An organic-inorganic intercalated spatial structure AAO / PVDF composite coating and its preparation method

By preparing an AAO/PVDF composite coating with an organic-inorganic intercalation structure on the surface of aluminum alloy, the problems of weak interfacial bonding strength and environmental pollution of organic antifouling coatings are solved, achieving long-term corrosion resistance and antibacterial and antifouling properties, which are suitable for marine engineering.

CN119710861BActive Publication Date: 2026-11-17SHANGHAI JIAOTONG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411881360.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-19
Publication Date
2026-11-17
Estimated Expiration
2044-12-19

AI Technical Summary

Technical Problem

Existing organic antifouling coatings have weak interfacial bonding strength in marine environments, are easily damaged, and release heavy metal ions that pollute the marine environment, making it difficult to achieve long-term corrosion and fouling protection.

Method used

An organic-inorganic intercalated spatial structure AAO/PVDF composite coating was prepared on the surface of aluminum alloy using a hard template-soft modification technique. PVDF was filled into the nanopores of anodic aluminum oxide by vacuum solution casting and then subjected to high-voltage polarization to form a piezoelectric AAO/PVDF composite coating. Environmental disturbances were used to excite surface charges to inhibit bacterial adhesion.

Benefits of technology

It achieves long-lasting anti-corrosion and anti-fouling effects with high interfacial bonding strength, good corrosion resistance, and resistance to mechanical damage. It is green and environmentally friendly, does not release toxic substances, and is suitable for anti-corrosion and anti-fouling of aluminum alloys in marine engineering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119710861B_ABST
    Figure CN119710861B_ABST
Patent Text Reader

Abstract

This invention discloses an organic-inorganic intercalated spatial structure AAO / PVDF composite coating and its preparation method. Based on hard template-soft modification technology, a hard porous anodic alumina layer is obtained on the surface of an aluminum alloy. Then, polyvinylidene fluoride (PVDF) solution is injected into the nanopores of the anodic alumina layer through vacuum pressure impregnation and solution casting to solidify and form a nanopillar array structure. The PVDF nanopillars are then subjected to high-voltage polarization treatment using corona polarization. This process can prepare an antibacterial, antifouling, and anticorrosion AAO / PVDF composite coating based on the piezoelectric effect and environmentally induced charge response. The AAO / PVDF coating of this invention exhibits excellent antibacterial properties, strong interfacial bonding, and stable piezoelectric characteristics. Furthermore, PVDF effectively seals the nanopores of AAO, significantly improving the corrosion resistance of the aluminum alloy. The anti-corrosion and antifouling process is long-lasting, environmentally friendly, and highly efficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of preventing marine biofouling on aluminum alloy surfaces. Specifically, it relates to a long-lasting anti-corrosion and antifouling AAO / PVDF composite coating with an organic-inorganic interlocking spatial structure and its preparation method, based on hard template-soft modification technology for PVDF soft modification of hard anodized aluminum. The coating possesses long-lasting anti-corrosion, antifouling and antibacterial properties. Background Technology

[0002] Lightweight, corrosion-resistant aluminum alloys hold promise as a partial replacement for steel materials commonly used in shipbuilding and marine engineering. They have potential applications in offshore platform oil and gas drilling equipment, port anchoring structures, and ship structural components. However, prolonged contact with seawater poses significant challenges to aluminum alloys, leading to severe biofouling and corrosion. Aluminum alloys corrode significantly in seawater environments, and biofouling accelerates this corrosion, shortening the service life of aluminum alloy components, impacting the safe operation of equipment systems, and increasing maintenance costs. Therefore, addressing biofouling and corrosion of aluminum alloys in marine environments is a pressing engineering challenge that needs to be tackled.

[0003] Currently, it is generally accepted that the matrix film induced by the adhesion of marine microorganisms is a key factor in the evolution and development of marine biofouling on material surfaces. Effectively inhibiting the adhesion of bacteria and fungi to material surfaces and controlling the formation of the initial matrix film has become a recognized method for preventing marine biofouling. Existing mainstream antifouling methods mainly regulate the surface morphology and functional components of materials to impart antibacterial adhesion properties. For example, applying organic coatings containing antifouling agents or bactericides to the material surface utilizes these agents to control bacterial and microbial adsorption and the formation of the initial matrix film, thereby eliminating or inhibiting the key process of marine biofouling formation. This is the most common technology in practical engineering applications. However, the interfacial bonding strength between organic antifouling coatings and metal substrates is relatively weak, and regular cleaning of surface fouling and recoating of the organic coating are required. The maintenance process is cumbersome and costly, and there are certain limitations in the performance requirements of organic antifouling coatings for mechanical damage resistance and erosion corrosion resistance. On the other hand, the release of heavy metal ions from organic antifouling coatings into seawater severely impacts the marine environment and organisms. The concentration of heavy metal elements in seabed silt is seriously excessive, and free heavy metal ions can cause genetic variations and abnormal development in marine organisms, and can also enter the human body through the food chain. In recent years, the marine environmental problems caused by various heavy metal ions released from organic antifouling coatings have become very significant. The International Maritime Organization (IMO) has called for full consideration of the pollution and damage of antifouling agents to the marine ecological environment and has banned the use of organotin compounds in antifouling coatings. Developing green and long-lasting antifouling and corrosion-resistant coatings has become a future trend in the prevention and control of marine biofouling.

