A dual-target demulsifier, its preparation method and application

A dual-target demulsifier, prepared by crosslinking polystyrene maleic anhydride with hydrophilic nanomaterials and polyether, solves the problems of difficult oil-water separation and sludge formation in binary composite flooding produced fluid, achieving simultaneous demulsification and expanding its application range.

CN119798905BActive Publication Date: 2026-11-10CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311305351.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-10
Publication Date
2026-11-10
Estimated Expiration
2043-10-10

AI Technical Summary

Technical Problem

Existing demulsifiers have problems such as difficulty in oil-water separation, oil sludge generation, complex processing procedures, and narrow application range when treating produced fluids from binary composite flooding. In particular, it is difficult to achieve simultaneous treatment of water-in-oil and oil-in-water emulsions.

Method used

A dual-targeting demulsifier was prepared by crosslinking polystyrene maleic anhydride with hydrophilic nanomaterials and polyether. By utilizing the surface effect of nanomaterials and the compatibility of benzene rings, it can simultaneously break down oil-in-water and water-in-oil emulsions, avoiding reactions with negatively charged substances in wastewater.

Benefits of technology

It achieves simultaneous crude oil dehydration and wastewater oil removal, avoids sludge formation, simplifies the treatment process, and expands the application range of demulsifiers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119798905B_ABST
    Figure CN119798905B_ABST
Patent Text Reader

Abstract

This invention discloses a dual-targeting demulsifier, which is formed by crosslinking the anhydride groups of polystyrene maleic anhydride with hydrophilic nanomaterials and polyethers, respectively. The dual-targeting demulsifier is composed of structural unit A from polystyrene maleic anhydride, structural unit B from hydrophilic nanomaterials, and structural unit C from polyethers. Based on the total mass of the dual-targeting demulsifier, the content of structural unit A is 10-62.5% by weight, the content of structural unit B is 7.1-25% by weight, and the content of structural unit C is 25-80% by weight. This invention also discloses the preparation method and application of the above-mentioned dual-targeting demulsifier. The dual-targeting demulsifier disclosed in this invention, under the synergistic effect of nanomaterials and a large number of styrene groups, has the function of simultaneously achieving crude oil dehydration and wastewater oil removal. Because the demulsifier molecule does not contain cations, it will not react with negatively charged substances in wastewater for binary flooding produced fluids, thus avoiding the generation of aged oil and sludge.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of oilfield chemistry, specifically to a dual-targeting demulsifier, its preparation method, and its application. Background Technology

[0002] Binary composite flooding refers to a tertiary oil recovery technology that uses a mixture of surfactants and polymers as the oil displacement agent. It can significantly improve crude oil recovery rate on the basis of water flooding and plays an important role in maintaining stable production in the middle and late stages of my country's oilfields.

[0003] The binary composite oil displacement process generates a large amount of produced fluid with complex composition and stable properties, exhibiting complex emulsion types and a high degree of emulsification. This is because residual polymers in the produced fluid increase the viscosity of the produced water, while the returned surfactants and active components such as gums and asphaltenes in the crude oil cause severe oil-water emulsification, making oil-water separation difficult. Therefore, it is necessary to add functional agents that break up oil-water emulsions—demulsifiers and reverse demulsifiers—to the produced fluid to achieve rapid oil-water separation. The process can be roughly divided into two steps: crude oil dehydration and wastewater oil removal. Specifically, demulsifiers break down crude oil emulsions that are mainly composed of water in oil, and reverse demulsifiers break down oily wastewater emulsions that are mainly composed of oil in water.

[0004] Oil-soluble polyether demulsifiers are commonly used to demulsify and dehydrate water-in-oil crude oil emulsions. For treating oily wastewater, cationic reverse demulsifiers (cleaning agents) and flocculants are added. The emulsified crude oil, negatively charged suspended solids, and other particles are removed through a charge neutralization reaction-flocculation method. However, this charge neutralization reaction and flocculation technology is non-selective towards negatively charged substances and particles in wastewater. It reacts not only with negatively charged emulsified oil but also with suspended solids and residual oil-displacing polymers, forming aggregated flocs containing crude oil and solid particles—i.e., oil sludge. The formation of oil sludge severely impacts normal oilfield production, causing pipeline blockages, filter malfunctions, and environmental pollution. Therefore, there is an urgent need to develop nonionic reverse demulsifiers to overcome the aforementioned shortcomings of cationic reverse demulsifiers; however, the results have not been ideal. Meanwhile, adding demulsifiers and reverse demulsifiers separately to the produced fluid means that at least two spaced dosing ports must be set up in the oil-water treatment process for these two functional agents, increasing the complexity of the treatment process and management points. Therefore, the development of dual-function oil-water treatment agents, especially non-ionic agents, that can simultaneously achieve crude oil dehydration and wastewater oil removal, i.e., simultaneously break down water-in-oil emulsions and oil-in-water emulsions, is an inevitable trend.

[0005] With the development of demulsifier and reverse demulsifier technologies, nano-demulsifiers have attracted attention due to the unique role of nanoparticles at the oil-water interface. For example, Chinese patent application CN106219669A discloses a method for preparing a magnetic graphene oxide demulsifier, which uses magnetic iron powder as a carrier to load graphene oxide on its surface. Its key feature is its reusability; however, the actual oil-water treatment industry is large-scale, and the amount of adsorbent material required for recycling the magnetic graphene oxide demulsifier is large, requiring considerable space and making industrial application difficult. Chinese patent CN 109054888 B discloses a demulsifier and its preparation method. This method includes: preparing hydroxylated carbon nanotubes; and in-situ grafting nano-silica onto the hydroxylated carbon nanotubes to obtain a carbon nanotube / nano-SiO2 composite nano-demulsifier. This invention also provides a demulsifier obtained by the above preparation method. However, the application scope of the above technical solutions is relatively narrow, targeting O / W crude oil emulsions with an oil content of 5%-10%. Chinese patent CN 110559691 B discloses a reusable carbon-based nano-demulsifier and its preparation method. The preparation method includes: reacting carbon nanotubes with a mixed acid solution to obtain carbon oxide nanotubes with hydroxyl and carboxyl groups on their surface; grafting nano-TiO2 generated from the hydrolysis of an organotitanium precursor onto the surface of the carbon oxide nanotubes to obtain the reusable carbon-based nano-demulsifier. This invention also discloses the demulsifier obtained by the above preparation method. However, the application scope of the above technical solution is still relatively narrow, only suitable for oily wastewater with an oil content of 1%. For nano-demulsifiers, their application scope still needs to be expanded, especially for demulsifying water-in-oil emulsions, and even for the simultaneous treatment of water-in-oil and oil-in-water emulsions. Summary of the Invention

[0006] Objective of the Invention: To address the shortcomings of existing technologies, the objective of this invention is to provide a dual-targeted demulsifier for binary flooding produced fluid treatment and its preparation method. A demulsifier bifunctionalized with both nanomaterials and polyether is obtained by crosslinking a hydrophilic nanomaterial (HNM, referred to as HNM in this application) with polystyrene maleic anhydride (SMA).

[0007] The polyether in the demulsifier's molecular structure is itself a highly efficient demulsifier, and after cross-linking with SMA, the molecular weight of the demulsifier is further increased.

[0008] The cross-linked nanomaterials in SMA are hydrophilic nanomaterials, which endow the demulsifier with excellent surface effects, small size effects and macroscopic quantum tunneling effects, thereby enhancing the demulsification effect of the dual-target demulsifier.

[0009] The large number of benzene rings in SMA endows this dual-target demulsifier with good compatibility with crude oil. Under the synergistic effect of hydrophilic nanomaterials and a large number of styrene groups, this dual-target demulsifier can simultaneously achieve crude oil dehydration and wastewater oil removal. Moreover, because the demulsifier molecule does not contain cations, it will not react with negatively charged substances in wastewater for binary flooding produced fluid, thus avoiding the generation of aged oil and sludge.

