Wafer integration method for improving bonding strength of gallium nitride and diamond
By etching the gallium nitride epitaxial layer and the diamond substrate to form grooves and protrusions, and performing joint bonding, the problem of insufficient bonding strength between gallium nitride and diamond substrate is solved, and a more stable bonding effect is achieved.
Patent Information
- Application Number
- CN202411905627.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-23
- Publication Date
- 2025-04-04
- Estimated Expiration
- 2044-12-23
AI Technical Summary
In the prior art, the bonding strength between gallium nitride and diamond substrate is poor, resulting in the easy fall of gallium nitride material.
By etching on the surface of the gallium nitride epitaxial layer to form grooves, etching on the surface of the diamond substrate to form protrusions, and the protrusions on the surface of the diamond substrate are interlocked with the grooves on the surface of the gallium nitride epitaxial layer for a second bonding, increasing the contact area and forming more chemical bonds.
The bonding strength between gallium nitride and diamond is significantly improved, the bonding stability is enhanced, and the fall of gallium nitride material is avoided.
Smart Images

Figure CN119764179A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductors, and in particular relates to a wafer integration method for improving the bonding strength between gallium nitride and diamond. Background Art
[0002] Gallium nitride (GaN) semiconductor materials have excellent properties such as large bandgap, high breakdown field strength, high carrier mobility, and easy formation of heterostructures. They are very suitable for the development of high-power electronic devices and high-frequency microwave devices, and play an important role in national defense science and technology, aerospace, 5G communication applications and other fields.
[0003] Since diamond has high thermal conductivity, using diamond instead of traditional substrates (sapphire, silicon carbide, silicon and other substrates) for GaN epitaxial films can improve the heat dissipation performance of GaN devices, thereby improving the service life and reliability of GaN devices.
[0004] At present, the common method for preparing gallium nitride and diamond substrates is to first peel the gallium nitride material from the original substrate, and then use wafer bonding technology to bond the gallium nitride material to the surface of the diamond substrate, so as to obtain a diamond-based gallium nitride wafer. However, when using this method, the bonding strength between the gallium nitride material and the diamond substrate is poor, which makes the gallium nitride material on the diamond substrate easy to fall off. Summary of the invention
[0005] In order to solve the above problems existing in the prior art, the present invention provides a wafer integration method for improving the bonding strength between gallium nitride and diamond. The technical problem to be solved by the present invention is achieved through the following technical solutions:
[0006] In a first aspect, the present invention provides a wafer integration method for improving the bonding strength between gallium nitride and diamond, comprising:
[0007] Step 1: providing a gallium nitride epitaxial wafer and a temporary substrate, wherein the gallium nitride epitaxial wafer includes a substrate layer and a gallium nitride epitaxial layer;
[0008] Step 2: preparing a bonding material layer, stacking the GaN epitaxial wafer, the bonding material layer and the temporary substrate in sequence and performing a first bonding to form a first bonded wafer, wherein the GaN epitaxial layer and the bonding material layer are in contact with each other;
[0009] Step 3: removing the substrate layer in the first bonded wafer to obtain a first sample;
[0010] Step 4: etching the GaN epitaxial layer in the first sample to form a groove on the surface of the GaN epitaxial layer;
[0011] Step 5: providing a diamond substrate, etching the diamond substrate to form protrusions on the surface of the diamond substrate, wherein the protrusions match the grooves;
[0012] Step 6: clamping the protrusions on the surface of the diamond substrate and the grooves on the surface of the gallium nitride epitaxial layer, and performing a second bonding on the diamond substrate and the gallium nitride epitaxial layer to obtain a second bonded wafer;
[0013] Step 7: Remove the temporary substrate and bonding material layer in the second bonded wafer to obtain a diamond-based gallium nitride wafer.
[0014] In one embodiment of the present invention, after step 1 and before step 2, the method further includes:
[0015] Cleaning GaN epitaxial wafers and temporary substrates;
[0016] The gallium nitride epitaxial wafer and the temporary substrate are first cleaned with hydrochloric acid having a mass solubility of 10% for 1 minute, and then rinsed with deionized water for 9 minutes, and finally the gallium nitride epitaxial wafer and the temporary substrate are dried.
[0017] In one embodiment of the present invention, step 2 specifically includes:
[0018] Step 201: using an electron beam evaporation process, depositing an adhesion layer and a bonding layer on the surface of the GaN epitaxial wafer and the surface of the temporary substrate in sequence, wherein the adhesion layer has a thickness of 40 nm and is made of Ti, and the bonding layer has a thickness of 400 nm and is made of Au;
[0019] Step 202: Lay the bonding layer on the surface of the GaN epitaxial wafer and the bonding layer on the surface of the temporary substrate together, clamp the GaN epitaxial wafer and the temporary substrate with a fixture and place them in a wafer bonding machine for hot pressing bonding, wherein the bonding temperature is 450° C. and the pressing time is 60 minutes.
[0020] In one embodiment of the present invention, step three specifically includes:
[0021] Step 301: attaching the bottom surface of the temporary substrate in the first bonding wafer to the UV film;
[0022] Step 302: placing the first bonded wafer into a wafer thinning machine, and thinning the substrate layer in the first bonded wafer by the wafer thinning machine, so that the thickness of the substrate layer is reduced to 100 μm;
[0023] Step 303: placing the first bonded wafer into a deep silicon etching device, and etching the substrate layer in the first bonded wafer by the deep silicon etching device to remove the substrate layer in the first bonded wafer;
[0024] Step 304: polishing the surface of the GaN epitaxial layer in the first bonded wafer to make the roughness of the surface of the GaN epitaxial layer less than 1 nm and obtain a first sample.
