magnet ferrite includes the following steps:

[0032] Step A: Blend the modified ferrite pre-calcined material, flux, and lubricant to obtain a blend;

[0033] Step B: Dry press the blend and sinter it.

[0034] Furthermore, step A satisfies at least one of the following conditions:

[0035] (1) The mass ratio of modified ferrite pre-sintered material to flux is (500-3000):(10-18), for example, it can be 500:10, 500:14, 500:18, 1000:10, 1000:14, 1000:18, 2000:10, 2000:14, 2000:18, 3000:10, 3000:14 and 3000:18, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably (1500-2500):(12-16);

[0036] (2) The mass ratio of the lubricant to the modified ferrite pre-calcined material is (1-25):(500-3000). For example, it can be 1:500, 1:1000, 1:1500, 1:2000, 1:2500, 1:3000, 7:500, 7:1000, 7:1500, 7:2000, 7:2500, 7:3000, 13:500, 13:1000, 13:1500, 13:2000, 13: 2500, 13:3000, 19:500, 19:1000, 19:1500, 19:2000, 19:2500, 19:3000, 25:500, 25:1000, 25:1500, 25:2000, 25:2500 or 25:3000, but not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably (8-16):(1500-2500);

[0037] (3) The fluxing agent includes one or more of La2O3, Al2O3 and CaCO3;

[0038] (4) The lubricant includes one or more of zinc stearate, magnesium stearate and calcium stearate, preferably zinc stearate.

[0039] Furthermore, step B satisfies at least one of the following conditions:

[0040] (1) The dry pressing is carried out in a magnetic field. Optionally, the magnetic field strength is 1000 to 1400 Oe, for example, it can be 1000 Oe, 1050 Oe, 1100 Oe, 1150 Oe, 1200 Oe, 1250 Oe, 1300 Oe, 1350 Oe or 1400 Oe, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0041] (2) The pressure of the dry pressing is 40 to 80 MPa, for example, it can be 40 MPa, 45 MPa, 50 MPa, 55 MPa, 60 MPa, 65 MPa, 70 MPa, 75 MPa or 80 MPa, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0042] (3) The sintering includes sequentially performing a first heating, a first holding, a second heating, a second holding, a third heating, a third holding, a fourth heating, and a fourth holding;

[0043] Optionally, the first heating rate is 2 to 10 °C / min, for example, it can be 2 °C / min, 3 °C / min, 4 °C / min, 5 °C / min, 6 °C / min, 7 °C / min, 8 °C / min, 9 °C / min or 10 °C / min, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably 5 to 8 °C / min.

[0044] Optionally, the endpoint temperature of the first heating is 300 to 500°C, for example, it can be 300°C, 320°C, 340°C, 360°C, 380°C, 400°C, 420°C, 440°C, 460°C, 480°C or 500°C, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0045] Optionally, the first heat preservation time is 1 to 6 hours, for example, it can be 1 hour, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably 2 to 3 hours.

[0046] Optionally, the second heating rate is 3 to 9 °C / min, for example, it can be 3 °C / min, 3.5 °C / min, 4 °C / min, 4.5 °C / min, 5 °C / min, 5.5 °C / min, 6 °C / min, 6.5 °C / min, 7 °C / min, 7.5 °C / min, 8 °C / min, 8.5 °C / min or 9 °C / min, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably 4 to 6 °C / min;

[0047] Optionally, the endpoint temperature of the second heating is 600 to 800°C, for example, it can be 600°C, 620°C, 640°C, 660°C, 680°C, 700°C, 720°C, 740°C, 760°C, 780°C or 800°C, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0048] Optionally, the second heat preservation time is 1 to 8 hours, for example, it can be 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours or 8 hours, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably 2 to 6 hours.

[0049] Optionally, the third heating rate is 2 to 7 °C / min, for example, it can be 2 °C / min, 2.5 °C / min, 3 °C / min, 3.5 °C / min, 4 °C / min, 4.5 °C / min, 5 °C / min, 5.5 °C / min, 6 °C / min, 6.5 °C / min or 7 °C / min, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably 3 to 6 °C / min;

[0050] Optionally, the endpoint temperature of the third heating is 900 to 1100°C, for example, it can be 900°C, 920°C, 940°C, 960°C, 980°C, 1000°C, 1020°C, 1040°C, 1060°C, 1080°C or 1100°C, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0051] Optionally, the third heat preservation time is 1 to 5 hours, for example, it can be 1 hour, 2 hours, 3 hours, 1 hour, 4 hours or 5 hours, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably 2 to 4 hours.

