Catalysts for the hydrogenation of carbon dioxide to methanol, their preparation methods and applications

By loading ultra-small palladium nanoclusters onto a lanthanum oxycarbonate support, the problem of low methanol selectivity in the CO2 hydrogenation to methanol process of noble metal Pd-based catalysts was solved, achieving efficient CO2 conversion and methanol production.

CN120169398BActive Publication Date: 2026-11-17LANZHOU UNIV +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510328673.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-03-19
Publication Date
2026-11-17
Estimated Expiration
2045-03-19

AI Technical Summary

Technical Problem

Existing noble metal Pd-based catalysts exhibit low methanol selectivity during CO2 hydrogenation to methanol production, readily generating byproducts such as methane and carbon monoxide, and are highly dependent on the support, making it difficult to effectively improve CO2 conversion and methanol selectivity.

Method used

Palladium with ultra-small nanoclusters was loaded onto a lanthanum oxycarbonate support. By controlling the size of the Pd clusters, the CO2 adsorption and activation capacity was enhanced, side reactions were suppressed, and methanol selectivity was improved.

Benefits of technology

The catalyst significantly improved CO2 conversion and methanol selectivity at low temperatures, achieved high methanol yield, and had a simple preparation method and short experimental cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005319622850000011
    Figure HDA0005319622850000011
  • Figure HDA0005319622850000012
    Figure HDA0005319622850000012
  • Figure HDA0005319622850000021
    Figure HDA0005319622850000021
Patent Text Reader

Abstract

This application relates to a catalyst for the hydrogenation of carbon dioxide to methanol, its preparation method, and its application. The catalyst provided in this application comprises a lanthanum oxycarbonate support and palladium metal supported on the support. The catalyst provided in this application exhibits high catalytic activity for the hydrogenation of carbon dioxide to methanol at low temperatures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of catalysis technology, and in particular relates to a catalyst for the hydrogenation of carbon dioxide to methanol, its preparation method and application. Background Technology

[0002] The widespread use of fossil fuels (coal, oil, and natural gas) has led to massive CO2 emissions, causing serious environmental problems such as global warming and ocean acidification. Therefore, reducing CO2 emissions and developing effective CO2 capture and utilization systems have become primary goals for solving environmental problems. Nobel laureate in Chemistry, George A. Olah, proposed the concept of a "methanol economy" in response to the global energy crisis, arguing that CO2 hydrogenation is one of the most promising renewable pathways for methanol production. Converting CO2 and green H2 into methanol (CO2 + 3H2 → CH3OH + H2O) is an efficient way to convert CO2 and store hydrogen, simultaneously addressing environmental issues and yielding the important basic chemical, methanol.

[0003] Currently, research on catalysts for CO2 hydrogenation to methanol mainly focuses on non-noble metal (Cu)-based catalysts, noble metal (Pd) catalysts, and bimetallic oxide catalysts. Noble metal Pd-based catalysts exhibit unique performance characteristics in the CO2 hydrogenation to methanol field. First, noble metal Pd-based catalysts are characterized by high efficiency at low temperatures and good resistance to poisoning. Pd nanoparticles show significant activation ability for H2 dissociation (H2→2H*), especially at low temperatures (<200℃), outperforming Cu-based catalysts and accelerating CO2 hydrogenation kinetics. Simultaneously, Pd has moderate adsorption capacity for intermediate products such as CO and is not easily deactivated by CO poisoning. Second, noble metal Pd-based catalysts have stable structures and exhibit anti-sintering and oxidation-resistant properties. Pd nanoparticles show strong anti-sintering ability in reducing atmospheres (maintaining high dispersion even at high temperatures), and Pd has a low oxidation tendency. Finally, noble metal Pd can synergistically interact with multifunctional supports. For example, when combined with reducible oxides (such as CeO2 and TiO2), Pd can induce oxygen vacancies (O2) on the support surface. V Pd-based catalysts promote CO2 adsorption and activation (CO2→CO2-). However, Pd-based catalysts exhibit low methanol selectivity. The Pd surface readily promotes deep hydrogenation of CO2 to produce methane (CH4) or carbon monoxide (CO), rather than methanol (CH3OH). Therefore, methanol selectivity needs to be improved through support additives or nanostructure modulation. Furthermore, Pd-based catalysts are significantly support-dependent. For example, while combining with a reducible support (such as ZrO2) can enhance the Pd-support interaction (SMSI), it may excessively inhibit H2 dissociation.