[0010] Technical solution: A dual-targeting demulsifier, comprising crosslinking the anhydride groups of polystyrene maleic anhydride with hydrophilic nanomaterials and polyether, wherein:

[0011] The dual-targeting demulsifier is composed of structural unit A derived from polystyrene maleic anhydride, structural unit B derived from hydrophilic nanomaterials, and structural unit C derived from polyether.

[0012] Based on the total mass of the dual-target demulsifier, the content of structural unit A is 10-62.5% by weight, the content of structural unit B is 7.1-25% by weight, and the content of structural unit C is 25-80% by weight.

[0013] A method for preparing the above-mentioned dual-target demulsifier, by weight, includes the following steps:

[0014] (1) 100 parts of hydrophilic nanomaterials were reacted with dopamine hydrochloride or tannic acid or silane coupling agent respectively to obtain polydopamine modified nanomaterials or tannic acid modified nanomaterials or silane coupling agent modified nanomaterials.

[0015] (2) Disperse polydopamine-modified nanomaterials, tannic acid-modified nanomaterials, or silane coupling agent-modified nanomaterials in solvent C, and react with 100-500 parts of polystyrene maleic anhydride to obtain nanomaterials grafted with polystyrene maleic anhydride.

[0016] (3) The nanomaterial grafted polystyrene maleic anhydride is dispersed in solvent C and reacted with 200-800 parts of polyether. After the reaction is completed, a dual-targeting demulsifier is obtained.

[0017] Furthermore, when the product of step (1) is a polydopamine-modified nanomaterial, the specific steps are as follows:

[0018] (11) Take appropriate amounts of dopamine hydrochloride and 100 parts of hydrophilic nanomaterials into a reaction vessel, respectively, wherein:

[0019] The mass ratio of dopamine hydrochloride to hydrophilic nanomaterials is (0.1-10):10;

[0020] (12) Add an appropriate amount of Tris-HCl buffer to the reaction vessel, seal it, and sonicate it in an ultrasonic oscillator to disperse the hydrophilic nanomaterials for at least 0.5 h to obtain a mixture, wherein:

[0021] The amount of the Tris-HCl buffer solution used is 2-20 times the mass of the hydrophilic nanomaterial;

[0022] (13) Transfer the mixture obtained in step (12) to a shaker and shake at room temperature for at least 4 hours to obtain a reaction solution;

[0023] (14) Centrifuge the reaction solution obtained in step (13), then wash it with ultrapure water and anhydrous ethanol at least 3 times in sequence, and vacuum dry it at 30-60℃ for at least 12 hours. After completion, polydopamine modified nanomaterials are obtained.

[0024] Furthermore, in step (13), the mixture obtained in step (12) is transferred to a shaker and shaken at a frequency of 100-300 rpm for 4-24 hours at room temperature.

[0025] Furthermore, when the product of step (1) is tannic acid-modified nanomaterial, the specific steps, by mass, are as follows:

[0026] S11. Take an appropriate amount of tannic acid and 100 parts of hydrophilic nanomaterials into a reaction vessel, wherein:

[0027] The mass ratio of the tannic acid to the hydrophilic nanomaterial is (0.1-10):10;

[0028] S12. Add solvent A to the reaction vessel, seal it, and sonicate it in an ultrasonic oscillator to disperse the hydrophilic nanomaterials for at least 2 hours to obtain a mixture, wherein:

[0029] The amount of solvent A added is 2-20 times the mass of the hydrophilic nanomaterial;

[0030] S13. Transfer the mixture obtained in step S12 to a shaker and shake at room temperature for at least 4 hours to obtain a reaction solution;

[0031] S14. The reaction solution obtained in step S13 is centrifuged and washed with ultrapure water and anhydrous ethanol at least 3 times in sequence. After vacuum drying at 30-60℃ for at least 12 hours, tannic acid modified nanomaterials are obtained.

[0032] Furthermore, solvent A is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, 1,4-dioxane, dimethyl sulfoxide, and N-methylpyrrolidone.

[0033] Furthermore, in step S13, the mixture obtained in step S12 is transferred to a shaker and shaken at a frequency of 100-300 rpm at room temperature for 4-24 hours.

[0034] Furthermore, when the product of step (1) is a silane coupling agent modified nanomaterial, the specific steps are as follows, based on mass parts:

[0035] Step 11: Take an appropriate amount of silane coupling agent and 100 parts of hydrophilic nanomaterials into a reaction vessel, wherein:

[0036] The mass ratio of the silane coupling agent to the hydrophilic nanomaterial is (0.1-10):10;

[0037] Step 12: Add solvent B to the reaction vessel and sonicate the hydrophilic nanomaterials in an ultrasonic oscillator for at least 0.5 hours to obtain a mixture, wherein:

[0038] The amount of solvent B added is 2-20 times the mass of the hydrophilic nanomaterial;

[0039] Step 13: Transfer the mixture obtained in Step 12 to a constant temperature magnetic stirrer and stir the reaction at 30-100℃ for 2-18 hours to obtain the reaction solution.

[0040] Step 14: Centrifuge the reaction solution obtained in Step 13, wash it with ultrapure water and anhydrous ethanol at least 3 times in sequence, and vacuum dry it at 30-60℃ for at least 12 hours to obtain silane coupling agent modified nanomaterials.

[0041] Furthermore, solvent B is at least one of methanol, ethanol, n-propanol, isopropanol, formic acid, and acetic acid.

[0042] Furthermore, the silane coupling agent is at least one of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and diethylenetriaminopropyltrimethoxysilane.

[0043] Furthermore, step (2) includes the following steps:

[0044] (21) Take polydopamine-modified nanomaterials, tannic acid-modified nanomaterials, or silane coupling agent-modified nanomaterials, catalyst, and 100-500 parts of polystyrene maleic anhydride into a reaction vessel, then add solvent C to the reaction vessel, and ultrasonically disperse in an ultrasonic oscillator for at least 0.5 h to obtain a mixture, wherein:

[0045] The mass ratio of polydopamine-modified nanomaterials, tannic acid-modified nanomaterials, silane coupling agent-modified nanomaterials, catalysts, and polystyrene maleic anhydride is (0.1-1):(0.1-1):1;

[0046] The amount of solvent C added is 2-6 times the amount of maleic anhydride used in polystyrene;

[0047] (22) Transfer the mixture obtained in step (21) to a constant temperature magnetic stirrer and stir at 40-120℃ for 4-24h. After the reaction is completed, centrifuge and separate the solid. Wash the solid with solvent C at least 3 times and vacuum dry at 60-80℃ for at least 12h to obtain nanomaterial grafted polystyrene maleic anhydride.

[0048] Furthermore, the catalyst is one of p-toluenesulfonic acid, sulfuric acid, hydrochloric acid, and phosphoric acid.

[0049] Furthermore, the solvent C is at least one selected from toluene, xylene, N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, dioxane, dimethyl sulfoxide, and N-methylpyrrolidone.

[0050] Furthermore, the specific steps of step (3) are as follows:

[0051] (31) Take nanomaterial-grafted polystyrene maleic anhydride, catalyst, and 200-800 parts of polyether into a reaction vessel, then add solvent C to the reaction vessel, and sonicate in an ultrasonic oscillator to disperse the nanomaterial-grafted polystyrene maleic anhydride for at least 0.5 h to obtain a mixture, wherein:

[0052] The mass ratio of nanomaterial-grafted polystyrene maleic anhydride, catalyst, and polyether is (0.1-1):(0.1-1):1;

[0053] The amount of solvent C added is 2-6 times the amount of polyether used;

[0054] (32) Transfer the mixture obtained in step (31) to a constant temperature magnetic stirrer and stir at 40-120℃ for 4-24h. After the reaction is completed, centrifuge and wash the solid with distilled water and anhydrous ethanol at least 3 times in sequence. Dry it under vacuum at 60-80℃ for at least 12h to obtain the dual-target demulsifier.

[0055] Furthermore, the molecular weight of the polystyrene maleic anhydride ranges from 2,000 to 100,000.

[0056] Furthermore, based on the mass of the polystyrene maleic anhydride, the content of structural units derived from maleic anhydride is 5-50% by weight.

