By optimizing the formula and process flow, the aging resistance of acrylate rubber mixed rubber is improved, and the problems of aging and unstable performance of rubber in the harsh environment in the prior art are solved, and better physical and mechanical properties and processing performance are achieved.
Patent Information
- Application Number
- CN202510079945.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-01-18
- Publication Date
- 2025-05-16
AI Technical Summary
The existing acrylate rubber compound is aged, hardened and deteriorated under environmental conditions such as high temperature, high humidity, ozone and ultraviolet rays, and it is difficult to achieve uniform mixing during the production process, resulting in unstable performance.
By optimizing the formulation composition and preparation process, a specific proportion of stearic acid, anti-aging agent, carbon black, mold release agent, plasticizer, accelerator and vulcanizing agent are used, combined with twin-screw refining, starting and vulcanizing process flows, the aging resistance of acrylate rubber is significantly improved.
It significantly improves the aging resistance of acrylate rubber, maintains the physical properties and service life of the rubber, optimizes the physical mechanical properties and processing properties, and ensures the consistency and repeatability of the product.
Smart Images

Figure BDA0005248295260000061 
Figure BDA0005248295260000062 
Figure BDA0005248295260000063
Abstract
Description
Technical Field
[0001] The invention belongs to the field of rubber chemistry and material science, and discloses an aging-resistant acrylic rubber compound and a preparation method thereof. Background Art
[0002] With the development of modern industry, rubber materials have been widely used in many fields, especially in the automotive, aviation, electronics and construction industries. Acrylic rubber has attracted wide attention in the rubber industry in recent years due to its excellent elasticity, wear resistance and excellent anti-aging properties. However, acrylic rubber still faces problems such as aging, hardening and performance degradation in actual use, especially under environmental conditions such as high temperature, high humidity, ozone and ultraviolet rays.
[0003] In order to solve these problems, researchers have been exploring various additives and modification methods to improve the aging resistance of acrylic rubber. Commonly used anti-aging agents include antioxidants, antioxidants and ultraviolet absorbers. At the same time, the use of vulcanizers and accelerators can also help to increase the cross-linking degree of rubber, thereby improving its aging resistance to a certain extent.
[0004] In traditional acrylic rubber compounds, although the performance can be improved by adding various chemical additives, it is often difficult to achieve the desired comprehensive performance due to compatibility issues between different materials and processing losses during the mixing process. In addition, many existing formulas fail to achieve sufficient uniform mixing during the production process, resulting in unstable performance of the materials in actual applications.
[0005] Therefore, developing a new type of aging-resistant acrylic rubber compound, by optimizing the formula composition and preparation process, can not only effectively improve the aging resistance of acrylic rubber, but also ensure the consistency and operability of the compound during the production process, which has become a technical problem that the industry urgently needs to solve.
[0006] In summary, the research and modification of the aging resistance of acrylic rubber, especially the in-depth exploration in material formulation and process optimization, will provide a more solid foundation and support for its application in the field of high-performance materials. Summary of the invention
[0007] The invention provides an aging-resistant acrylic rubber compound and a preparation method thereof, which significantly improves the aging resistance of acrylic rubber by optimizing the formula composition and the preparation process, and solves the problems of unstable performance and accelerated aging in the prior art.
[0008] To achieve the purpose of the invention, the technical solution adopted by the present invention is: an aging-resistant acrylic rubber compound, which is composed of 100 parts of acrylic rubber, 0.5-2 parts of stearic acid, 0.5-2 parts of antioxidant A, 0.5-2 parts of antioxidant B, 40-80 parts of carbon black, 1-5 parts of release agent, 1-6 parts of plasticizer, 0.3-4 parts of accelerator and 0.3-3 parts of vulcanizer.
[0009] According to an aging-resistant acrylic rubber compound, the antioxidant A is one or more of antioxidant 445, antioxidant 405, antioxidant 630F, antioxidant 2246, antioxidant 4010NA, and antioxidant 4020.
[0010] According to an ageing-resistant acrylic rubber compound, the antioxidant B is one or more of antioxidant 245, antioxidant 618, antioxidant 565 and antioxidant GM.
[0011] According to an aging-resistant acrylic rubber compound, the carbon black is one or more of carbon black N330, carbon black N550, carbon black N660, carbon black N774, and carbon black N990.