[0004] In the catalyst provided in this application, palladium metal is supported on a lanthanum oxycarbonate support in the form of ultrasmall nanoclusters. When the size of the Pd clusters approaches the Fermi wavelength (approximately 1 nm), their electronic energy levels change from a continuous state to a discrete state, causing a shift in the d-band center position, thereby altering the adsorption strength for reactant molecules (such as H2 and CO2). For example, Pd... 30 The d-band center of the cluster is shifted 0.3 eV higher than that of the bulk Pd, enhancing its adsorption and activation capacity for CO2. In the hydrogenation of CO2 to methanol, precise control of cluster size can suppress side reactions (such as the formation of methane and CO) and improve the selectivity and space-time yield of methanol. Summary of the Invention

[0005] To address the problems in the prior art, this application provides a catalyst for the hydrogenation of carbon dioxide to methanol, its preparation method, and its application.

[0006] In one aspect, this application provides a catalyst for the hydrogenation of carbon dioxide to methanol, comprising a lanthanum oxycarbonate (La2O2CO3) support and a palladium metal supported on the support.

[0007] In some embodiments, palladium is loaded onto the carrier in the form of ultrasmall nanoclusters.

[0008] In some embodiments, the palladium loading is 0.5%-12% based on the mass of the catalyst, for example, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 5.7%, 6%, 6.3%, 6.5%, 6.7%, 7%, 7.3%, 7.5%, 7.7%, 8%, 8.3%, 8.5%, 9%, 9.5%, 10%, 11%, or any value between them. In some embodiments, the palladium loading is 1%-10%. In some embodiments, the palladium loading is 2%-8%.

[0009] In some implementations, the diameter of the ultrasmall nanoclusters is less than or equal to 2 nm, for example, 0.5 nm, 1 nm, 1.3 nm, 1.5 nm or 1.7 nm.

[0010] In some embodiments, the lanthanum oxycarbonate support is selected from nanorod-shaped lanthanum oxycarbonate supports. Compared to other morphologies, nanorod-shaped lanthanum oxycarbonate supports can provide abundant oxygen vacancies, which is beneficial for CO2 adsorption and activation.

[0011] In some embodiments, the length of the nanorod is less than or equal to 50 nm, for example, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, or any value between them. In some embodiments, the length of the nanorod is 30 nm to 40 nm.

[0012] In some embodiments, the diameter of the nanorods is 5 nm to 15 nm, for example, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, or any value between them. In some embodiments, the diameter of the nanorods is 5 nm to 12 nm. In some embodiments, the diameter of the nanorods is 8 nm to 10 nm.

[0013] Secondly, this application provides a method for preparing a catalyst for the hydrogenation of carbon dioxide to methanol, comprising the following steps:

[0014] S1: The first mixture containing lanthanum source is mixed with an alkaline solution to obtain a mixture containing lanthanum hydroxide;

[0015] S2: The mixture from step S1 is subjected to a hydrothermal reaction, and the hydrothermal reaction product is subjected to a first calcination to obtain lanthanum carbonate support.

[0016] S3: The second mixture containing the lanthanum oxycarbonate support from step S2 is mixed with the third mixture containing the palladium source to obtain the fourth mixture;

[0017] S4: The fourth mixture is subjected to a precipitation reaction, and the precipitated product is calcined a second time and reduced to obtain the catalyst.

[0018] This application presents a two-step synthesis of a catalyst (Pd / La2O2CO3) for the hydrogenation of carbon dioxide to methanol. The preparation method is simple and has a short experimental cycle. Furthermore, the prepared catalyst exhibits a high methanol yield.

[0019] In some embodiments, the mass of the palladium source is 0.5%-15% of the mass of the lanthanum oxycarbonate support, for example, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 5.7%, 6%, 6.3%, 6.5%, 6.7%, 7%, 7.3%, 7.5%, 7.7%, 8%, 8.3%, 8.5%, 8.7%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 13%, 14%, or any value between them. In some embodiments, the mass of the palladium source is 2%-12% of the mass of the lanthanum oxycarbonate support. In some embodiments, the mass of the palladium source is 6%-10% of the mass of the lanthanum oxycarbonate support.

[0020] In some embodiments, in step S1, the first mixture containing the lanthanum source is selected from an aqueous solution of the lanthanum source.

[0021] In some embodiments, in step S1, the lanthanum source is selected from one or more of lanthanum nitrate, lanthanum chloride, lanthanum sulfate, and lanthanum acetate.