[0057] Furthermore, the hydrophilic nanomaterial is at least one of nano-TiO2, nano-ZnO, nano-SiO2, graphene oxide, and carbon nanotubes.

[0058] Furthermore, the nanomaterials have a particle size of 1-100 nm.

[0059] Further, the polyether is a diblock polyether polymerized with propylene oxide or ethylene oxide using at least one of the following as an initiator: an alkyl alcohol with 4-18 carbon atoms, an alkylamine with 4-18 carbon atoms, propylene glycol, glycerol, pentaerythritol, polyethylene polyamine, polyethyleneimine, phenolic amine resin, phenolic resin, or polyamide-amine.

[0060] A triblock polyether polymerized with propylene oxide, ethylene oxide, or propylene glycol as an initiator, comprising at least one of the following: alkyl alcohols with 4-18 carbon atoms, alkylamines with 4-18 carbon atoms, propylene glycol, glycerol, pentaerythritol, polyethylene polyamine, polyethyleneimine, phenolic amine resin, phenolic resin, or polyamide-amine; or

[0061] A triblock polyether polymerized with ethylene oxide, propylene oxide, or ethylene oxide using at least one of the following as initiators: alkyl alcohols with 4-18 carbon atoms, alkylamines with 4-18 carbon atoms, propylene glycol, glycerol, pentaerythritol, polyethylene polyamine, polyethyleneimine, phenolic amine resin, phenolic resin, or polyamide-amine.

[0062] Furthermore, the molecular weight of the polyether is 2000-50000.

[0063] A dual-target demulsifier, prepared by any one of the preparation methods described above.

[0064] The application of any of the above-mentioned dual-target demulsifiers in oil extraction, especially as demulsifiers in the treatment of binary composite flooding produced fluids.

[0065] Beneficial Effects: The dual-targeting demulsifier, its preparation method, and its application disclosed in this invention have the following beneficial effects:

[0066] The dual-target demulsifier structure contains nanomaterials, demulsifiers and a large number of benzene rings. The nanomaterials endow the dual-target demulsifier with excellent surface effects, small size effects and macroscopic quantum tunneling effects, while the large number of benzene rings endow the dual-target demulsifier with good compatibility with crude oil. Under the synergistic effect of nanomaterials and a large number of styrene groups, the dual-target demulsifier can simultaneously achieve crude oil dehydration and wastewater oil removal.

[0067] Because the demulsifier molecule does not contain cations, it will not react with negatively charged substances in wastewater for binary flooding produced fluid, thus avoiding the generation of aged oil and sludge. Attached Figure Description

[0068] Figure 1 This is a flowchart of a method for preparing a dual-targeting demulsifier disclosed in this invention. Detailed Implementation

[0069] The specific embodiments of the present invention are described in detail below.

[0070] In this application: hydrophilic nano material (hereinafter referred to as HNM).

[0071] Example 1

[0072] A dual-target demulsifier is formed by crosslinking the anhydride groups of polystyrene maleic anhydride with hydrophilic nanomaterials and polyether, wherein:

[0073] The dual-targeting demulsifier is composed of structural unit A derived from polystyrene maleic anhydride, structural unit B derived from hydrophilic nanomaterials, and structural unit C derived from polyether.

[0074] Based on the total mass of the dual-target demulsifier, the content of structural unit A is 10% by weight, the content of structural unit B is 10% by weight, and the content of structural unit C is 80% by weight.

[0075] Example 2

[0076] A dual-target demulsifier is formed by crosslinking the anhydride groups of polystyrene maleic anhydride with hydrophilic nanomaterials and polyether, wherein:

[0077] The dual-targeting demulsifier is composed of structural unit A derived from polystyrene maleic anhydride, structural unit B derived from hydrophilic nanomaterials, and structural unit C derived from polyether.

[0078] Based on the total mass of the dual-target demulsifier, the content of structural unit A is 10% by weight, the content of structural unit B is 25% by weight, and the content of structural unit C is 65% by weight.

[0079] Example 3

[0080] A dual-target demulsifier is formed by crosslinking the anhydride groups of polystyrene maleic anhydride with hydrophilic nanomaterials and polyether, wherein:

[0081] The dual-targeting demulsifier is composed of structural unit A derived from polystyrene maleic anhydride, structural unit B derived from hydrophilic nanomaterials, and structural unit C derived from polyether.

[0082] Based on the total mass of the dual-target demulsifier, the content of structural unit A is 62.5% by weight, the content of structural unit B is 7.1% by weight, and the content of structural unit C is 30.4% by weight.

[0083] Example 4

[0084] A dual-target demulsifier is formed by crosslinking the anhydride groups of polystyrene maleic anhydride with hydrophilic nanomaterials and polyether, wherein:

[0085] The dual-targeting demulsifier is composed of structural unit A derived from polystyrene maleic anhydride, structural unit B derived from hydrophilic nanomaterials, and structural unit C derived from polyether.

[0086] Based on the total mass of the dual-target demulsifier, the content of structural unit A is 62.5% by weight, the content of structural unit B is 12.5% ​​by weight, and the content of structural unit C is 25% by weight.

[0087] Example 5

[0088] A dual-target demulsifier is formed by crosslinking the anhydride groups of polystyrene maleic anhydride with hydrophilic nanomaterials and polyether, wherein:

[0089] The dual-targeting demulsifier is composed of structural unit A derived from polystyrene maleic anhydride, structural unit B derived from hydrophilic nanomaterials, and structural unit C derived from polyether.

[0090] Based on the total mass of the dual-target demulsifier, the content of structural unit A is 45% by weight, the content of structural unit B is 25% by weight, and the content of structural unit C is 30% by weight.

[0091] Example 6

[0092] A method for preparing a dual-targeting demulsifier, comprising the following steps, by weight:

[0093] (1) 100 parts of hydrophilic nanomaterials were reacted with dopamine hydrochloride to obtain polydopamine modified nanomaterials;

[0094] (2) The polydopamine-modified nanomaterials were dispersed in solvent C and reacted with 100 parts of polystyrene maleic anhydride to obtain nanomaterials grafted with polystyrene maleic anhydride (SMA-g-HNM).

[0095] (3) The nanomaterial grafted polystyrene maleic anhydride was dispersed in solvent C and reacted with 200 parts of polyether. After the reaction was completed, a dual-targeting demulsifier was obtained.

[0096] Furthermore, the specific steps of step (1) are as follows:

[0097] (11) Take appropriate amounts of dopamine hydrochloride and 100 parts of hydrophilic nanomaterials into a reaction vessel, respectively, wherein:

[0098] The mass ratio of dopamine hydrochloride to hydrophilic nanomaterials is 0.1:10;

[0099] (12) Add an appropriate amount of Tris-HCl buffer to the reaction vessel, seal it, and sonicate it in an ultrasonic oscillator for 0.5 h to disperse the hydrophilic nanomaterials to obtain a mixture, wherein:

[0100] The amount of the Tris-HCl buffer solution used is twice the mass of the hydrophilic nanomaterial;

[0101] (13) Transfer the mixture obtained in step (12) to a shaker and shake at room temperature for 4 hours to obtain a reaction solution (in the above process, dopamine hydrochloride is polymerized to generate polydopamine hydrochloride, which adheres to the surface of hydrophilic nanomaterials. The catechol groups in polydopamine hydrochloride react with the hydroxyl groups on the surface of hydrophilic nanomaterials to achieve loading).

[0102] (14) The reaction solution obtained in step (13) is centrifuged and then washed three times with ultrapure water and anhydrous ethanol. It is then vacuum dried at 30°C for 24 hours. After completion, polydopamine modified nanomaterials are obtained.

[0103] Furthermore, in step (13), the mixture obtained in step (12) is transferred to a shaker and shaken at a frequency of 100 rpm for 24 hours at room temperature.

