Sheath-core composite fiber and preparation method thereof

By using leather-core composite anti-permeable fibers in textiles, nanoparticles are used to enhance the light reflection and absorption capacity of the fibers, the problem that textiles are difficult to take into account between lightness, clearance and ultraviolet functions is solved, and efficient anti-permeable and ultraviolet effects are achieved, while maintaining the lightness and comfort of the fibers.

CN119980511APending Publication Date: 2025-05-13新兴际华(上海)工程科技研究院有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510154175.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-02-12
Publication Date
2025-05-13

AI Technical Summary

Technical Problem

When existing textiles pursue lightweight, perspective-proof and UV-proof functions, it is difficult to take into account comfort and production costs, and the multi-layer weaving method is complex and difficult to balance perspective-proof, sweat-free and comfortable.

Method used

The skin-core composite anti-permeable fiber is used, which consists of a core layer made of a low melting point polymer and a nanoparticle-enhanced cortex. Through the addition of nanoparticles in the cortex, the fibers can reflect, absorb and scatter the visible light, thereby achieving anti-permeability and ultraviolet rays, while maintaining the light and comfortable properties.

Benefits of technology

While ensuring thinness, leather-core composite fiber products have excellent anti-perspectiveness, anti-UV and hidden sweat marks, solving the problem that traditional textiles are difficult to balance between functionality and comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a sheath-core composite fiber and a preparation method thereof. The skin-core composite anti-permeable fiber is prepared from a core layer and a skin layer, the raw material of the core layer is a polymer A, the raw material of the skin layer comprises a polymer B and nanoparticles, and the addition amount of the nanoparticles is 2-20 wt% of the raw material of the skin layer. The nano particles are added into the raw materials of the skin layer, so that the reflection, absorption and scattering of visible light by the fiber are increased, and the quantity of light penetrating through the textile is reduced, so that the light and thin performance of the product is ensured, and the product still has excellent anti-perspective performance and ultraviolet resistance and has a sweat mark hiding effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of textile technology, and specifically relates to a sheath-core composite fiber and a preparation method thereof. Background Art

[0002] For some specific application scenarios, such as summer light clothing, outdoor clothing, etc., people require textiles to be light and thin to meet the comfort and fashion of wearing, and also expect them to have excellent sweat-free, anti-see-through, and UV protection functions to protect personal privacy and physical health.

[0003] Most textiles on the market today often have difficulty striking a good balance between lightness and functionality. Traditional fabrics usually achieve anti-see-through effects by increasing the thickness of the fabric or using a special multi-layer woven structure, which inevitably leads to a worse feel and increased heaviness of the textiles, affecting the comfort and aesthetics of wearing. In addition, the multi-layer woven method has high production costs and complex processes, and it is difficult to find a balance between anti-see-through, no sweat marks and comfort.

[0004] Therefore, it is urgent to study a kind of anti-penetration fiber for the preparation of light, comfortable, anti-see-through and sweat-free fabrics. Summary of the invention

[0005] In order to overcome the defect that traditional fabrics usually achieve anti-see-through effects by increasing the fabric thickness or adopting a special multi-layer woven structure and cannot take into account both lightness and functionality, the present invention provides a skin-core composite anti-see-through fiber and a preparation method thereof.

[0006] The core-skin composite anti-permeability fiber provided by the present invention is made of a core layer and a skin layer, wherein the core layer raw material is polymer A, and the skin layer raw material includes polymer B and nanoparticles, wherein the added amount of the nanoparticles is 2-20wt% of the skin layer raw material (based on the total weight of the skin component being 100, the weight of the nanoparticles is not less than 2%).

[0007] The addition of nanoparticles in polymer B can increase the reflection, absorption and scattering of visible light by the fiber, and reduce the amount of light passing through the textile, so that the product can ensure lightness and thinness while still having excellent anti-see-through and UV protection, and can hide sweat marks.