[0004] Numerous studies have developed various antifouling coatings from an eco-friendly perspective. For example, superhydrophobic surfaces have shown good performance in laboratory microbiological experiments (see Chinese patent, application number CN202410848829.0). However, their performance in marine field tests remains insufficient. Low surface energy organic substances are easily degraded, and the brittle hydrophobic network structure cannot withstand harsh mechanical damage and fluid erosion. Dynamically dissolving and releasing self-polishing antifouling coatings (see Chinese patents, application numbers CN202410660043.6, CN202411010200.5) have shown good antifouling effects in both laboratory microbiological experiments and marine field tests. However, in actual service, the long-term antifouling performance and resistance to mechanical damage of the coatings have not met expectations. The surface antifouling performance of organic coatings drops sharply after scratching or abrasion, the dynamic dissolution rate is difficult to control stably, and the interfacial bonding strength between the organic coating and the substrate is still insufficient. Therefore, the service life of organic antifouling coatings lacks long-term effectiveness. High interfacial bonding strength, resistance to mechanical damage, and long-term effectiveness have become bottleneck problems in the application of antifouling coatings in the field of marine engineering. Therefore, exploring new design methods for long-term anti-corrosion and antifouling coatings on aluminum alloy surfaces for marine engineering applications has urgent practical significance. Summary of the Invention

[0005] To address the shortcomings of existing eco-friendly organic antifouling coatings, this invention aims to provide a method for preparing a long-lasting anti-corrosion and antifouling AAO / PVDF composite coating with an organic-inorganic intercalated spatial structure based on hard template-soft modification technology. Utilizing the nanoporous structure of hard anodic alumina, PVDF is filled into the nanopores of anodic alumina through a vacuum solution casting process. After curing, an organic-inorganic intercalated spatial structure is formed. High-voltage polarization yields a long-lasting anti-corrosion and antifouling AAO / PVDF composite coating with piezoelectric properties. This coating can spontaneously generate and release surface charges through environmental disturbances, interacting with bacteria and inhibiting the formation of bacterial matrix films on aluminum alloy surfaces. The AAO / PVDF composite coating exhibits advantages such as high interfacial bonding strength, good corrosion resistance, resistance to mechanical damage, and long-lasting effectiveness. The antibacterial and antifouling process is environmentally friendly and has potential applications in the field of marine biofouling prevention and corrosion protection of aluminum alloys for marine engineering.

[0006] Most bacteria possess charged groups on their surfaces, and imparting surface charge properties to materials can influence bacterial adhesion. Based on the principle of bacterial-charge interaction, designing charge properties on aluminum alloy surfaces can effectively inhibit bacterial and microbial adhesion. Methods for charging material surfaces mainly include triboelectric charging, contact charging, and inductive charging. Inductive charging is the most feasible technique in marine environments. Piezoelectric materials are typical inductively charged materials, and the dynamic response of the piezoelectric coating surface can be excited by marine environmental disturbances to generate induced charges. Polyvinylidene fluoride (PVDF) is one of the most typical piezoelectric materials, possessing advantages such as flexibility, low density, corrosion resistance, wear resistance, impact resistance, and aging resistance. Furthermore, the molding process of PVDF is simple. Therefore, PVDF organic piezoelectric coatings can be prepared on aluminum alloy surfaces, utilizing the piezoelectric properties of the PVDF coating to inhibit bacterial adhesion to the aluminum alloy surface, thereby controlling marine biofouling on aluminum alloy surfaces.

[0007] This invention provides a method for preparing a long-lasting anti-corrosion and anti-fouling coating on aluminum alloy surfaces based on the piezoelectric effect. The method involves constructing anodized aluminum oxide (AAO) with a nanoporous structure on the aluminum alloy surface using an anodizing process, followed by vacuum solution casting to fill the nanopores of the anodized aluminum layer with PVDF. The AAO / PVDF composite coating exhibits significant piezoelectric response characteristics after high-voltage corona polarization. This invention proposes a hard template-soft modification process for soft modification of hard anodized aluminum with PVDF. The anti-corrosion and anti-fouling AAO / PVDF composite coating prepared using this method has the following characteristics: ① PVDF seals the nanopores of the AAO coating, effectively preventing chloride ions in seawater from penetrating to the bottom of the AAO coating and corroding the aluminum substrate. PVDF itself is chemically extremely stable and resistant to seawater corrosion, resulting in superior corrosion resistance for the AAO / PVDF composite coating; ② The nanopores provide numerous interfaces between PVDF and AAO, significantly improving the interfacial bonding strength between PVDF and the aluminum alloy, effectively solving the problem of organic... The coating addresses the weak interfacial bonding problem on inorganic aluminum alloy surfaces; ③ The hard and wear-resistant AAO coating has good resistance to mechanical damage and fluid erosion, which can prevent the flexible PVDF coating from being damaged too quickly by external mechanical forces. The piezoelectric PVDF nanopillar array in the nanopores can still achieve the long-term effect of the coating inhibiting bacterial adhesion; ④ With the help of ocean waves and seawater impact disturbance, the piezoelectric PVDF is continuously excited and induced to form and release surface charges by external forces, achieving effective inhibition of marine biofouling on aluminum alloy surfaces. This environmentally excited charge response antibacterial process has significant green and environmentally friendly characteristics for the marine environment.