[0104] Furthermore, step (2) includes the following steps:

[0105] (21) Take polydopamine-modified nanomaterials, catalyst, and 100 parts of polystyrene maleic anhydride into a reaction vessel, then add solvent C to the reaction vessel, and ultrasonically disperse in an ultrasonic oscillator for 0.5 h to obtain a mixture, wherein:

[0106] The mass ratio of polydopamine-modified nanomaterials, catalyst, and polystyrene maleic anhydride is 0.1:0.1:1;

[0107] The amount of solvent C added is twice the amount of maleic anhydride used in polystyrene;

[0108] (22) Transfer the mixture obtained in step (21) to a constant temperature magnetic stirrer and stir at 40°C for 24 hours. After the reaction is completed, centrifuge and separate the solid. Wash the solid three times with solvent C and dry it under vacuum at 60°C for 12 hours to obtain nanomaterial grafted polystyrene maleic anhydride.

[0109] Furthermore, the catalyst is p-toluenesulfonic acid.

[0110] Furthermore, the solvent C is toluene.

[0111] Furthermore, the specific steps of step (3) are as follows:

[0112] (31) Take nanomaterial-grafted polystyrene maleic anhydride, catalyst, and 200 parts of polyether into a reaction vessel, then add solvent C to the reaction vessel, and sonicate in an ultrasonic oscillator to disperse the nanomaterial-grafted polystyrene maleic anhydride for 0.5 h to obtain a mixed solution, wherein:

[0113] The mass ratio of nanomaterial-grafted polystyrene maleic anhydride, catalyst, and polyether is 0.1:0.1:1.

[0114] The amount of solvent C added is twice the amount of polyether used;

[0115] (32) Transfer the mixture obtained in step (31) to a constant temperature magnetic stirrer and stir at 40°C for 24 hours. After the reaction is completed, centrifuge and wash the solid three times with distilled water and anhydrous ethanol. Dry it under vacuum at 60°C for 12 hours to obtain the dual-target demulsifier.

[0116] Furthermore, the polystyrene maleic anhydride has a molecular weight of 2000.

[0117] Furthermore, based on the mass of the polystyrene maleic anhydride, the content of structural units derived from maleic anhydride is 5% by weight.

[0118] Furthermore, the hydrophilic nanomaterial is nano-TiO2.

[0119] Furthermore, the nanomaterial has a particle size of 1 nm.

[0120] Furthermore, the polyether is a diblock polyether polymerized with propylene oxide and ethylene oxide using an alkyl alcohol having 4 carbon atoms as an initiator.

[0121] Furthermore, the polyether has a molecular weight of 2000.

[0122] A dual-target demulsifier, prepared by any one of the preparation methods described above.

[0123] The application of any of the above-mentioned dual-target demulsifiers in oil extraction, especially as demulsifiers in the treatment of binary composite flooding produced fluids.

[0124] Example 7

[0125] A method for preparing a dual-targeting demulsifier, comprising the following steps, by weight:

[0126] (1) 100 parts of hydrophilic nanomaterials were reacted with dopamine hydrochloride to obtain polydopamine modified nanomaterials;

[0127] (2) The polydopamine-modified nanomaterials were dispersed in solvent C and reacted with 500 parts of polystyrene maleic anhydride to obtain nanomaterials grafted with polystyrene maleic anhydride (SMA-g-HNM).

[0128] (3) The nanomaterial grafted polystyrene maleic anhydride was dispersed in solvent C and reacted with 800 parts of polyether. After the reaction was completed, a dual-targeting demulsifier was obtained.

[0129] Furthermore, the specific steps of step (1) are as follows:

[0130] (11) Take appropriate amounts of dopamine hydrochloride and 100 parts of hydrophilic nanomaterials into a reaction vessel, respectively, wherein:

[0131] The mass ratio of dopamine hydrochloride to hydrophilic nanomaterials is 10:10;

[0132] (12) Add an appropriate amount of Tris-HCl buffer to the reaction vessel, seal it, and sonicate it in an ultrasonic oscillator for 2 hours to disperse the hydrophilic nanomaterials to obtain a mixture, in which:

[0133] The amount of the Tris-HCl buffer solution used is 20 times the mass of the hydrophilic nanomaterial;

[0134] (13) Transfer the mixture obtained in step (12) to a shaker and shake at room temperature for 8 hours to obtain a reaction solution (in the above process, dopamine hydrochloride is polymerized to generate polydopamine hydrochloride, which adheres to the surface of hydrophilic nanomaterials. The catechol groups in polydopamine hydrochloride react with the hydroxyl groups on the surface of hydrophilic nanomaterials to achieve loading).

[0135] (14) The reaction solution obtained in step (13) is centrifuged and then washed with ultrapure water and anhydrous ethanol five times in sequence. It is then vacuum dried at 60°C for 12 hours. After completion, polydopamine modified nanomaterials are obtained.

[0136] Furthermore, in step (13), the mixture obtained in step (12) is transferred to a shaker and shaken at a frequency of 300 rpm for 4 hours at room temperature.

[0137] Furthermore, step (2) includes the following steps:

[0138] (21) Take polydopamine-modified nanomaterials, catalyst, and 500 parts of polystyrene maleic anhydride into a reaction vessel, then add solvent C to the reaction vessel, and ultrasonically disperse in an ultrasonic oscillator for 2 hours to obtain a mixture, wherein:

[0139] The mass ratio of polydopamine-modified nanomaterials, catalysts, and polystyrene maleic anhydride is 1:1:1;

[0140] The amount of solvent C added is 6 times the amount of polystyrene maleic anhydride used;

[0141] (22) Transfer the mixture obtained in step (21) to a constant temperature magnetic stirrer and stir at 120°C for 4 hours. After the reaction is completed, centrifuge and separate the solid. Wash the solid 5 times with solvent C and vacuum dry at 80°C for 12 hours to obtain nanomaterial grafted polystyrene maleic anhydride.

[0142] Furthermore, the catalyst is sulfuric acid. In another embodiment, the catalyst is hydrochloric acid. In yet another embodiment, the catalyst is phosphoric acid.

[0143] Furthermore, solvent C is toluene. In another embodiment, solvent C is a mixture of equal masses of toluene, xylene, N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, dioxane, dimethyl sulfoxide, and N-methylpyrrolidone. In another embodiment, solvent C is xylene. In another embodiment, solvent C is N,N-dimethylformamide. In another embodiment, solvent C is N,N-dimethylacetamide. In another embodiment, solvent C is tetrahydrofuran. In another embodiment, solvent C is dioxane. In another embodiment, solvent C is dimethyl sulfoxide. In another embodiment, solvent C is N-methylpyrrolidone.

[0144] Furthermore, the specific steps of step (3) are as follows:

[0145] (31) Take nanomaterial-grafted polystyrene maleic anhydride, catalyst, and 800 parts of polyether into a reaction vessel, then add solvent C to the reaction vessel, and sonicate in an ultrasonic oscillator to disperse the nanomaterial-grafted polystyrene maleic anhydride for 2 hours to obtain a mixed solution, wherein:

[0146] The mass ratio of nanomaterial-grafted polystyrene maleic anhydride, catalyst, and polyether is 1:1:1.

[0147] The amount of solvent C added is 6 times the amount of polyether used;

[0148] (32) Transfer the mixture obtained in step (31) to a constant temperature magnetic stirrer and stir at 120°C for 4 hours. After the reaction is completed, centrifuge and wash the solid with distilled water and anhydrous ethanol five times in sequence. Dry it under vacuum at 80°C for 12 hours to obtain the dual-target demulsifier.

[0149] Furthermore, the polystyrene maleic anhydride has a molecular weight of 100,000.

[0150] Furthermore, based on the mass of the polystyrene maleic anhydride, the content of structural units derived from maleic anhydride is 50% by weight.

[0151] Further, the hydrophilic nanomaterial is nano-TiO2. In another embodiment, the hydrophilic nanomaterial is nano-ZnO. In another embodiment, the hydrophilic nanomaterial is nano-SiO2. In another embodiment, the hydrophilic nanomaterial is graphene oxide. In another embodiment, the hydrophilic nanomaterial is carbon nanotubes. In yet another embodiment, the hydrophilic nanomaterial is a mixture of nano-TiO2, nano-ZnO, nano-SiO2, graphene oxide, and carbon nanotubes in equal mass ratios.