[0025] In one embodiment of the present invention, step 4 specifically includes:
[0026] Step 401: placing a first sample on a sample plate of a coating device, dripping photoresist at the center of the surface of the GaN epitaxial layer of the first sample, setting the rotation speed of the coating device to 4000 r / min, and setting the movement time to 30 seconds, so that the photoresist is evenly distributed on the surface of the GaN epitaxial layer;
[0027] Step 402: placing the first sample on a hot plate at 100° C. and drying for 90 seconds;
[0028] Step 403: placing the first sample in a photolithography machine, exposing the first sample for 2.3 seconds based on a first preset mask and developing for 45 seconds, so as to copy the pattern of the first preset mask onto the photoresist of the first sample;
[0029] Step 404: placing the first sample on a hot plate at 100° C. and drying for 120 seconds to cure the photoresist on the first sample;
[0030] Step 405: etching the surface of the GaN epitaxial layer in the first sample using an ICP process;
[0031] Step 406: Clean the first sample with acetone, anhydrous ethanol and deionized water in sequence to remove the remaining photoresist on the first sample, and then dry the first sample.
[0032] In one embodiment of the present invention, step five specifically includes:
[0033] Step 501: providing a diamond substrate, placing the diamond substrate on a sample plate of a coating device, dripping photoresist on the center of the surface of the diamond substrate, setting the rotation speed of the coating device to 3000 r / min, and setting the movement time to 30 seconds, so that the photoresist is evenly distributed on the surface of the diamond substrate;
[0034] Step 502: placing the diamond substrate on a hot plate at 110° C. and drying it for 70 seconds;
[0035] Step 503: placing the diamond substrate in a photolithography machine, exposing the diamond substrate for 45 seconds and developing for 60 seconds based on a second preset mask, so as to copy the pattern of the second preset mask onto the photoresist of the diamond substrate;
[0036] Step 504: etching the surface of the diamond substrate using an ICP process;
[0037] Step 505: Clean the diamond substrate with acetone, anhydrous ethanol and deionized water in sequence to remove the remaining photoresist on the diamond substrate, and then dry the diamond substrate.
[0038] In one embodiment of the present invention, the first preset mask and the second preset mask are the same mask, and one of step four and step five uses a positive resist, and the other uses a negative resist.
[0039] In one embodiment of the present invention, step six specifically includes:
[0040] Step 601: growing SiO2 on the surface of the first sample after photolithography and on the surface of the diamond substrate respectively;
[0041] Step 602: performing oxygen plasma treatment on the surface of the first sample and the surface of the diamond substrate respectively;
[0042] Step 603: rinse the first sample and the diamond substrate with RCA1 solution and deionized water in sequence and spin dry, so that the surface of the first sample and the surface of the diamond substrate have hydrophilicity;
[0043] Step 604: placing the first sample and the diamond substrate into a bonding alignment module of a photolithography machine, aligning the grooves on the surface of the gallium nitride epitaxial layer and the protrusions on the surface of the diamond substrate through a microscope, and clamping and fixing them;
[0044] Step 605: placing the first sample and the diamond substrate into a wafer bonding device for bonding, setting the bonding temperature of the wafer bonding device to 30° C., the bonding pressure to 12000 N, and the pressurization time to 5 hours;
[0045] Step 606: annealing the bonded first sample and diamond substrate at 400° C. for 1 hour to obtain a second bonded wafer.
[0046] In one embodiment of the present invention, step six includes:
[0047] Step 601: performing hydrophilic treatment on the surface of the first sample and the surface of the diamond substrate after photolithography;
[0048] Step 602: placing the diamond substrate in a NH4OH / H2O2 mixed solution and soaking it at 70°C for 10-15 minutes, placing the first sample in an HCl solution and soaking it at 70°C for 10-15 minutes, so that OH ends are generated on the surface of the diamond substrate and the surface of the gallium nitride epitaxial layer of the first sample;
[0049] Step 603: placing the first sample and the diamond substrate into a bonding alignment module of a photolithography machine, aligning the grooves on the surface of the gallium nitride epitaxial layer and the protrusions on the surface of the diamond substrate through a microscope, and clamping and fixing them;
[0050] Step 604: Place the first sample and the diamond substrate into a wafer bonding device for bonding, set the bonding temperature of the wafer bonding device to 200° C., the bonding pressure to 12000N, and the pressurizing time to 2 hours to obtain a second bonded wafer.
[0051] In one embodiment of the present invention, step seven includes:
[0052] Step 701: attaching the bottom surface of the diamond substrate in the second bonding wafer to the UV film;
[0053] Step 702: placing the second bonded wafer into a wafer thinning machine, and performing a thinning process on the temporary substrate in the second bonded wafer, so that the thickness of the temporary substrate is reduced to 100 μm;
[0054] Step 703: using a solution composed of acetic acid, nitric acid and hydrofluoric acid to corrode the temporary substrate remaining on the second bonded wafer;
[0055] Step 704: Use potassium iodide and hydrofluoric acid solution to remove the bonding material layer to obtain a diamond-based gallium nitride wafer.