[0052] Optionally, the fourth heating rate is 1 to 5 °C / min, for example, it can be 1 °C / min, 2 °C / min, 3 °C / min, 4 °C / min or 5 °C / min, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably 2 to 4 °C / min.

[0053] Optionally, the final temperature of the fourth heating step is 1200-1300℃, for example, it can be 1200℃, 1210℃, 1220℃, 1230℃, 1240℃, 1250℃, 1260℃, 1270℃, 1280℃, 1290℃ or 1300℃, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0054] Optionally, the fourth heat preservation time is 1 to 12 hours, for example, it can be 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours or 12 hours, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably 3 to 10 hours.

[0055] Furthermore, the permanent magnet ferrite blanks cooled in the furnace are ground and cleaned.

[0056] Fourthly, the present invention provides a permanent magnet ferrite, which is prepared according to the above preparation method.

[0057] Optionally, the step of mixing the ferrite pre-sintered substrate, silicon source, and solvent in step 1 includes stirring.

[0058] Optionally, the step of blending the modified ferrite pre-sintered material, flux, and lubricant in step A includes stirring.

[0059] After sintering, the furnace is cooled.

[0060] The technical solution of this invention has the following advantages:

[0061] 1. The preparation method of the modified ferrite pre-sintered material of the present invention includes the following steps: Step 1, mixing the ferrite pre-sintered material substrate, silicon source and solvent to obtain a mixture; the mass ratio of the ferrite pre-sintered material substrate to the silicon source is (500-3000):(10-100); Step 2, mixing the mixture with a catalyst and ball milling; the catalyst includes an aqueous solution of acid or an aqueous solution of alkali; Step 3, solid-liquid separation to obtain the modified ferrite pre-sintered material.

[0062] A silicon source, catalyzed by a catalyst, hydrolyzes and condenses to form a nano-silica surface layer on the surface of a ferrite pre-sintered substrate. This invention utilizes a simple in-situ growth method to generate nano-silica on the surface of the ferrite pre-sintered substrate. Nano-silica modifies individual ferrite pre-sintered substrate grains, improving grain uniformity and increasing specific surface area. During dry pressing and sintering, it increases grain boundary strength, reduces inter-grain porosity, and prevents cracking caused by excessive stress in the sintering region, thereby improving the magnetic properties of the permanent magnet ferrite.

[0063] The mass ratio of ferrite pre-sintered material to silicon source is (500–3000):(10–100). Within this range, insufficient modification of the grains by nano-silica can be avoided, while excessive nano-silica can also have an adverse effect on performance.

[0064] 2. The mass ratio of modified ferrite pre-sintered material to flux is (500~3000):(10~18).

[0065] In the dry pressing process for preparing permanent magnet ferrites, to ensure high magnetic properties, it is necessary to address issues such as poor grain uniformity and the reduction in magnetic properties caused by disordered grain growth during sintering. Currently, in actual mass production, grain uniformity is controlled solely through processes like sieving, and disordered grain growth is controlled by adding certain additives, ultimately achieving the regulation of internal porosity changes and improved grain boundary strength. While sieving ferrite pre-sintered particles can improve grain uniformity to some extent, individual grains still exhibit irregular morphologies with protrusions and depressions, and certain voids remain between grains. Adding flux can compensate for some voids during liquid phase formation, but as grains grow, excessive stress can occur in certain areas, ultimately leading to defects and reduced magnetic properties in the magnet.

[0066] This invention endows each ferrite grain with a certain degree of high-melting-point nano-silica shell. By controlling the amount of silicon source added and the processing technology, the growth of nano-silica is controlled. This not only better modifies the morphology of the ferrite grains but also improves the strength of each ferrite grain, preventing excessive stress in the region caused by disordered growth. At the same time, it can also reduce the amount of other additives (fluxes and lubricants) used, thereby improving production efficiency.

[0067] This invention targets the preparation of permanent magnet ferrite magnets. Based on the dry preparation process, it modifies the ferrite pre-sintered material by in-situ growth of nano-silica, and modifies and strengthens the surface of the ferrite pre-sintered material, aiming to further improve the magnetic properties of the magnet and enhance product competitiveness.