[0152] Furthermore, the nanomaterial has a particle size of 100 nm.

[0153] Further, the polyether is a diblock polyether polymerized with propylene oxide and ethylene oxide using an alkyl alcohol with 18 carbon atoms as an initiator. In another embodiment, the polyether is a diblock polyether polymerized with propylene oxide and ethylene oxide using an alkyl alcohol with 12 carbon atoms as an initiator. In another embodiment, the polyether is a diblock polyether polymerized with propylene oxide and ethylene oxide using an alkylamine with 4 carbon atoms as an initiator. In another embodiment, the polyether is a diblock polyether polymerized with propylene oxide and ethylene oxide using an alkylamine with 18 carbon atoms as an initiator. In another embodiment, the polyether is a diblock polyether polymerized with propylene oxide and ethylene oxide using an alkylamine with 8 carbon atoms as an initiator. In yet another embodiment, the polyether is a diblock polyether polymerized with propylene glycol as an initiator. In another embodiment, the polyether is a diblock polyether polymerized with propylene oxide and ethylene oxide using glycerol as an initiator. In another embodiment, the polyether is a diblock polyether polymerized with propylene oxide and ethylene oxide using pentaerythritol as an initiator. In another embodiment, the polyether is a diblock polyether polymerized with propylene oxide and ethylene oxide using polyethylene polyamine as an initiator. In another embodiment, the polyether is a diblock polyether polymerized with propylene oxide and ethylene oxide using polyethyleneimine as an initiator. In another embodiment, the polyether is a diblock polyether polymerized with propylene oxide and ethylene oxide using phenolic resin as an initiator. In another embodiment, the polyether is a phenolic resin. In another embodiment, the polyether is a diblock polyether polymerized with propylene oxide and ethylene oxide using polyamide-amine as an initiator. In another embodiment, the polyether is a diblock polyether polymerized with propylene oxide and ethylene oxide using an equal mass ratio of a mixture of a 6-carbon alkyl alcohol, a 9-carbon alkylamine, propylene glycol, glycerol, pentaerythritol, polyethylenepolyamine, polyethyleneimine, phenolic amine resin, phenolic resin, and polyamide-amine as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with propylene oxide, ethylene oxide, and propylene oxide using a 4-carbon alkyl alcohol as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with propylene oxide, ethylene oxide, and propylene oxide using an 18-carbon alkyl alcohol as an initiator. In yet another embodiment, the polyether is a triblock polyether polymerized with propylene oxide, ethylene oxide, and propylene oxide using a 14-carbon alkyl alcohol as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with propylene oxide, ethylene oxide, and propylene oxide using a 4-carbon alkylamine as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with propylene oxide, ethylene oxide, and propylene oxide using an 18-carbon alkylamine as an initiator. In yet another embodiment, the polyether is a triblock polyether polymerized with propylene oxide, ethylene oxide, and propylene oxide using a 12-carbon alkylamine as an initiator.In another embodiment, the polyether is a triblock polyether polymerized with propylene glycol as an initiator and propylene oxide, ethylene oxide, and propylene oxide. In another embodiment, the polyether is a triblock polyether polymerized with glycerol as an initiator and propylene oxide, ethylene oxide, and propylene oxide. In another embodiment, the polyether is a triblock polyether polymerized with pentaerythritol as an initiator and propylene oxide, ethylene oxide, and propylene oxide. In another embodiment, the polyether is a triblock polyether polymerized with polyethyleneimine as an initiator and propylene oxide, ethylene oxide, and propylene oxide. In another embodiment, the polyether is a triblock polyether polymerized with polyethyleneimine as an initiator and propylene oxide, ethylene oxide, and propylene oxide. In yet another embodiment, the polyether is a triblock polyether polymerized with phenolic amine resin as an initiator and propylene oxide, ethylene oxide, and propylene oxide. In another embodiment, the polyether is a triblock polyether polymerized with propylene oxide, ethylene oxide, and propylene oxide using phenolic resin as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with propylene oxide, ethylene oxide, and propylene oxide using polyamide-amine as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with propylene oxide, ethylene oxide, and propylene oxide using an equal mass ratio of a mixture of an 8-carbon alkyl alcohol, a 12-carbon alkylamine, propylene glycol, glycerol, pentaerythritol, polyethylenepolyamine, polyethyleneimine, phenolic amine resin, phenolic resin, and polyamide-amine as an initiator. In yet another embodiment, the polyether is a triblock polyether polymerized with ethylene oxide, propylene oxide, and ethylene oxide using an 4-carbon alkyl alcohol as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with ethylene oxide, propylene oxide, and ethylene oxide using an 18-carbon alkyl alcohol as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with ethylene oxide, propylene oxide, and ethylene oxide using an 12-carbon alkyl alcohol as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with ethylene oxide, propylene oxide, and ethylene oxide using an 4-carbon alkylamine as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with ethylene oxide, propylene oxide, and ethylene oxide using an 18-carbon alkylamine as an initiator. In yet another embodiment, the polyether is a triblock polyether polymerized with ethylene oxide, propylene oxide, and ethylene oxide using an 12-carbon alkylamine as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with propylene glycol as an initiator and ethylene oxide, propylene oxide, and ethylene oxide. In another embodiment, the polyether is a triblock polyether polymerized with glycerol as an initiator and ethylene oxide, propylene oxide, and ethylene oxide. In yet another embodiment, the polyether is a triblock polyether polymerized with pentaerythritol as an initiator and ethylene oxide, propylene oxide, and ethylene oxide.In another embodiment, the polyether is a triblock polyether polymerized with ethylene oxide, propylene oxide, and ethylene oxide using polyethyleneimine as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with ethylene oxide, propylene oxide, and ethylene oxide using polyethyleneimine as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with ethylene oxide, propylene oxide, and ethylene oxide using phenolic resin as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with ethylene oxide, propylene oxide, and ethylene oxide using phenolic resin as an initiator. In yet another embodiment, the polyether is a triblock polyether polymerized with ethylene oxide, propylene oxide, and ethylene oxide using polyamide-amine as an initiator. In another embodiment, the polyether is a triblock polyether polymerized with ethylene oxide, propylene oxide, and ethylene oxide using an equal mass ratio of a mixture of alkyl alcohols with four carbon atoms, alkylamines with four carbon atoms, propylene glycol, glycerol, pentaerythritol, polyethylene polyamine, polyethyleneimine, phenolic amine resin, phenolic resin, and polyamide-amine as an initiator.

[0154] Furthermore, the polyether has a molecular weight of 50,000.

[0155] A dual-target demulsifier, prepared by any one of the preparation methods described above.

[0156] The application of any of the above-mentioned dual-target demulsifiers in oil extraction, especially as demulsifiers in the treatment of binary composite flooding produced fluids.

[0157] Example 8

[0158] A method for preparing a dual-targeting demulsifier, comprising the following steps, by weight:

[0159] (1) 100 parts of hydrophilic nanomaterials were reacted with dopamine hydrochloride to obtain polydopamine modified nanomaterials;

[0160] (2) The polydopamine-modified nanomaterials were dispersed in solvent C and reacted with 300 parts of polystyrene maleic anhydride to obtain nanomaterials grafted with polystyrene maleic anhydride (SMA-g-HNM).

[0161] (3) The nanomaterial grafted polystyrene maleic anhydride was dispersed in solvent C and reacted with 400 parts of polyether. After the reaction was completed, a dual-targeting demulsifier was obtained.