[0012] According to an aging-resistant acrylic rubber compound, the release agent is one or more of release agent 18D, microcrystalline wax, polyethylene wax, release agent WB212, and release agent FG-200.
[0013] According to an aging-resistant acrylic rubber compound, the plasticizer is one or more of plasticizer TP95, plasticizer TP759, plasticizer RS107, plasticizer RS700, and plasticizer RS735.
[0014] According to an aging-resistant acrylic rubber compound, the accelerator is one or more of accelerator DOTG, accelerator DOTG-75, accelerator XLA-60, accelerator ACT-70, accelerator ACT-55, sodium stearate, and potassium stearate.
[0015] According to an aging-resistant acrylic rubber compound, the vulcanizing agent is one or more of insoluble sulfur, thiocyanuric acid, N,N dicinnamyl-1,-hexanediamine, ammonium benzoate, phthalic anhydride / imidazole, guanidine sulfur, hexamethylenediamine carbamate, isocyanuric acid / trimethyloctadecylammonium bromide, thiocyanuric acid / zinc dibutyldithiocarbamate, diisopropylbenzene peroxide, vulcanizing agent NPC-50, and vulcanizing agent NPC-100.
[0016] According to a method for preparing an aging-resistant acrylic rubber compound, the preparation method comprises the following process:
[0017] S1 weighs 100 parts of raw acrylic rubber and puts it into a twin-screw internal mixer, and mixes it at 80-100°C for 5-10 minutes to ensure that the rubber is evenly mixed and avoid material degradation caused by excessive heating;
[0018] After the S2 internal mixing is completed, the following raw materials are added in sequence: 0.5-2 parts of stearic acid, 0.5-2 parts of antioxidant A, 0.5-2 parts of antioxidant B, 40-80 parts of carbon black, 1-5 parts of release agent, 1-6 parts of plasticizer, and the internal mixing is continued at 80-100°C for 5-10 minutes until all materials are evenly distributed; after the internal mixing is completed, the rubber compound is discharged from the internal mixer in time to avoid degradation caused by long-term retention, and the rubber compound is cooled to 20-25°C;
[0019] S3: Transfer the cooled rubber material to a two-roller mixing mill, set the roller distance to 2-4 mm, start the mixing mill and stir at a speed of 60-80 rpm / min to ensure that the rubber material is evenly dispersed on the rollers, and stir for 30-40 minutes; then cool the rubber material to 80-100°C;
[0020] S4: Put the rubber material back into the open mill, add 0.3-4 parts of accelerator and 0.3-3 parts of vulcanizer, keep the rubber material evenly stirred in the open mill for 3-5 minutes to ensure that the accelerator and vulcanizer are evenly distributed; after stirring evenly, set the open mill to perform 4-6 thin-pass operations;
[0021] S5 After the thin pass is completed, adjust the roller gap to 1-2 mm, remove the mixed rubber from the open mixer, and place it on a flat workbench to wait for the rubber to cool to 20-25°C;
[0022] S6: Place the mixed rubber into the configured mold to ensure that the mold is well closed to avoid leakage; place the mold into a flat vulcanizer, set the vulcanization temperature to 170-200°C, the vulcanizer pressure to 20MPa, and the initial vulcanization time to 10-20 minutes to ensure that the rubber fully fills the mold to avoid defects; after the initial vulcanization is completed, take the mold out of the flat vulcanizer, cool it to 80-100°C, and place the mold in a preheated oven for secondary vulcanization; set the temperature in the oven to 170-200°C and the vulcanization time to 2-6 hours to ensure that the rubber is evenly heated under the flow of hot air;
[0023] After the second stage vulcanization is completed in step S7, the mold is taken out, and after the mold is cooled to 20-25°C, the mold is opened to obtain the desired mixed rubber. Compared with the prior art, the present invention has the following advantages:
[0024] (1) Significantly improve aging resistance: By optimizing the formula and rationally selecting antioxidants and anti-aging agents, the aging process of rubber in high temperature, humidity and ultraviolet light environments can be effectively delayed, thereby maintaining the physical properties and service life of the rubber.
[0025] (2) Excellent physical and mechanical properties: By using high-quality carbon black and plasticizers, the elasticity, strength and wear resistance of rubber are improved, so that it can still maintain excellent mechanical properties under harsh conditions.