[0056] In one embodiment of the present invention, a plurality of grooves are formed on the surface of the gallium nitride epitaxial layer, and the plurality of grooves are sequentially arranged along the length direction of the gallium nitride epitaxial layer;
[0057] A plurality of protrusions are formed on the surface of the diamond substrate. The plurality of protrusions are arranged in sequence along the length direction of the diamond substrate. The plurality of protrusions correspond to the plurality of grooves one by one.
[0058] Compared with the prior art, the present invention has the following beneficial effects:
[0059] In the above scheme of the present application, first, a gallium nitride epitaxial wafer and a temporary substrate are provided, and the gallium nitride epitaxial wafer includes a substrate layer and a gallium nitride epitaxial layer, so that the gallium nitride epitaxial layer can be formed by growing a gallium nitride thin film on the substrate layer. Secondly, a bonding material layer is prepared, and the gallium nitride epitaxial wafer, the bonding material layer and the temporary substrate are stacked in sequence and bonded for the first time to form a first bonded wafer. The gallium nitride epitaxial layer and the bonding material layer are in contact, so that the surface of the gallium nitride epitaxial wafer can be bonded to the temporary substrate, which facilitates the removal of the substrate layer using the temporary substrate. Afterwards, the substrate layer in the first bonded wafer is removed to obtain a first sample, so that the substrate layer is peeled off from the gallium nitride epitaxial wafer. Afterwards, the gallium nitride epitaxial layer in the first sample is etched to form a groove on the surface of the gallium nitride epitaxial layer, a diamond substrate is provided, and the diamond substrate is etched to form a protrusion on the surface of the diamond substrate, the protrusion and the groove match, the protrusion on the surface of the diamond substrate and the groove on the surface of the gallium nitride epitaxial layer are clamped, and the diamond substrate and the gallium nitride epitaxial layer are bonded for a second time to obtain a second bonded wafer. Finally, the temporary substrate and the bonding material layer in the second bonded wafer are removed to obtain a diamond-based gallium nitride wafer. Using this method, by etching a groove on the surface of the gallium nitride epitaxial layer and etching a protrusion on the surface of the diamond substrate, the contact area between the gallium nitride epitaxial layer and the diamond substrate can be increased, so that more chemical bonds can be formed between the gallium nitride epitaxial layer and the diamond substrate, thereby enhancing the bonding strength between the gallium nitride epitaxial layer and the diamond substrate. Furthermore, when the protrusion on the diamond substrate is engaged with the groove on the gallium nitride epitaxial layer, the locking structure between the protrusion and the groove can be utilized to make the bonding between the gallium nitride epitaxial layer and the diamond substrate more firm and reliable, thereby improving the stability of the bonding between the gallium nitride epitaxial layer and the diamond substrate.
[0060] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 is a schematic diagram of a wafer integration method for improving the bonding strength between gallium nitride and diamond provided by an embodiment of the present invention;
[0062] Figure 2 is a schematic diagram of a gallium nitride epitaxial wafer in an embodiment of the present invention;
[0063] Figure 3 is a schematic diagram of a temporary substrate in an embodiment of the present invention;
[0064] Figure 4 is a schematic diagram of a first bonded wafer in an embodiment of the present invention;
[0065] Figure 5 is a schematic diagram of the position of the first bonded wafer in the wafer thinning machine according to an embodiment of the present invention;
[0066] Figure 6 is a schematic diagram of the embodiment of the present invention when the substrate layer is thinned to 100 μm;
[0067] Figure 7 is a schematic diagram of a first sample in an embodiment of the present invention;
[0068] Figure 8 is a schematic diagram of etching a groove on the surface of a gallium nitride epitaxial layer in an embodiment of the present invention;
[0069] Fig. 9 is a schematic diagram of etching protrusions on the surface of a diamond substrate in an embodiment of the present invention;
[0070] Fig.10 is a schematic diagram corresponding to a gallium nitride epitaxial layer and a gallium nitride epitaxial layer in an embodiment of the present invention;
[0071] Fig.11 is a schematic diagram of a second bonded wafer provided with silicon dioxide in an embodiment of the present invention;
[0072] Fig.12 is a schematic diagram of the position of the second bonded wafer provided with silicon dioxide in a wafer thinning machine in an embodiment of the present invention;
[0073] Fig.13 is a schematic diagram of a diamond-based gallium nitride wafer provided with silicon dioxide in an embodiment of the present invention;
[0074] Fig.14 is a schematic diagram of a second bonded wafer without silicon dioxide in an embodiment of the present invention;
[0075] Fig.15 is a schematic diagram of the position of the second bonded wafer without silicon dioxide in the wafer thinning machine in an embodiment of the present invention;
[0076] Fig.16 is a schematic diagram of a GaN-on-diamond wafer without silicon dioxide in an embodiment of the present invention. DETAILED DESCRIPTION
[0077] The present invention is further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto.