[0162] Furthermore, the specific steps of step (1) are as follows:

[0163] (11) Take appropriate amounts of dopamine hydrochloride and 100 parts of hydrophilic nanomaterials into a reaction vessel, respectively, wherein:

[0164] The mass ratio of dopamine hydrochloride to hydrophilic nanomaterials is 5:10;

[0165] (12) Add an appropriate amount of Tris-HCl buffer to the reaction vessel, seal it, and sonicate it in an ultrasonic oscillator for 1 hour to disperse the hydrophilic nanomaterials to obtain a mixture, wherein:

[0166] The amount of the Tris-HCl buffer solution used is 10 times the mass of the hydrophilic nanomaterial;

[0167] (13) Transfer the mixture obtained in step (12) to a shaker and shake at room temperature for 6 hours to obtain a reaction solution (in the above process, dopamine hydrochloride is polymerized to generate polydopamine hydrochloride, which adheres to the surface of hydrophilic nanomaterials. The catechol groups in polydopamine hydrochloride react with the hydroxyl groups on the surface of hydrophilic nanomaterials to achieve loading).

[0168] (14) The reaction solution obtained in step (13) is centrifuged and then washed with ultrapure water and anhydrous ethanol four times in sequence. It is then vacuum dried at 45°C for 16 hours. After completion, polydopamine modified nanomaterials are obtained.

[0169] Furthermore, in step (13), the mixture obtained in step (12) is transferred to a shaker and shaken at a frequency of 200 rpm for 12 h at room temperature.

[0170] Furthermore, step (2) includes the following steps:

[0171] (21) Take polydopamine-modified nanomaterials, catalyst, and 300 parts of polystyrene maleic anhydride into a reaction vessel, then add solvent C to the reaction vessel, and ultrasonically disperse in an ultrasonic oscillator for 1 hour to obtain a mixture, wherein:

[0172] The mass ratio of polydopamine-modified nanomaterials, catalyst, and polystyrene maleic anhydride is 0.5:0.5:1.

[0173] The amount of solvent C added is 4 times the amount of polystyrene maleic anhydride used;

[0174] (22) Transfer the mixture obtained in step (21) to a constant temperature magnetic stirrer and stir at 80°C for 12 hours. After the reaction is completed, centrifuge and separate the solid. Wash the solid 4 times with solvent C and dry it under vacuum at 70°C for 16 hours to obtain nanomaterial grafted polystyrene maleic anhydride.

[0175] Furthermore, the catalyst is hydrochloric acid.

[0176] Furthermore, the solvent C is N,N-dimethylformamide.

[0177] Furthermore, the specific steps of step (3) are as follows:

[0178] (31) Take nanomaterial-grafted polystyrene maleic anhydride, catalyst, and 400 parts of polyether into a reaction vessel, then add solvent C to the reaction vessel, and sonicate in an ultrasonic oscillator to disperse the nanomaterial-grafted polystyrene maleic anhydride for 1 hour to obtain a mixed solution, wherein:

[0179] The mass ratio of nanomaterial-grafted polystyrene maleic anhydride, catalyst, and polyether is 0.5:0.5:1.

[0180] The amount of solvent C added is 4 times the amount of polyether used;

[0181] (32) Transfer the mixture obtained in step (31) to a constant temperature magnetic stirrer and stir at 60°C for 12 hours. After the reaction is completed, centrifuge and wash the solid with distilled water and anhydrous ethanol four times in sequence. Dry it under vacuum at 70°C for 16 hours to obtain the dual-target demulsifier.

[0182] Furthermore, the molecular weight of the polystyrene maleic anhydride is in the range of 40,000.

[0183] Furthermore, based on the mass of the polystyrene maleic anhydride, the content of structural units derived from maleic anhydride is 26.2% by weight.

[0184] Furthermore, the hydrophilic nanomaterial is nano-SiO2.

[0185] Furthermore, the nanomaterial has a particle size of 20 nm.

[0186] Furthermore, a triblock polyether is polymerized with ethylene oxide, propylene oxide, and ethylene oxide using a 6-carbon alkyl alcohol as an initiator.

[0187] Furthermore, the polyether has a molecular weight of 20,000.

[0188] A dual-target demulsifier, prepared by any one of the preparation methods described above.

[0189] The application of any of the above-mentioned dual-target demulsifiers in oil extraction, especially as demulsifiers in the treatment of binary composite flooding produced fluids.

[0190] Example 9

[0191] Similar to Example 8, except that in step (1), tannic acid is used to modify the hydrophilic nanomaterial to obtain tannic acid-modified nanomaterials:

[0192] Furthermore, the product of step (1) is tannic acid-modified nanomaterials, and the specific steps are as follows, based on mass parts:

[0193] S11. Take an appropriate amount of tannic acid and 100 parts of hydrophilic nanomaterials into a reaction vessel, wherein:

[0194] The mass ratio of the tannic acid to the hydrophilic nanomaterial is 0.1:10;

[0195] S12. Add solvent A to the reaction vessel, seal it, and sonicate it in an ultrasonic oscillator for 2 hours to disperse the hydrophilic nanomaterials, obtaining a mixed solution, wherein:

[0196] The amount of solvent A added is twice the mass of the hydrophilic nanomaterial;

[0197] S13. Transfer the mixture obtained in step S12 to a shaker and shake at room temperature for 4 hours to obtain a reaction solution; (In the above process, tannic acid adheres to the surface of the hydrophilic nanomaterial to achieve loading);

[0198] S14. The reaction solution obtained in step S13 is centrifuged and washed three times with ultrapure water and anhydrous ethanol. After vacuum drying at 30°C for 24 hours, tannic acid modified nanomaterials are obtained.

[0199] Furthermore, solvent A is N,N-dimethylformamide.

[0200] Furthermore, in step S13, the mixture obtained in step S12 is transferred to a shaker and shaken at a frequency of 100 rpm for 24 hours at room temperature.

[0201] Example 10

[0202] Similar to Example 8, except that in step (1), tannic acid is used to modify the hydrophilic nanomaterial to obtain tannic acid-modified nanomaterials:

[0203] Furthermore, the product of step (1) is tannic acid-modified nanomaterials, and the specific steps are as follows, based on mass parts:

[0204] S11. Take an appropriate amount of tannic acid and 100 parts of hydrophilic nanomaterials into a reaction vessel, wherein:

[0205] The mass ratio of the tannic acid to the hydrophilic nanomaterial is 10:10;

[0206] S12. Add solvent A to the reaction vessel, seal it, and sonicate it in an ultrasonic oscillator for 6 hours to disperse the hydrophilic nanomaterials, resulting in a mixed solution, wherein:

[0207] The amount of solvent A added is 20 times the mass of the hydrophilic nanomaterial;

[0208] S13. Transfer the mixture obtained in step S12 to a shaker and shake at room temperature for 8 hours to obtain a reaction solution; (In the above process, tannic acid adheres to the surface of the hydrophilic nanomaterial to achieve loading);

[0209] S14. The reaction solution obtained in step S13 is centrifuged and washed five times with ultrapure water and anhydrous ethanol, and then vacuum dried at 60°C for 12 hours to obtain tannic acid modified nanomaterials.

[0210] Furthermore, solvent A is N,N-dimethylacetamide.

[0211] Furthermore, in step S13, the mixture obtained in step S12 is transferred to a shaker and shaken at a frequency of 300 rpm for 4 hours at room temperature.

[0212] Example 11

[0213] Similar to Example 8, except that in step (1), tannic acid is used to modify the hydrophilic nanomaterial to obtain tannic acid-modified nanomaterials:

[0214] Furthermore, the product of step (1) is tannic acid-modified nanomaterials, and the specific steps are as follows, based on mass parts:

[0215] S11. Take an appropriate amount of tannic acid and 100 parts of hydrophilic nanomaterials into a reaction vessel, wherein:

[0216] The mass ratio of the tannic acid to the hydrophilic nanomaterial is 5:10;

[0217] S12. Add solvent A to the reaction vessel, seal it, and sonicate it in an ultrasonic oscillator for 3 hours to disperse the hydrophilic nanomaterials, obtaining a mixed solution, wherein:

[0218] The amount of solvent A added is 10 times the mass of the hydrophilic nanomaterial;

[0219] S13. Transfer the mixture obtained in step S12 to a shaker and shake at room temperature for 6 hours to obtain a reaction solution; (In the above process, tannic acid adheres to the surface of the hydrophilic nanomaterial to achieve loading);

[0220] S14. The reaction solution obtained in step S13 is centrifuged and washed four times with ultrapure water and anhydrous ethanol. After vacuum drying at 50°C for 16 hours, tannic acid modified nanomaterials are obtained.