[0026] (3) Good processing performance: The optimized preparation process ensures the uniformity of the mixed rubber during the production process, improves the processing performance of the rubber, and reduces the energy consumption and time during the processing.
[0027] (4) Improve product consistency: Under certain manufacturing process conditions, the prepared rubber compound has high consistency and repeatability, ensuring the stability of product performance in large-scale production and reducing production defects. DETAILED DESCRIPTION
[0028] Embodiment 1
[0029] Weigh 100 parts of acrylic rubber raw rubber and put it into a twin-screw internal mixer, and mix it at 80°C for 5 minutes to ensure that the rubber is evenly mixed and avoid material degradation caused by overheating; after the internal mixing is completed, add the following raw materials in sequence: 0.5 parts of stearic acid, 0.5 parts of antioxidant A, 0.5 parts of antioxidant B, 40 parts of carbon black, 1 part of release agent, and 1 part of plasticizer, and continue to mix at 80°C in the internal mixer for 5 minutes until all materials are evenly distributed; after the internal mixing is completed, discharge the rubber from the internal mixer in time to avoid degradation caused by long-term residence, and cool the rubber to 20°C; transfer the cooled rubber to a two-roll open mill, set the roller distance to 2mm, start the open mill and stir at a speed of 60rpm / min to ensure that the rubber is evenly dispersed on the roller, and the stirring time is 30 minutes; then cool the rubber temperature to 80°C; put the rubber back into the open mill, add 0.3 parts of accelerator and 0.3 parts of vulcanizer, and keep the rubber evenly dispersed in the open mill Stir evenly for 3 minutes to ensure that the accelerator and vulcanizer are evenly distributed; after stirring evenly, set the open mill to perform 4 thin-pass operations; after the thin-pass operation is completed, adjust the roller gap to 1mm, remove the mixed rubber from the open mill, and place it on a flat workbench until the rubber cools to 20°C; put the mixed rubber into the configured mold to ensure that the mold is well closed to avoid leakage; put the mold into a flat vulcanizer, set the vulcanization temperature to 170°C, the vulcanizer pressure to 20MPa, and the initial vulcanization time to 10 minutes to ensure that the rubber fully fills the mold to avoid defects; after the initial vulcanization is completed, take out the mold from the flat vulcanizer, cool it to 80°C, and put the mold into a preheated oven for two-stage vulcanization; set the temperature in the oven to 170°C and the vulcanization time to 2 hours to ensure that the rubber is evenly heated under the flow of hot air; after the two-stage vulcanization is completed, take out the mold, wait for the mold to cool to 20°C, open the mold, and obtain the required mixed rubber.
[0030] Embodiment 2
[0031] Weigh 100 parts of raw acrylic rubber and put them into a twin-screw internal mixer. Mix them at 90°C for 8 minutes to ensure that the rubber is evenly mixed and avoid material degradation caused by overheating. After the mixing is completed, add the following raw materials in sequence: 1 part of stearic acid, 1 part of antioxidant A, 1 part of antioxidant B, 60 parts of carbon black, 3 parts of release agent, and 3 parts of plasticizer. Continue to mix them at 90°C in the internal mixer for 8 minutes until all materials are evenly distributed. After the mixing is completed, discharge the rubber from the internal mixer in time to avoid degradation caused by long-term residence, and cool the rubber to 23°C. Transfer the cooled rubber to a two-roll open mill, set the roller distance to 3mm, start the open mill and stir at a speed of 70rpm / min to ensure that the rubber is evenly dispersed on the roller. The stirring time is 35 minutes. Then cool the rubber temperature to 90°C. Put the rubber back into the open mill, add 2 parts of accelerator and 2 parts of vulcanizer, and keep the rubber evenly stirred in the open mill for 4 minutes. , ensure that the accelerator and vulcanizer are evenly distributed; after stirring evenly, set the open mill to perform 5 thin-pass operations; after the thin-pass operation is completed, adjust the roller gap to 1.5mm, remove the mixed rubber from the open mill, and place it on a flat workbench, and wait for the rubber to cool to 22°C; put the mixed rubber into the configured mold to ensure that the mold is well closed to avoid leakage; put the mold into the flat vulcanizer, set the vulcanization temperature to 190°C, the vulcanizer pressure to 20MPa, and the initial vulcanization time to 15 minutes to ensure that the rubber fully fills the mold and avoids defects; after the initial vulcanization is completed, take out the mold from the flat vulcanizer, cool it to 90°C, and put the mold into a preheated oven for two-stage vulcanization; set the temperature in the oven to 190°C and the vulcanization time to 4 hours to ensure that the rubber is evenly heated under the flow of hot air; after the two-stage vulcanization is completed, take out the mold, wait for the mold to cool to 22°C, open the mold, and obtain the required mixed rubber.