[0078] See also Figures 1 to 16 , an embodiment of the present invention provides a wafer integration method for improving the bonding strength between gallium nitride and diamond, comprising:
[0079] Step 1: providing a gallium nitride epitaxial wafer and a temporary substrate, wherein the gallium nitride epitaxial wafer includes a substrate layer and a gallium nitride epitaxial layer;
[0080] Step 2: preparing a bonding material layer, stacking the GaN epitaxial wafer, the bonding material layer and the temporary substrate in sequence and performing a first bonding to form a first bonded wafer, wherein the GaN epitaxial layer and the bonding material layer are in contact with each other;
[0081] Step 3: removing the substrate layer in the first bonded wafer to obtain a first sample;
[0082] Step 4: etching the GaN epitaxial layer in the first sample to form a groove on the surface of the GaN epitaxial layer;
[0083] Step 5: providing a diamond substrate, etching the diamond substrate to form protrusions on the surface of the diamond substrate, wherein the protrusions match the grooves;
[0084] Step 6: clamping the protrusions on the surface of the diamond substrate and the grooves on the surface of the gallium nitride epitaxial layer, and performing a second bonding on the diamond substrate and the gallium nitride epitaxial layer to obtain a second bonded wafer;
[0085] Step 7: Remove the temporary substrate and bonding material layer in the second bonded wafer to obtain a diamond-based gallium nitride wafer.
[0086] In some embodiments of the present application, the gallium nitride epitaxial wafer includes but is not limited to a silicon-based gallium nitride epitaxial wafer, a sapphire-based gallium nitride epitaxial wafer, and a silicon carbide-based gallium nitride epitaxial wafer.
[0087] In some embodiments of the present application, the substrate layer is a silicon substrate.
[0088] In some embodiments of the present application, the temporary substrate includes but is not limited to a silicon wafer, a sapphire wafer, a silicon carbide wafer, etc. The temporary substrate in this embodiment is a silicon substrate.
[0089] In some embodiments of the present application, the temporary bonding layer material may be a dielectric, various layers of metal, or bonding glue.
[0090] In some embodiments of the present application, the method for removing the substrate layer on the gallium nitride epitaxial wafer may be mechanical grinding, dry etching or laser removal.
[0091] In some embodiments of the present application, the size of the gallium nitride epitaxial wafer is equal to the size of the temporary substrate.
[0092] In some embodiments of the present application, the groove may be a rectangular groove opening toward the diamond substrate, and the protrusion may be a rectangular protrusion protruding toward the gallium nitride epitaxial layer.
[0093] In the above scheme of the present application, first, a gallium nitride epitaxial wafer and a temporary substrate are provided, and the gallium nitride epitaxial wafer includes a substrate layer and a gallium nitride epitaxial layer, so that the gallium nitride epitaxial layer can be formed by growing a gallium nitride thin film on the substrate layer. Secondly, a bonding material layer is prepared, and the gallium nitride epitaxial wafer, the bonding material layer and the temporary substrate are stacked in sequence and bonded for the first time to form a first bonded wafer. The gallium nitride epitaxial layer and the bonding material layer are in contact, so that the surface of the gallium nitride epitaxial wafer can be bonded to the temporary substrate, which facilitates the removal of the substrate layer using the temporary substrate. Afterwards, the substrate layer in the first bonded wafer is removed to obtain a first sample, so that the substrate layer is peeled off from the gallium nitride epitaxial wafer. Afterwards, the gallium nitride epitaxial layer in the first sample is etched to form a groove on the surface of the gallium nitride epitaxial layer, a diamond substrate is provided, and the diamond substrate is etched to form a protrusion on the surface of the diamond substrate, the protrusion and the groove match, the protrusion on the surface of the diamond substrate and the groove on the surface of the gallium nitride epitaxial layer are clamped, and the diamond substrate and the gallium nitride epitaxial layer are bonded for a second time to obtain a second bonded wafer. Finally, the temporary substrate and the bonding material layer in the second bonded wafer are removed to obtain a diamond-based gallium nitride wafer. Using this method, by etching a groove on the surface of the gallium nitride epitaxial layer and etching a protrusion on the surface of the diamond substrate, the contact area between the gallium nitride epitaxial layer and the diamond substrate can be increased, so that more chemical bonds can be formed between the gallium nitride epitaxial layer and the diamond substrate, thereby enhancing the bonding strength between the gallium nitride epitaxial layer and the diamond substrate. Furthermore, when the protrusions on the diamond substrate are snapped into the grooves on the gallium nitride epitaxial layer, the locking structure between the protrusions and the grooves can be used to make the bonding between the gallium nitride epitaxial layer and the diamond substrate more secure and reliable, thereby improving the stability of the bonding between the gallium nitride epitaxial layer and the diamond substrate. Among them, the corresponding patterns of the concave and convex formed on the surfaces of the gallium nitride and diamond substrate after photolithography are similar to the mortise and tenon structure in architecture, that is, the protruding part is the tenon, and the concave part is the mortise. When the wafers are bonded, the tenons and mortise are inlaid, bitten, squeezed, and rubbed against each other, so that the gallium nitride and the diamond substrate are tightly connected together, the surfaces of the two are closely fitted, the intermolecular force is enhanced, and then a strong binding force is generated, so that a firm connection is achieved, which is difficult to separate easily, making the bonding between the gallium nitride and the diamond substrate more secure and reliable, and more stable.