[0221] Furthermore, solvent A is tetrahydrofuran. In another embodiment, solvent A is 1,4-dioxane. In another embodiment, solvent A is dimethyl sulfoxide. In another embodiment, solvent A is N-methylpyrrolidone. In yet another embodiment, solvent A is a mixture of N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, 1,4-dioxane, dimethyl sulfoxide, and N-methylpyrrolidone in equal mass ratios.

[0222] Furthermore, in step S13, the mixture obtained in step S12 is transferred to a shaker and shaken at a frequency of 200 rpm for 12 hours at room temperature.

[0223] Example 12

[0224] Similar to Example 8, except that in step (1), a silane coupling agent is used to modify the hydrophilic nanomaterial to obtain silane coupling agent modified nanomaterials:

[0225] Furthermore, when the product of step (1) is a silane coupling agent modified nanomaterial, the specific steps are as follows, based on mass parts:

[0226] Step 11: Take an appropriate amount of silane coupling agent and 100 parts of hydrophilic nanomaterials into a reaction vessel, wherein:

[0227] The mass ratio of the silane coupling agent to the hydrophilic nanomaterial is 0.1:10;

[0228] Step 12: Add solvent B to the reaction vessel and sonicate the hydrophilic nanomaterials in an ultrasonic oscillator for 0.5 hours to obtain a mixture, wherein:

[0229] The amount of solvent B added is twice the mass of the hydrophilic nanomaterial;

[0230] Step 13: Transfer the mixture obtained in Step 12 to a constant temperature magnetic stirrer and stir at 30°C for 18 hours to obtain the reaction solution.

[0231] Step 14: Centrifuge the reaction solution obtained in Step 13, wash it three times with ultrapure water and anhydrous ethanol, and vacuum dry it at 30°C for 24 hours to obtain silane coupling agent modified nanomaterials.

[0232] Furthermore, the solvent B is methanol.

[0233] Furthermore, the silane coupling agent is 3-aminopropyltrimethoxysilane (APTMS).

[0234] Example 13

[0235] Similar to Example 8, except that in step (1), a silane coupling agent is used to modify the hydrophilic nanomaterial to obtain silane coupling agent modified nanomaterials:

[0236] Furthermore, when the product of step (1) is a silane coupling agent modified nanomaterial, the specific steps are as follows, based on mass parts:

[0237] Step 11: Take an appropriate amount of silane coupling agent and 100 parts of hydrophilic nanomaterials into a reaction vessel, wherein:

[0238] The mass ratio of the silane coupling agent to the hydrophilic nanomaterial is 10:10;

[0239] Step 12: Add solvent B to the reaction vessel and sonicate the hydrophilic nanomaterials in an ultrasonic oscillator for 2 hours to obtain a mixed solution, wherein:

[0240] The amount of solvent B added is 20 times the mass of the hydrophilic nanomaterial;

[0241] Step 13: Transfer the mixture obtained in Step 12 to a constant temperature magnetic stirrer and stir at 100°C for 2 hours to obtain the reaction solution.

[0242] Step 14: Centrifuge the reaction solution obtained in Step 13, wash it 6 times with ultrapure water and anhydrous ethanol, and vacuum dry it at 60°C for 12 hours to obtain silane coupling agent modified nanomaterials.

[0243] Furthermore, solvent B is ethanol.

[0244] Furthermore, the silane coupling agent is 3-aminopropyltriethoxysilane (KH550).

[0245] Example 14

[0246] Similar to Example 8, except that in step (1), a silane coupling agent is used to modify the hydrophilic nanomaterial to obtain silane coupling agent modified nanomaterials:

[0247] Furthermore, when the product of step (1) is a silane coupling agent modified nanomaterial, the specific steps are as follows, based on mass parts:

[0248] Step 11: Take an appropriate amount of silane coupling agent and 100 parts of hydrophilic nanomaterials into a reaction vessel, wherein:

[0249] The mass ratio of the silane coupling agent to the hydrophilic nanomaterial is 5:10;

[0250] Step 12: Add solvent B to the reaction vessel and sonicate the hydrophilic nanomaterials in an ultrasonic oscillator for 1 hour to obtain a mixed solution, wherein:

[0251] The amount of solvent B added is 10 times the mass of the hydrophilic nanomaterial;

[0252] Step 13: Transfer the mixture obtained in Step 12 to a constant temperature magnetic stirrer and stir at 60°C for 9 hours to obtain the reaction solution.

[0253] Step 14: Centrifuge the reaction solution obtained in Step 13, wash it four times with ultrapure water and anhydrous ethanol, and vacuum dry it at 45°C for 16 hours to obtain silane coupling agent modified nanomaterials.

[0254] Furthermore, solvent B is n-propanol. In another embodiment, solvent B is isopropanol. In another embodiment, solvent B is formic acid. In another embodiment, solvent B is acetic acid. In yet another embodiment, solvent B is a mixture of methanol, ethanol, n-propanol, isopropanol, formic acid, and acetic acid in equal mass ratios.

[0255] Furthermore, the silane coupling agent is diethylenetriaminopropyltrimethoxysilane. In another embodiment, the silane coupling agent is a mixture of 3-aminopropyltrimethoxysilane (APTMS), 3-aminopropyltriethoxysilane (KH550), and diethylenetriaminopropyltrimethoxysilane in equal mass ratios.

[0256] Performance characterization:

[0257] The dual-targeting demulsifier prepared according to Example 6-14 of the Chinese petroleum and natural gas industry standard SY / T 5281-2000 "Test Method for Performance of Crude Oil Demulsifier (Bottle Test Method)" was tested on-site in a bottle test on the produced fluid of the binary flooding at the Gudong Oil Production Plant of Shengli Oilfield.

[0258] The specific experimental steps are as follows:

[0259] A complex multiphase emulsion was prepared by mixing 20 mL of oil phase (mainly W / O emulsion) and 80 mL of aqueous phase (mainly O / W emulsion) from the drain fluid of the Gudong No. 2 well in a 100 mL demulsification bottle. The mixture was kept at a constant temperature of 45℃ for 45 min. Then, 100 mg / L of the demulsifier to be tested was added to the demulsification bottle, shaken 200 times, and placed back in a constant temperature water bath for constant temperature.

[0260] Observe the oil-water phase separation after 12 hours.

[0261] Test the water content in the oil and the oil content in the water after demulsification.

[0262] The polymer content in the demulsified wastewater was determined by liquid chromatography, and the polymer retention rate was obtained by comparing it with the polymer content in the extracted fluid.

[0263] The experimental results are shown in Table 1. In Table 1, the reagents added (items 1-4) are a polyether demulsifier and a field-applied reverse demulsifier, each at a concentration of 50 mg / L. As can be seen from Table 1, the dual-targeted demulsifier prepared in this invention has a good demulsification and water-clearing effect on binary flooding produced fluid, and can retain polymers in the wastewater.

[0264] Table 1 Results of Emulsion Breaking and Clear Water Production from Crude Oil Emulsion

[0265]

[0266]

[0267] The embodiments of the present invention have been described in detail above. However, the present invention is not limited to the above embodiments, and various changes can be made within the scope of knowledge possessed by those skilled in the art without departing from the spirit of the present invention.