[0022] In some embodiments, in step S1, the alkaline solution is selected from one or more of potassium hydroxide solution, sodium hydroxide solution, ammonia solution, and urea solution.

[0023] In some embodiments, the temperature of the hydrothermal reaction in step S2 is 150℃-250℃, for example, 160℃, 170℃, 180℃, 190℃, 200℃, 210℃, 220℃, 230℃, or 240℃. In some embodiments, the temperature of the hydrothermal reaction is 180℃-200℃.

[0024] In some embodiments, the hydrothermal reaction time in step S2 is 5h-30h, for example, 8h, 10h, 12h, 15h, 18h, 20h, 24h, or 28h. In some embodiments, the hydrothermal reaction time is 10h-20h.

[0025] In some embodiments, the temperature of the first firing in step S2 is 400℃-700℃, for example, 450℃, 500℃, 550℃, 600℃ or 650℃. In some embodiments, the temperature of the first firing is 500℃-600℃.

[0026] In some embodiments, in step S2, the hydrothermal reaction product is washed and dried before being calcined for the first time.

[0027] In some embodiments, in step S3, the second mixture is selected from an aqueous solution containing a lanthanum oxycarbonate support.

[0028] In some embodiments, in step S3, the third mixture containing the palladium source is selected from an aqueous solution of the palladium source.

[0029] In some embodiments, in step S3, the palladium source is selected from one or more of palladium nitrate, palladium chloride, palladium acetate, and sodium tetrachloropalladium.

[0030] In some embodiments, in step S4, an alkaline source is used to adjust the pH of the fourth mixture to 8-9, causing a precipitation reaction in the fourth mixture. In some embodiments, the alkaline solution is selected from potassium hydroxide solution and / or sodium hydroxide solution.

[0031] In some embodiments, in step S4, the temperature of the second firing is 350°C-600°C, for example, 400°C, 450°C, 500°C, or 550°C. In some embodiments, the temperature of the second firing is 400°C-500°C.

[0032] In some embodiments, in step S4, the precipitated reaction product is washed and dried before being calcined a second time.

[0033] In some implementations, in step S4, the reduction temperature is 250°C-350°C, for example, 270°C, 300°C or 330°C.

[0034] In some implementations, in step S4, the reduction is carried out in a hydrogen atmosphere.

[0035] In some embodiments, the preparation method includes the following specific steps:

[0036] (1) Preparation of La2O2CO3:

[0037] Lanthanum nitrate hexahydrate (La(NO3)3·6H2O, 0.9855 g) was dissolved in 40 mL of deionized water and magnetically stirred for 10 min. Then, freshly prepared KOH solution (KOH, 10%, 20 mL) was added dropwise to a beaker using a pipette until the mixture turned milky white, forming La(OH)3. The mixture was stirred for 2 h, then transferred to a 100 mL hydrothermal reactor and hydrothermated at 180 °C for 12 h. The hydrothermated solution was filtered and washed with deionized water until neutral, then dried overnight at 80 °C. The dried solid was calcined at 550 °C for 2 h (with air circulation) to form rod-shaped La2O2CO3.

[0038] (2) Preparation of Pd / La2O2CO3:

[0039] 0.5 g of rod-shaped La₂O₂CO₃ was dispersed in 120 mL of deionized water and sonicated for 30 min. A measured amount of Pd(NO₃)₂·2H₂O was added to the above solution, and the mixture was magnetically stirred for 2 h. Subsequently, freshly prepared NaOH solution (0.1 M) was added dropwise to the mixed solution, and the solution was allowed to settle at pH 8-9 at room temperature for 2 h. The precipitated solution was filtered and washed with deionized water until neutral, and then dried overnight at 110 °C. The dried solid was calcined at 450 °C for 4 h (with air circulation) to obtain the Pd / La₂O₂CO₃ catalyst.

[0040] Thirdly, this application provides the application of the catalyst described in the first aspect or the catalyst prepared by the preparation method described in the second aspect in the hydrogenation of carbon dioxide to methanol.

[0041] Fourthly, this application provides a method for producing methanol by hydrogenation of carbon dioxide, comprising reacting carbon dioxide and hydrogen in the presence of the catalyst described in the first aspect or the catalyst prepared by the preparation method described in the second aspect.