[0094] In some embodiments of the present application, after step 1 and before step 2, the following steps are further included:
[0095] Cleaning GaN epitaxial wafers and temporary substrates;
[0096] Among them, the gallium nitride epitaxial wafer and the temporary substrate are first cleaned with hydrochloric acid with a mass solubility of 10% for 1 minute, and then the gallium nitride epitaxial wafer and the temporary substrate are rinsed with deionized water for 9 minutes, and finally the gallium nitride epitaxial wafer and the temporary substrate are dried. In this method, the gallium nitride epitaxial wafer and the temporary substrate can be fully cleaned before bonding the gallium nitride epitaxial wafer and the temporary substrate, thereby improving the cleanliness of the gallium nitride epitaxial wafer and the temporary substrate during bonding, thereby achieving a better bonding effect between the gallium nitride epitaxial wafer and the temporary substrate.
[0097] In some embodiments of the present application, the gallium nitride epitaxial wafer and the temporary substrate may be placed in a spin dryer for spin drying. The spin drying time may be 13 minutes to ensure the dryness of the gallium nitride epitaxial wafer and the temporary substrate.
[0098] In some embodiments of the present application, Figure 2 , Figure 3 and Figure 4 As shown, step 2 specifically includes:
[0099] Step 201: using an electron beam evaporation process, depositing an adhesion layer and a bonding layer on the surface of the GaN epitaxial wafer and the surface of the temporary substrate in sequence, wherein the adhesion layer has a thickness of 40 nm and is made of Ti (titanium), and the bonding layer has a thickness of 400 nm and is made of Au (gold);
[0100] Step 202: The bonding layer on the surface of the GaN epitaxial wafer is laminated with the bonding layer on the surface of the temporary substrate, and the GaN epitaxial wafer and the temporary substrate are clamped by a fixture and placed in a wafer bonding machine for hot pressing bonding, wherein the bonding temperature is 450° C. and the pressing time is 60 minutes. This method can improve the reliability of the bonding between the GaN epitaxial layer and the temporary substrate.
[0101] In some embodiments of the present application, a gallium nitride epitaxial wafer and a temporary substrate are clamped with a fixture and placed in a wafer bonding machine for hot pressing bonding for 60 minutes, and then the pressure is removed and the temperature is lowered. After the temperature slowly drops to room temperature, the bonded first bonded wafer is taken out.
[0102] In some embodiments of the present application, Figure 5 , Figure 6 and Figure 7 As shown, step three specifically includes:
[0103] Step 301: attaching the bottom surface of the temporary substrate in the first bonding wafer to the UV film;
[0104] Step 302: placing the first bonded wafer into a wafer thinning machine, and thinning the substrate layer in the first bonded wafer by the wafer thinning machine, so that the thickness of the substrate layer is reduced to 100 μm;
[0105] Step 303: placing the first bonded wafer into a deep silicon etching device, and etching the substrate layer in the first bonded wafer by the deep silicon etching device to remove the substrate layer in the first bonded wafer;
[0106] Step 304: Polishing the surface of the GaN epitaxial layer in the first bonded wafer to make the surface roughness of the GaN epitaxial layer less than 1 nm and obtain a first sample. In this method, by first thinning the substrate layer, then etching and removing the substrate layer, and finally polishing the surface of the GaN epitaxial layer in the first bonded wafer, the substrate layer in the GaN epitaxial wafer can be fully removed, the effect of subsequent bonding is improved, and it is more convenient to remove the substrate layer.
[0107] In some embodiments of the present application, Figure 8 As shown, step four specifically includes:
[0108] Step 401: placing a first sample on a sample plate of a coating device, dripping photoresist at the center of the surface of the GaN epitaxial layer of the first sample, setting the rotation speed of the coating device to 4000 r / min, and setting the movement time to 30 seconds, so that the photoresist is evenly distributed on the surface of the GaN epitaxial layer;
[0109] Step 402: placing the first sample on a hot plate at 100° C. and drying for 90 seconds;
[0110] Step 403: placing the first sample in a photolithography machine, exposing the first sample for 2.3 seconds based on a first preset mask and developing for 45 seconds, so as to copy the pattern of the first preset mask onto the photoresist of the first sample;
[0111] Step 404: placing the first sample on a hot plate at 100° C. and drying for 120 seconds to cure the photoresist on the first sample;
[0112] Step 405: etching the surface of the GaN epitaxial layer in the first sample using an ICP process;
[0113] Step 406: sequentially clean the first sample with acetone, anhydrous ethanol and deionized water to remove the remaining photoresist on the first sample, and then dry the first sample. In this way, a groove can be formed on the surface of the gallium nitride epitaxial layer of the first sample by etching using a photolithography process.
[0114] In some embodiments of the present application, the model of the photoresist may be AZ6130.
[0115] In some embodiments of the present application, when developing the first sample, the first sample can be placed in a developer for development.
[0116] In some embodiments of the present application, the ICP process (Inductively Coupled Plasma) is mainly used in integrated circuit packaging and semiconductor manufacturing. The main purpose of the ICP process is to protect the chip, provide electrical connections and heat dissipation functions, and ensure the reliability, stability and performance of the chip. ICP etching technology is inductively coupled plasma etching, and its working principle is to ionize the working gas through a high-frequency electromagnetic field to form a plasma. These plasmas induce current under the action of the magnetic field, generate heat and reach a high temperature state. Under vacuum and low pressure, these plasmas bombard the surface of the substrate, break the chemical bonds of the substrate material, generate volatile substances and are extracted. ICP etching technology has the advantages of fast etching rate, high selectivity, high anisotropy, and small etching damage, and is widely used in the etching of materials such as silicon, silicon dioxide, III-V compounds, and metals.