[0068] Modified ferrite pre-sintered material is processed through mixing, dry pressing, and sintering to produce magnets with excellent magnetic properties. Magnets prepared from modified ferrite pre-sintered material effectively address problems such as excessive porosity, low grain boundary strength, and uneven internal stress that lead to reduced magnetic performance and cracking. It shows great promise for application in the field of dry-pressed permanent magnet ferrites. Detailed Implementation

[0069] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.

[0070] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.

[0071] Example 1

[0072] This embodiment provides a method for preparing permanent magnet ferrite, including the following steps:

[0073] (1) Preparation of modified ferrite pre-sintered material:

[0074] Step 1: Pre-sinter the ferrite pre-fired substrate Sr 0.86 La 0.14 Fe 11.86 Co 0.14 O 19 Tetraethyl orthosilicate and anhydrous ethanol were mixed and ultrasonically dispersed. The mass ratio of ferrite pre-sintered material to tetraethyl orthosilicate was 2000:70, and the mass ratio of ferrite pre-sintered material to anhydrous ethanol was 2000:4500.

[0075] Step 2: Place the mixture into a ball mill jar for ball milling. After ball milling for half an hour, add the catalyst dilute hydrochloric acid (1 mol / L).

[0076] The mass ratio of ferrite pre-calcined material to dilute hydrochloric acid was 2000:5, the ball milling rate was 300 r / min, and the ball milling time was 8 h.

[0077] Step 3: Solid-liquid separation. Spread the solid product out to air dry, and then sieve it through a 30-mesh sieve to obtain the modified ferrite pre-calcined material.

[0078] (2) Preparation of permanent magnet ferrite:

[0079] Step A: Blend the modified ferrite pre-calcined material, flux La2O3, and lubricant zinc stearate to obtain a blend.

[0080] The mass ratio of modified ferrite pre-calcined material, La2O3, and zinc stearate is 2000:15:14.

[0081] Step B: Dry-press the blend and sinter it.

[0082] After dry pressing in a magnetic field with a strength of 1200 Oe and a pressure of 50 MPa, the temperature is increased to 400℃ at a rate of 6℃ / min and held for 2 hours, then increased to 700℃ at a rate of 5℃ / min and held for 4 hours, then increased to 1000℃ at a rate of 4℃ / min and held for 3 hours, then increased to 1260℃ at a rate of 3℃ / min and held for 6 hours, and then cooled in the furnace to obtain permanent magnet ferrite.

[0083] Example 2

[0084] This embodiment provides a method for preparing permanent magnet ferrite, which is basically the same as that in Example 1, except that the mass ratio of ferrite pre-sintered material to tetraethyl orthosilicate is 500:100.

[0085] Example 3

[0086] This embodiment provides a method for preparing permanent magnet ferrite, which is basically the same as that in Example 1, except that the mass ratio of ferrite pre-sintered material to tetraethyl orthosilicate is 3000:10.

[0087] Example 4

[0088] This embodiment provides a method for preparing permanent magnet ferrite, which is basically the same as that in Embodiment 1, except that the ball milling speed is 600 r / min.

[0089] Example 5

[0090] This embodiment provides a method for preparing permanent magnet ferrite, which is basically the same as that in Embodiment 1, except that the ball milling speed is 200 r / min.

[0091] Example 6

[0092] This embodiment provides a method for preparing permanent magnet ferrite, which is basically the same as that in Embodiment 1, except that the ball milling time is 10 hours.

[0093] Example 7

[0094] This embodiment provides a method for preparing permanent magnet ferrite, which is basically the same as that in Embodiment 1, except that the ball milling time is 6 hours.

[0095] Example 8

[0096] This embodiment provides a method for preparing permanent magnet ferrite, which is basically the same as that in Example 1, except that the mass ratio of modified ferrite pre-calcined material to La2O3 is 500:18.

[0097] Example 9

[0098] This embodiment provides a method for preparing permanent magnet ferrite, which is basically the same as that in Example 1, except that the mass ratio of modified ferrite pre-calcined material to La2O3 is 3000:10.