[0008] The objective of this invention is achieved through the following technical solution: In a first aspect, the present invention provides a method for preparing a long-lasting anti-corrosion and anti-fouling AAO / PVDF composite coating with an organic-inorganic intercalated spatial structure based on hard template-soft modification technology, comprising the following steps: S1. Anodizing treatment: The aluminum alloy substrate is anodized in an electrolyte to obtain an anodized aluminum layer, and then a pore-expansion treatment is performed to increase the diameter of the nanopores in the anodized aluminum layer. S2, Vacuum solution casting: The anodic aluminum oxide layer obtained in step S1 is subjected to vacuum degassing treatment, and then PVDF solution is fully introduced into the nanopores of the anodic aluminum oxide layer under high-purity nitrogen pressure treatment for filling. After filling, PVDF curing treatment is performed. S3. Corona polarization treatment: The cured anodic aluminum oxide layer is subjected to corona polarization treatment to obtain an AAO / PVDF composite coating with an organic-inorganic intercalation structure and piezoelectric properties.

[0009] As some specific embodiments of the present invention, in step S1, the aluminum alloy substrate must undergo pretreatment before anodizing, specifically including: grinding, polishing and ultrasonic cleaning of the aluminum alloy, then removing surface organic matter and oxide layer by alkaline washing and acid washing, and electrochemical polishing in a solution containing perchloric acid to obtain an aluminum alloy substrate in a reflective mirror state.

[0010] As some specific embodiments of the present invention, the polishing is performed by sequentially polishing the aluminum alloy with SiC waterproof sandpaper of 180#, 400#, 800#, 1500# and 3000#. The polishing process involves sequentially applying diamond polishing slurries with particle sizes of 9μm, 3μm, and 1μm to the polished aluminum alloy for 2-5 minutes. The ultrasonic cleaning process involves sequentially ultrasonically cleaning the ground and polished aluminum alloy in acetone, pure water, and ethanol for 3-5 minutes each.

[0011] As some specific embodiments of the present invention, the alkaline solution used for alkaline washing is a 25-40 g / L NaOH solution; the acid solution used for acid washing is a 20-25% HNO3 solution; the alkaline washing time is 3-5 min, which removes organic matter from the aluminum alloy surface; the acid washing time is 5-10 min, which removes surface oxides and residual alkaline solution.

[0012] As some specific embodiments of the present invention, the electrochemical polishing is carried out in a perchloric acid / ethanol electrolyte under a DC voltage of 20-25V and a water bath condition of 0-5℃; the electrochemical polishing time is 4-10min, and an aluminum alloy substrate with a reflective mirror state is obtained after polishing; in the electrolyte, the volume ratio of HClO4 to C2H5OH is 1:3-1:5.

[0013] Preferably, the volume ratio of HClO4 to C2H5OH solution is V1:V2=1:4.

[0014] As some specific embodiments of the present invention, the pretreatment steps for the aluminum alloy substrate specifically include: grinding with SiC waterproof sandpaper of 180#, 400#, 800#, 1500# and 3000# in sequence; polishing with diamond polishing liquid of 9μm, 3μm and 1μm particle size in sequence for 2-5 minutes after grinding; ultrasonic cleaning in acetone, pure water and ethanol in sequence for 3-5 minutes after polishing; immersing the cleaned aluminum alloy in alkaline solution and acid solution to remove surface organic matter and oxide layer; then ultrasonic cleaning in acetone, pure water and ethanol in sequence for 3-5 minutes; electrochemical polishing of the aluminum alloy in perchloric acid / ethanol electrolyte at 20-25V DC voltage and 0-5℃ water bath conditions for 4-10 minutes to finally obtain aluminum alloy in a reflective mirror state; then ultrasonic cleaning in acetone, pure water and ethanol in sequence for 3-5 minutes; and drying with cold air for later use.

[0015] As some specific embodiments of the present invention, in step S1, during the anodizing process, an aluminum alloy substrate is used as the anode working electrode and an inert conductive electrode is used as the cathode. The anode aluminum alloy is treated under constant pressure for 15-60 minutes in an acidic electrolyte and a constant temperature water bath.

[0016] As some specific embodiments of the present invention, the inert conductive electrode includes at least one of carbon plate, titanium plate, platinum sheet, and gold sheet.

[0017] As some specific embodiments of the present invention, the acidic electrolyte is at least one of phosphoric acid, sulfuric acid, and oxalic acid solution.

[0018] As some specific embodiments of the present invention, the acidic electrolyte is a phosphoric acid solution with a mass fraction of 5-20%, the constant temperature water bath temperature is 15-25℃, the voltage is 40-70V, and the time is 15-45min; And / or, the acidic electrolyte is a sulfuric acid solution with a mass fraction of 10-20%, a constant temperature water bath temperature of 0-5℃, a voltage of 20-35V, and a time of 15-45min; And / or, the acidic electrolyte is an oxalic acid solution with a mass fraction of 3-10%, a constant temperature water bath temperature of 0-5℃, a voltage of 40-65V, and a time of 20-60min.