[0032] Embodiment 3
[0033] Weigh 100 parts of acrylic rubber raw rubber and put it into a twin-screw internal mixer. Mix it at 100°C for 10 minutes to ensure that the rubber is evenly mixed and avoid material degradation caused by overheating. After the internal mixing is completed, add the following raw materials in sequence: 2 parts of stearic acid, 2 parts of antioxidant A, and 2 parts of antioxidant B. 2 parts, 80 parts of carbon black, 5 parts of release agent, 6 parts of plasticizer, continue to mix in the internal mixer at 100℃ for 10 minutes until all materials are evenly distributed; after the internal mixing is completed, the rubber material is discharged from the internal mixer in time to avoid degradation caused by long-term retention, and the rubber material is cooled to 25℃; the cooled rubber material is transferred to a two-roll open mill, the roller spacing is set to 4mm, and the open mill is started to stir at a speed of 80rpm / min to ensure that the rubber material is evenly dispersed on the roller, and the stirring time is 40 minutes; then the rubber material temperature is cooled to 100℃; the rubber material is put back into the open mill, 4 parts of accelerator and 3 parts of vulcanizer are added, and the rubber material is kept evenly stirred in the open mill for 5 minutes to ensure that the accelerator and vulcanizer are evenly distributed; after stirring evenly, set the open mill to perform 6 thin-pass operations; after the thin-pass operation is completed, Adjust the roller gap to 2mm, remove the rubber mix from the open mixer and place it on a flat workbench, and wait for the rubber to cool to 25℃; put the rubber mix into the configured mold and ensure that the mold is well closed to avoid leakage; put the mold into a flat vulcanizer, set the vulcanization temperature to 200℃, the vulcanizer pressure to 20MPa, and the initial vulcanization time to 20 minutes to ensure that the rubber fully fills the mold and avoids defects; after the initial vulcanization is completed, take out the mold from the flat vulcanizer, cool it to 100℃, and put the mold into a preheated oven for secondary vulcanization; set the temperature in the oven to 200℃ and the vulcanization time to 6 hours to ensure that the rubber is evenly heated under the flow of hot air; after the secondary vulcanization is completed, take out the mold, wait for the mold to cool to 25℃, open the mold, and obtain the required rubber mix.
[0034] Embodiment 4
[0035] 100 parts of double cross-linked heat-resistant acrylic rubber were selected as raw rubber and put into an internal mixer for 3 minutes; 2.0 parts of stearic acid, 1.0 parts of 445, 1.0 parts of 245, 60 parts of N550, 1.0 parts of microcrystalline wax, 2.0 parts of FG-200, and 3.0 parts of TP95 were added to the internal mixer and mixed for 5 minutes; the rubber was discharged after internal mixing and cooled to 60°C for 5 minutes; the rubber was put into an open mixer, and after mixing for 1 minute, 2.0 parts of diisopropylbenzene peroxide and 0.5 parts of NPC-50 were added and stirred evenly; then it was thinned and passed 4 times; rolled into sheets; the mixed rubber obtained above was subjected to a first-stage vulcanization on a flat vulcanizer at 180°C for 10 minutes, and then a second-stage vulcanization was carried out in an oven at 180°C for 4 hours, and tested after vulcanization.
[0036] Embodiment 5
[0037] 100 parts of epoxy cold-resistant acrylate rubber were selected as raw rubber and put into an internal mixer for 3 minutes; 1.5 parts of stearic acid, 1.0 parts of 630F, 1.0 parts of 618, 30 parts of N330, 30 parts of N660, 2.0 parts of microcrystalline wax, and 3.0 parts of TP759 were added to the internal mixer and mixed for 6 minutes; the rubber was discharged after internal mixing and cooled to 70°C for 5 minutes; the rubber was put into an open mixer, and 1.0 parts of ammonium benzoate was added after mixing for 1 minute, and stirred evenly; then it was thinned and passed 5 times; rolled into sheets; the mixed rubber obtained above was subjected to a first-stage vulcanization on a flat vulcanizer at 180°C for 10 minutes, and then a second-stage vulcanization was carried out in an oven at 180°C for 4 hours, and then tested after vulcanization.