[0008] The polymer A and polymer B are both high polymers with a melting point lower than the decomposition temperature, such as polyester, nylon, polypropylene, etc.; The polymer A and polymer B may be the same polymer or different polymers; The average particle size of the nanoparticles is 50-500nm; The nanoparticles are one or more of titanium dioxide, silicon dioxide, calcium carbonate, barium sulfate, zinc oxide and the like; The amount of the nanoparticles added is 2%-20% of the total weight of the cortex; In the core-skin composite anti-penetration fiber, the weight ratio of the core layer to the skin layer is 1:4-4:1, specifically 3:7 or 4:6.

[0009] The single fiber fineness of the core-sheath composite anti-permeability fiber is 0.1-5 dtex.

[0010] The above-mentioned skin-core composite anti-penetration fiber is prepared by a method comprising the following steps: 1) Mix the masterbatch containing nanoparticles with polymer B and add them into the cortex material storage tank as the cortex raw material; 2) Add polymer A into the core layer storage tank as the core layer raw material; 3) The core layer raw material and the skin layer raw material are extruded through the core layer screw and the skin layer screw extruder respectively. After melting, they are extruded into the skin-core composite spinning assembly according to a certain mass ratio to form filaments. After the filaments are stretched and deformed, the skin-core composite anti-permeability fiber is obtained.

[0011] No matter what form the processed fiber exists in, it will not affect the anti-see-through, UV protection and sweat mark hiding effects of the skin-core composite fiber.

[0012] The yarn and fabric made from the above-mentioned core-sheath composite barrier fiber also fall within the protection scope of the present invention.

[0013] The fabric can be made from yarn made from the core-sheath composite anti-permeability fiber using a flat knitting machine, a circular knitting machine, a warp knitting machine, or a weaving machine.

[0014] The fabric has excellent lightness, thinness, UV protection and perspective resistance, and has the effect of hiding sweat marks.

[0015] The present invention adds nanoparticles to the skin material to increase the reflection, absorption and scattering of visible light by the fiber and reduce the amount of light passing through the textile, so that the product has excellent anti-see-through and anti-ultraviolet properties while ensuring lightness and thinness, and has the effect of hiding sweat marks. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a schematic diagram of the cross-section of the fiber prepared in Example 1 of the present invention.

[0017] Figure 2 This is a schematic diagram of the cross-section of the fiber prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0018] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.

[0019] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.

[0020] The anti-see-through performance, UV protection performance and sweat stain hiding effect described in the following examples are measured by the following methods: (1) Anti-see-through performance Test standard: GB / T 42698-2023 Testing and evaluation of anti-see-through properties of textiles Test equipment: colorimeter, white board for test, black board for test Test method: Take 3 samples of each fabric, the size of the sample should be able to fully cover the test hole of the instrument, put the back of the sample flat against the white board, and the front of the sample facing the test hole of the colorimeter, and measure the lightness value L w , place the back of the sample flat against the blackboard, with the front facing the colorimeter test hole, and measure the lightness value L b , Anti-perspective index S=L b / L w Among them, the anti-perspective index S is less than 93, and the anti-perspective performance is poor; 93≤S<97, it has certain anti-perspective performance; S≥97, it has good anti-perspective performance.

[0021] (2) Anti-ultraviolet performance and sweat stain hiding effect Test standard: GB / T 18830-2009 Evaluation of UV protection performance of textiles Test equipment: Spectrophotometer UV-3150 Test method: Take 4 samples of each fabric and place them in front of the entrance of the integrating sphere to obtain the UPF value. When UPF>50, the sample has good UV protection. In addition, the smaller the difference in UPF value between dry and wet states, the better the sweat stain hiding effect of the fabric.