[0042] In some embodiments, the reaction temperature is 200°C-350°C, for example, 220°C, 240°C, 260°C, 280°C, 300°C, 320°C, or 340°C. In some embodiments, the reaction temperature is 280°C-300°C.

[0043] In some embodiments, the reaction pressure is 2 MPa-5 MPa, for example 2.5 MPa, 3 MPa, 3.5 MPa, 4 MPa, or 4.5 MPa. In some embodiments, the reaction pressure is 2.5 MPa-3.5 MPa.

[0044] In some embodiments, the space velocity of the reaction is 8000 mL g. cat -1 h -1 -36000mL g cat -1 h -1 For example, 10000mL g cat -1 h -1 15000mLg cat -1 h -1 20000mL g cat -1 h -1 25000mL g cat -1 h -1 30000mLg cat -1 h -1 Or 35000mL g cat -1 h -1 In some embodiments, the space velocity of the reaction is 18000 mL g. cat -1 h -1 -30000mL g cat - 1 h -1 .

[0045] Compared with the prior art, the beneficial effects of this application are as follows:

[0046] 1. In the synthesized Pd / La2O2CO3 catalyst, Pd is supported on La2O2CO3 in the form of nanoclusters.

[0047] 2. The Pd / La2O2CO3 catalyst preparation method in this application is simple, has a short experimental cycle, and achieves a high methanol yield, with a space-time yield of 0.36 g of methanol at 290℃. CH3OH g cat -1 h -1 .

[0048] 3. The synthesized Pd / La2O2CO3 catalyst can effectively catalyze CO2 conversion. Experimental results show that the CO2 conversion rate reaches 15.7% at 290℃. Attached Figure Description

[0049] Figure 1 The XRD patterns of the samples prepared in Comparative Example 1 and Examples 1-4 are shown.

[0050] Figure 2 Transmission electron microscope (TEM) images, high-resolution TEM images, high-angle annular dark-field scanning TEM images, and elemental distribution maps of the 8wt% Pd / La2O2CO3 sample prepared in Example 3.

[0051] Figure 3 High-angle annular dark-field scanning transmission electron microscope image of the 8wt% Pd / La2O2CO3 sample prepared in Example 3.

[0052] Figure 4 The figures show the performance test results of the samples prepared in Comparative Example 1 and Examples 1-4, where Figure (a) shows the methanol selectivity, Figure (b) shows the CO2 conversion rate, and Figure (c) shows the space-time yield of methanol. Detailed Implementation

[0053] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with embodiments and accompanying drawings. The specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, descriptions of well-known structures and technologies are omitted in the following description to avoid unnecessarily obscuring the concepts of this disclosure. Such structures and technologies have also been described in numerous publications.

[0054] The present application will be further described below through specific embodiments.

[0055] Unless otherwise specified, all reagents used in the following examples and comparative examples were obtained commercially.

[0056] Unless otherwise specified, the pressures mentioned in the following examples and comparative examples are gauge pressures.

[0057] Comparative Example 1

[0058] Lanthanum nitrate hexahydrate (La(NO3)3·6H2O, 0.9855 g) was dissolved in 40 mL of deionized water and magnetically stirred for 10 min. Then, freshly prepared KOH solution (KOH, 10%, 20 mL) was added dropwise to a beaker using a pipette until the mixture turned milky white, forming La(OH)3. The mixture was stirred for 2 h, and then transferred to a 100 mL hydrothermal reactor and hydrothermated at 180 °C for 12 h. The hydrothermated solution was filtered and washed with deionized water until neutral, then dried overnight at 80 °C. The dried solid was calcined at 550 °C for 2 h (with air) to form rod-shaped La2O2CO3. The resulting sample was designated as 0 wt% Pd / La2O2CO3 (0 wt% Pd / LOC).

[0059] Example 1

[0060] (1) Preparation of rod-shaped La2O2CO3

[0061] Lanthanum nitrate hexahydrate (La(NO3)3·6H2O, 0.9855 g) was dissolved in 40 mL of deionized water and magnetically stirred for 10 min. Freshly prepared KOH solution (KOH, 10%, 20 mL) was then added dropwise to a beaker using a pipette until the mixture turned milky white, forming La(OH)3. The mixture was stirred for 2 h, then transferred to a 100 mL hydrothermal reactor and hydrothermated at 180 °C for 12 h. The hydrothermated solution was filtered and washed with deionized water until neutral, then dried overnight at 80 °C. The dried solid was calcined at 550 °C for 2 h (with air circulation) to form rod-shaped La2O2CO3.