[0019] Preferably, the acidic electrolyte is a phosphoric acid solution with a mass fraction of 15%, the constant temperature water bath is 20°C, the voltage is 50-60V, and the time is 30min. And / or, the acidic electrolyte is a sulfuric acid solution with a mass fraction of 15%, the constant temperature water bath is at 0°C, the voltage is 25-30V, and the time is 30min; And / or, the acidic electrolyte is an oxalic acid solution with a mass fraction of 5%, the constant temperature water bath is at 0°C, the voltage is 50-60V, and the time is 60min.

[0020] As some specific embodiments of the present invention, in step S1, the solution used for the pore-expanding treatment is a phosphoric acid solution with a mass fraction of 3-5%, the pore-expanding treatment time is 5-30 minutes, and the temperature is 40-60°C. The pore-expanding treatment accelerates the rate at which the PVDF solution penetrates into the AAO nanopores, reducing the preparation time of the vacuum-pressurized solution casting process.

[0021] As some specific embodiments of the present invention, in step S2, the PVDF solution is prepared by dissolving PVDF powder in an organic solvent, the mass fraction of PVDF in the PVDF solution is 30-70%, and the organic solvent is N,N-dimethylformamide (DMF).

[0022] Specifically, PVDF powder is dissolved in DMF by magnetic stirring at a speed of 50-300 rpm for 1-3 hours.

[0023] As some specific embodiments of the present invention, in step S2, the vacuum degassing treatment and high-purity nitrogen pressurization treatment are carried out in a high-pressure tank. During the vacuum degassing treatment, the high-pressure tank is first evacuated to 0-0.1 bar and held for 1-2 minutes. Then, the PVDF solution is brought into contact with the anodic aluminum oxide layer under the condition of 0-0.1 bar and held for 10-60 minutes. After introducing high-purity nitrogen, the pressure is increased to 10... 6 -10 7 Pa, maintain for 20-60 minutes. The air inside the nanopores of the anodic aluminum oxide is removed through vacuum degassing. First, a vacuum is drawn, then the anodic aluminum oxide and PVDF solution are brought into contact under vacuum. This effectively removes air from the pores, reducing the resistance to PVDF filling. Then, high-purity nitrogen is introduced for pressurization, ensuring the PVDF fully fills the nanopores of the anodic aluminum oxide.

[0024] In some specific embodiments, the anodized aluminum is fixed to the austenitic stainless steel tank sealing cap using two magnets. One magnet is placed on the outer surface of the sealing cap, and the other magnet is placed on the inner surface of the sealing cap, with the anodized aluminum sandwiched between the magnets and the sealing cap. After the PVDF / DMF solution is poured into the tank, the tank is sealed. The tank is evacuated until the pressure gauge shows 0.1 bar, and this is maintained for 1-2 minutes. Then, the valve connected to the vacuum pump is closed. The magnet on the outer surface of the sealing cap is then removed, allowing the anodized aluminum to fall into the PVDF / DMF solution. This is maintained below 0.1 bar for 10-60 minutes. This step removes the air from the nanopores within the anodized aluminum layer. Afterward, the valve connected to the high-purity nitrogen cylinder is opened, and nitrogen is injected until the pressure gauge shows 10.6 After the pressure reaches above 10 Pa, close the valve connecting the high-purity nitrogen cylinder. 6 Maintaining a pressure above 20 Pa for 20-60 minutes allows the PVDF / DMF solution to fully fill the nanopores of the anodic aluminum oxide during the entire treatment process.

[0025] As some specific embodiments of the present invention, in step S2, the curing process is carried out in an oven or heat treatment furnace. During the curing process, the temperature is first kept at 60-80℃ for 1-3 hours, and then kept at 110-140℃ for 3-8 hours.

[0026] As some specific embodiments of the present invention, in step S3, during the corona polarization treatment, the electric field strength is 3-10 kV / cm, the polarization time is 30-60 min, and the voltage polarization is carried out in a high-voltage polarization device; during corona polarization, the voltage and the distance between the high-voltage needle tip and the anodic aluminum oxide can be adjusted, the corona polarization voltage is 4-20 kV, and the distance between the needle tip and the anodic aluminum oxide surface is 3-15 mm.

[0027] Preferably, the electric field strength is 10kV / cm, the corona polarization voltage is 10kV, and the distance between the high-voltage needle tip and the anodic aluminum oxide is 10mm.

[0028] As some specific embodiments of the present invention, the corona-polarized needle tip can be either a single-needle structure or a multi-needle array structure. The polarization voltage and the spacing between the needle tip and the anodic aluminum oxide are the same for the multi-needle array structure as for the single-needle structure. The spacing of the multi-needle array structure is 5-10 mm, and the arrangement of the multi-needle array structure is designed according to the area of ​​the aluminum alloy. For example, a 50 mm × 50 mm square aluminum alloy can use a multi-needle array structure, which can be an array structure formed by combining 9 single needles in a 3×3 configuration.

