Organic electroluminescent compound and organic electroluminescent device

By reasonably introducing deuterium atoms into OLED materials to active sites and positions with high electron cloud density of amine compounds containing fluorenyl substituents into OLED materials, the shortcomings in life and efficiency of OLED materials are solved, and the performance of materials and devices are improved and cost control is achieved.

CN119977821APending Publication Date: 2025-05-13NANJING TOPTO MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510149650.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-02-11
Publication Date
2025-05-13

AI Technical Summary

Technical Problem

There are shortcomings in existing OLED materials in terms of life and efficiency, especially in the case of expanded display area, how to improve the performance of materials and devices within cost control becomes a challenge.

Method used

The structure of organic electroluminescent materials is optimized by reasonably introducing deuterium atoms into fluorenyl-containing amine compounds, especially at the active sites of the compound and at high electron cloud density.

Benefits of technology

It significantly improves the thermal stability, chemical stability and photoelectric stability of the material, extends the service life of the device, improves the luminous efficiency, and controls the raw material costs, achieving better economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119977821A_ABST
    Figure CN119977821A_ABST
Patent Text Reader

Abstract

The invention provides an organic electroluminescent compound and an organic electroluminescent device. The organic electroluminescent compound has a structure as shown in a formula (1). According to the invention, through reasonable introduction of deuterium atoms, compared with non-deuterated materials, the amine compounds containing fluorenyl substituent groups have the advantages that the stability of the material structure, such as thermal stability, chemical stability and photoelectric stability, can be obviously improved; the deuteration position of the compound is located at the active site of the compound and the position with high electron cloud density, so that the performance of the organic electroluminescent material and the corresponding device is improved to a certain level by using relatively few deuterium raw materials; the raw material cost and the production cost required by the organic electroluminescent material are controlled and optimized, and better economic benefits are achieved. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic electroluminescence, in particular to an organic electroluminescent compound and an organic electroluminescent device. Background Art

[0002] OLED, the full name of which is Organic Light-Emitting Diode, is a current-type organic light-emitting device. Its working principle is that under the action of an electric field, the holes generated by the anode and the electrons generated by the cathode move, are injected into the hole transport layer and the electron transport layer respectively, and migrate to the light-emitting layer. When the holes and electrons meet in the light-emitting layer, energy excitons are generated, thereby exciting the molecules of the light-emitting material and finally generating visible light. In organic light-emitting devices, the biggest problems are lifespan and efficiency, and as the display area becomes larger and larger, such efficiency or lifespan problems must be solved.

[0003] Deuterium (D) is a stable non-radioactive isotope in nature with a larger atomic mass than hydrogen. Studies have shown that introducing deuterium atoms into OLED materials can stabilize the molecular structure, improve the luminous efficiency and stability of OLED devices, and extend the service life. However, through practical verification, whether the introduction of deuterium can specifically improve the performance of materials and devices is also related to the method of introduction, including the deuterium substitution rate of the material and the location of the deuterium substitution reaction, and the introduction of deuterium will lead to a significant increase in material costs. Therefore, at a certain cost, how to reasonably modify the compound and introduce deuterium atoms at the appropriate site to achieve more cost-effective performance improvement of materials and devices is a direction worthy of research. Summary of the invention

[0004] The technical purpose of the present invention is to introduce deuterium atoms into amine compounds containing fluorenyl substituents in a more reasonable manner, so as to provide more optimized organic electroluminescent compounds and organic electroluminescent devices.

[0005] The technical solution provided by the present invention is:

[0006] An organic electroluminescent compound, characterized in that it has a structural formula as shown in formula (1):

[0007]

[0008] in:

[0009] R1 is one of substituted or unsubstituted C1-C4 alkyl groups, and the substituent of R1 is selected from deuterium, methyl or deuterated methyl;

[0010] R2 and R3 each independently represent a substituted or unsubstituted C6-C30 aryl group, R2 and R3 are different groups, and one of them is selected from a substituted or unsubstituted fluorenyl group;

[0011] The substituents of R2 and R3 are independently selected from one or more of methyl, deuterated methyl, phenyl substituted by methyl and phenyl substituted by deuterated methyl.