[0117] In some embodiments of the present application, Fig. 9 As shown, step five specifically includes:
[0118] Step 501: providing a diamond substrate, placing the diamond substrate on a sample plate of a coating device, dripping photoresist on the center of the surface of the diamond substrate, setting the rotation speed of the coating device to 3000 r / min, and setting the movement time to 30 seconds, so that the photoresist is evenly distributed on the surface of the diamond substrate;
[0119] Step 502: placing the diamond substrate on a hot plate at 110° C. and drying it for 70 seconds;
[0120] Step 503: placing the diamond substrate in a photolithography machine, exposing the diamond substrate for 45 seconds and developing for 60 seconds based on a second preset mask, so as to copy the pattern of the second preset mask onto the photoresist of the diamond substrate;
[0121] Step 504: etching the surface of the diamond substrate using an ICP process;
[0122] Step 505: Use acetone, anhydrous ethanol and deionized water to clean the diamond substrate in sequence to remove the remaining photoresist on the diamond substrate, and then dry the diamond substrate. In this way, a protrusion can be formed on the surface of the diamond substrate by etching using a photolithography process.
[0123] In some embodiments of the present application, the model of the photoresist may be AZ6130.
[0124] In some embodiments of the present application, when developing the diamond substrate, the diamond substrate may be placed in a developer for development.
[0125] In some embodiments of the present application, the first preset mask and the second preset mask are the same mask, and one of step 4 and step 5 uses a positive resist and the other uses a negative resist. By adopting this method, the size of the groove on the surface of the gallium nitride epitaxial layer and the protrusion on the surface of the diamond substrate can be equal and correspond to each other, which facilitates the engagement of the protrusion and the groove, improves the stability and fit of the engagement of the protrusion and the groove, and thus improves the subsequent bonding effect between the gallium nitride epitaxial layer and the diamond substrate.
[0126] In an alternative approach, Fig.10 , Fig.11 , Fig.12 and Fig.13 As shown, step six specifically includes:
[0127] Step 601: growing SiO2 on the surface of the first sample after photolithography and on the surface of the diamond substrate respectively;
[0128] Step 602: performing oxygen plasma treatment on the surface of the first sample and the surface of the diamond substrate respectively;
[0129] Step 603: rinse the first sample and the diamond substrate with RCA1 solution and deionized water in sequence and spin dry, so that the surface of the first sample and the surface of the diamond substrate have hydrophilicity;
[0130] Step 604: placing the first sample and the diamond substrate into a bonding alignment module of an MA6 lithography machine, and aligning the grooves on the surface of the gallium nitride epitaxial layer and the protrusions on the surface of the diamond substrate through a microscope and clamping and fixing them;
[0131] Step 605: placing the first sample and the diamond substrate into a wafer bonding device for bonding, setting the bonding temperature of the wafer bonding device to 30° C., the bonding pressure to 12000 N, and the pressurization time to 5 hours;
[0132] Step 606: anneal the bonded first sample and diamond substrate at 400° C. for 1 hour to obtain a second bonded wafer. This method can improve the strength and reliability of the bond between the GaN epitaxial layer and the diamond substrate, and prevent the GaN epitaxial layer from falling off the diamond substrate.
[0133] In some embodiments of the present application, the first sample after photolithography and the diamond substrate can be placed in a PE CVD device to grow SiO2 (silicon dioxide). PECVD equipment (Plasma Enhanced Chemical Vapor Deposition) is a device that uses plasma technology to promote chemical reactions and is mainly used to deposit high-quality thin film materials on the surface of a substrate. PECVD equipment has the characteristics of high deposition rate, high uniformity and high adhesion, and can prepare high-quality and high-performance thin film materials.
[0134] In some embodiments of the present application, RIE equipment can be used to perform oxygen plasma treatment on the first sample and diamond substrate after the growth of SiO2. RIE (Reactive Ion Etching) equipment is a dry etching equipment. Its working principle is to generate plasma between electrodes by using radio frequency power in a vacuum environment. The active ions in the plasma are accelerated to bombard the sample surface under the action of the electric field, and chemically react with the sample material to generate volatile products that are pumped away by the vacuum pump, thereby achieving material etching.
[0135] In some embodiments of the present application, RCA1 solution is a cleaning solution used in semiconductor manufacturing, mainly used to remove organic pollutants and particles on silicon wafers. RCA1 solution is composed of three chemical substances: ammonium hydroxide, hydrogen peroxide and deionized water, with a ratio of 1:1:51.
[0136] In another alternative, if Fig.10 , Fig.14 , Fig.15 and Fig.16 As shown, step six includes:
[0137] Step 601: performing hydrophilic treatment on the surface of the first sample and the surface of the diamond substrate after photolithography;
[0138] Step 602: placing the diamond substrate in a NH4OH / H2O2 mixed solution and soaking it at 70°C for 10-15 minutes, placing the first sample in an HCl solution and soaking it at 70°C for 10-15 minutes, so that OH ends are generated on the surface of the diamond substrate and the surface of the gallium nitride epitaxial layer of the first sample;
[0139] Step 603: placing the first sample and the diamond substrate into a bonding alignment module of a photolithography machine, aligning the grooves on the surface of the gallium nitride epitaxial layer and the protrusions on the surface of the diamond substrate through a microscope, and clamping and fixing them;
[0140] Step 604: Place the first sample and the diamond substrate in a wafer bonding device for bonding, set the bonding temperature of the wafer bonding device to 200°C, the bonding pressure to 12000N, and the pressing time to 2 hours to obtain a second bonded wafer. This method can improve the strength and reliability of the bonding between the GaN epitaxial layer and the diamond substrate, and prevent the GaN epitaxial layer from falling off the diamond substrate.