[0099] Example 10

[0100] This embodiment provides a method for preparing permanent magnet ferrite, which is basically the same as that in Example 1, except that the mass ratio of modified ferrite pre-calcined material to zinc stearate is 500:25.

[0101] Example 11

[0102] This embodiment provides a method for preparing permanent magnet ferrite, which is basically the same as that in Example 1, except that the mass ratio of modified ferrite pre-calcined material to zinc stearate is 3000:1.

[0103] Example 12

[0104] This embodiment also provides a method for preparing permanent magnet ferrite, including the following steps:

[0105] (1) Preparation of modified ferrite pre-sintered material:

[0106] Step 1: Pre-sinter the ferrite pre-fired substrate Sr 0.86 La 0.14 Fe 11.86 Co 0.14 O 19 Tetraethyl orthosilicate and anhydrous ethanol were mixed and ultrasonically dispersed. The mass ratio of ferrite pre-sintered material to tetraethyl orthosilicate was 2000:70, and the mass ratio of ferrite pre-sintered material to anhydrous ethanol was 2000:4500.

[0107] Step 2: Place the mixture into a ball mill jar for ball milling, and add dilute hydrochloric acid (1 mol / L) as a catalyst during the ball milling process.

[0108] The mass ratio of ferrite pre-calcined material to dilute hydrochloric acid was 2000:5, the ball milling rate was 300 r / min, and the ball milling time was 8 h.

[0109] Step 3: Solid-liquid separation. Spread the solid product out to air dry, and then sieve it through a 30-mesh sieve to obtain the modified ferrite pre-calcined material.

[0110] (2) Preparation of permanent magnet ferrite:

[0111] Step A: Blend the modified ferrite pre-calcined material, flux Al2O3, and lubricant calcium stearate to obtain a blend.

[0112] The mass ratio of modified ferrite pre-calcined material, Al2O3, and calcium stearate is 2000:15:14.

[0113] Step B: Dry-press the blend and sinter it.

[0114] After dry pressing in a magnetic field with a strength of 1200 Oe and a pressure of 50 MPa, the temperature is increased to 400℃ at a rate of 6℃ / min and held for 2 hours, then increased to 700℃ at a rate of 5℃ / min and held for 4 hours, then increased to 1000℃ at a rate of 4℃ / min and held for 3 hours, then increased to 1260℃ at a rate of 3℃ / min and held for 6 hours, and then cooled in the furnace to obtain permanent magnet ferrite.

[0115] Example 13

[0116] This embodiment also provides a method for preparing permanent magnet ferrite, including the following steps:

[0117] (1) Preparation of modified ferrite pre-sintered material:

[0118] Step 1: Pre-sinter the ferrite pre-fired substrate Sr 0.86 La 0.14 Fe 11.86 Co 0.14 O 19 Tetraethyl orthosilicate and anhydrous ethanol were mixed and ultrasonically dispersed. The mass ratio of ferrite pre-sintered material to tetraethyl orthosilicate was 2000:70, and the mass ratio of ferrite pre-sintered material to anhydrous ethanol was 2000:4500.

[0119] Step 2: Place the mixture into a ball mill jar for ball milling, and add ammonia water (concentration 12mol / L) as a catalyst during the ball milling process.

[0120] The mass ratio of ferrite pre-calcined material to dilute hydrochloric acid was 2000:5, the ball milling rate was 300 r / min, and the ball milling time was 8 h.

[0121] Step 3: Solid-liquid separation. Spread the solid product out to air dry, and then sieve it through a 30-mesh sieve to obtain the modified ferrite pre-calcined material.

[0122] (2) Preparation of permanent magnet ferrite:

[0123] Step A: Blend the modified ferrite pre-calcined material, flux La2O3, and lubricant zinc stearate to obtain a blend.

[0124] The mass ratio of modified ferrite pre-calcined material, La2O3, and zinc stearate is 2000:15:14.

[0125] Step B: Dry-press the blend and sinter it.

[0126] After dry pressing in a magnetic field with a strength of 1200 Oe and a pressure of 50 MPa, the temperature is increased to 400℃ at a rate of 6℃ / min and held for 2 hours, then increased to 700℃ at a rate of 5℃ / min and held for 4 hours, then increased to 1000℃ at a rate of 4℃ / min and held for 3 hours, then increased to 1260℃ at a rate of 3℃ / min and held for 6 hours, and then cooled in the furnace to obtain permanent magnet ferrite.