[0012] In a preferred embodiment, the organic electroluminescent compound contains 1 to 3 deuterated methyl groups, or 3 to 12 deuterium atoms.

[0013] In a preferred embodiment, R1 is a substituted or unsubstituted methyl, ethyl, isopropyl, or tert-butyl group, and its substituent is selected from deuterium or deuterated methyl;

[0014] Preferably, R1 is selected from one of the following groups: deuterated methyl, deuterated ethyl, deuterated isopropyl, tert-butyl or deuterated tert-butyl;

[0015] Further preferably, the R1 is selected from one of the following groups: deuterated methyl, deuterated ethyl, deuterated isopropyl or tert-butyl;

[0016] More preferably, the structural formula of R1 is Where * indicates the attachment site.

[0017] In a preferred embodiment, R2 and R3 each independently represent a substituted or unsubstituted phenyl, biphenyl, fluorenyl, naphthyl or carbazolyl group;

[0018] Preferably, one of R2 and R3 is selected from the following substituted or unsubstituted groups: biphenyl, biphenyl substituted by methyl, biphenyl substituted by deuterated methyl;

[0019] More preferably, one of R2 and R3 is dimethylfluorene, and the other is diphenyl substituted with at least one methyl group or at least one deuterated methyl group;

[0020] More preferably, R2 and R3 are each independently selected from a group represented by formula (1-1), formula (1-2) or formula (1-3):

[0021]

[0022] wherein R4 and R5 each independently represent a methyl group or a deuterated methyl group;

[0023] m and n independently represent 0 or 1;

[0024] * indicates the attachment site.

[0025] As a preferred embodiment, the compound of the present invention is any one of the following compounds:

[0026]

[0027]

[0028]

[0029]

[0030]

[0031]

[0032]

[0033]

[0034]

[0035] An organic electroluminescent device comprises an anode, a cathode and an organic layer formed between the anode and the cathode, wherein the organic layer contains the organic electroluminescent compound as described in any one of the above schemes.

[0036] Furthermore, the organic layer comprises a hole injection layer, a first hole transport layer, a second hole transport layer, a light-emitting layer, a hole blocking layer, an electron transport layer and an electron injection layer, and the first hole transport layer or the second hole transport layer contains any of the above organic electroluminescent compounds.

[0037] Beneficial effects of the present invention:

[0038] 1) The present invention aims to introduce deuterium atoms in a reasonable manner so that a class of amine compounds containing fluorenyl substituents can be significantly improved in terms of material structure stability, such as thermal stability, chemical stability, and photoelectric stability, compared with such materials that are not deuterated, thereby improving the lifespan and luminous efficiency of devices using such compounds, and making the deuterated position of the compound located at the active site of the compound and a position with high electron cloud density, so as to achieve the use of relatively small amounts of deuterium raw materials to improve the performance of organic electroluminescent materials and corresponding devices to a certain level, thereby controlling and optimizing the raw material cost and production cost required for the organic electroluminescent material, and achieving better economic benefits.

[0039] 2) The present invention improves the carrier mobility of the material while ensuring the stability of the material by introducing modifying groups such as alkyl or deuterated alkyl, broadens the exciton recombination area, and further improves the life and luminous efficiency of the device using the material of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 A schematic diagram of the structure of an organic electroluminescent device provided by the present invention;

[0041] Figure 2HPLC chart of compound G3 prepared in Example of the present invention;

[0042] Figure 3 The DSC spectrum of compound G3 prepared in the embodiment of the present invention is shown in FIG. Figure 3 It can be seen that the Tm value of compound G3 is 189.61°C;

[0043] Figure 4 The TGA spectrum of compound G3 prepared in the embodiment of the present invention is shown in FIG. Figure 4 It can be seen that the melting point temperature Td value of compound G3 is 402.86°C.