[0022] Example 1: Preparation of sheath-core composite anti-penetration fiber The preparation of the skin-core composite anti-penetration fiber includes the following steps: Step 1: Mix the masterbatch with a titanium dioxide content of 30wt% (the average particle size of titanium dioxide is 500nm) and the full-dull nylon chips in a mass ratio of 7:97 and add them into the skin storage tank. The mixture with a titanium dioxide content of 2wt% is used as the raw material of skin B; Step 2: Add the full-dull nylon slices into the core layer storage tank as the raw material of the core layer A; Step 3: The core layer raw material and the skin layer raw material are respectively passed through the core layer screw extruder (the temperature of each zone is 290℃, 300℃, 300℃) and the skin layer screw extruder (the temperature of each zone is 290℃, 300℃, 300℃), and distributed through the pipeline into the spinning box with a temperature of 310℃, and then filtered through the double-layer filter screen in the skin-core composite spinning assembly at a mass ratio of 1:4, and then sprayed out from the circular spinneret hole to form a tow, and then cooled by side blowing, bundled oiling, stretched and heat-set, and finally wound to obtain a skin-core composite fiber with a single fiber fineness of 5dtex (cross-section as shown Figure 1 55D yarn composed of 1.6 wt% silica particles.

[0023] Step 4: The obtained yarn is knitted into a knitted fabric using a small circular weft machine. The relevant properties are shown in Table 1.

[0024] Example 2: Preparation of sheath-core composite anti-penetration fiber Step 1: Mix the masterbatch containing 30wt% zinc oxide particles (average zinc oxide particle size is 50nm) and the semi-dull nylon slices in a mass ratio of 67:33 and add them into the cortex storage tank. The mixture with a zinc oxide content of 20wt% is used as the raw material of cortex B; Step 2: Add the semi-dull polyester slices into the core layer storage tank as the raw material of the core layer A; Step 3: The core layer raw material and the skin layer raw material are respectively passed through the core layer screw extruder (the temperature of each zone is 285℃, 290℃, and 295℃) and the skin layer screw extruder (the temperature of each zone is 290℃, 300℃, and 300℃), and are distributed through pipelines into the spinning box with a temperature of 300℃ and 310℃, and then filtered through the double-layer filter screen in the skin-core composite spinning assembly at a mass ratio of 4:1, and then sprayed out from the pentagonal spinneret to form a tow, and then cooled by side blowing, bundled oiling, stretched and heat-set, and finally wound to obtain a skin-core composite fiber with a single fiber fineness of 0.1dtex (cross-section as shown in Figure 2 40D yarn composed of 200% nylon (as shown in FIG. 1 ). In the yarn, the silica particles account for 4 wt%.

[0025] Step 4: The obtained yarn is knitted into a knitted fabric using a small circular weft machine. The relevant properties are shown in Table 1.

[0026] Example 3: Preparation of sheath-core composite anti-penetration fiber Step 1: Mix the masterbatch containing 30wt% silica particles (average silica particle size is 200nm) and the full-dull polyester chips in a mass ratio of 4:6 and add them into the cortex storage tank. The mixed mixture with a silica content of 12wt% is used as the raw material of cortex B; Step 2: Add the full-dull polyester slices into the core layer storage tank as the raw material of the core layer A; Step 3: The core layer raw material and the skin layer raw material are respectively passed through the core layer screw extruder (the temperature of each zone is 285°C, 290°C, and 295°C) and the skin layer screw extruder (the temperature of each zone is 285°C, 290°C, and 295°C), and are distributed through pipelines into a spinning box with a temperature of 300°C. Then, they are filtered through a double-layer filter screen in the skin-core composite spinning assembly at a mass ratio of 1:1, and then sprayed out from the circular spinneret hole to form a tow, and then cooled by side blowing, bundled and oiled, stretched and heat-set, and finally wound to obtain a skin-core composite fiber with a single fiber fineness of 1.1dtex (cross-section as shown in FIG. Figure 1 50D yarn composed of 100% nylon (as shown in FIG. 1 ). In the yarn, the silica particles account for 6 wt%.

[0027] Step 4: The obtained yarn is knitted into a knitted fabric using a small circular weft machine. The relevant properties are shown in Table 1.

[0028] Comparative Example 1 Step 1: Mix the masterbatch containing 30wt% silica particles (average silica particle size is 200nm) and the full matte polyester chips in a mass ratio of 1:4 and add them into the storage tank. After being extruded by a screw extruder (temperatures in each zone are 285℃, 290℃, and 295℃), they are distributed through a pipeline into a spinning box at a temperature of 300℃, and sprayed out from a circular spinneret hole to form a tow. After side-blowing cooling, bundling and oiling, drawing and heat setting, and finally winding, a sheath-core composite fiber with a single-filament fineness of 1.1dtex (cross-section as shown in FIG. 1 ) is obtained. Figure 1 50D yarn composed of 100% nylon (as shown in FIG. 1 ). In the yarn, the silica particles account for 6 wt%.