[0127] Comparative Example 1

[0128] This comparative example provides a method for preparing permanent magnet ferrite, including the following steps:

[0129] Step A: The ferrite pre-sintered substrate Sr 0.86 La 0.14 Fe 11.86 Co 0.14 O 19The flux La2O3 and the lubricant zinc stearate were blended to obtain a blend.

[0130] The mass ratio of ferrite pre-sintered base material, La2O3, and zinc stearate is 2000:15:14.

[0131] Step B: Dry-press the blend and sinter it.

[0132] After dry pressing in a magnetic field with a strength of 1200 Oe and a pressure of 50 MPa, the temperature is increased to 400℃ at a rate of 6℃ / min and held for 2 hours, then increased to 700℃ at a rate of 5℃ / min and held for 4 hours, then increased to 1000℃ at a rate of 4℃ / min and held for 3 hours, then increased to 1260℃ at a rate of 3℃ / min and held for 6 hours, and then cooled in the furnace to obtain permanent magnet ferrite.

[0133] Comparative Example 2

[0134] This comparative example provides a method for preparing permanent magnet ferrite, including the following steps:

[0135] (1) Preparation of modified ferrite pre-sintered material:

[0136] Step 1: Pre-sinter the ferrite pre-fired substrate Sr 0.86 La 0.14 Fe 11.86 Co 0.14 O 19 It is mixed with tetraethyl orthosilicate and anhydrous ethanol and ultrasonically dispersed. The mass ratio of ferrite pre-sintered material to tetraethyl orthosilicate is 2000:500, and the mass ratio of ferrite pre-sintered material to anhydrous ethanol is 2000:4500.

[0137] Step 2: Place the mixture into a ball mill jar for ball milling. After ball milling for half an hour, add the catalyst dilute hydrochloric acid (1 mol / L).

[0138] The mass ratio of ferrite pre-calcined material to dilute hydrochloric acid was 2000:5, the ball milling rate was 300 r / min, and the ball milling time was 8 h.

[0139] Step 3: Solid-liquid separation. Spread the solid product out to air dry, and then sieve it through a 30-mesh sieve to obtain the modified ferrite pre-calcined material.

[0140] (2) Preparation of permanent magnet ferrite:

[0141] Step A: Blend the above modified ferrite pre-calcined material, flux La2O3, and lubricant zinc stearate to obtain a blend.

[0142] The mass ratio of modified ferrite pre-calcined material, La2O3, and zinc stearate is 2000:15:14.

[0143] Step B: Dry-press the blend and sinter it.

[0144] After dry pressing in a magnetic field with a strength of 1200 Oe and a pressure of 50 MPa, the temperature is increased to 400℃ at a rate of 6℃ / min and held for 2 hours, then increased to 700℃ at a rate of 5℃ / min and held for 4 hours, then increased to 1000℃ at a rate of 4℃ / min and held for 3 hours, then increased to 1260℃ at a rate of 3℃ / min and held for 6 hours, and then cooled in the furnace to obtain permanent magnet ferrite.

[0145] The magnetic properties of the permanent magnet ferrites prepared in the examples and comparative examples were tested using a BH performance tester. The X-ray diffraction (XRD) of the modified ferrite pre-sintered materials prepared in examples 2 and 2, and the ferrite pre-sintered material substrates in comparative example 1 were tested using a particle size analyzer. 50 The test results are shown in Table 1.

[0146] Table 1

[0147]

[0148] B r For remanence, H cb For coercivity, H cj This refers to intrinsic self-control (BH). max For the maximum magnetic energy product, X 50 This refers to the particle size at which the cumulative particle size distribution percentage reaches 50%.

[0149] As shown in Table 1, the magnetic properties of the permanent magnet ferrite prepared by the method of the present invention are significantly improved. In Comparative Example 1, the ferrite pre-sintered substrate was not modified. Due to the inconsistent grain regularity, grain movement or rotation was often difficult during the dry preparation process, resulting in low orientation. Furthermore, the interfacial strength between grains was low during crystal growth, leading to voids and a decrease in magnet performance. In Comparative Example 2, excessive use of tetraethyl orthosilicate also resulted in a poor coating effect. 50 The size increases significantly, and the grain uniformity deteriorates, resulting in a decrease in magnet performance.