[0044] Figure 1 The reference numerals in the drawings represent respectively:

[0045] 1- anode, 2- hole injection layer, 3- first hole transport layer, 4- second hole transport layer, 5- light emitting layer, 6- hole blocking layer, 7- electron transport layer, 8- electron injection layer, 9- cathode. DETAILED DESCRIPTION

[0046] In order to further illustrate the technical solution of the present invention, the present invention is introduced in more detail below in conjunction with specific embodiments.

[0047] The term "deuterated" herein refers to at least one hydrogen of a group being re-coordinated with a deuterium substituent group. "Deuterium" refers to a stable isotope of hydrogen, also known as heavy hydrogen, with the element symbol D.

[0048] The term "aryl" herein, unless otherwise specified, refers to a group containing one or more aromatic rings, where the aromatic rings include but are not limited to benzene, naphthalene, phenanthrene, fluorene, acenaphthene, pyridine, pyrimidine, pyrrole, furan, thiophene, etc. C6-C30 aryl means that the group contains 6-30 carbon atoms.

[0049] The term "alkyl" herein, unless otherwise specified, includes but is not limited to methyl, hexyl, propyl, butyl, etc. C1-C4 alkyl means that the group contains 1-4 carbon atoms.

[0050] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0051] Embodiment 1:

[0052]

[0053] The above compound G3 was prepared according to the following method:

[0054] Step S1:

[0055]

[0056] Under nitrogen protection, CP8557-SM1 (122 g, 596 mmol, 1.1 eq) was added to the reaction vessel, dissolved in tetrahydrofuran (500 mL), cooled to -78 ° C, n-BuLi (260 mL, 650 mmol, 1.2 eq) was added dropwise, and stirred at -78 ° C for 1 hour. CP8557-SM2 (140 g, 542 mmol, 1.0 eq) was dissolved in tetrahydrofuran (250 mL) and added dropwise to the reaction system. After the dropwise addition was completed, the temperature was raised to room temperature and stirred for 8 hours.

[0057] Saturated ammonium chloride solution was added to terminate the reaction, and the organic phase was collected and dried by adding anhydrous magnesium sulfate. The solvent was removed by a rotary evaporator, and the solid was dried to obtain 177 g of crude product with a yield of 85%, which was directly used for the next step without purification.

[0058] Step S2:

[0059]

[0060] Under nitrogen protection, CP8557-ZJ1 (175 g, 455 mmol, 1.0 eq) was dissolved in 500 mL of dichloromethane, cooled to 0°C, and methanesulfonic acid (87.5 g, 910 mmol, 2 eq) was added dropwise. After the addition, the mixture was naturally warmed to room temperature and stirred for 30 minutes. The reaction progress was monitored by TLC plate until the reaction of the raw material completely stopped.

[0061] The reaction solution was added with ethanol, concentrated under reduced pressure to remove dichloromethane, the precipitated solid was filtered, and the filter cake was collected to obtain a crude product. The crude product was added with ethanol / toluene = 9:1 (500 mL), heated to 80°C and stirred overnight, cooled to room temperature naturally, filtered, and the filter cake was collected and dried to obtain 140 g of an intermediate with a yield of 84%.

[0062] Step S3:

[0063]

[0064] Under nitrogen protection, CP8557-ZJ2 (120 g, 327 mmol, 1 eq), silver carbonate (18 g, 65.4 mmol, 0.2 eq), potassium carbonate (45.2 g, 327 mmol, 1 eq) were added to the reaction bottle, 120 ml of toluene was added, and the mixture was stirred evenly. Diphenylcyclohexylphosphine (44 g, 163.5 mmol, 0.5 eq) and heavy water (130 g) were added, and the mixture was stirred and refluxed at 100 ° C for 24 hours.

[0065] The reaction solution was separated, the aqueous phase was extracted twice with ethyl acetate, the combined organic phases were dried, and spin-dried to obtain 116 g of product with a yield of 96%.