[0038] Embodiment 6
[0039] 100 parts of active chlorine super cold-resistant acrylic rubber were selected as raw rubber and put into an internal mixer for 4 minutes; 2.0 parts of stearic acid, 1.0 parts of 2246, 1.0 parts of 565, 55 parts of N660, 1.0 parts of polyethylene wax, 2.0 parts of WB212, and 4.0 parts of RS107 were added to the internal mixer and mixed for 8 minutes; the rubber was discharged during internal mixing and cooled for 5 minutes; the rubber was put into an open mixer, mixed for 1 minute, cooled to less than 60°C, and then 0.3 parts of potassium stearate, 3.0 parts of sodium stearate, and 0.3 parts of insoluble sulfur were added and stirred evenly; then it was thinned and passed 5 times; rolled into sheets; the mixed rubber obtained above was subjected to a first-stage vulcanization on a flat vulcanizer at 180°C for 10 minutes, and then a second-stage vulcanization was carried out in an oven at 180°C for 4 hours, and tested after vulcanization.
[0040] Embodiment 7
[0041] 100 parts of carboxyl extremely cold-resistant acrylic rubber were selected as raw rubber and put into an internal mixer for 5 minutes; 1.0 part of stearic acid, 2.0 parts of GM, 50 parts of N550, 10 parts of N550, 0.5 parts of 18D, 1.0 part of microcrystalline wax, 2.0 parts of FG-200, and 5.0 parts of RS735 were added to the internal mixer and mixed for 10 minutes; the rubber was discharged after internal mixing and cooled for 5 minutes; the rubber was put into an open mixer and mixed for 2 minutes, cooled to less than 80°C, 2.0 parts of DOTG-75 and 0.6 parts of 1# vulcanizing agent were added, and stirred evenly; then it was thinned and passed 6 times; rolled into sheets; the mixed rubber obtained above was subjected to a first-stage vulcanization on a flat vulcanizer at 180°C for 10 minutes, and then a second-stage vulcanization was carried out in an oven at 180°C for 4 hours, and tested after vulcanization.
[0042] Embodiment 8
[0043] The antioxidants A and B in Examples 4, 5, 6 and 7 were all replaced by conventional antioxidant 445, and control samples 1-1, 2-1, 3-1 and 4-1 were obtained respectively; in order to obtain products with good aging resistance, this technical solution was developed, and samples 1-2, 2-2, 3-2 and 4-2 corresponded to the products of Examples 4, 5, 6 and 7 respectively. The analysis data are shown in the following table:
[0044] Table 1 Aging resistance test data
[0045]
[0046] Table 2 Aging resistance test data
[0047]
[0048] Table 3 Aging resistance test data
[0049]
[0050]
[0051] It can be seen from Table 1, Table 2 and Table 3 that, except for the epoxy type product, the aging performance of the four samples in the embodiment was poor before the invention, with the strength change rate exceeding 30% and the elongation change rate exceeding 40% at 190℃×72h. After the invention, the aging resistance was significantly improved, with the strength change rate at 190℃×72h not exceeding 20% and the elongation change rate below 30%, indicating that the technical solution can better improve the aging resistance.
[0052] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An aging-resistant acrylic rubber compound, characterized in that: The ageing-resistant acrylic rubber compound comprises, by weight, 100 parts of acrylic rubber, 0.5 to 2 parts of stearic acid, 0.5 to 2 parts of antioxidant A, 0.5 to 2 parts of antioxidant B, 40 to 80 parts of carbon black, 1 to 5 parts of release agent, 1 to 6 parts of plasticizer, 0.3 to 4 parts of accelerator and 0.3 to 3 parts of vulcanizer.
2. An ageing-resistant acrylic rubber compound as claimed in claim 1, characterized in that: The antioxidant A is one or more of antioxidant 445, antioxidant 405, antioxidant 630F, antioxidant 2246, antioxidant 4010NA, and antioxidant 4020.