[0029] Preferably, the corona-polarized needle tip is a multi-needle array structure formed by combining 9 single needles in a 3×3 configuration. The polarization voltage of the multi-needle array structure is set to 10kV, the distance between the needle tip and the anodic aluminum oxide is 10mm, the electric field strength is 10kV / cm, and the needle tip spacing of the array structure is 5mm.

[0030] Secondly, the present invention provides an AAO / PVDF composite coating with an organic-inorganic intercalation structure having piezoelectric properties, which is prepared by the method described in any one of the above-mentioned methods.

[0031] Invention patent CN104959045B discloses a method for preparing polyvinylidene fluoride (PVDF) nanoporous membranes. Specifically, PVDF is prepared on anodic aluminum oxide by dripping a PVDF solution into the nanopores of the anodic aluminum oxide at room temperature and pressure. After dripping, the surface PVDF solution is blown off with nitrogen gas to expose the anodic aluminum oxide. The aim is to use the nanopores of the anodic aluminum oxide as a template to synthesize PVDF nanoporous membranes. However, when preparing PVDF nanoporous membranes using this method, the PVDF solution is difficult to fully penetrate and fill the nanopores of the anodic aluminum oxide, resulting in the inability to form highly intact PVDF nanopillars and an organic-inorganic intercalated spatial structure, thus lacking corrosion resistance.

[0032] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention prepares a long-lasting anti-corrosion and anti-fouling AAO / PVDF composite coating on the surface of aluminum alloy based on hard template-soft modification technology. The coating can continuously induce the generation and release of charges on the surface of PVDF piezoelectric coating by the dynamic disturbance pressure of the environment, reduce the adhesion of bacteria on the surface of aluminum alloy, and thus inhibit the formation of marine biofouling. The antibacterial and antifouling process of PVDF piezoelectric coating will not release toxic substances that affect marine organisms and the ecological environment, and has significant eco-friendly characteristics.

[0033] (2) This invention utilizes the nanoporous structure of hard anodized aluminum to fill PVDF, forming an organic-inorganic interlocking spatial structure between the aluminum alloy substrate and the PVDF coating, which greatly improves the interfacial bonding strength between the organic PVDF piezoelectric coating and the aluminum alloy, and cleverly solves the problem of weak organic-inorganic interfacial bonding.

[0034] (3) PVDF fills the nanopores of anodic aluminum oxide, effectively preventing corrosive chloride ions in seawater from eroding the aluminum alloy substrate. The PVDF coating has stable chemical properties and is corrosion resistant, ensuring the superior corrosion resistance of the AAO / PVDF composite coating.

[0035] (4) Hard and wear-resistant anodized aluminum has good resistance to mechanical damage and fluid erosion, ensuring that even after the PVDF coating is peeled off or damaged by severe mechanical forces, the PVDF nanopillar array embedded in the nanopores can still maintain a stable piezoelectric effect, thus achieving the long-term antibacterial and anti-corrosion functions of the AAO / PVDF composite coating. Only this interlocking structure can achieve such an effect, and the PVDF / AAO composite coating integrates antibacterial and anti-corrosion functions. Attached Figure Description

[0036] Other features, objects, and advantages of the present invention will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings: Figure 1A schematic diagram of the structure of the AAO / PVDF composite coating formed on an aluminum substrate; Figure 2 A schematic diagram of the vacuum pressure solution casting process; Figure 3 Here is a cross-sectional SEM image of the AAO / PVDF composite coating in Example 1; Figure 4 SEM images of the surface coatings of Comparative Examples 1-3 and Examples 2-4; Figure 5 The XRD phase structure maps of Comparative Example 2 and Examples 2-4 are shown. Figure 6 The piezoelectric coefficient d of Comparative Example 2 and Examples 2-4 after corona polarization 33 Resulting image; Figure 7 Macroscopic photographs of the composite coatings used in Comparative Examples 1-2 and Examples 2-4 to visualize airborne Escherichia coli and Staphylococcus aureus on coated plates. Figure 8 SEM morphology of bacterial adhesion of Escherichia coli and Staphylococcus aureus on the surface of composite coatings in Comparative Examples 1-2 and Examples 2-4; Figure 9 Electrochemical curves and immersion corrosion morphology images of aluminum substrates, comparative examples 1, 3, and example 4. Detailed Implementation

[0037] The present invention will now be described in detail with reference to specific embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.

[0038] Example 1 This embodiment provides a method for preparing a long-lasting anti-corrosion and anti-fouling AAO / PVDF composite coating with an organic-inorganic intercalated spatial structure based on hard template-soft modification technology, including the following steps: (1) Aluminum alloy pretreatment: A 50mm x 50mm piece of 6061 aluminum alloy was successively polished using 180#, 400#, 800#, 1500#, and 3000# SiC waterproof sandpaper. When changing the sandpaper grit, the aluminum alloy was rotated 90° in the polishing direction. After polishing, it was polished for 2 minutes each time with diamond polishing slurries with 9μm, 3μm, and 1μm grit, followed by ultrasonic cleaning for 3 minutes each time in acetone, pure water, and ethanol.

[0039] The cleaned aluminum alloy was immersed in a 30 g / L NaOH solution for 3 minutes to remove surface organic matter, and then immersed in a 25% HNO3 solution for 5 minutes to remove surface oxides and residual alkali. Finally, it was ultrasonically cleaned for 3 minutes with acetone, pure water and ethanol.