[0029] Step 2: The obtained yarn is knitted into a knitted fabric using a small circular weft machine. The relevant properties are shown in Table 1.

[0030] Comparative Example 2 The difference from Example 3 is that the raw materials of the skin layer B and the core layer A are interchanged. In the prepared yarn, the silica particles account for 6wt%. The obtained yarn is knitted using a small circular weft machine, and its related properties are shown in Table 1.

[0031] Table 1 Fabric performance test results

[0032] From the results in Table 1, it can be seen that the knitted fabrics in Examples 1-3 all have good anti-see-through, anti-ultraviolet performance and sweat stain hiding effects. Except for the distribution of silica particles, other conditions such as the proportion of silica particles in Example 3 are the same as those in Comparative Examples 1 and 2. In terms of effect, Example 3>Comparative Example 2>Comparative Example 1. This is because Example 3 adds nanoparticles into the cortex raw material, which can directly reflect, absorb and scatter visible light, so the effect is the best; Comparative Example 2 adds nanoparticles into the core layer raw material, and some visible light will penetrate from the cortex of each fiber, so its effect is slightly worse; Comparative Example 1 adds nanoparticles uniformly to the entire fiber, which reduces the concentration of particles, resulting in the worst effect.

[0033] The present invention has been described in detail above. For those skilled in the art, without departing from the purpose and scope of the present invention, and without the need to carry out unnecessary experimental conditions, the present invention can be implemented in a wide range under equivalent parameters, concentrations and conditions. Although the present invention provides specific embodiments, it should be understood that the present invention can be further improved. In a word, according to the principles of the present invention, the application is intended to include any changes, uses or improvements to the present invention, including departure from the disclosed scope in the application, and changes made with conventional techniques known in the art.

Claims

1. A core-skin composite anti-penetration fiber, made of a core layer and a skin layer, wherein the core layer material is polymer A, and the skin layer material includes polymer B and nanoparticles, wherein: The added amount of the nanoparticles is 2-20wt% of the skin layer raw material.

2. The core-sheath composite anti-permeability fiber according to claim 1, characterized in that: The polymer A and polymer B are both high polymers with a melting point lower than the decomposition temperature; the polymer A and polymer B are the same polymer or different polymers.

3. The core-sheath composite anti-permeability fiber according to claim 1, characterized in that: The average particle size of the nanoparticles is 50-500nm; The nanoparticles are one or more of titanium dioxide, silicon dioxide, calcium carbonate, barium sulfate, and zinc oxide particles.

4. The core-sheath composite anti-penetration fiber according to claim 1, characterized in that: In the core-skin composite anti-penetration fiber, the weight ratio of the core layer to the skin layer is 1:4-4:

1.

5. The core-sheath composite anti-permeability fiber according to claim 1, characterized in that: The single fiber fineness of the core-sheath composite anti-penetration fiber is 0.1-5 dtex.

6. A method for preparing the core-sheath composite barrier fiber according to any one of claims 1 to 5, comprising the following steps: 1) Mix the masterbatch containing nanoparticles with polymer B and add them into the cortex material storage tank as the cortex raw material; 2) Add polymer A into the core layer storage tank as the core layer raw material; 3) The core layer raw material and the skin layer raw material are extruded through the core layer screw and the skin layer screw extruder respectively. After melting, they are extruded into the skin-core composite spinning component according to a certain mass ratio to form filaments. After the filaments are stretched and deformed, the skin-core composite anti-permeability fiber is obtained.

7. Yarn or fabric made from the core-sheath composite barrier fiber described in any one of claims 1 to 5.

8. The fabric according to claim 7, characterized in that The fabric is made of yarn made from the core-sheath composite anti-permeability fiber described in any one of claims 1 to 5 using a flat knitting machine, a circular knitting machine, a warp knitting machine, or a weaving machine.