[0066] Step S4:

[0067]

[0068] Under nitrogen protection, CP8557-ZJ3 (116 g, 315 mmol, 1 eq), sodium tert-butoxide (30.3 g, 315 mmol, 1 eq), deuterated dimethyl sulfoxide (265 g, 3.15 mol, 10 eq) were added to the reaction bottle, and 500 mL of tetrahydrofuran was added and stirred at 80°C for 48 hours.

[0069] After cooling to room temperature, tetrahydrofuran was removed by rotary evaporation, 1L of water was added and stirred evenly, and then 300mL of ethyl acetate was added to extract the liquid, and the mixture was repeated 4 times. The combined organic phase was washed with brine twice and dried. The crude product was spin-dried to obtain a crude product. 500mL of ethanol was added to the crude product for pulping, and the filter cake was collected by filtration and dried to obtain 95g of the product, with a yield of 81%.

[0070] Step S5:

[0071]

[0072] Under nitrogen protection, CP8557-SM3 (100 g, 337 mmol, 1 eq), phenylboric acid (45.2 g, 370 mmol, 1 eq), potassium carbonate (93 g, 674 mmol, 3 eq) and tetrakistriphenylphosphine palladium (5.84 g, 5 mmol, 0.015 eq) were added to the reaction bottle, and 900 mL of toluene, 450 mL of ethanol and 270 mL of water were added, and the mixture was stirred and refluxed at 80 ° C for 8 hours. The reaction progress was monitored by HPLC until the reaction of the raw materials was completely stopped.

[0073] The liquid was separated, and 300 mL of ethyl acetate was added to the aqueous phase for extraction and separation, and the combined organic phase was washed twice with brine and dried to obtain 83 g of product with a yield of 99%.

[0074] Step S6:

[0075] Under nitrogen protection, CP8557-ZJ6 (83 g, 337 mmol, 1 eq), sodium tert-butoxide (32.4 g, 337 mmol, 1 eq), deuterated dimethyl sulfoxide (283 g, 3.37 mol, 10 eq) were added to the reaction bottle, and 500 mL of tetrahydrofuran was added and stirred at 80°C for 48 hours.

[0076] After cooling to room temperature, tetrahydrofuran was removed by rotary evaporation, 1L of water was added and stirred evenly, and then 500mL of ethyl acetate was added to extract the liquid, and the mixture was repeated 4 times. The combined organic phase was washed twice with brine and dried. The crude product was spin-dried to obtain a crude product. The crude product was purified by column chromatography (petroleum ether) to obtain 69g of product, with a yield of 82%.

[0077] Step S7:

[0078]

[0079] Under nitrogen protection, CP8557-ZJ7 (65 g, 260 mmol, 1 eq), CP8557-SM6 (60 g, 286 mmol, 1.1 eq) and sodium tert-butoxide (50 g, 520 mol, 2 eq) were added to the reaction bottle, 800 mL of toluene was added, and tri-tert-butylphosphine (19.5 mL, 0.04 eq) and Pd2(dba)3 (4.76 g, 5.2 mmol, 0.02 eq) were added, and the temperature was raised to 105°C and stirred under reflux for 4 hours. The reaction progress was monitored by HPLC until the reaction of the raw materials was completely stopped.

[0080] The reaction solution was passed through silica gel while hot, and the filtrate was dried by rotary evaporation to obtain a crude product. The crude product was purified by ethanol beating to obtain 80 g of product with a yield of 81%.

[0081] Step S8:

[0082]

[0083] Under nitrogen protection, CP8557-ZJ4 (45 g, 121 mmol, 1 eq), CP8557-ZJ5 (45.8 g, 121 mmol, 1 eq) and sodium tert-butoxide (17.4 g, 181 mol, 1.5 eq) were added to the reaction bottle, and 500 mL of toluene was added, and palladium acetate (0.55 g, 2.42 mmol, 0.02 eq) and 2-dicyclohexylphosphine-2', 4', 6'-triisopropylbiphenyl (2.3 g, 4.84 mmol, 0.04 eq) were added, and the temperature was raised to 105 ° C. and stirred under reflux for 4 hours. The reaction progress was monitored by HPLC until the reaction of the raw materials was completely stopped.