[0040] Electrochemical polishing was performed for 5 minutes in an electrolyte solution of HClO4 and C2H5OH with a volume ratio of 1:3, under a DC voltage of 20V and a water bath at 0℃. Then, ultrasonic cleaning was performed for 3 minutes in acetone, pure water and ethanol, followed by drying with cold air.

[0041] (2) Anodizing treatment: A carbon plate was used as the cathode, and a pretreated aluminum alloy substrate was used as the anode working electrode. A 5% oxalic acid solution was used as the electrolyte. A constant voltage of 60V was applied in a constant temperature water bath at 0℃ to perform anodizing treatment on the aluminum alloy substrate for 60 minutes. The anodized aluminum was then rinsed with pure water and then immersed in a 5% phosphoric acid solution at 50℃ to expand the pores for 30 minutes.

[0042] (3) Vacuum solution casting: PVDF powder was dissolved in DMF by magnetic stirring at a speed of 150 rpm for 2 hours to obtain a PVDF solution with a mass fraction of 70%.

[0043] Place one magnet on the outer surface of the austenitic stainless steel tank sealing cap, and place another magnet on the inner surface of the sealing cap. Clamp the anodized aluminum between the magnet and the sealing cap, thus fixing the anodized aluminum to the austenitic stainless steel tank sealing cap with two magnets. Pour the PVDF solution into the tank.

[0044] like Figure 2 As shown, first evacuate the tank to a vacuum level below 0.1 bar, maintain this for 1 minute, then close the valve connected to the vacuum pump. Next, remove the magnet from the sealing cap to allow the anodized aluminum to fall into the PVDF / DMF solution. Maintain this below 0.1 bar for 30 minutes, then open the valve connected to the high-purity nitrogen cylinder and inject nitrogen until the pressure gauge shows 10. 6 After the pressure reaches above 10 Pa, close the valve connecting the high-purity nitrogen cylinder. 6 Maintain a pressure above 30 Pa for 30 minutes. Then, the anodized aluminum was removed and PVDF cured, and kept at 70℃ for 2 hours in a forced-air drying oven, followed by 130℃ for 6 hours.

[0045] (4) Corona polarization treatment: The cured anodized aluminum was polarized using a high-voltage device with a single needle structure, an electric field strength of 7kV / cm, a voltage of 7kV, a needle tip distance of 10mm from the anodized aluminum surface, and a polarization time of 30min.

[0046] like Figure 3 The image shown is a cross-sectional SEM image of the AAO / PVDF composite coating prepared in this embodiment. It can be seen that PVDF completely covers the surface of the anodic aluminum oxide (AAO), and the entire nanopore is filled with PVDF. Therefore, the method provided by this invention can realize the preparation of organic-inorganic intercalated spatial structures.

[0047] like Figure 1 The diagram shows the structure of the AAO / PVDF composite coating prepared on an aluminum substrate by the above steps of the present invention. Anodized aluminum AAO framework is formed on the aluminum substrate by anodizing treatment, and then PVDF is filled into the nanopores of AAO by vacuum solution casting and covers the upper surface of AAO to form a three-layer interlocking structure.

[0048] Example 2 This embodiment provides a method for preparing an antibacterial and antifouling AAO / PVDF composite coating with an organic-inorganic intercalated spatial structure based on hard template-soft modification technology. The specific steps are basically the same as in Example 1, except that: (1) In the pretreatment of aluminum alloy, a 40 g / L NaOH solution was used, the volume ratio of HClO4 and C2H5OH electrolyte was 1:4, and the voltage of electrochemical polishing was 25 V.

[0049] (2) In the corona polarization treatment, a 3×3 multi-needle array structure is used as the polarization needle tip, the needle tip spacing is 5mm, the distance between the needle tip and the surface of the anodic aluminum oxide is set to 10mm, the voltage is set to 5kV, the electric field strength is 5kV / cm, and the polarization time is 30min.

[0050] Example 3 This embodiment provides a method for preparing an antibacterial and antifouling AAO / PVDF composite coating with an organic-inorganic intercalated spatial structure based on hard template-soft modification technology. The specific steps are basically the same as those in Embodiment 2, except that: in the corona polarization treatment, a 3×3 multi-needle array structure is used as the polarization needle tip, the needle tip spacing is 5mm, the distance between the needle tip and the surface of the anodic aluminum oxide is set to 10mm, the voltage is set to 7kV, and the electric field strength is 7kV / cm.

[0051] Example 4 This embodiment provides a method for preparing an antibacterial and antifouling AAO / PVDF composite coating with an organic-inorganic intercalated spatial structure based on hard template-soft modification technology. The specific steps are basically the same as in Embodiment 3, except that: In the corona polarization treatment, a 3×3 multi-needle array structure is used as the polarization needle tip, the needle tip spacing is 5mm, the distance between the needle tip and the surface of the anodic aluminum oxide is set to 10mm, the voltage is set to 10kV, and the electric field strength is 10kV / cm.

[0052] Comparative Example 1 The specific steps in this comparative example are basically the same as in Example 4, except that this comparative example only performs anodizing treatment on the aluminum alloy substrate, without subsequent PVDF soft modification process. The preparation method in this comparative example can only obtain anodized aluminum (AAO).