3. The aging-resistant acrylic rubber compound according to claim 1, characterized in that: The antioxidant B is one or more of antioxidant 245, antioxidant 618, antioxidant 565, and antioxidant GM.
4. The aging-resistant acrylic rubber compound according to claim 1, characterized in that: The carbon black is one or more of carbon black N330, carbon black N550, carbon black N660, carbon black N774, and carbon black N990.
5. The aging-resistant acrylic rubber compound according to claim 1, characterized in that: The release agent is one or more of release agent 18D, microcrystalline wax, polyethylene wax, release agent WB212, and release agent FG-200.
6. The aging-resistant acrylic rubber compound according to claim 1, characterized in that: The plasticizer is one or more of plasticizer TP95, plasticizer TP759, plasticizer RS107, plasticizer RS700, and plasticizer RS735.
7. The aging-resistant acrylic rubber compound according to claim 1, characterized in that: The accelerator is one or more of accelerator DOTG, accelerator DOTG-75, accelerator XLA-60, accelerator ACT-70, accelerator ACT-55, sodium stearate, and potassium stearate.
8. The aging-resistant acrylic rubber compound according to claim 1, characterized in that: The vulcanizing agent is one or more of insoluble sulfur, thiocyanuric acid, N,N-dicinnamyl-1,-hexanediamine, ammonium benzoate, phthalic anhydride / imidazole, guanidine sulfur, hexamethylenediamine carbamate, isocyanuric acid / trimethyloctadecylammonium bromide, thiocyanuric acid / zinc dibutyldithiocarbamate, diisopropylbenzene peroxide, vulcanizing agent NPC-50, and vulcanizing agent NPC-100.
9. The method for preparing an ageing-resistant acrylic rubber compound according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: S1 Weigh 100-120 parts of acrylic rubber raw rubber into a twin-screw internal mixer and mix at 80-100°C for 5-10 minutes to ensure that the rubber is evenly mixed and avoid material degradation caused by excessive heating; After the S2 internal mixing is completed, the following raw materials are added in sequence: 0.5-2 parts of stearic acid, 0.5-2 parts of antioxidant A, 0.5-2 parts of antioxidant B, 40-80 parts of carbon black, 1-5 parts of release agent, 1-6 parts of plasticizer, and the internal mixing is continued at 80-100°C for 5-10 minutes until all materials are evenly distributed; after the internal mixing is completed, the rubber compound is discharged from the internal mixer in time to avoid degradation caused by long-term retention, and the rubber compound is cooled to 20-25°C; S3: Transfer the cooled rubber material to a two-roller mixing mill, set the roller distance to 2-4 mm, start the mixing mill and stir at a speed of 60-80 rpm / min to ensure that the rubber material is evenly dispersed on the rollers, and stir for 30-40 minutes; then cool the rubber material to 80-100°C; S4: Put the rubber material back into the open mill, add 0.3-4 parts of accelerator and 0.3-3 parts of vulcanizer, keep the rubber material evenly stirred in the open mill for 3-5 minutes to ensure that the accelerator and vulcanizer are evenly distributed; after stirring evenly, set the open mill to perform 4-6 thin-pass operations; S5 After the thin pass is completed, adjust the roller gap to 1-2 mm, remove the mixed rubber from the open mixer, and place it on a flat workbench to wait for the rubber to cool to 20-25°C; S6: Place the mixed rubber into the configured mold to ensure that the mold is well closed to avoid leakage; place the mold into a flat vulcanizer, set the vulcanization temperature to 170-200°C, the vulcanizer pressure to 20MPa, and the initial vulcanization time to 10-20 minutes to ensure that the rubber fully fills the mold to avoid defects; after the initial vulcanization is completed, take the mold out of the flat vulcanizer, cool it to 80-100°C, and place the mold in a preheated oven for secondary vulcanization; set the temperature in the oven to 170-200°C and the vulcanization time to 2-6 hours to ensure that the rubber is evenly heated under the flow of hot air; After the second stage vulcanization of S7 is completed, the mold is taken out and the mold is cooled to 20-25°C, then the mold is opened to obtain the required compound rubber.
Citation Information
Cited By
Wear-resistant sealing ring for discharging pipe of concrete pumping truck and preparation method of wear-resistant sealing ring
CN121271326A