[0062] (2) Preparation of 2wt% Pd / La2O2CO3 catalyst

[0063] The rod-shaped La₂O₂CO₃ (0.5 g) prepared in step (1) was dissolved in 120 mL of deionized water and sonicated for 30 min. 0.025 g of Pd(NO₃)₂·2H₂O was added to the above solution and magnetically stirred for 2 h. Then, freshly prepared NaOH solution (0.1 M) was added dropwise to the mixed solution. The solution was allowed to settle at pH 8-9 at room temperature for 2 h. The precipitated solution was filtered and washed with deionized water until neutral, then dried overnight at 110 °C. The dried solid was calcined at 450 °C for 4 h (with air), followed by reduction at 300 °C for 1 h under a hydrogen atmosphere. The resulting sample was denoted as 2 wt% Pd / La₂O₂CO₃ (2 wt% Pd / LOC).

[0064] Example 2

[0065] The only difference from Example 1 is that the mass of Pd(NO3)2·2H2O added in step (2) is 0.05g, and the resulting sample is recorded as 4wt%Pd / La2O2CO3 (4wt%Pd / LOC).

[0066] Example 3

[0067] The only difference from Example 1 is that the mass of Pd(NO3)2·2H2O added in step (2) is 0.1002 g, and the resulting sample is recorded as 8wt%Pd / La2O2CO3 (8wt%Pd / LOC).

[0068] Example 4

[0069] The only difference from Example 1 is that the mass of Pd(NO3)2·2H2O added in step (2) is 0.1502 g, and the resulting sample is recorded as 12wt%Pd / La2O2CO3 (12wt%Pd / LOC).

[0070] Structural characterization

[0071] Figure 1 The XRD patterns of samples prepared in Comparative Example 1 and Examples 1-4 (0 wt% Pd / La₂O₂CO₃, 2 wt% Pd / La₂O₂CO₃, 4 wt% Pd / La₂O₂CO₃, 8 wt% Pd / La₂O₂CO₃, and 12 wt% Pd / La₂O₂CO₃) are shown. The XRD patterns of 0 wt% Pd / La₂O₂CO₃, 2 wt% Pd / La₂O₂CO₃, 4 wt% Pd / La₂O₂CO₃, 8 wt% Pd / La₂O₂CO₃, and 12 wt% Pd / La₂O₂CO₃ show diffraction peaks of hexagonal La₂O₂CO₃, indicating the successful synthesis of the hexagonal La₂O₂CO₃ support, and that Pd loading did not alter the crystal form of the hexagonal La₂O₂CO₃ support.

[0072] Figure 2 Transmission electron microscope (TEM) images, high-resolution TEM images, high-angle annular dark-field scanning TEM images, and elemental distribution maps of the 8 wt% Pd / La₂O₂CO₃ sample prepared in Example 3 are provided. Figure 2 (a) Transmission electron microscopy images show a clear microstructure; the 8wt% Pd / La2O2CO3 sample maintains a nanorod-like structure with nanorods less than 50 nm in length (approximately 20-50 nm) and diameters of 5-12 nm. Figure 2 (b) The high-resolution transmission image shows the lattice fringes of La2O2CO3, where the characteristic lattice distance is 0.35 nm, which matches the (100) crystal plane of hexagonal La2O2CO3. Figure 2 (c) The high-angle annular dark-field scanning transmission electron microscope image and the corresponding elemental distribution map show that Pd is uniformly dispersed on the surface of the support La2O2CO3.

[0073] The presence of Pd atoms in the 8wt% Pd / La2O2CO3 sample prepared in Example 3 was further investigated using aberration-corrected transmission electron microscopy. Figure 3 As shown. Atomic-level high-angle annular dark-field scanning transmission electron microscopy revealed that Pd atoms were loaded onto the La2O2CO3 surface in the form of clusters smaller than 2 nm. Figure 3 (Highlights).

[0074] The actual Pd loading (ICP data) of the samples obtained from Comparative Example 1 and Examples 1-4 are shown in Table 1.

[0075] Table 1

[0076] sample Comparative Example 1 Example 1 Example 2 Example 3 Example 4 Pd(wt%) 0% 1.54% 2.78% 6.62% 8.47%

[0077] Thermal catalytic effect test

[0078] The thermocatalytic performance of the Pd / La2O2CO3 catalysts prepared in Comparative Example 1 and Examples 1-4 was tested using the following methods:

[0079] Performance testing of CO2 hydrogenation to CH3OH was conducted in a Ward fixed-bed flow microreactor, and product distribution was detected using a Fuli 9790Ⅱ online gas chromatograph.