[0053] Comparative Example 2 The specific steps of this comparative example are basically the same as those of Example 4, except that the AAO / PVDF composite coating in this comparative example did not undergo the high-voltage corona polarization treatment in step 4.

[0054] Comparative Example 3 The specific steps of this comparative example are basically the same as those of Example 4. The difference is that the aluminum alloy in this comparative example is not anodized. Instead, a PVDF coating is directly prepared on the surface of the aluminum alloy. After that, the PVDF coating is subjected to the same corona polarization treatment as in Example 4.

[0055] Effect Example Figure 4The images show SEM morphology photographs of Comparative Examples 1, 2, 3, 2, 3, and 4. The coatings of Comparative Examples 1, 2, 3, 2, 3, and 4 are labeled AAO, A / P-0, A1 / P-10, A / P-5, A / P-7, and A / P-10, respectively. The images show that the nanopores of AAO are uniformly dispersed, with a relatively uniform pore size and an average pore size of approximately 40 nm. The surface of the unpolarized A / P-0 coating shows the original morphology of the PVDF coating, with all nanopores completely covered. With increasing polarization electric field, the PVDF surface undergoes significant deformation. Under corona polarization at an electric field strength of 5 kV / cm, the flocculent amorphous microstructure of PVDF on the A / P-0 coating surface transforms into elongated, silkworm-like crystalline domains composed of spherical particles. When the electric field strength increases to 7 kV / cm and 10 kV / cm, the A / P-7 coating surface exhibits a leaf-like or plate-like structure, while the A / P-10 coating surface becomes a dense rod-shaped crystal. The increasing polarization electric field strength gradually increases the crystallinity of the AAO / PVDF composite coating, significantly affecting its piezoelectric properties. Comparative Example 3, where PVDF is prepared on an aluminum alloy surface without the nanoporous structure of anodic aluminum oxide, does not form an organic-inorganic intercalated spatial structure of AAO / PVDF, and its surface morphology after applying voltage is also different from that of Example 4.

[0056] Figure 5 For the XRD patterns of Comparative Example 2 (A / P-0) and Examples 2 (A / P-5), 3 (A / P-7), and 4 (A / P-10), the diffraction peak at 20.6° represents the (110) and (200) diffraction planes of the piezoelectric β-PVDF crystalline phase. Figure 5 It can be seen that the content of piezoelectric β-PVDF crystalline phase increases with the increase of electric field strength.

[0057] Figure 6 The piezoelectric coefficient d of Comparative Example 2 (A / P-0) and Examples 2 (A / P-5), 3 (A / P-7) and 4 (A / P-10) 33 As the electric field strength increases from 0 kV / cm to 10 kV / cm, d 33 The average value increased from 4.5 pC / N to 31.4 pC / N, indicating that the increased content of the piezoelectric β-PVDF crystalline phase enhances the piezoelectric properties of the AAO / PVDF composite coating as the electric field strength increases.

[0058] Figure 7Macroscopic photographs of the coated plates of airborne Escherichia coli and Staphylococcus aureus in Comparative Example 1 (AAO), Comparative Example 2 (A / P-0), Example 2 (A / P-5), Example 3 (A / P-7), and Example 4 (A / P-10). As the piezoelectric properties of the AAO / PVDF composite coating increase, the number of airborne bacterial colonies on the agar plates in the coated plate experiment gradually decreases. Figure 8 The SEM morphology of *Escherichia coli* and *Staphylococcus aureus* in Comparative Example 1 (AAO), Comparative Example 2 (A / P-0), Example 2 (A / P-5), Example 3 (A / P-7), and Example 4 (A / P-10) shows that as the piezoelectric properties of the AAO / PVDF composite coating increase, the number of adhered bacteria gradually decreases, and the structure of the adhered bacteria undergoes significant deformation. Figure 7 and Figure 8 It can be seen that the A / P-10 coating has the best antibacterial performance, with an antibacterial rate of 99%. The bacteria adhering to the surface all showed obvious cytoplasmic leakage and apoptosis.

[0059] Figure 9 Electrochemical curves for aluminum substrate (Al), Comparative Example 1 (AAO), Comparative Example 3 (Al / P-10), and Example 4 (A / P-10) are shown. Comparative analysis of the polarization curves of Comparative Example 1 and the aluminum substrate indicates that anodic oxidation treatment increased the self-corrosion potential of the aluminum alloy and reduced the corrosion current. The AAO layer significantly improved the corrosion resistance of the aluminum alloy. Meanwhile, the polarization curve of Comparative Example 3 (Al / P-10) demonstrates that PVDF can isolate the aluminum alloy from corrosive media; the polarization curve at this point is a horizontal line, indicating weak electrode reactions on the sample surface. The polarization curve of Example 4 (A / P-10) further demonstrates that after PVDF seals the nanopores of AAO, the potentiodynamic polarization curve exhibits an even lower horizontal line characteristic. At this point, the current density signal has no accurate value, indicating that there are no observable electrode reactions on the surface of the AAO / PVDF composite coating. The corrosion resistance of the AAO / PVDF composite coating has reached its optimal state, and the aluminum alloy has not corroded. The interlocking spatial structure between PVDF and AAO completely inhibits the penetration of corrosive media.