Claims

1. A method for preparing a dual-targeting demulsifier, characterized in that, By weight, the following steps are included: (1) 100 parts of hydrophilic nanomaterials were reacted with dopamine hydrochloride or tannic acid respectively to obtain polydopamine modified nanomaterials or tannic acid modified nanomaterials. (2) Disperse polydopamine-modified nanomaterials or tannic acid-modified nanomaterials in solvent C and react with 100-500 parts of polystyrene maleic anhydride to obtain nanomaterials grafted with polystyrene maleic anhydride. (3) The nanomaterial grafted polystyrene maleic anhydride is dispersed in solvent C and reacted with 200-800 parts of polyether. After the reaction is completed, a dual-targeting demulsifier is obtained, wherein: The dual-target demulsifier is formed by crosslinking the anhydride groups in polystyrene maleic anhydride with hydrophilic nanomaterials and polyether, respectively. The dual-target demulsifier is composed of structural unit A derived from polystyrene maleic anhydride, structural unit B derived from hydrophilic nanomaterials, and structural unit C derived from polyether. Based on the total mass of the dual-target demulsifier, the content of structural unit A is 10-62.5% by weight, the content of structural unit B is 7.1-25% by weight, and the content of structural unit C is 25-80% by weight. The hydrophilic nanomaterial is at least one of nano-TiO2, nano-ZnO, graphene oxide, and carbon nanotubes; The hydrophilic nanomaterial has a particle size of 1-100 nm; When the product of step (1) is polydopamine-modified nanomaterial, the specific steps are as follows: (11) Take appropriate amounts of dopamine hydrochloride and 100 parts of hydrophilic nanomaterials into a reaction vessel, wherein: The mass ratio of dopamine hydrochloride to hydrophilic nanomaterials is (0.1-10):10; (12) Add an appropriate amount of Tris-HCl buffer to the reaction vessel, seal it, and sonicate it in an ultrasonic oscillator to disperse the hydrophilic nanomaterials for at least 0.5 h to obtain a mixture, wherein: The amount of the Tris-HCl buffer solution used is 2-20 times the mass of the hydrophilic nanomaterial; (13) Transfer the mixture obtained in step (12) to a shaker and shake at room temperature for at least 4 hours to obtain a reaction solution; (14) Centrifuge the reaction solution obtained in step (13), then wash it with ultrapure water and anhydrous ethanol at least 3 times in sequence, and vacuum dry it at 30-60 °C for at least 12 h. After completion, polydopamine modified nanomaterials are obtained. When the product of step (1) is tannic acid-modified nanomaterial, the specific steps are as follows, based on mass parts: S11. Take an appropriate amount of tannic acid and 100 parts of hydrophilic nanomaterials into a reaction vessel, wherein: The mass ratio of the tannic acid to the hydrophilic nanomaterial is (0.1-10):10; S12. Add solvent A to the reaction vessel, seal it, and sonicate it in an ultrasonic oscillator to disperse the hydrophilic nanomaterials for at least 2 hours to obtain a mixture, wherein: The amount of solvent A added is 2-20 times the mass of the hydrophilic nanomaterial; S13. Transfer the mixture obtained in step S12 to a shaker and shake at room temperature for at least 4 hours to obtain a reaction solution; S14. The reaction solution obtained in step S13 is centrifuged and washed with ultrapure water and anhydrous ethanol at least 3 times in sequence. After vacuum drying at 30-60 °C for at least 12 h, tannic acid modified nanomaterials are obtained.

2. The method for preparing a dual-targeting demulsifier as described in claim 1, characterized in that, In step (13), the mixture obtained in step (12) is transferred to a shaker and shaken at a frequency of 100-300 rpm for 4-24 hours at room temperature.

3. The method for preparing a dual-targeting demulsifier as described in claim 1, characterized in that, The solvent A is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, 1,4-dioxane, dimethyl sulfoxide, and N-methylpyrrolidone. In step S13, the mixture obtained in step S12 is transferred to a shaker and shaken at a frequency of 100-300 rpm at room temperature for 4-24 hours.

4. The method for preparing a dual-targeting demulsifier as described in claim 1, characterized in that, Step (2) includes the following steps: (21) Take polydopamine-modified nanomaterials or tannic acid-modified nanomaterials, catalyst, and 100-500 parts of polystyrene maleic anhydride into a reaction vessel, then add solvent C to the reaction vessel, and ultrasonically disperse in an ultrasonic oscillator for at least 0.5 h to obtain a mixture, wherein: The mass ratio of polydopamine-modified nanomaterials or tannic acid-modified nanomaterials, catalysts, and polystyrene maleic anhydride is (0.1-1):(0.1-1):1; The amount of solvent C added is 2-6 times the amount of maleic anhydride used in polystyrene; (22) Transfer the mixture obtained in step (21) to a constant temperature magnetic stirrer and stir at 40-120 °C for 4-24 h. After the reaction is completed, centrifuge and separate the solid. Wash the solid with solvent C at least 3 times and vacuum dry at 60-80 °C for at least 12 h to obtain nanomaterial grafted polystyrene maleic anhydride.

5. The method for preparing a dual-targeting demulsifier as described in claim 4, characterized in that, The solvent C is at least one of toluene, xylene, N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, dioxane, dimethyl sulfoxide, and N-methylpyrrolidone.

6. The method for preparing a dual-targeted demulsifier as described in claim 1, characterized in that, The specific steps of step (3) are as follows: (31) Take nanomaterial-grafted polystyrene maleic anhydride, catalyst, and 200-800 parts of polyether into a reaction vessel, then add solvent C to the reaction vessel, and sonicate in an ultrasonic oscillator to disperse the nanomaterial-grafted polystyrene maleic anhydride for at least 0.5 h to obtain a mixture, wherein: The mass ratio of nanomaterial-grafted polystyrene maleic anhydride, catalyst, and polyether is (0.1-1):(0.1-1):1; The amount of solvent C added is 2-6 times the amount of polyether used; (32) Transfer the mixture obtained in step (31) to a constant temperature magnetic stirrer and stir at 40-120 °C for 4-24 h. After the reaction is completed, centrifuge and wash the solid with distilled water and anhydrous ethanol at least 3 times in sequence. Dry it under vacuum at 60-80 °C for at least 12 h to obtain the dual-target demulsifier.

7. The method for preparing a dual-targeting demulsifier as described in claim 6, characterized in that, The catalyst is one of p-toluenesulfonic acid, sulfuric acid, hydrochloric acid, and phosphoric acid.

8. The method for preparing a dual-targeting demulsifier as described in claim 1, characterized in that, The molecular weight range of the polystyrene maleic anhydride is 2000-100000.

9. The method for preparing a dual-targeting demulsifier as described in claim 1, characterized in that, The content of structural units derived from maleic anhydride is 5-50% by weight, based on the mass of the polystyrene maleic anhydride.

10. The method for preparing a dual-targeting demulsifier as described in claim 1, characterized in that, The polyether is a diblock polyether polymerized with propylene oxide or ethylene oxide using at least one of the following as an initiator: an alkyl alcohol with 4-18 carbon atoms, an alkylamine with 4-18 carbon atoms, propylene glycol, glycerol, pentaerythritol, polyethylene polyamine, polyethyleneimine, phenolic amine resin, phenolic resin, or polyamide-amine. A triblock polyether polymerized with propylene oxide, ethylene oxide, or propylene glycol as an initiator, comprising at least one of the following: alkyl alcohols with 4-18 carbon atoms, alkylamines with 4-18 carbon atoms, propylene glycol, glycerol, pentaerythritol, polyethylene polyamine, polyethyleneimine, phenolic amine resin, phenolic resin, or polyamide-amine; or A triblock polyether polymerized with ethylene oxide, propylene oxide, or ethylene oxide using at least one of the following as initiators: alkyl alcohols with 4-18 carbon atoms, alkylamines with 4-18 carbon atoms, propylene glycol, glycerol, pentaerythritol, polyethylene polyamine, polyethyleneimine, phenolic amine resin, phenolic resin, or polyamide-amine.

11. The method for preparing a dual-targeting demulsifier as described in claim 1, characterized in that, The polyether has a molecular weight of 2000-50000.

12. A dual-targeting demulsifier, characterized in that, It is prepared by the preparation method according to any one of claims 1-11.

Citation Information

Patent Citations

  • Preparation method of magnetic graphene oxide demulsifying agent

    CN106219669A

  • A demulsifier and its preparation method

    CN109054888B

  • A reusable carbon-based nano-demulsifier and its preparation method

    CN110559691B

  • Nano SiO2-TA162824 composite demulsifier and preparation method thereof

    CN112370817A

  • Hyperbranched polyether grafted polystyrene maleic anhydride oil-water synchronous demulsification water clarifier

    CN115368577A