[0084] The reaction solution was passed through silica gel while hot, and the filtrate was dried by rotary evaporation to obtain a crude product. The crude product was slurried once with ethanol to precipitate solids, and the solid product obtained by filtration was purified by recrystallization of toluene and ethanol (1:1) for 5 times to obtain 57.3 g of product, with a yield of 66.2% and a purity of 99.95%.

[0085] The following compounds G2, G4, G10, G11, G17, G18, G24, G31, G34, G35, G38, G40, G42, G44, G47, G49, G50, G52, G55, G59, G67, G68, G69, G72, G73, G79, G81, G82, G83, G86, G88, G92, G93, G94, G95, G96, G97, G98, G99, G100, G111, G122, G133, G134, G135, G136, G137, G138, G139, G140, G141, G142, G143, G144, G145 94, G98, G100, G106, G107, G108, G111, G112, G118, G120, G121, G125, G126, G127, G129, G132, G133, G134, G137, G141, G143, G146, G148, G149 and G153, see Table 1-1, Table 1-2 and Table 1-3 below for details.

[0086] Table 1-1

[0087]

[0088]

[0089]

[0090]

[0091] Table 1-2

[0092]

[0093]

[0094]

[0095]

[0096] Table 1-3

[0097]

[0098]

[0099]

[0100]

[0101]

[0102] The synthesis and identification results of the compounds prepared above and in Table 1-1, Table 1-2 and Table 1-3 are shown in Table 2 below.

[0103] Table 2

[0104]

[0105]

[0106] The above materials were subjected to basic performance tests, including thermal weight loss temperature Td and melting point temperature Tm. The test results are shown in Table 3 below.

[0107] Compounds G2, G3, G4, G10, G11, G17, G18, G24, G31, G34, G35, G38, G40, G42, G44, G47, G49, G50, G52, G55, G59, G67, G68, G69, G72, G73, G79, G81, G82, G83, G86, G88, G92, G94, G98 The test results of thermal weight loss temperature Td and melting point temperature Tm of G100, G106, G107, G108, G111, G112, G118, G120, G121, G125, G126, G127, G129, G132, G133, G134, G137, G141, G143, G146, G148, G149 and G153 are shown in Table 3:

[0108] Table 3

[0109]

[0110]

[0111] Note: Thermogravimetric temperature Td is the temperature at which the weight loss is 5% in a nitrogen atmosphere, and is measured on a TGA N-1000 thermogravimetric analyzer with a nitrogen flow rate of 10 mL / min. The melting point temperature Tm is measured by differential scanning calorimetry (DSC, Shinco DSC N-650) with a heating rate of 10°C / min.

[0112] It can be seen from the above data that the compound synthesized in the present invention has excellent thermal stability and can meet the requirements for use of organic electroluminescent materials.

[0113] Device performance test:

[0114] Application Example 1:

[0115] The organic electroluminescent device is prepared by the following process:

[0116] ITO was used as the reflective layer anode substrate material, and its surface was treated with water, acetone, and N2 plasma in sequence;

[0117] On top of the ITO anode substrate, 10 nm of HT-1 doped with 5% NDP-9 was deposited to form a hole injection layer (HIL);

[0118] 100 nm of HT-1 was evaporated on the hole injection layer (HIL) to form the first hole transport layer (HTL);

[0119] Vacuum evaporating the compound G3 of the present invention on the first hole transport layer (HTL) to form a second hole transport layer (GPL) with a thickness of 10 nm;