[0060] Furthermore, after immersion in a 3.5% NaCl solution for 30 days, the aluminum substrate and the surface of Comparative Example 1 showed severe corrosion, and the corrosion behavior of Comparative Example 3 was also quite obvious. However, the AAO / PVDF composite coating in Example 4 still showed no obvious corrosion, indicating that the PVDF layer on the surface of the aluminum alloy alone cannot effectively isolate the aluminum alloy from the corrosive medium. Only when PVDF and AAO form an interlocking spatial structure can the aluminum alloy be protected from the corrosive medium for a long time, proving that the AAO / PVDF composite coating has long-term corrosion resistance.

[0061] The specific embodiments of the present invention have been described above. It should be understood that the present invention is not limited to the specific embodiments described above, and those skilled in the art can make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A method for preparing a long-lasting anti-corrosion and anti-fouling AAO / PVDF composite coating with an organic-inorganic intercalated spatial structure based on hard template-soft modification technology, characterized in that, Includes the following steps: S1. Anodizing treatment: The aluminum alloy substrate is anodized in an electrolyte to obtain an anodized aluminum layer, and then the hole is enlarged. S2, Vacuum solution casting: The anodic aluminum oxide layer obtained in step S1 is subjected to vacuum degassing treatment, and then PVDF solution is fully introduced into the nanopores of the anodic aluminum oxide layer under high-purity nitrogen pressure treatment for filling. After filling, PVDF curing treatment is performed. The vacuum degassing and high-purity nitrogen pressurization processes are carried out in a high-pressure tank. During vacuum degassing, the high-pressure tank is first evacuated to 0-0.1 bar and held for 1-2 minutes. Then, the PVDF solution is brought into contact with the anodic aluminum oxide layer at 0-0.1 bar and held for 10-60 minutes. After introducing high-purity nitrogen, the pressure is increased to 10... 6 -10 7 Pa, maintain for 20-60 minutes; During the curing process, first keep it at 60-80℃ for 1-3 hours, and then keep it at 110-140℃ for 3-8 hours. S3. Corona polarization treatment: The cured anodic aluminum oxide layer is subjected to corona polarization treatment to obtain an AAO / PVDF composite coating with an organic-inorganic intercalation structure and piezoelectric properties.

2. The method according to claim 1, characterized in that, In step S1, the aluminum alloy substrate must undergo pretreatment before anodizing, specifically including grinding, polishing and ultrasonic cleaning of the aluminum alloy, followed by alkaline washing and acid washing, and then electrochemical polishing in a solution containing perchloric acid to obtain an aluminum alloy substrate with a reflective mirror surface.

3. The method according to claim 2, characterized in that, The alkaline solution used for alkaline washing is a 25-40 g / L NaOH solution; the acid solution used for acid washing is a 20-25% (w / w) HNO3 solution. And / or, the electrochemical polishing is carried out in a perchloric acid / ethanol electrolyte under a DC voltage of 20-25V and a water bath condition of 0-5℃; the volume ratio of perchloric acid to ethanol in the electrolyte is 1:3-1:

5.

4. The method according to claim 1, characterized in that, In step S1, during the anodizing process, an aluminum alloy substrate is used as the anode working electrode, and an inert conductive electrode is used as the cathode. The anode aluminum alloy is treated under constant pressure for 15-60 minutes in an acidic electrolyte and a constant temperature water bath. The inert conductive electrode includes at least one of carbon plate, titanium plate, platinum sheet, and gold sheet. The acidic electrolyte includes at least one of phosphoric acid, sulfuric acid, and oxalic acid solution.

5. The method according to claim 1, characterized in that, In step S1, the solution used for the pore-expanding treatment is a phosphoric acid solution with a mass fraction of 3-5%, the temperature of the pore-expanding treatment is 40-60℃, and the time is 5-30 min.

6. The method according to claim 1, characterized in that, In step S2, the PVDF solution is prepared by dissolving PVDF powder in an organic solvent, wherein the mass fraction of PVDF in the PVDF solution is 30-70%, and the organic solvent is N,N-dimethylformamide.

7. The method according to claim 1, characterized in that, In step S3, during the corona polarization treatment, the electric field strength is 3-20 kV / cm, the voltage is 4-20 kV, the distance between the needle tip and the surface of the anodic aluminum oxide is 3-15 mm, and the treatment time is 30-60 min.

8. A long-lasting anti-corrosion and anti-fouling AAO / PVDF composite coating with an organic-inorganic intercalated spatial structure, characterized in that, It is prepared by the method described in any one of claims 1-7.

Citation Information

Patent Citations

  • A kind of method for preparing polyvinylidene fluoride nano-array porous membrane

    CN104959045B

  • Preparation method of aluminum alloy super-hydrophobic membrane with anti-corrosion, anti-fouling and self-repairing functions

    CN118773698A

  • Preparation method of piezoelectric antibacterial and antifouling film layer on surface of maritime work metal material

    CN114907729A

  • Aluminum alloy plate for outdoor building and coating process of aluminum alloy plate

    CN117822794A