[0080] The above catalyst was compressed into tablets, granulated, and sieved to obtain catalyst particles of 40-65 mesh (230-400 μm). 0.3 g of the catalyst was mixed evenly with 0.7 g of quartz of the same particle size and packed into the isothermal zone (id = 6 mm) of the quartz tube in a fixed-bed reactor for catalytic performance testing. H2 and CO2 were used as feed gases, and Ar was used as the equilibrium gas. The reaction conditions were: P = 3 MPa, T = 240-320℃, V(H2) / V(CO2) / V(Ar) = 72 / 24 / 4, and space velocity was 24000 mL g. cat -1 h -1 The catalyst was at 300℃, with H2 (40 ml / min) –1 The system was pretreated at atmospheric pressure for 1 hour, then cooled to the reaction temperature and pressurized. The proportion of reactant gases was adjusted using a mass flow meter, and the system pressure was controlled to 3 MPa using a back pressure valve.

[0081] The main products after the reaction were CH3OH, CH4, and CO. CO, Ar, and unreacted CO2 were separated and quantitatively analyzed using a thermal conductivity detector (TCD) packed column (Lanzhou Donglilong Information Technology Co., Ltd., TDX-01, 2m × 3mm). Methanol, methane, and alkanes were analyzed using a flame ionization detector (FID) capillary column (Agilent HP-Plot Q, 30m × 0.53mm × 40μm). Methane (CH4) served as a bridge between FID and TCD for quantitative analysis. The temperature between the reactor and the gas phase was maintained at 130℃ to prevent product condensation.

[0082] At each reaction temperature, at least five stable data points were collected and averaged to calculate the CO2 conversion rate and product selectivity during the catalytic process. The carbon balance was 100 ± 3%. At each temperature, the reaction time was maintained for at least 3 hours, and the last five sets of stable gas-phase data for the products were collected.

[0083] The test results of the samples prepared in Comparative Example 1 and Examples 1-4 are as follows: Figure 4 As shown. Figure 4 (a) The results show that the methanol selectivity of the 8wt% Pd / La2O2CO3 sample is optimal. Figure 4 (b) The results show that the CO2 conversion rate was significantly improved after loading with Pd, and the CO2 conversion rate of the 8wt% Pd / La2O2CO3 sample was greater than 15% at 290℃. Figure 4 (c) The results showed that the space-time yield of methanol in the 8wt% Pd / La2O2CO3 sample reached 0.36 g at 290 °C. CH3OH g cat -1 h -1 .

[0084] The results of methanol selectivity, CO2 conversion and methanol space-time yield in the thermocatalytic effect test of the samples prepared in Comparative Example 1 and Examples 1-4 at 290°C are shown in Table 2.

[0085] Table 2

[0086] sample <![CDATA[CO2 conversion rate]]> Methanol selectivity Methanol space-time yield Comparative Example 1 0% 0% 0 Example 1 10.38% 24.98% <![CDATA[0.21g CH3OH g cat -1 h -1 ]]> Example 2 13.31% 27.34% <![CDATA[0.30g CH3OH g cat -1 h -1 ]]> Example 3 15.76% 27.61% <![CDATA[0.36g CH3OH g cat -1 h -1 ]]> Example 4 14.72% 22.60% <![CDATA[0.27g CH3OH g cat -1 h -1 ]]>

[0087] The above results indicate that the Pd / La2O2CO3 catalyst provided in this application has high catalytic activity for the hydrogenation of CO2 to methanol at low temperatures.

[0088] The preferred embodiments of this application have been described in detail above; however, this application is not limited thereto. Within the scope of the technical concept of this application, various simple modifications can be made to the technical solution of this application, including combining various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in this application and are all within the protection scope of this application.

Claims

1. The application of a catalyst for the hydrogenation of carbon dioxide to methanol, the catalyst comprising a lanthanum oxycarbonate support and a palladium metal supported on the support; Palladium is loaded onto the support in the form of ultrasmall nanoclusters, the diameter of which is less than or equal to 2 nm; the loading of palladium is 1%-12% based on the mass of the catalyst. The lanthanum oxycarbonate support is selected from nanorod-shaped lanthanum oxycarbonate supports, the length of the nanorods is less than or equal to 50 nm, the diameter of the nanorods is 5 nm-15 nm, and the lanthanum oxycarbonate support has a hexagonal lanthanum oxycarbonate (100) crystal plane. in, The temperature for the hydrogenation of carbon dioxide to methanol is 200℃-350℃, and the space velocity is... .