[0120] GH-2 and GH-1 were co-evaporated at a ratio of 5:5 (mass ratio) as the main luminescent materials, and GD-1 was evaporated as the doping material (the amount of GD-1 was 8% of the total weight of GH-1 and GH-2) on the second hole transport layer (GPL) to form a luminescent layer with a thickness of 20 nm;

[0121] HB-1 was evaporated onto the light-emitting layer to obtain a hole blocking layer (HBL) with a thickness of 20 nm;

[0122] ET-1 and LiQ were co-evaporated onto the hole blocking layer (HBL) in a ratio of 5:5 to obtain an electron transport layer (ETL) with a thickness of 30 nm;

[0123] Magnesium (Mg) and silver (Ag) were mixed in a ratio of 9:1 and evaporated onto the electron transport layer (ETL) to form an electron injection layer (EIL) with a thickness of 50 nm;

[0124] Thereafter, silver (Ag) is evaporated onto the electron injection layer to form a cathode with a thickness of 100 nm, and DNTPD with a thickness of 50 nm is deposited on the cathode sealing layer;

[0125] In addition, the cathode surface is sealed with a UV curable adhesive and a seal cap containing a dehumidifier to protect the organic electroluminescent device from being affected by oxygen or moisture in the atmosphere, thereby preparing an organic electroluminescent device.

[0126] The structural formula of the compound used in the above process is as follows:

[0127]

[0128]

[0129] Application Example 2-58:

[0130] Compounds G2, G3, G4, G10, G11, G17, G18, G24, G31, G34, G35, G38, G40, G42, G44, G47, G49, G50, G52, G55, G59, G67, G68, G69, G72, G73, G79, G81, G82, G83, G86, G88, G92, G94, G98, G100, G106 , G107, G108, G111, G112, G118, G120, G121, G125, G126, G127, G129, G132, G133, G134, G137, G141, G143, G146, G148, G149 and G153 are used as the second hole transport layer materials, and the other parts are consistent with the conditions in Application Example 1, to produce the organic electroluminescent device of Application Example 2-58.

[0131] The luminescent color of the organic electroluminescent device of Application Example 2-58 has an x ​​value in the range of about 0.21-0.28 and a y value in the range of about 0.68-0.75 in the CIE coordinates.

[0132] Comparative Examples 1-5:

[0133] Compounds D1, D2, D3, D4 and D5 were used as the second hole transport layer materials respectively, and other parts were in the same conditions as those in Application Example 1 to prepare organic electroluminescent devices of Control Examples 1-5.

[0134] The structures of the compounds D1, D2, D3, D4 and D5 are as follows:

[0135]

[0136] The characteristics of the organic electroluminescent device manufactured in the above application example and the organic electroluminescent device manufactured in the control example are as follows: 2 The results were shown in Table 4 below.

[0137] Table 4

[0138]

[0139]

[0140]

[0141] It can be seen from the above table that the introduction of deuterium at certain sites of the compound improves the luminous efficiency of the organic electroluminescent device at the same current density, reduces the starting voltage of the device, and reduces the power consumption of the device. However, it can also be seen that the introduction of deuterium at different sites of this type of compound will result in different degrees of improvement in the luminous efficiency of the corresponding organic electroluminescent device at the same current density.

[0142] Compared with the above embodiments, when the deuterated sites are distributed in an meta-position on the benzene ring connected to the amino group N atom on diphenylfluorene, the luminous efficiency of the device is significantly improved. At the same time, the modification of the compound by methyl, especially deuterated methyl, further improves the luminous efficiency of the corresponding device, such as representative compounds G3, G11, G17, G31, G35, etc., while compared with control examples 4 and 5 and the compounds of the present invention with more deuterated groups R2 and R3, the luminous efficiency of the corresponding device is not significantly improved.

[0143] Because the introduction of deuterium will significantly increase the synthesis cost of the material, in general, the more deuterium there is, the higher the cost, and the more deuterium positions there are, the more complicated the process is. Therefore, considering the process and production cost, identifying the active sites of the deuterium reaction of the compound and the sites with high electron cloud density, and introducing deuterium at the corresponding positions can more effectively improve the performance of materials and devices, save production costs, and achieve better economic benefits.