[0141] In some embodiments of the present application, Fig.12 , Fig.13 , Fig.15 and Fig.16 As shown, step seven includes:
[0142] Step 701: attaching the bottom surface of the diamond substrate in the second bonding wafer to the UV film;
[0143] Step 702: placing the second bonded wafer into a wafer thinning machine, and performing a thinning process on the temporary substrate in the second bonded wafer, so that the thickness of the temporary substrate is reduced to 100 μm;
[0144] Step 703: using a solution composed of acetic acid, nitric acid and hydrofluoric acid to corrode the temporary substrate remaining on the second bonded wafer;
[0145] Step 704: Use potassium iodide and hydrofluoric acid solution to remove the bonding material layer to obtain a diamond-based gallium nitride wafer. Using this method, the temporary substrate and the bonding material layer on the second bonded wafer can be removed to obtain the required diamond-based gallium nitride wafer.
[0146] In some embodiments of the present application, when the bonding material layer is removed using potassium iodide and hydrofluoric acid solution, Au (gold) and Ti (titanium) in the bonding material layer can be removed.
[0147] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0148] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0149] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.
Claims
1. A wafer integration method for improving the bonding strength between gallium nitride and diamond, characterized in that: include: Step 1: providing a gallium nitride epitaxial wafer and a temporary substrate, wherein the gallium nitride epitaxial wafer comprises a substrate layer and a gallium nitride epitaxial layer; Step 2: preparing a bonding material layer, stacking the GaN epitaxial wafer, the bonding material layer and the temporary substrate in sequence and performing a first bonding to form a first bonded wafer, wherein the GaN epitaxial layer is in contact with the bonding material layer; Step 3: removing the substrate layer in the first bonded wafer to obtain a first sample; Step 4: etching the gallium nitride epitaxial layer in the first sample to form a groove on the surface of the gallium nitride epitaxial layer; Step 5: providing a diamond substrate, etching the diamond substrate to form a protrusion on the surface of the diamond substrate, wherein the protrusion matches the groove; Step 6: clamping the protrusions on the surface of the diamond substrate and the grooves on the surface of the gallium nitride epitaxial layer, and performing a second bonding on the diamond substrate and the gallium nitride epitaxial layer to obtain a second bonded wafer; Step seven: removing the temporary substrate and the bonding material layer in the second bonded wafer to obtain a diamond-based gallium nitride wafer.
2. The wafer integration method for improving the bonding strength between gallium nitride and diamond according to claim 1, characterized in that: After step 1 and before step 2, the following steps are also included: Cleaning the gallium nitride epitaxial wafer and the temporary substrate; The gallium nitride epitaxial wafer and the temporary substrate are first cleaned with hydrochloric acid having a mass solubility of 10% for 1 minute, and then rinsed with deionized water for 9 minutes, and finally the gallium nitride epitaxial wafer and the temporary substrate are dried.
3. The wafer integration method for improving the bonding strength between gallium nitride and diamond according to claim 1, characterized in that: The step 2 specifically includes: Step 201: using an electron beam evaporation process, depositing an adhesion layer and a bonding layer on the surface of the gallium nitride epitaxial wafer and the surface of the temporary substrate in sequence, wherein the adhesion layer has a thickness of 40 nm and is made of Ti, and the bonding layer has a thickness of 400 nm and is made of Au; Step 202: Lay the bonding layer on the surface of the GaN epitaxial wafer and the bonding layer on the surface of the temporary substrate together, clamp the GaN epitaxial wafer and the temporary substrate with a clamp and place them in a wafer bonding machine for hot pressing bonding, wherein the bonding temperature is 450° C. and the pressing time is 60 minutes.
4. The wafer integration method for improving the bonding strength between gallium nitride and diamond according to claim 1, characterized in that: The step three specifically includes: Step 301: attaching the bottom surface of the temporary substrate in the first bonding wafer to a UV film; Step 302: placing the first bonded wafer into a wafer thinning machine, and thinning the substrate layer in the first bonded wafer by the wafer thinning machine, so that the thickness of the substrate layer is reduced to 100 μm; Step 303: placing the first bonded wafer into a deep silicon etching device, and etching the substrate layer in the first bonded wafer by the deep silicon etching device to remove the substrate layer in the first bonded wafer; Step 304: polishing the surface of the gallium nitride epitaxial layer in the first bonded wafer to make the roughness of the surface of the gallium nitride epitaxial layer less than 1 nm and obtain a first sample.