[0150] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A method for preparing permanent magnet ferrite, characterized in that, Includes the following steps: Step A: Blend the modified ferrite pre-calcined material, flux, and lubricant to obtain a blend; The mass ratio of the modified ferrite pre-sintered material to the flux is (500~2000):(15~18); Step B: Dry press the blend into shape and sinter it; The dry pressing is carried out in a magnetic field with a strength of 1000~1400 Oe; The preparation method of the modified ferrite pre-sintered material includes the following steps: Step 1: Mix the ferrite pre-sintered material substrate, silicon source, and solvent to obtain a mixture; The mass ratio of the ferrite pre-sintered material to the silicon source is 2000:70; Step 2: Mix the mixture with the catalyst and ball mill it; The catalyst is an aqueous solution of an acid; The mass ratio of the silicon source to the catalyst is (10~100):(1~10). The aqueous solution of the acid includes one or more of hydrochloric acid and selenic acid; The rotational speed of the ball mill is 300~600 r / min; The ball milling time is 6-10 hours; The silicon source is catalyzed by the catalyst to hydrolyze and condense on the surface of the ferrite pre-sintered substrate to form a nano-silica surface layer. Step 3: Solid-liquid separation to obtain modified ferrite pre-calcined material.

2. The method for preparing permanent magnet ferrite according to claim 1, characterized in that, Step 1 satisfies at least one of the following conditions: (1) The mass ratio of the silicon source to the solvent is (10~100):(3000~6000); (2) After mixing the ferrite pre-sintered material substrate, silicon source and solvent, the mixture is ultrasonically dispersed to obtain a mixture; (3) The silicon source includes one or more of methyl orthosilicate, ethyl orthosilicate, and sodium silicate; (4) The solvent includes water and / or an organic solvent, wherein the organic solvent includes one or more of anhydrous ethanol, acetone and toluene.

3. The method for preparing permanent magnet ferrite according to any one of claims 1 or 2, characterized in that, Step 3 includes drying the solid product after solid-liquid separation.

4. The method for preparing permanent magnet ferrite according to claim 3, characterized in that, The drying method is air drying.

5. The method for preparing permanent magnet ferrite according to claim 3, characterized in that, Step 3 further includes crushing and sieving the dried product using a 10-100 mesh sieve.

6. The method for preparing permanent magnet ferrite according to claim 1, characterized in that, Step A satisfies at least one of the following conditions: (1) The mass ratio of the lubricant to the modified ferrite pre-calcined material is (1~25):(500~3000); (2) The flux includes one or more of La2O3, Al2O3 and CaCO3; (3) The lubricant includes one or more of zinc stearate, magnesium stearate and calcium stearate.

7. The method for preparing permanent magnet ferrite according to claim 1 or 6, characterized in that, The pressure for dry pressing is 40~80MPa; And / or, the sintering includes sequentially performing a first heating, a first holding, a second heating, a second holding, a third heating, a third holding, a fourth heating, and a fourth holding.

8. The method for preparing permanent magnet ferrite according to claim 7, characterized in that, The first heating rate is 2~10℃ / min; And / or, the endpoint temperature of the first heating is 300~500℃; And / or, the first heat preservation time is 1~6 hours.

9. The method for preparing permanent magnet ferrite according to claim 7, characterized in that, The second heating rate is 3~9℃ / min; And / or, the endpoint temperature of the second heating is 600~800℃; And / or, the second heat preservation time is 1~8h.

10. The method for preparing permanent magnet ferrite according to claim 7, characterized in that, The third heating rate is 2~7℃ / min; And / or, the endpoint temperature of the third heating is 900~1100℃; And / or, the third insulation time is 1~5h.

11. The method for preparing permanent magnet ferrite according to claim 7, characterized in that, The rate of the fourth heating is 1~5℃ / min; And / or, the final temperature of the fourth heating step is 1200~1300℃; And / or, the fourth heat preservation time is 1~12h.

12. A permanent magnet ferrite, characterized in that, Prepared by the preparation method according to any one of claims 1-11.

Citation Information

Patent Citations

  • High-coercivity ferrite and preparation method thereof

    CN113087513A

  • Dry-pressed permanent magnetic ferrite, preparation method thereof, magnetic device and application of magnetic device

    CN118754636A

  • Magnetically hard material

    US20100155651A1