2. The application according to claim 1, characterized in that, The loading of palladium metal is 1%-10% based on the mass of the catalyst.

3. The application according to claim 1, characterized in that, The loading of palladium metal is 2%-8% based on the mass of the catalyst.

4. The application according to claim 1, characterized in that, The nanorods are 30nm-40nm long and 8nm-10nm in diameter.

5. The application according to any one of claims 1-4, characterized in that, The method for preparing the catalyst includes the following steps: S1: The first mixture containing lanthanum source is mixed with an alkaline solution to obtain a mixture containing lanthanum hydroxide; S2: The mixture from step S1 is subjected to a hydrothermal reaction, and the hydrothermal reaction product is subjected to a first calcination to obtain lanthanum carbonate support. S3: The second mixture containing the lanthanum oxycarbonate support from step S2 is mixed with the third mixture containing the palladium source to obtain the fourth mixture; S4: The fourth mixture is subjected to a precipitation reaction, and the precipitated product is calcined a second time and reduced to obtain the catalyst.

6. The application according to claim 5, characterized in that, The mass of the palladium source is 0.5%-15% of the mass of the lanthanum oxycarbonate support, based on the mass of palladium.

7. The application according to claim 5, characterized in that, The mass of the palladium source is 2%-12% of the mass of the lanthanum oxycarbonate support, based on the mass of the palladium.

8. The application according to claim 5, characterized in that, The mass of the palladium source is 6%-10% of the mass of the lanthanum oxycarbonate support, based on the mass of the palladium.

9. The application according to claim 5, characterized in that, In step S1, the first mixture containing the lanthanum source is selected from an aqueous solution of the lanthanum source; and / or The lanthanum source is selected from one or more of lanthanum nitrate, lanthanum chloride, lanthanum sulfate, and lanthanum acetate; and / or The alkaline solution is selected from one or more of potassium hydroxide solution, sodium hydroxide solution, ammonia water, and urea solution.

10. The application according to claim 5, characterized in that, In step S2, the temperature of the hydrothermal reaction is 150℃-250℃; and / or The hydrothermal reaction time is 5h-30h; and / or The temperature of the first roasting is 400℃-700℃; and / or After washing and drying the hydrothermal reaction products, a first calcination is performed.

11. The application according to claim 10, characterized in that, In step S2, the temperature of the hydrothermal reaction is 180℃-200℃; and / or The hydrothermal reaction time is 10-20 hours; and / or The temperature of the first roasting is 500℃-600℃.

12. The application according to claim 5, characterized in that, In step S3, the second mixture is selected from an aqueous solution containing a lanthanum oxycarbonate support; and / or The third mixture containing the palladium source is selected from an aqueous solution of the palladium source; and / or The palladium source is selected from one or more of palladium nitrate, palladium chloride, palladium acetate, and sodium tetrachloropalladium; and / or In step S4, the pH of the fourth mixture is adjusted to 8-9 using an alkali source to induce a precipitation reaction; and / or The temperature of the second roasting is 350℃-600℃; and / or After washing and drying the precipitated product, it is then calcined a second time. and / or The reduction temperature is 250℃-350℃.

13. The application according to claim 12, characterized in that, The alkali source is selected from potassium hydroxide solution and / or sodium hydroxide solution; and / or The temperature for the second roasting is 350℃-600℃.

14. A method for producing methanol by hydrogenation of carbon dioxide, comprising reacting carbon dioxide and hydrogen in the presence of a catalyst, said catalyst being the catalyst defined in any one of claims 1-13; The reaction temperature is 200℃-350℃; The reaction pressure is 2MPa-5MPa; The space velocity of the reaction is .

15. The method according to claim 14, characterized in that, The reaction temperature is 280℃-300℃; The reaction pressure is 2.5 MPa-3.5 MPa; The space velocity of the reaction is .

Citation Information

Patent Citations

  • A palladium / carbon nanotube catalyst, a preparing method thereof and applications of the catalyst

    CN105727942A

  • Preparation method and application of La2O2CO3 nano triangular plate loaded Pd catalyst

    CN109999871A