5. The wafer integration method for improving the bonding strength between gallium nitride and diamond according to claim 1, characterized in that: The step 4 specifically includes: Step 401: placing the first sample on a sample plate of a coating device, dripping photoresist at the center of the surface of the GaN epitaxial layer of the first sample, setting the rotation speed of the coating device to 4000 r / min and the movement time to 30 seconds, so that the photoresist is evenly distributed on the surface of the GaN epitaxial layer; Step 402: placing the first sample on a hot plate at 100° C. and drying for 90 seconds; Step 403: placing the first sample in a photolithography machine, exposing the first sample for 2.3 seconds based on a first preset mask and developing the first sample for 45 seconds, so as to copy the pattern of the first preset mask onto the photoresist of the first sample; Step 404: placing the first sample on a hot plate at 100° C. and drying for 120 seconds to cure the photoresist on the first sample; Step 405: etching the surface of the gallium nitride epitaxial layer in the first sample using an ICP process; Step 406: Clean the first sample with acetone, anhydrous ethanol and deionized water in sequence to remove the remaining photoresist on the first sample, and then dry the first sample.
6. The wafer integration method for improving the bonding strength between gallium nitride and diamond according to claim 5, characterized in that: The step five specifically includes: Step 501: providing a diamond substrate, placing the diamond substrate on a sample plate of a coating device, dripping photoresist at the center of the surface of the diamond substrate, setting the rotation speed of the coating device to 3000 r / min, and the movement time to 30 seconds, so that the photoresist is evenly distributed on the surface of the diamond substrate; Step 502: placing the diamond substrate on a hot plate at 110° C. and drying for 70 seconds; Step 503: placing the diamond substrate in a photolithography machine, exposing the diamond substrate for 45 seconds and developing for 60 seconds based on a second preset mask, so as to copy the pattern of the second preset mask onto the photoresist of the diamond substrate; Step 504: etching the surface of the diamond substrate using an ICP process; Step 505: Clean the diamond substrate with acetone, anhydrous ethanol and deionized water in sequence to remove the remaining photoresist on the diamond substrate, and then dry the diamond substrate.
7. The wafer integration method for improving the bonding strength between gallium nitride and diamond according to claim 6, characterized in that: The first preset mask and the second preset mask are the same mask, and one of the step four and the step five uses a positive resist, and the other uses a negative resist.
8. The wafer integration method for improving the bonding strength between gallium nitride and diamond according to claim 1, characterized in that: The step six specifically includes: Step 601: growing SiO2 on the surface of the first sample and the surface of the diamond substrate after photolithography respectively; Step 602: performing oxygen plasma treatment on the surface of the first sample and the surface of the diamond substrate respectively; Step 603: washing the first sample and the diamond substrate with RCA1 solution and deionized water in sequence and drying them, so that the surface of the first sample and the surface of the diamond substrate have hydrophilicity; Step 604: placing the first sample and the diamond substrate into a bonding alignment module of a photolithography machine, and aligning the grooves on the surface of the gallium nitride epitaxial layer and the protrusions on the surface of the diamond substrate through a microscope and clamping and fixing them; Step 605: placing the first sample and the diamond substrate into a wafer bonding device for bonding, setting the bonding temperature of the wafer bonding device to 30° C., the bonding pressure to 12000 N, and the pressurization time to 5 hours; Step 606: annealing the bonded first sample and the diamond substrate at 400° C. for 1 hour to obtain a second bonded wafer.
9. The wafer integration method for improving the bonding strength between gallium nitride and diamond according to claim 1, characterized in that: The step six comprises: Step 601: performing hydrophilic treatment on the surface of the first sample and the surface of the diamond substrate after photolithography; Step 602: placing the diamond substrate in a NH4OH / H2O2 mixed solution and soaking it at 70°C for 10-15 minutes, placing the first sample in an HCl solution and soaking it at 70°C for 10-15 minutes, so that OH ends are generated on the surface of the diamond substrate and the surface of the gallium nitride epitaxial layer of the first sample; Step 603: placing the first sample and the diamond substrate into a bonding alignment module of a photolithography machine, aligning the grooves on the surface of the gallium nitride epitaxial layer and the protrusions on the surface of the diamond substrate through a microscope, and clamping and fixing them; Step 604: Place the first sample and the diamond substrate into a wafer bonding device for bonding, set the bonding temperature of the wafer bonding device to 200° C., the bonding pressure to 12000 N, and the pressurizing time to 2 hours to obtain a second bonded wafer.
10. The wafer integration method for improving the bonding strength between gallium nitride and diamond according to claim 1, characterized in that: The step seven comprises: Step 701: attaching the bottom surface of the diamond substrate in the second bonded wafer to a UV film; Step 702: placing the second bonded wafer into a wafer thinning machine, and performing a thinning process on the temporary substrate in the second bonded wafer, so that the thickness of the temporary substrate is reduced to 100 μm; Step 703: using a solution composed of acetic acid, nitric acid and hydrofluoric acid to corrode the temporary substrate remaining on the second bonded wafer; Step 704: Use potassium iodide and hydrofluoric acid solution to remove the bonding material layer to obtain a diamond-based gallium nitride wafer.
Citation Information
Patent Citations
Method utilizing thermal stress chemical corrosion method to separate sapphire from gallium nitride base epitaxial layer
CN102709415A
GaN high-electron-mobility device based on SOI-structured diamond composite substrate, and manufacturing method thereof
CN107731903A
Direct bonding method for gallium nitride / diamond
CN108597993A
Method of integrating diamond and gallium nitride
CN110838438A
Diamond-based gallium nitride composite wafer and bonding preparation method thereof
CN111900200A
Cited By
GaN epitaxial wafer and preparation method thereof
CN121218666A
Bonding structure and method of large-size single crystal GaN wafer and single crystal diamond
CN121473007A