[0144] Next, the organic electroluminescent devices prepared in the control examples 1-5 and the application examples 1-11, the application examples 22-27 and the application examples 56-58 were further subjected to luminescence lifetime tests to obtain the luminescence lifetime T97% data (the time when the luminescence brightness decreases to 97% of the initial brightness). The test equipment is the TEO luminescent device lifetime test system. The lifetime test results are based on the control example 1.

[0145] As shown in Table 5:

[0146]

[0147]

[0148] As can be seen from the above table, compared with control examples 1-3, the compounds of the present invention are used in organic electroluminescent devices, and the service life of the devices is greatly improved at the same current density. Compared with control examples 4-5 in which the compounds have more deuterated positions, the organic electroluminescent devices using the compounds of the present invention have basically the same service life at the same current density. However, due to the reduction in the number of deuterated positions in the materials, the cost of production materials can be effectively reduced.

[0149] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. An organic electroluminescent compound, characterized in that: It has the structural formula shown in formula (1): in: R1 is a substituted or unsubstituted C1-C4 alkyl group, and the substituent of R1 is selected from deuterium, methyl or deuterated methyl; R2 and R3 each independently represent a substituted or unsubstituted C6-C30 aryl group, R2 and R3 are different groups, and one of them is selected from a substituted or unsubstituted fluorenyl group; The substituents of R2 and R3 are independently selected from one or more of methyl, deuterated methyl, phenyl substituted by methyl and phenyl substituted by deuterated methyl.

2. The organic electroluminescent compound according to claim 1, characterized in that Formula (1) contains 1 to 3 deuterated methyl groups or 3 to 12 deuterium atoms.

3. The organic electroluminescent compound according to claim 1, characterized in that The R1 is a substituted or unsubstituted methyl, ethyl, isopropyl, or tert-butyl group, and its substituent is selected from deuterium or deuterated methyl; The R2 and R3 each independently represent a substituted or unsubstituted phenyl, biphenyl, fluorenyl, naphthyl or carbazolyl group; 4. The organic electroluminescent compound according to claim 1, characterized in that The R1 is selected from one of the following groups: deuterated methyl, deuterated ethyl, deuterated isopropyl, tert-butyl or deuterated tert-butyl; One of R2 and R3 is selected from the following substituted or unsubstituted groups: biphenyl, biphenyl substituted by methyl, biphenyl substituted by deuterated methyl.

5. The organic electroluminescent compound according to claim 1, characterized in that The R1 is selected from one of the following groups: deuterated methyl, deuterated ethyl, deuterated isopropyl or tert-butyl; One of R2 and R3 is dimethylfluorene, and the other is a diphenyl group substituted with at least one methyl group or at least one deuterated methyl group.

6. The organic electroluminescent compound according to claim 1, characterized in that The structural formula of R1 is Where * indicates the attachment site.

7. The organic electroluminescent compound according to claim 1, characterized in that The R2 and R3 are each independently selected from a group represented by formula (1-1), formula (1-2) or formula (1-3): wherein R4 and R5 each independently represent a methyl group or a deuterated methyl group; m and n independently represent 0 or 1; * indicates the attachment site.

8. The organic electroluminescent compound according to claim 1, characterized in that Any one of the following compounds:

9. An organic electroluminescent device, comprising an anode, a cathode and an organic layer formed between the anode and the cathode, wherein the organic layer contains the organic electroluminescent compound according to any one of claims 1 to 8.

10. The organic electroluminescent device according to claim 9, characterized in that: The organic layer comprises a hole injection layer, a first hole transport layer, a second hole transport layer, a light emitting layer, a hole blocking layer, an electron transport layer and an electron injection layer, wherein the first hole transport layer or the second hole transport layer contains the organic electroluminescent compound according to any one of claims 1 to 8.